A high-crystallinity, micro-crosslinked, ultra-high molecular weight polyethylene resin and its preparation method

By introducing the amidation reaction of maleic anhydride-grafted polyethylene and m-phenylenediamine and the synergistic crosslinking of long-chain non-conjugated α,ω-dienes into the ultra-high molecular weight polyethylene matrix, the problems of thermo-oxidative stability and mechanical properties of ultra-high molecular weight polyethylene materials were solved, and a balance between high crystallinity and excellent mechanical strength was achieved.

CN123107219APending Publication Date: 2026-11-17WEIFANG JUPU NEW MATERIAL TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611613438.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing ultra-high molecular weight polyethylene materials exhibit poor long-term thermo-oxidative stability and impaired mechanical properties after irradiation, and uneven irradiation dose distribution leads to poor performance consistency.

Method used

By introducing maleic anhydride-grafted polyethylene and m-phenylenediamine into the ultra-high molecular weight polyethylene matrix through an amidation reaction, a sparse covalent cross-linked network is formed. Combined with the synergistic cross-linking of long-chain non-conjugated α,ω-diene and 1,3-bis(tert-butylperoxyisopropyl)benzene, the crystal structure and mechanical properties are optimized.

Benefits of technology

While maintaining high crystallinity, the rigidity, heat resistance and processing performance of the material are improved, and the restriction of molecular chain segment movement by the cross-linked structure is reduced, so as to achieve a balance between high crystallinity and excellent mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application relates to the field of polymer materials technology, specifically disclosing a high-crystallinity, micro-crosslinked ultra-high molecular weight polyethylene (UHMWPE) resin and its preparation method. The high-crystallinity, micro-crosslinked UHMWPE resin is made from the following raw materials in parts by weight: 100 parts UHMWPE, 10-20 parts linear low-density polyethylene, 15-25 parts high-density polyethylene, 5-10 parts low-density polyethylene, 10-20 parts maleic anhydride-grafted polyethylene, 0.08-0.15 parts m-phenylenediamine, 2-5 parts filler, 0.5-1.5 parts long-chain non-conjugated α,ω-diene, 0.4-0.8 parts antioxidant, 0.5-1 part lubricant, and 0.5-1 part light stabilizer. The resin obtained by this application has the advantages of high crystallinity and a balance of rigidity and toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of polymer materials technology, and more specifically, it relates to a special resin for highly crystalline micro-crosslinked ultra-high molecular weight polyethylene and its preparation method. Background Technology

[0002] Ultra-high molecular weight polyethylene (UHMWPE) possesses excellent wear resistance, self-lubrication, impact resistance, and chemical corrosion resistance, and is widely used in medical artificial joints, lithium battery separators, wear-resistant liners, and high-strength fibers. However, due to its extremely long and tightly entangled molecular chains, its melt viscosity is extremely high, making it difficult to mold using conventional thermoplastic processing methods. Furthermore, the material exhibits defects such as low surface hardness, poor heat creep resistance, and susceptibility to environmental stress cracking, limiting its application under high load and high temperature conditions.

[0003] To improve the above properties, especially to enhance its morphological stability, creep resistance, and fatigue resistance, crosslinking modification technology is typically employed. Patent application CN119661915A discloses a method for preparing an ultra-high molecular weight polyethylene (UHMWPE) composition, comprising the following steps: 1) uniformly mixing UHMWPE resin, a hindered amine stabilizer, and a portion of an antioxidant to obtain a premixed composition; 2) irradiating the premixed composition with a high-energy electron beam of 15-50 kGy or a cobalt source, then adding the remaining antioxidant and peroxide to obtain the UHMWPE composition; based on 100 parts by weight of the UHMWPE resin, the hindered amine stabilizer comprises 0.01-0.05 parts by weight, the antioxidant comprises 0.4-0.8 parts by weight, and the peroxide comprises 0.03-0.2 parts by weight.

[0004] In this technical solution, irradiation pretreatment generates some active sites to reduce the amount of peroxide added subsequently, thereby improving crosslinking efficiency and mitigating the oxidative degradation problem caused by excessive peroxide to some extent. However, the free radicals remaining after irradiation will continue to cause oxidative degradation during long-term use of the material, leading to significant loss of crystallinity, which in turn causes a decrease in molecular weight and mechanical properties. Furthermore, the uneven distribution of irradiation dose in thick products can easily cause large differences in the degree of crosslinking between the surface and the interior, resulting in poor product performance consistency. Summary of the Invention

[0005] In order to overcome the problems of poor long-term thermo-oxidative stability and impaired mechanical properties after irradiation in the prior art, this application provides a special resin for highly crystalline micro-crosslinked ultra-high molecular weight polyethylene and its preparation method.

[0006] A special resin for highly crystalline micro-crosslinked ultra-high molecular weight polyethylene is made from the following raw materials in parts by weight: The composition includes 100 parts ultra-high molecular weight polyethylene, 10-20 parts linear low-density polyethylene, 15-25 parts high-density polyethylene, 5-10 parts low-density polyethylene, 10-20 parts maleic anhydride-grafted polyethylene, 0.08-0.15 parts m-phenylenediamine, 2-5 parts filler, 0.5-1.5 parts long-chain non-conjugated α,ω-diene, 0.4-0.8 parts antioxidant, 0.5-1 part lubricant, and 0.5-1 part light stabilizer.

[0007] By adopting the above technical solution, during subsequent processing, the primary amino group of m-phenylenediamine undergoes an amidation reaction with the maleic anhydride-grafted polyethylene side chain anhydride. Some of the product is dehydrated by heating to generate an imide structure, forming chemical cross-linking sites inside the polyethylene matrix. Maleic anhydride-grafted polyethylene is compatible with various polyethylene matrices in the system and co-crystallizes, so that the cross-linking sites are uniformly dispersed. Long-chain non-conjugated α,ω-dienes can undergo a small amount of grafting under thermal shearing, achieving a balance between the mechanical properties and crystallinity of the material without significantly sacrificing crystallinity.

[0008] Preferably, the long-chain non-conjugated α,ω-diene is 1,9-decadiene.

[0009] Preferably, the high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin further includes 0.03~0.07 parts by weight of 1,3-bis(tert-butylperoxyisopropyl)benzene.

[0010] By adopting the above technical solution, a trace amount of 1,3-bis(tert-butylperoxyisopropyl)benzene is introduced as an auxiliary initiator, which works synergistically with amidation crosslinking to improve the grafting efficiency of long-chain non-conjugated α,ω-dienes and form a micro-crosslinked network that combines rigidity and flexibility.

[0011] Preferably, the viscosity-average molecular weight of the ultra-high molecular weight polyethylene is 3 million to 6 million.

[0012] Preferably, the filler is two of the following: nano-montmorillonite, nano-silica, ultrafine wollastonite, and silicon carbide micro powder.

[0013] Preferably, the filler undergoes the following pretreatment steps before use: S1: Prepare a 3%~5% (w / w) aqueous solution of silane coupling agent in ethanol, adjust the pH to 4.0~5.0, and hydrolyze for 40~60 min to obtain a pre-hydrolyzed solution; S2: Mix the packing material and the pre-hydrolyzed solution, heat to 50~70℃, react for 2~4 hours, separate the solid and liquid, wash, and dry to obtain the pretreated packing material.

[0014] By adopting the above technical solution, the silane coupling agent is hydrolyzed and grafted onto the surface of the filler, introducing organic hydrophobic segments to improve the interfacial compatibility between the filler and the non-polar polyethylene matrix; the modified filler helps to optimize the crystal structure, refine the grains, and maintain the crystallization level of the system.

[0015] Preferably, the silane coupling agent is silane coupling agent KH-550 or silane coupling agent KH-570.

[0016] Preferably, the antioxidant includes antioxidant 1010 and antioxidant 168.

[0017] Preferably, the lubricant is calcium stearate or polyethylene wax.

[0018] Preferably, the light stabilizer is light stabilizer 944.

[0019] Preferably, the high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin further includes 0.2 to 0.4 parts by weight of alicyclic non-conjugated diene.

[0020] Preferably, the alicyclic non-conjugated diene is dicyclopentadiene.

[0021] By adopting the above technical solution, dicyclopentadiene can participate in free radical graft crosslinking under the condition of containing 1,3-bis(tert-butylperoxyisopropyl)benzene, and a small number of rigid alicyclic crosslinking nodes are introduced into the flexible long-chain crosslinking network to moderately improve the rigidity of the crosslinking network and the high-temperature structural stability.

[0022] Preferably, the high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin further includes 3-5 parts by weight of ethylene-octene copolymer elastomer.

[0023] By adopting the above technical solution, the ethylene-octene copolymer elastomer has good compatibility with the polyolefin matrix and can be uniformly dispersed in the amorphous region of the matrix. It absorbs impact energy through chain segment slippage and deformation, compensating for the toughness loss of the micro-crosslinked system.

[0024] Preferably, the high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin further includes 0.8 to 1.2 parts by weight of 2-butyl-1-octene.

[0025] By adopting the above technical solution, single-terminal α-olefins can participate in the free radical reaction of the system, moderately consume excess macromolecular free radicals, and regulate the crosslinking density of the system.

[0026] This application also provides a method for preparing a special resin for highly crystalline micro-crosslinked ultra-high molecular weight polyethylene, comprising the following steps: Ultra-high molecular weight polyethylene, linear low-density polyethylene, high-density polyethylene, low-density polyethylene, maleic anhydride-grafted polyethylene, m-phenylenediamine, filler, long-chain non-conjugated α,ω-diene, optional 1,3-bis(tert-butylperoxyisopropyl)benzene, optional alicyclic non-conjugated diene, optional ethylene-octene copolymer elastomer, and optional 2-butyl-1-octene are mixed and heated to 140~160℃ and kneaded for 8~12 min. The temperature is then raised to 180~200℃ and kneaded for 12~15 min. The temperature is lowered to 145~150℃, antioxidants, lubricants, and light stabilizers are added, and the mixture is kneaded for 3~5 min. The mixture is then extruded, cooled, granulated, and dried to obtain a high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin.

[0027] By adopting the above technical solution, the low-melting-point component melts first in the low-temperature stage to form a continuous liquid phase, which encapsulates the ultra-high molecular weight polyethylene particles to achieve plasticization and dispersion. During this stage, the reaction rate between m-phenylenediamine and the anhydride is low, and the degree of crosslinking is limited. In the high-temperature mixing stage, the primary amine groups of m-phenylenediamine undergo ring-opening amidation with the anhydride groups of maleic anhydride-grafted polyethylene, and partially cyclize into an imide structure, forming a sparse micro-crosslinked network between polyethylene chains, bridged by amide / imide bonds. Because the polyethylene backbone of maleic anhydride-grafted polyethylene has a similar structure to the polyethylene components in the matrix, the material maintains a high level of crystallinity even at low crosslinking density. Simultaneously, long-chain non-conjugated α,ω-dienes are introduced as auxiliary modifying components, which can effectively enhance melt strength and improve processing rheological behavior through micro-crosslinking or the formation of long-chain branched structures.

[0028] More preferably, the following pretreatment steps are performed before adding the filler, long-chain non-conjugated α,ω-diene, and m-phenylenediamine: Under an inert atmosphere, the packing material, long-chain non-conjugated α,ω-diene, and m-phenylenediamine are added to the reactor and mixed at 40-60°C for 1-3 hours, then aged for later use.

[0029] By adopting the above technical solution, the pre-adsorption of filler helps to achieve uniform dispersion of diene and m-phenylenediamine in the matrix.

[0030] In summary, this application has the following beneficial effects: This application constructs a sparse covalent cross-linked network in an ultra-high molecular weight polyethylene (UHMWPE) matrix through an amidation reaction between maleic anhydride-grafted polyethylene and m-phenylenediamine. Simultaneously, the polyethylene backbone of the maleic anhydride-grafted polyethylene has a similar chemical structure to the polyethylene components in the matrix, allowing for co-crystallization and chain entanglement during melt processing. This enables the material to maintain a high level of crystallinity even at low cross-linking densities. Furthermore, in systems containing 1,3-bis(tert-butylperoxyisopropyl)benzene, it can co-construct a micro-cross-linked system with the amidation cross-linking sites, moderately enhancing the bonding forces between molecular chains. This strengthens the material's rigidity and heat resistance while reducing the restriction of the cross-linked structure on molecular chain movement and the crystallization process. Additionally, the formation of long-chain branched structures optimizes melt rheological behavior, improving the difficulty of processing pure UHMWPE. Ultimately, this achieves a balance between high crystallinity, excellent mechanical strength, and good processing performance. Detailed Implementation

[0031] The present application will be further described in detail below with reference to the embodiments.

[0032] Unless otherwise specified, the raw materials used in the embodiments and comparative examples of this application are all commercially available.

[0033] Ultra-high molecular weight polyethylene, with a viscosity-average molecular weight of 4 million, is used as a powder after drying at 60°C for 4 hours. Linear low-density polyethylene, butene copolymer, melt flow rate 2.0 g / 10 min (190℃, 2.16 kg). High-density polyethylene: injection molding grade, melt flow rate 5.0 g / 10 min (190℃, 21.6 kg). Low-density polyethylene: extrusion grade, melt flow rate 2.0 g / 10 min (190℃, 2.16 kg). Ethylene-octene copolymer elastomer, octene content 25wt%, melt flow rate 5.0g / 10min (190℃, 2.16kg); Maleic anhydride-grafted polyethylene, with a grafting rate of 0.8~1.2wt% and a melt flow rate of 1.0~3.0g / 10min (190℃, 2.16kg). Nano-montmorillonite: Organic quaternary ammonium salt modified type, commercially available model is Fenghong DK-1, with a single crystal layer thickness of 1~2nm, a lateral size of 100~500nm, and an interlayer spacing ≥1.8nm; silicon carbide micro powder, particle size 5~10μm; nano-silica, specific surface area 200m². 2 / g, particle size 20~50nm; ultrafine wollastonite, needle-like structure, aspect ratio 10~15:1, median particle size 1~5μm.

[0034] Preparation Examples 1-3: Pretreated Packing Materials Preparation Example 1 The preparation method of the pretreated packing material in this preparation example includes the following steps: S1: Prepare a 3% (w / w) aqueous solution of silane coupling agent KH-550 in ethanol, wherein the volume ratio of anhydrous ethanol to deionized water in the aqueous solution is 9:1. Adjust the pH to 5.0 using an 8% (w / w) acetic acid solution and hydrolyze for 60 min with continuous stirring at 200 r / min to obtain a pre-hydrolyzed solution. S2: Nano-montmorillonite and silicon carbide micro powder are mixed evenly at a mass ratio of 2:1, and then added to a stirred reactor with pre-hydrolyzed solution at a solid-liquid ratio of 1g:10mL. The stirring is turned on at 200r / min, and the temperature is raised to 50℃. The reaction is kept at a constant temperature for 4h. After the reaction is completed, the filter is filtered under reduced pressure while hot. The filter cake is washed three times with anhydrous ethanol and dried at 105℃ and -0.09MPa for 4h. The filter cake is then ground and dispersed to obtain the pretreated filler.

[0035] Preparation Example 2 The preparation method of the pretreated packing material in this preparation example includes the following steps: S1: Prepare a 5% (w / w) aqueous solution of silane coupling agent KH-570 in ethanol, wherein the volume ratio of anhydrous ethanol to deionized water in the aqueous solution is 9:1. Adjust the pH to 4.0 using an 8% (w / w) acetic acid solution and hydrolyze for 40 min with continuous stirring at 200 r / min to obtain a pre-hydrolyzed solution. S2: Nano-silica and silicon carbide micro powders were mixed evenly at a mass ratio of 2:1, and then added to a stirred reactor with pre-hydrolyzed solution at a solid-liquid ratio of 1g:10mL. The stirring was turned on at 200r / min, and the temperature was raised to 70℃. The reaction was kept at a constant temperature for 2h. After the reaction was completed, the filter was filtered under reduced pressure while hot. The filter cake was washed three times with anhydrous ethanol and dried at 105℃ and -0.09MPa for 4h. The filter cake was then ground and dispersed to obtain the pretreated filler.

[0036] Preparation Example 3 The preparation method of the pretreated packing material in this preparation example includes the following steps: S1: Prepare a 4% (w / w) aqueous solution of silane coupling agent KH-570 in ethanol, wherein the volume ratio of anhydrous ethanol to deionized water in the aqueous solution is 9:1. Adjust the pH to 4.5 using an 8% (w / w) acetic acid solution and hydrolyze for 50 min with continuous stirring at 200 r / min to obtain a pre-hydrolyzed solution. S2: After mixing ultrafine wollastonite and silicon carbide micro powder at a mass ratio of 2:1, add them to a stirred reactor with pre-hydrolyzed solution at a solid-liquid ratio of 1g:10mL. Start stirring at 200r / min and heat to 60℃. React at a constant temperature for 3h. After the reaction is completed, filter under reduced pressure while hot. Wash the filter cake three times with anhydrous ethanol. Dry it at 105℃ and -0.09MPa for 4h. Grind and disperse to obtain the pretreated filler.

[0037] Example 1 The preparation method of the high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin in this embodiment includes the following steps: 1000g of ultra-high molecular weight polyethylene, 150g of linear low-density polyethylene, 200g of high-density polyethylene, 70g of low-density polyethylene, 150g of maleic anhydride-grafted polyethylene, 1.2g of m-phenylenediamine, 30g of filler from Preparation Example 1, and 10g of 1,9-decadiene were added to a high-speed mixer and mixed evenly. The mixture was then transferred to an internal mixer at a speed of 50 r / min, heated to 150°C, and mixed for 10 min. The temperature was then raised to 190°C, the speed was adjusted to 40 r / min, and the mixture was mixed for 12 min. The temperature was then lowered to 145°C, and 3g of antioxidant 1010, 3g of antioxidant 168, 8g of calcium stearate, and 8g of light stabilizer 944 were added. The mixture was mixed for 4 min, extruded using a single-screw extruder, cooled, granulated, and dried to obtain a special resin for highly crystalline micro-crosslinked ultra-high molecular weight polyethylene.

[0038] The parameters for the single-screw extruder are as follows: feeding section 120℃, compression section 180℃, metering section 200℃, die head 200℃, and screw speed 20r / min.

[0039] Example 2 The preparation method of the high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin in this embodiment includes the following steps: (1) 30g of the pretreated filler obtained in Preparation Example 1 was put into a closed reactor with stirring. Nitrogen gas was introduced to replace the filler three times to maintain a slightly positive pressure inert atmosphere of 0.02~0.05MPa in the reactor. 10g of 1,9-decadiene and 1.2g of m-phenylenediamine were slowly added. After the addition was completed, stirring was started and the speed was controlled at 150r / min. The temperature was raised to 50℃ and mixed at a constant temperature for 2h. Stirring was stopped and the mixture was sealed and aged in a nitrogen atmosphere for 12h to obtain the premix. (2) 1000g of ultra-high molecular weight polyethylene, 150g of linear low-density polyethylene, 200g of high-density polyethylene, 70g of low-density polyethylene, 150g of maleic anhydride-grafted polyethylene and premix were added to a high-speed mixer and mixed evenly. The mixture was then transferred to an internal mixer at a speed of 50r / min, heated to 150℃ and mixed for 10min. The temperature was then raised to 190℃, the speed was adjusted to 40r / min and mixed for 12min. The temperature was then lowered to 150℃ and antioxidant 1010 3g, antioxidant 168 3g, polyethylene wax 8g and light stabilizer 944 8g were added and mixed for 3min. The mixture was then extruded through a single screw extruder, cooled, granulated and dried to obtain a special resin for high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene.

[0040] The parameters for the single-screw extruder are as follows: feeding section 120℃, compression section 180℃, metering section 200℃, die head 200℃, and screw speed 20r / min.

[0041] Example 3 The difference between this embodiment and Embodiment 2 is as follows: (2) 1000g of ultra-high molecular weight polyethylene, 150g of linear low-density polyethylene, 200g of high-density polyethylene, 70g of low-density polyethylene, 150g of maleic anhydride-grafted polyethylene, premix and 0.5g of 1,3-bis(tert-butylperoxyisopropyl)benzene were added to a high-speed mixer and mixed evenly. The mixture was then transferred to an internal mixer at a speed of 50r / min, heated to 150℃, and mixed for 10min. The temperature was then raised to 190℃, the speed was adjusted to 40r / min, and mixed for 12min. The temperature was then lowered to 150℃, and 3g of antioxidant 1010, 3g of antioxidant 168, 8g of polyethylene wax and 8g of light stabilizer 944 were added. The mixture was mixed for 3min, extruded by a single screw extruder, cooled, granulated and dried to obtain a special resin for high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene.

[0042] The parameters for the single-screw extruder are as follows: feeding section 120℃, compression section 180℃, metering section 200℃, die head 200℃, and screw speed 20r / min.

[0043] Everything else is the same as in Example 2.

[0044] Example 4 The preparation method of the high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin in this embodiment includes the following steps: (1) 20g of the pretreated filler obtained in Preparation Example 2 was put into a closed reactor with a stirrer, and nitrogen was introduced to replace it 3 times. The reactor was kept under a slightly positive pressure inert atmosphere of 0.02~0.05MPa. 5g of 1,9-decadiene and 0.8g of m-phenylenediamine were slowly added. After the addition was completed, the stirrer was turned on and the speed was controlled at 150r / min. The temperature was raised to 40℃ and mixed at a constant temperature for 1h. The stirring was stopped and the mixture was sealed and aged under a nitrogen atmosphere for 12h to obtain the premix. (2) 1000g of ultra-high molecular weight polyethylene, 100g of linear low-density polyethylene, 150g of high-density polyethylene, 50g of low-density polyethylene, 100g of maleic anhydride-grafted polyethylene, premix and 0.3g of 1,3-bis(tert-butylperoxyisopropyl)benzene were added to a high-speed mixer and mixed evenly. The mixture was then transferred to an internal mixer at a speed of 50r / min, heated to 140℃, and mixed for 12min. The temperature was then raised to 180℃, the speed was adjusted to 40r / min, and mixed for 15min. The temperature was then lowered to 150℃, and 2g of antioxidant 1010, 2g of antioxidant 168, 5g of calcium stearate and 5g of light stabilizer 944 were added. The mixture was mixed for 3min, extruded through a single screw extruder, cooled, granulated and dried to obtain a special resin for high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene.

[0045] The parameters for the single-screw extruder are as follows: feeding section 120℃, compression section 180℃, metering section 200℃, die head 200℃, and screw speed 20r / min.

[0046] Example 5 The preparation method of the high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin in this embodiment includes the following steps: (1) 50g of the pretreated filler obtained in Preparation Example 3 was put into a closed reactor with a stirrer, and nitrogen was introduced to replace it 3 times. The reactor was kept under a slightly positive pressure inert atmosphere of 0.02~0.05MPa. 15g of 1,9-decadiene and 1.5g of m-phenylenediamine were slowly added. After the addition was completed, the stirrer was turned on and the speed was controlled at 150r / min. The temperature was raised to 60℃ and mixed at a constant temperature for 3h. The stirring was stopped and the mixture was sealed and aged under a nitrogen atmosphere for 12h to obtain the premix. (2) 1000g of ultra-high molecular weight polyethylene, 200g of linear low-density polyethylene, 250g of high-density polyethylene, 100g of low-density polyethylene, 200g of maleic anhydride-grafted polyethylene, premix and 0.7g of 1,3-bis(tert-butylperoxyisopropyl)benzene were added to a high-speed mixer and mixed evenly. The mixture was then transferred to an internal mixer at a speed of 50r / min, heated to 160℃ and mixed for 8min. The temperature was then raised to 200℃, the speed was adjusted to 40r / min and mixed for 15min. The temperature was then lowered to 150℃, and 4g of antioxidant 1010, 4g of antioxidant 168, 10g of calcium stearate and 10g of light stabilizer 944 were added and mixed for 5min. The mixture was then extruded through a single-screw extruder, cooled, granulated and dried to obtain a special resin for high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene.

[0047] The parameters for the single-screw extruder are as follows: feeding section 120℃, compression section 180℃, metering section 200℃, die head 200℃, and screw speed 20r / min.

[0048] Example 6 The difference between this embodiment and embodiment 5 is as follows: (2) 1000g of ultra-high molecular weight polyethylene, 200g of linear low-density polyethylene, 250g of high-density polyethylene, 100g of low-density polyethylene, 200g of maleic anhydride-grafted polyethylene, premix, 0.7g of 1,3-bis(tert-butylperoxyisopropyl)benzene and 2g of dicyclopentadiene were added to a high-speed mixer and mixed evenly. The mixture was then transferred to an internal mixer at a speed of 50r / min, heated to 160℃, and mixed for 8min. The temperature was then raised to 200℃, the speed was adjusted to 40r / min, and mixed for 15min. The temperature was then lowered to 150℃, and 4g of antioxidant 1010, 1684g of antioxidant, 10g of calcium stearate and 10g of light stabilizer 944 were added. The mixture was mixed for 5min, extruded through a single-screw extruder, cooled, granulated and dried to obtain a special resin for high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene.

[0049] The rest is the same as in Example 5.

[0050] Example 7 The difference between this embodiment and embodiment 6 is that: (2) 1000g of ultra-high molecular weight polyethylene, 200g of linear low-density polyethylene, 250g of high-density polyethylene, 100g of low-density polyethylene, 200g of maleic anhydride-grafted polyethylene, premix, 0.7g of 1,3-bis(tert-butylperoxyisopropyl)benzene, 4g of dicyclopentadiene and 30g of ethylene-octene copolymer elastomer were added to a high-speed mixer and mixed evenly. The mixture was then transferred to an internal mixer at a speed of 50r / min, heated to 160℃ and mixed for 8min. The temperature was then raised to 200℃, the speed was adjusted to 40r / min and mixed for 15min. The temperature was then lowered to 150℃, and 4g of antioxidant 1010, 4g of antioxidant 168, 10g of calcium stearate and 10g of light stabilizer 944 were added and mixed for 5min. The mixture was then extruded through a single screw extruder, cooled, granulated and dried to obtain a special resin for high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene.

[0051] The rest is the same as in Example 6.

[0052] Example 8 The difference between this embodiment and embodiment 7 is that: (2) 1000g of ultra-high molecular weight polyethylene, 200g of linear low-density polyethylene, 250g of high-density polyethylene, 100g of low-density polyethylene, 200g of maleic anhydride-grafted polyethylene, premix, 0.7g of 1,3-bis(tert-butylperoxyisopropyl)benzene, 4g of dicyclopentadiene and 50g of ethylene-octene copolymer elastomer were added to a high-speed mixer and mixed evenly. The mixture was then transferred to an internal mixer at a speed of 50r / min, heated to 160℃ and mixed for 8min. The temperature was then raised to 200℃, the speed was adjusted to 40r / min and mixed for 15min. The temperature was then lowered to 150℃, and 4g of antioxidant 1010, 4g of antioxidant 168, 10g of calcium stearate and 10g of light stabilizer 944 were added and mixed for 5min. The mixture was then extruded through a single screw extruder, cooled, granulated and dried to obtain a special resin for high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene.

[0053] The rest is the same as in Example 7.

[0054] Example 9 The difference between this embodiment and embodiment 8 is as follows: (2) 1000g of ultra-high molecular weight polyethylene, 200g of linear low-density polyethylene, 250g of high-density polyethylene, 100g of low-density polyethylene, 200g of maleic anhydride-grafted polyethylene, premix, 0.7g of 1,3-bis(tert-butylperoxyisopropyl)benzene, 4g of dicyclopentadiene, 30g of ethylene-octene copolymer elastomer and 8g of 2-butyl-1-octene were added to a high-speed mixer and mixed evenly. The mixture was then transferred to an internal mixer at a speed of 50r / min, heated to 160℃ and mixed for 8min. The temperature was then raised to 200℃, the speed was adjusted to 40r / min and mixed for 15min. The temperature was then lowered to 150℃, and 4g of antioxidant 1010, 4g of antioxidant 168, 10g of calcium stearate and 10g of light stabilizer 944 were added and mixed for 5min. The mixture was then extruded through a single screw extruder, cooled, granulated and dried to obtain a special resin for high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene.

[0055] The rest is the same as in Example 8.

[0056] Example 10 The difference between this embodiment and embodiment 9 is as follows: (2) 1000g of ultra-high molecular weight polyethylene, 200g of linear low-density polyethylene, 250g of high-density polyethylene, 100g of low-density polyethylene, 200g of maleic anhydride-grafted polyethylene, premix, 0.7g of 1,3-bis(tert-butylperoxyisopropyl)benzene, 4g of dicyclopentadiene, 30g of ethylene-octene copolymer elastomer and 12g of 2-butyl-1-octene were added to a high-speed mixer and mixed evenly. The mixture was then transferred to an internal mixer at a speed of 50r / min, heated to 160℃ and mixed for 8min. The temperature was then raised to 200℃, the speed was adjusted to 40r / min and mixed for 15min. The temperature was then lowered to 150℃, and 4g of antioxidant 1010, 4g of antioxidant 168, 10g of calcium stearate and 10g of light stabilizer 944 were added and mixed for 5min. The mixture was then extruded through a single screw extruder, cooled, granulated and dried to obtain a special resin for high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene.

[0057] The rest is the same as in Example 9.

[0058] Comparative Example 1 The difference between this comparative example and Example 1 is as follows: No m-phenylenediamine was added; Everything else is the same as in Example 1.

[0059] Comparative Example 2 The preparation method of the high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene resin in this comparative example includes the following steps: (1) 30g of the pretreated filler obtained in Preparation Example 1 was put into a closed reactor with a stirrer, and nitrogen was introduced to replace it 3 times. The reactor was kept under a slightly positive pressure inert atmosphere of 0.02~0.05MPa. 10g of 1,9-decadiene was slowly added. After the addition was completed, the stirrer was turned on and the speed was controlled at 150r / min. The temperature was raised to 50℃ and mixed at a constant temperature for 2h. The stirring was stopped and the mixture was sealed and aged under a nitrogen atmosphere for 12h to obtain the premix. (2) 1000g of ultra-high molecular weight polyethylene, 150g of linear low-density polyethylene, 200g of high-density polyethylene, 70g of low-density polyethylene, premix and 0.5g of 1,3-bis(tert-butylperoxyisopropyl)benzene were added to a high-speed mixer and mixed evenly. The mixture was then transferred to an internal mixer at a speed of 50r / min, heated to 150℃ and mixed for 10min. The temperature was then raised to 190℃, the speed was adjusted to 40r / min and mixed for 12min. The temperature was then lowered to 150℃, and 3g of antioxidant 1010, 3g of antioxidant 168, 8g of polyethylene wax and 8g of light stabilizer 944 were added and mixed for 3min. The mixture was then extruded through a single screw extruder, cooled, granulated and dried to obtain a special resin for high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene.

[0060] The parameters for the single-screw extruder are as follows: feeding section 120℃, compression section 180℃, metering section 200℃, die head 200℃, and screw speed 20r / min.

[0061] Performance testing The high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resins prepared in Examples 1-10 and Comparative Examples 1-2 were weighed and placed into the mold of a flat vulcanizing apparatus. The molding temperature was controlled at 190-200℃ using a mold temperature controller. Low-pressure preheating was performed for 8 minutes to remove air, followed by pressurization to 12MPa and holding for 10 minutes. Finally, under the holding pressure, the mold was opened and the sheets were removed by water cooling to below 60℃. The following performance tests were conducted, with reference standards as follows: GB / T 2411-2008; GB / T 1633-2000; GB / T 1043.1-2008; GB / T 1040.2-2022; GB / T 19466.3-2004; ASTM D2765-16 (2024). The test results are shown in Table 1.

[0062] Table 1. Performance test data of the ultra-high molecular weight polyethylene special resins prepared in Examples 1-10 and Comparative Examples 1-2

[0063] The performance test data in Table 1 is analyzed in detail as follows: As can be seen from Example 1 and Comparative Example 1, after introducing m-phenylenediamine and undergoing an amidation reaction with maleic anhydride-grafted polyethylene, the material's hardness and heat resistance improved, the yield strength increased slightly, the impact toughness and elongation at break decreased, and the gel content increased, indicating that the amidation reaction introduced a cross-linked structure into the system. The crystallinity of Example 1 decreased only slightly, indicating that the micro-cross-linked structure did not significantly impair the crystallinity of the polyethylene chain segments.

[0064] As can be seen from the performance changes in Examples 1-5, the rigidity and toughness of the material show an inverse adjustment trend with the increase of reactive components and auxiliary initiators. Examples 3 and 5 correspond to higher crosslinking densities, higher hardness and Vicat softening temperature, and lower impact strength and elongation at break; Example 4 corresponds to a lower crosslinking density, but maintains better toughness. Example 2 uses a filler pre-adsorption process, which slightly optimizes the overall performance.

[0065] Compared with Comparative Example 2, Example 3 achieved better rigidity and heat resistance at a similar level of crosslinking, with a more gradual decrease in hardness and heat resistance, but a significant decrease in impact strength and elongation at break. Example 3 achieved better overall performance by combining amidation and free radical crosslinking.

[0066] As can be seen from the performance changes in Examples 6-10, the introduction of rigid alicyclic dienes further improved the material's hardness and heat resistance, decreased its impact toughness, and slightly increased its gelation rate. After adding ethylene-octene copolymer elastomer, the impact strength and elongation at break rebounded, while rigidity and heat resistance declined, and the gelation rate gradually decreased due to the elastomer's dilution effect. With increasing 2-butyl-1-octene content, the gelation rate gradually decreased due to chain transfer, and the various properties tended to reach equilibrium within a narrow range. Overall, the gelation rates of Examples 6-10 remained within the micro-crosslinking range, and although the crystallinity decreased slightly, it remained at a high level, maintaining the basic characteristics of highly crystalline micro-crosslinked systems.

Claims

1. A special resin for highly crystalline micro-crosslinked ultra-high molecular weight polyethylene, characterized in that, Made from the following parts by weight of raw materials: The composition includes 100 parts ultra-high molecular weight polyethylene, 10-20 parts linear low-density polyethylene, 15-25 parts high-density polyethylene, 5-10 parts low-density polyethylene, 10-20 parts maleic anhydride-grafted polyethylene, 0.08-0.15 parts m-phenylenediamine, 2-5 parts filler, 0.5-1.5 parts long-chain non-conjugated α,ω-diene, 0.4-0.8 parts antioxidant, 0.5-1 part lubricant, and 0.5-1 part light stabilizer.

2. The high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin according to claim 1, characterized in that, The long-chain non-conjugated α,ω-diene is 1,9-decadiene.

3. The high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin according to claim 1, characterized in that, The high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin also includes 0.03~0.07 parts by weight of 1,3-bis(tert-butylperoxyisopropyl)benzene.

4. The high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin according to claim 1, characterized in that, The filler is two of the following: nano-montmorillonite, nano-silica, ultrafine wollastonite, and silicon carbide micro powder.

5. The high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin according to claim 4, characterized in that, Before use, the filler undergoes the following pretreatment steps: S1: Prepare a 3%~5% (w / w) aqueous solution of silane coupling agent in ethanol, adjust the pH to 4.0~5.0, and hydrolyze for 40~60 min to obtain a pre-hydrolyzed solution; S2: Mix the packing material and the pre-hydrolyzed solution, heat to 50~70℃, react for 2~4 hours, separate the solid and liquid, wash, and dry to obtain the pretreated packing material.

6. The high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin according to claim 1, characterized in that, The high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin also includes 0.2 to 0.4 parts by weight of alicyclic non-conjugated diene.

7. The high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin according to claim 1, characterized in that, The high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin also includes 3-5 parts by weight of ethylene-octene copolymer elastomer.

8. The high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin according to claim 1, characterized in that, The high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin also includes 0.8 to 1.2 parts by weight of 2-butyl-1-octene.

9. A method for preparing a special resin for highly crystalline micro-crosslinked ultra-high molecular weight polyethylene as described in any one of claims 1 to 8, characterized in that, Includes the following steps: Ultra-high molecular weight polyethylene, linear low-density polyethylene, high-density polyethylene, low-density polyethylene, maleic anhydride-grafted polyethylene, m-phenylenediamine, filler, long-chain non-conjugated α,ω-diene, optional 1,3-bis(tert-butylperoxyisopropyl)benzene, optional alicyclic non-conjugated diene, optional ethylene-octene copolymer elastomer, and optional 2-butyl-1-octene are mixed and heated to 140~160℃ and kneaded for 8~12 min. The temperature is then raised to 180~200℃ and kneaded for 12~15 min. The temperature is lowered to 145~150℃, antioxidants, lubricants, and light stabilizers are added, and the mixture is kneaded for 3~5 min. The mixture is then extruded, cooled, granulated, and dried to obtain a high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin.

10. The method for preparing the high-crystallinity micro-crosslinked ultra-high molecular weight polyethylene special resin according to claim 9, characterized in that, Before adding the filler, long-chain non-conjugated α,ω-diene, and m-phenylenediamine, the following pretreatment steps are performed: Under an inert atmosphere, the packing material, long-chain non-conjugated α,ω-diene, and m-phenylenediamine are added to the reactor and mixed at 40-60°C for 1-3 hours, then aged for later use.

Citation Information

Patent Citations