A foamed carbon fiber reinforced composite material consumable for 3D printing, its preparation method and printing method

By preparing foamed carbon fiber reinforced composite materials, the problems of lightweighting and high performance of 3D printing consumables have been solved, achieving a reduction in material density and an improvement in mechanical properties, making them suitable for applications in multiple fields.

CN123107325APending Publication Date: 2026-11-17MAANSHAN ANYI INTELLIGENT TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611172469.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing 3D printing consumables are difficult to achieve in terms of lightweight and high performance. Carbon fiber reinforced composite materials suffer from poor interfacial bonding, uneven dispersion, narrow process window, and 3D printing process compatibility issues during the foaming process, which leads to a decline in material performance.

Method used

A combination of thermoplastic matrix resin, chopped carbon fiber, foaming agent, interface modifier and processing aid is used to prepare foamed carbon fiber reinforced composite consumables through twin-screw extrusion granulation and single-screw wire drawing processes. The printing process parameters are optimized to achieve lightweight and high strength of the material.

Benefits of technology

It achieves a 35-60% reduction in material density, a significant increase in tensile strength and flexural modulus, improved uniformity of cell structure, and enhanced interfacial bonding, making it suitable for industrial production and use in existing FDM equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107325A_ABST
    Figure CN123107325A_ABST
Patent Text Reader

Abstract

This invention discloses a foamed carbon fiber reinforced composite material consumable for 3D printing, its preparation method, and printing method. The consumable, by mass percentage, consists of 72-85% thermoplastic matrix resin, 5-15% chopped carbon fiber, 1-5% foaming agent, 0.5-3% silane coupling agent, and 0.5-5% processing aids. The preparation method employs a two-step process: first, carbon fiber is mixed with a portion of the resin and dispersant to obtain a pre-dispersed masterbatch; then, it is mixed with the remaining components and granulated by twin-screw extrusion; finally, it is segmented and temperature-controlled drawn into fibers by a single screw extruder, and wound using water-cooling, air-cooling, and laser online diameter measurement. This invention refines the pore size to 5-15 μm through heterogeneous nucleation of carbon fiber and achieves dual interface modification with the silane coupling agent, solving the interface competition problem between foaming and reinforcement. The density of this consumable is 0.50-0.85 g / cm³. 3 With a tensile strength of 45-75 MPa, a flexural modulus of 2.5-4.5 GPa, and a weight reduction of 35-60%, it is suitable for aerospace, automotive, and medical orthopedic applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer composite materials and additive manufacturing technology, specifically to a foamed carbon fiber reinforced composite material consumable for 3D printing, its preparation method, and printing method. Background Technology

[0002] In recent years, fused deposition modeling (FDM) 3D printing technology has been widely used in aerospace, automotive manufacturing, medical devices, and consumer electronics due to its advantages such as low equipment cost, ease of operation, and wide material applicability. However, the high density of traditional FDM printed parts makes it difficult to meet the extreme lightweight requirements of drones and aerospace applications. Therefore, the development of 3D printing composite material consumables aimed at lightweighting and high performance has become an important research direction in the current additive manufacturing field.

[0003] Carbon fiber reinforced thermoplastic composites are considered an important development direction for high-performance 3D printing consumables due to their advantages such as high specific strength, high specific modulus, corrosion resistance, and recyclability. Currently, various carbon fiber reinforced 3D printing consumables are available on the market, such as PLA-CF (polylactic acid-based carbon fiber reinforced consumables), PETG-CF, and PA-CF (nylon-based carbon fiber reinforced consumables). These products significantly improve the tensile strength, flexural modulus, and heat resistance of printed parts by adding 5-30% short-cut carbon fibers to a thermoplastic matrix. However, due to the high density of carbon fibers themselves (approximately 1.75 g / cm³) and the large amount added, the density of these consumables is typically in the range of 1.2-1.4 g / cm³, which is higher than the density of pure matrix resin (PLA approximately 1.25 g / cm³), making it difficult to achieve lightweighting goals.

[0004] Foaming technology is an effective method for preparing lightweight polymer materials. By introducing a foaming agent into the polymer matrix, gas is generated during processing to form a cellular structure, which can significantly reduce the material density. In recent years, foamed 3D printing consumables have also received increasing attention. For example, the PLALLAWAERO series of foamed consumables launched by the Dutch company ColorFabb can achieve a weight reduction of 40-65% by adding a chemical foaming agent. However, the foaming process leads to a significant decrease in the mechanical properties of the material—the tensile strength of pure foamed PLA typically drops to 15-25 MPa, and the flexural modulus drops to 1.0-1.5 GPa, making it difficult to use for load-bearing structural components.

[0005] Combining carbon fiber reinforcement with foaming technology holds promise for achieving both lightweighting and high performance. Carbon fiber can act as a reinforcement to improve the mechanical properties of foamed materials, while the foamed structure can significantly reduce the density of carbon fiber reinforced composites. However, research on foamed carbon fiber reinforced composites remains in its infancy in the field of 3D printing consumables, and there are currently no related products on the market. This is mainly due to the following technical challenges:

[0006] (1) Interface competition problem. Both the cell surface and the carbon fiber surface formed during the foaming process need to form a good interfacial bond with the matrix resin. Under the limited amount of interface modifier, the modification of the two interfaces is competitive. If the distribution is not proper, it will lead to debonding of the cell-matrix or carbon fiber-matrix interface, which will seriously affect the material properties.

[0007] (2) Dispersion uniformity problem. Carbon fiber has poor dispersion in polymer melt and is prone to agglomeration; the foaming agent decomposes rapidly at the processing temperature and releases gas in a concentrated manner. If the dispersion is uneven, it can easily lead to a wide distribution of cell size, cell merging, or even rupture.

[0008] (3) The problem of narrow process window. The foaming temperature window of the foaming agent and the processing temperature window of carbon fiber reinforced composite material often do not overlap. Too high a foaming temperature will cause carbon fiber to break and matrix to degrade; too low a temperature will result in incomplete foaming and poor weight reduction effect.

[0009] (4) 3D printing process adaptation issues. The melt flow behavior, foaming timing control, and interlayer bonding of foamed carbon fiber reinforced consumables in the FDM printing process are complex and require targeted optimization of printing process parameters. Summary of the Invention

[0010] To address the problems mentioned in the background art, the present invention provides the following technical solution: a foamed carbon fiber reinforced composite material consumable for 3D printing, comprising the following components by mass percentage;

[0011] Thermoplastic matrix resin 72-85%;

[0012] Short-cut carbon fiber 5-15%;

[0013] Foaming agent 1-5%;

[0014] Interface modifier 0.5-3%;

[0015] Processing aids 0.5-5%;

[0016] The thermoplastic matrix resin is selected from one or more of polylactic acid, polyethylene terephthalate-1,4-cyclohexanediol ester, or thermoplastic polyurethane.

[0017] The length of the chopped carbon fiber is 100-200 μm;

[0018] The foaming agent is selected from one or more of azodicarbonamide, 4,4'-oxobisbenzenesulfonylhydrazine, or expandable microspheres;

[0019] The interface modifier is a silane coupling agent selected from γ-aminopropyltriethoxysilane or γ-glycidoxypropyltrimethoxysilane.

[0020] The processing aids include lubricants, antioxidants, and dispersants.

[0021] Preferably, the thermoplastic matrix resin is polylactic acid with a relative molecular weight of 8 × 10⁻⁶. 4 -1.5×10 5 Under test conditions of 190°C / 2.16kg, the melt index was 5-15g / 10min.

[0022] Preferably, the chopped carbon fiber has a length of 120-180 μm and a diameter of 5-7 μm.

[0023] Preferably, the foaming agent is azodicarbonamide, with a particle size of 5-15 μm, a decomposition temperature of 140-220°C, and a gas generation rate of 220-250 mL / g.

[0024] Preferably, the foaming agent is an expandable microsphere, the outer shell of which is a thermoplastic acrylic copolymer, the core material is isobutane, the initial expansion temperature is 140-180°C, and the maximum expansion temperature is 180-220°C.

[0025] Preferably, the silane coupling agent is γ-aminopropyltriethoxysilane, with a molecular weight of 221.37 and a density of 0.940-0.950 g / cm³.

[0026] Preferably, the lubricant is selected from one or more of zinc stearate, polyethylene wax, or ethylene bis-stearamide, and the dosage is 0.3-2%; the antioxidant is selected from one or more of antioxidant 1010, antioxidant 168, or antioxidant 1098, and the dosage is 0.1-1%; the dispersant is selected from one or more of stearic acid, titanate coupling agent, or aluminate coupling agent, and the dosage is 0.1-2%.

[0027] Preferably, the mass ratio of the foaming agent to the chopped carbon fiber is 1:3 to 1:5, so as to utilize the carbon fiber as a heterogeneous nucleating agent to refine the cell structure during the foaming process, with an average cell diameter of 5-15 μm and a cell density of 1×10⁻⁶. 8 -5×10 9 pcs / cm³

[0028] Preferably, the filament has a wire diameter of 1.75±0.02mm or 2.85±0.02mm, an ellipticity of no more than 0.01mm, and a moisture content of no more than 0.02wt%, and is suitable for fused deposition modeling 3D printing.

[0029] Preferably, the consumable has a density of 0.50-0.85 g / cm³, a tensile strength of 45-75 MPa, and a flexural modulus of 2.5-4.5 GPa.

[0030] This invention also proposes a method for preparing the above-mentioned consumables, which specifically includes the following steps:

[0031] S1. Preparation of carbon fiber predispersed masterbatch: Short carbon fibers, a portion of thermoplastic matrix resin and dispersant are added into an internal mixer at a mass ratio of (5-15):(10-20):(0.1-1). The mixture is then internally mixed for 10-20 minutes at 160-180°C and 40-60 rpm to uniformly disperse the carbon fibers in the matrix resin. After crushing, carbon fiber predispersed masterbatch is obtained.

[0032] S2: Twin-screw extrusion granulation—The remaining thermoplastic matrix resin, foaming agent, interface modifier, processing aid, and carbon fiber pre-dispersion masterbatch obtained in step S1 are added to a high-speed mixer according to the formula ratio and mixed for 5-10 minutes at a speed of 800-1200 rpm to obtain a premix; the premix is ​​fed into a twin-screw extruder and melt-extruded at a temperature of 160-220°C, a screw speed of 80-120 rpm, and a vacuum degree of -0.06 to -0.09 MPa. After water cooling and pelletizing, composite material granules are obtained.

[0033] S3: Single-screw filament forming—The composite material granules obtained in step S2 are vacuum dried at 80-100°C for 4-8 hours to reduce the moisture content to below 0.02wt%; the dried granules are fed into a single-screw extruder and melt-extruded at a temperature of 180-210°C and a screw speed of 20-40rpm. The filaments are drawn out through a circular die with a diameter of 1.75mm or 2.85mm, cooled by a primary water bath at 20-30°C, followed by a secondary air cooling at room temperature, laser online diameter measurement, and traction winding to obtain the foamed carbon fiber reinforced composite material consumable for 3D printing.

[0034] Preferably, the temperature settings of the twin-screw extruder in step S2 are: 160-170°C for the feeding section, 170-190°C for the compression section, 180-200°C for the homogenization section, and 190-210°C for the die head; the temperature settings of the single-screw extruder in step S3 are: 180-190°C for the feeding section, 190-200°C for the compression section, 200-210°C for the homogenization section, and 200-210°C for the die head.

[0035] Preferably, the twin-screw extruder in step S2 adopts a co-rotating twin-screw with a screw length-to-diameter ratio of 36-48:1. The screw assembly includes a conveying element, a shearing element, and a mixing element, wherein the shearing gap of the shearing element is 0.5-1.0 mm; the single-screw extruder in step S3 has a screw length-to-diameter ratio of 25-30:1 and a compression ratio of 2.5-3.5.

[0036] Preferably, the accuracy of the laser online diameter measurement in step S3 is ±0.001mm, and the traction speed is automatically adjusted when the wire diameter deviation exceeds ±0.005mm; the traction and winding speed is 50-150m / min, and the winding tension is 0.5-2N.

[0037] In addition to the above-mentioned preparation method of consumables, there is also the process of using consumables. Specifically, 3D printing is performed using consumables, and the printing adopts the fused deposition modeling process. The process parameters are as follows: the nozzle temperature is 10-30°C higher than the initial decomposition temperature or initial expansion temperature of the foaming agent; the heated bed temperature is 50-70°C; the printing speed is 30-50 mm / s; the layer height is 0.1-0.3 mm; the extrusion ratio is 0.4-0.6; the filling density is 15-40%; after printing, the material is annealed at 60-100°C for 6-12 hours; during the printing process, the cooling fan of the printing cavity is turned off or the fan speed is kept below 30% to maintain the melt temperature and pressure required for foaming.

[0038] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0039] 1. Achieving both significant weight reduction and high strength. This invention organically combines carbon fiber reinforcement with foaming technology to prepare 3D printing consumables with a density of only 0.50-0.85 g / cm³, which is 35-60% lighter than traditional carbon fiber reinforced consumables (1.2-1.4 g / cm³). At the same time, due to the reinforcement effect of carbon fiber, the tensile strength reaches 45-75 MPa and the flexural modulus reaches 2.5-4.5 GPa, which is far higher than that of pure foam consumables (tensile strength 15-25 MPa).

[0040] 2. Carbon fiber heterogeneous nucleation refines cell structure and improves foam uniformity. This invention utilizes carbon fiber as a heterogeneous nucleating agent, providing numerous nucleation sites during the foaming process. This reduces the average cell diameter from 21.4 μm in the pure foam system to 5-15 μm, and the cell density from 10... 5 The quantity per cm³ has increased to 10. 8 -10 9 The cell count is on the order of 1 / cm³. The fine and uniform cell structure not only improves the weight reduction efficiency but also reduces stress concentration points and improves the mechanical properties of the material.

[0041] 3. Dual Interface Modification with Silane Coupling Agent to Enhance Interfacial Bonding. This invention uses a silane coupling agent as the interface modifier, which acts simultaneously on both the carbon fiber-matrix resin interface and the cell-matrix resin interface, creating a "dual interface modification" effect. The increased bonding strength at the carbon fiber-matrix interface allows for effective load transfer to the carbon fibers; the increased bonding strength at the cell-matrix interface reduces stress concentration at the cell edges. The synergistic effect of this dual interface modification enables the material of this invention to maintain high mechanical properties while achieving weight reduction during foaming.

[0042] 4. The process is simple and suitable for industrial production and existing FDM equipment. This invention adopts a mature two-step process of twin-screw extrusion granulation and single-screw wire drawing, resulting in low equipment investment and high production efficiency. The consumables can be directly used in most FDM 3D printers on the market without requiring equipment modification, demonstrating good market adaptability.

[0043] 5. Wide range of applications. The consumables of this invention are applicable to applications with strict requirements for lightweighting and mechanical performance, such as UAV fuselage frames, aerospace structural components, automotive interior parts, medical orthotics, and sports equipment. Attached Figure Description

[0044] Figure 1 SEM image of the cross section of the foamed carbon fiber reinforced composite material;

[0045] Figure 2 SEM images comparing carbon fiber surface modification before and after modification;

[0046] Figure 3 A comparison chart of the tensile strength of different materials;

[0047] Figure 4 A comparison chart of the flexural modulus of different materials;

[0048] Figure 5 A comparison chart of notched impact strength of different materials;

[0049] Figure 6 A comparison chart of the heat distortion temperatures of different materials;

[0050] Figure 7 This is a comparison of surface roughness of 3D printed parts (layer height 0.2mm).

[0051] Figure 8 This diagram illustrates the control of pore structure and the distribution of bubble size. Detailed Implementation

[0052] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0053] The raw materials used in the following examples are all commercially available industrial-grade products:

[0054] Polylactic acid (PLA): NatureWorks 4043D, melt index 8g / 10min (190°C / 2.16kg), density 1.24g / cm³;

[0055] Polyethylene terephthalate-1,4-cyclohexanediethanol (PETG): EastEastar GN007, melt index 10g / 10min (220°C / 2.16kg), density 1.27g / cm³;

[0056] Thermoplastic polyurethane (TPU): BASF Elastollan 1185A, Shore hardness 85A, melt index 20g / 10min (190°C / 2.16kg), density 1.12g / cm³;

[0057] Short-cut carbon fiber: T700S grade, 150μm in length, 7μm in diameter, and 1.78g / cm³ in density, supplied by Toray Industries, Inc., Japan;

[0058] Azodicarbonamide (AC): Hangzhou Haihong Fine Chemical Plant, particle size 10μm, decomposition temperature 200°C, gas evolution 230mL / g;

[0059] Expandable microspheres: AkzoNobel Expansel 930DU40, initial expansion temperature 150°C, maximum expansion temperature 200°C;

[0060] γ-aminopropyltriethoxysilane (KH550): Nanjing Shuguang Chemical Group Co., Ltd.;

[0061] γ-glycidyl etheroxypropyltrimethoxysilane (KH560): Nanjing Shuguang Chemical Group Co., Ltd.;

[0062] Zinc stearate: Tianjin Damao Chemical Reagent Factory;

[0063] Polyethylene wax: BASF Luwax A;

[0064] Antioxidant 1010: BASF Irganox 1010;

[0065] Antioxidant 168: BASF Irgafos 168.

[0066] Example 1: PLA-based foamed carbon fiber reinforced composite consumable (PLA-CF-AC)

[0067] In this embodiment, polylactic acid (PLA) is used as the matrix resin and azodicarbonamide (AC) is used as the foaming agent to prepare foamed carbon fiber reinforced composite material consumables.

[0068] (1) Formulation composition (by mass percentage):

[0069] Components Content (wt%) Polylactic acid (PLA) 82.5% Short-cut carbon fiber (150μm) 10% Azodicarbonamide (AC) 3% γ-aminopropyltriethoxysilane (KH550) 2% Zinc stearate 1% Antioxidant 1010 0.2% Antioxidant 168 0.1% Polyethylene wax 0.7% Stearic acid (dispersant) 0.5% total 100%

[0070] (2) Preparation method:

[0071] S1: Preparation of carbon fiber predispersed masterbatch

[0072] 1.0 kg of chopped carbon fiber, 2.0 kg of polylactic acid, and 0.1 kg of stearic acid were added to an internal mixer and mixed for 15 minutes at 170°C and 50 rpm. During the mixing process, the carbon fiber gradually dispersed in the PLA matrix under the action of a strong shear field, and the material gradually changed from loose powder to uniform blackish-gray lumps. After the mixing was completed, the material was removed and cooled at room temperature for 30 minutes, and then crushed into particles with a particle size of about 4 mm to obtain carbon fiber pre-dispersion masterbatch (carbon fiber content of about 33.3%).

[0073] S2: Twin-screw extrusion granulation

[0074] 5.85 kg of polylactic acid, 0.3 kg of azodicarbonamide (AC), 0.2 kg of KH550, 0.1 kg of zinc stearate, 0.02 kg of antioxidant 1010, 0.01 kg of antioxidant 168, 0.07 kg of polyethylene wax, and 3.1 kg of carbon fiber predispersed masterbatch obtained in step S1 (containing 1.0 kg of carbon fiber, 2.0 kg of PLA, and 0.1 kg of stearic acid) were added into a high-speed mixer and mixed for 8 minutes at 1000 rpm to obtain a premix.

[0075] The premixed material is fed into a co-rotating twin-screw extruder. The temperature settings of the twin-screw extruder are: feeding section 165°C, compression section 180°C, homogenization section 190°C, and die head 200°C. The screw speed is 100 rpm, and the vacuum degree in the vacuum devolatilization section is -0.08 MPa. After the molten material is extruded from the die head, it is cooled to room temperature in a 20°C water cooling tank and then fed into a pelletizer to cut it into cylindrical pellets with a particle size of 3-4 mm and a length of 3-5 mm.

[0076] S3: Single-screw wire drawing forming

[0077] The granules obtained in step S2 were dried at 90°C and a vacuum of -0.09 MPa for 6 hours to reduce the moisture content to 0.015 wt%. The dried granules were then fed into a single-screw extruder. The temperatures of the single-screw extruder were set as follows: feeding section 185°C, compression section 195°C, homogenization section 205°C, and die head 205°C. The screw speed was 30 rpm, and the molten material was drawn into filaments through a circular die with a diameter of 1.75 mm. After being cooled in a 25°C water bath and then by air cooling at room temperature, the filament diameter was monitored online using a laser diameter gauge (accuracy ±0.001 mm). When the filament diameter deviation exceeded ±0.005 mm, the traction speed was automatically adjusted. The traction and winding speed was 80 m / min, and the winding tension was 1 N, resulting in foamed carbon fiber reinforced PLA consumables with a filament diameter of 1.75 ± 0.02 mm.

[0078] (3) 3D printing and post-processing:

[0079] The prepared filament was vacuum dried at 70°C for 4 hours before being used for FDM 3D printing. The printing equipment was a Raise3DPro2, with the following parameters: nozzle temperature 240°C, heated bed temperature 60°C, printing speed 40 mm / s, layer height 0.2 mm, extrusion ratio 0.5, and infill density 25%. The cavity cooling fan was turned off during printing. After printing, the sample was annealed in an 80°C oven for 8 hours.

[0080] (4) Performance test results:

[0081] Performance indicators Test methods Test Results density GB / T 1033.1-2008 0.68g / cm³ Tensile strength GB / T 1040.2-2006 65MPa Flexural modulus GB / T 9341-2008 4.2 GPa Impact strength (notch in a simply supported beam) GB / T 1043.1-2008 9.5 kJ / m² Heat distortion temperature (0.45 MPa) GB / T 1634.2-2004 72°C Average diameter of bubbles SEM image analysis 5μm weight loss rate Compared to pure PLA 45.2%

[0082] Example 2: PETG-based foamed carbon fiber reinforced composite material consumables (PETG-CF-EM)

[0083] In this embodiment, polyethylene terephthalate-1,4-cyclohexanediethanol ester (PETG) is used as the matrix resin and expandable microspheres are used as the foaming agent to prepare foamed carbon fiber reinforced composite material consumables.

[0084] (1) Formulation composition (by mass percentage):

[0085] Components Content (wt%) PETG 76% Short-cut carbon fiber (150μm) 15% Expandable microspheres (Expancel 930DU40) 4% γ-glycidyl oxypropyltrimethoxysilane (KH560) 2.5% Ethylene bis-stearamide (EBS) 1.5% Antioxidant 1010 0.3% Antioxidant 168 0.2% Titanate coupling agents (dispersants) 0.5% total 100%

[0086] (2) Preparation method:

[0087] S1: Preparation of carbon fiber predispersed masterbatch

[0088] 1.2 kg of chopped carbon fiber, 2.0 kg of PETG, and 0.05 kg of titanate coupling agent were added to an internal mixer and mixed for 18 minutes at 175°C and 55 rpm. After mixing, the material was cooled and crushed to obtain carbon fiber pre-dispersion masterbatch (carbon fiber content approximately 36.4%).

[0089] S2: Twin-screw extrusion granulation

[0090] 5.6 kg of PETG, 0.4 kg of expandable microspheres, 0.25 kg of KH560, 0.15 kg of EBS, 0.03 kg of antioxidant 1010, 0.02 kg of antioxidant 168, and 3.25 kg of carbon fiber pre-dispersed masterbatch obtained in step S1 were added to a high-speed mixer and mixed for 6 minutes at 1100 rpm. The premix was then fed into a twin-screw extruder with the following temperature settings: feeding section 170°C, compression section 185°C, homogenization section 195°C, die head 205°C, screw speed 110 rpm, and vacuum degree -0.07 MPa. The extrudate was water-cooled and pelletized to obtain composite material granules.

[0091] S3: Single-screw wire drawing forming

[0092] The granules were dried at 85°C and a vacuum of -0.085 MPa for 7 hours. The dried granules were then fed into a single-screw extruder with the following temperatures set: feeding section 190°C, compression section 200°C, homogenization section 208°C, die head 208°C, and screw speed 35 rpm. The filaments were drawn through a 1.75 mm diameter die, and after water cooling, air cooling, laser diameter measurement, and traction winding (speed 100 m / min, tension 1.2 N), finished consumables with a filament diameter of 1.75 ± 0.015 mm were obtained.

[0093] (3) 3D printing and post-processing:

[0094] The printing equipment was an Ultimaker S5, and the printing parameters were: nozzle temperature 245°C, heated bed temperature 65°C, printing speed 35mm / s, layer height 0.15mm, extrusion ratio 0.45, and filling density 30%. After printing, the sample was annealed in a 90°C oven for 10 hours.

[0095] (4) Performance test results:

[0096] Performance indicators Test methods Test Results density GB / T 1033.1-2008 0.58g / cm³ Tensile strength GB / T 1040.2-2006 62MPa Flexural modulus GB / T 9341-2008 3.5GPa Impact strength (notch in a simply supported beam) GB / T 1043.1-2008 12.5 kJ / m² Heat distortion temperature (0.45 MPa) GB / T 1634.2-2004 90°C Average diameter of bubbles SEM image analysis 5μm weight loss rate Compared to pure PETG 54.3%

[0097] Example 3: TPU-based foamed carbon fiber reinforced composite material consumables (TPU-CF-OBSH)

[0098] In this embodiment, thermoplastic polyurethane (TPU) is used as the matrix resin and 4,4'-oxobisbenzenesulfonyl hydrazine (OBSH) is used as the foaming agent to prepare foamed carbon fiber reinforced composite consumables with excellent flexibility.

[0099] (1) Formulation composition (by mass percentage):

[0100] Components Content (wt%) TPU 85% Short-cut carbon fiber (120μm) 9% OBSH 2% γ-aminopropyltriethoxysilane (KH550) 1.5% Zinc stearate 0.8% Antioxidant 1010 0.2% Antioxidant 168 0.1% Aluminate coupling agents (dispersants) 0.4% Polyethylene wax 0.5% stearic acid 0.5% total 100%

[0101] (2) Preparation method:

[0102] S1: Preparation of carbon fiber predispersed masterbatch

[0103] 0.8 kg of chopped carbon fibers (120 μm in length), 1.5 kg of TPU, and 0.04 kg of aluminate coupling agent were added to an internal mixer and mixed for 12 minutes at 165°C and 45 rpm. TPU has a narrow processing temperature window and requires mixing at a lower temperature to prevent degradation. After mixing, the material was cooled and crushed to obtain carbon fiber pre-dispersion masterbatch (carbon fiber content approximately 33.9%).

[0104] S2: Twin-screw extrusion granulation

[0105] 6.55 kg TPU, 0.2 kg OBSH, 0.15 kg KH550, 0.08 kg zinc stearate, 0.02 kg antioxidant 1010, 0.01 kg antioxidant 168, 0.05 kg polyethylene wax, 0.05 kg stearic acid, and 2.34 kg carbon fiber pre-dispersion masterbatch obtained in step S1 were added to a high-speed mixer and mixed for 10 minutes at 900 rpm. The premix was then fed into a twin-screw extruder with the following temperatures set: feeding section 165°C, compression section 175°C, homogenization section 185°C, and die head 195°C; screw speed 90 rpm; and vacuum degree -0.06 MPa.

[0106] Because TPU is sensitive to moisture, vacuum devolatilization in twin-screw extruders is particularly important. At a vacuum level of -0.06 MPa, moisture and water vapor generated from OBSH decomposition in the TPU are effectively removed, preventing foaming and degradation of the extrudate.

[0107] S3: Single-screw wire drawing forming

[0108] The granules were dried for 8 hours at 80°C and a vacuum of -0.09MPa. Due to the high hygroscopicity of TPU, thorough drying is crucial for ensuring the quality of the filaments. The dried granules were fed into a single-screw extruder with the following temperature settings: feeding section 180°C, compression section 190°C, homogenization section 200°C, die head 200°C, and screw speed 25 rpm. Because TPU has low melt viscosity and good flowability, the screw speed is lower than that of PLA and PETG systems. The filaments were drawn through a 1.75mm diameter die, cooled in a 30°C water bath, cooled to room temperature by air, laser diameter measurement, and traction winding (speed 60m / min, tension 0.8N) to obtain finished consumables with a filament diameter of 1.75±0.018mm.

[0109] (3) 3D printing and post-processing:

[0110] The printing equipment was a Prusa i3 MK3S+, and the printing parameters were: nozzle temperature 235°C, heated bed temperature 55°C, printing speed 30mm / s, layer height 0.2mm, extrusion ratio 0.55, and infill density 20%. After printing, the sample was annealed in a 70°C oven for 12 hours.

[0111] (4) Performance test results:

[0112] Performance indicators Test methods Test Results density GB / T 1033.1-2008 0.75g / cm³ Tensile strength GB / T 1040.2-2006 48MPa Elongation at break GB / T 1040.2-2006 85% Flexural modulus GB / T 9341-2008 0.22 GPa Impact strength (notch in a simply supported beam) GB / T 1043.1-2008 28kJ / m² Shore hardness GB / T 2411-2008 82A Average diameter of bubbles SEM image analysis 5μm weight loss rate Compared to pure TPU 33.0%

[0113] Comparative Example 1: Pure PLA foam consumables (without carbon fiber)

[0114] To illustrate the effect of carbon fiber on the material properties of the present invention, Comparative Example 1 was set up. The formulation of Comparative Example 1 was the same as that of Example 1, but short-cut carbon fiber and KH550 were not added. The mass percentages of each component were adjusted as follows: PLA 88.5%, AC 3%, zinc stearate 1%, antioxidant 1010 0.2%, antioxidant 168 0.1%, polyethylene wax 0.7%, and stearic acid 0.5%.

[0115] The preparation method is the same as steps S2 and S3 of Example 1 (step S1 is not required). The 3D printing parameters are the same as those of Example 1.

[0116] Performance test results: density 0.52 g / cm³, tensile strength 28 MPa, flexural modulus 1.5 GPa, impact strength 2.1 kJ / m², heat distortion temperature 45°C, average cell diameter 50 μm.

[0117] Compared to Example 1, Comparative Example 1 has a lower density (0.52 vs 0.68 g / cm³), but its mechanical properties are significantly reduced—the tensile strength is only 35.5% of that of Example 1, the flexural modulus is only 34.2%, and the heat distortion temperature is reduced by 46°C. Meanwhile, the average cell diameter of Comparative Example 1 (50 μm) is 10 times that of Example 1 (5 μm), and the cell structure is coarse and uneven. This comparison fully demonstrates the dual role of carbon fiber in this invention: firstly, as a reinforcement to improve mechanical properties, and secondly, as a heterogeneous nucleating agent to refine the cell structure.

[0118] Comparative Example 2: Pure carbon fiber reinforced PLA consumables (without foaming agent)

[0119] Comparative Example 2 was set up to illustrate the effect of foaming on the density of the material of the present invention. The formulation of Comparative Example 2 was the same as that of Example 1, but AC foaming agent was not added, the PLA content was adjusted to 81.5%, and the contents of the other components remained unchanged.

[0120] The preparation method is basically the same as in Example 1, but vacuum devolatilization is not required during the twin-screw extrusion process. The 3D printing parameters are: nozzle temperature 220°C, heated bed temperature 60°C, printing speed 50 mm / s, layer height 0.2 mm, extrusion ratio 0.95, and infill density 100%.

[0121] Performance test results: density 1.32 g / cm³, tensile strength 82 MPa, flexural modulus 5.8 GPa, impact strength 5.8 kJ / m², heat distortion temperature 68°C.

[0122] Compared to Example 1, Comparative Example 2 has slightly higher mechanical properties, but its density is as high as 1.32 g / cm³, resulting in no weight reduction. Example 1, while maintaining 72.9% of the tensile strength and 73.1% of the flexural modulus of Comparative Example 2, achieved a significant weight reduction of 45.2%, demonstrating a significant overall performance advantage.

[0123] Comparative Example 3: PLA-CF-AC consumables without the use of carbon fiber pre-dispersion masterbatch

[0124] Comparative Example 3 was set up to illustrate the importance of carbon fiber pre-dispersion masterbatch technology. The formulation of Comparative Example 3 was exactly the same as that of Example 1, but the preparation method was different: instead of the internal mixing and pre-dispersion in step S1, all raw materials were directly fed into a high-speed mixer and then fed into a twin-screw extruder.

[0125] Performance test results: density 0.72 g / cm³, tensile strength 45 MPa, flexural modulus 2.8 GPa, impact strength 4.5 kJ / m², heat distortion temperature 58°C.

[0126] Compared to Example 1, all mechanical properties of Comparative Example 3 decreased significantly. This is because the undispersed carbon fibers were unevenly dispersed in the twin-screw extruder, forming numerous agglomerates. These agglomerates not only weakened the reinforcing effect but also became stress concentration points, reducing the material's strength and toughness. This comparative example demonstrates the crucial role of carbon fiber pre-dispersion masterbatch technology in ensuring the uniformity and stability of material properties.

[0127] Interpretation of the attached diagram

[0128] Figure 1 The image shows the SEM morphology of a cross-section of a foamed carbon fiber reinforced composite material. The black lines / rod-like structures in the image represent carbon fibers (CF), while the porous network structure and micropores represent the cell structure formed inside the foamed matrix.

[0129] Figure 2 These are SEM comparison images of carbon fiber before and after surface modification. Figure 2 (a) shows the surface of the unmodified carbon fiber. Figure 2 (b) shows the surface of carbon fiber modified with KH560, with the etched pits and adhesive coating layer formed on the surface clearly marked.

[0130] Figures 3 to 7 The comparison results of different materials in various properties are shown. The meanings of the bar charts are consistent: gray (solid color) bars represent pure matrix resin, dark gray bars represent carbon fiber reinforced composite materials, light gray bars represent foamed lightweight materials, and red bars represent the foamed and carbon fiber co-reinforced composite materials provided by this invention. Specifically, Figure 3 This is a comparison chart of the tensile strength of different materials. Figure 4 A comparison chart of the flexural modulus of different materials. Figure 5 This is a comparison chart of the notched impact strength of different materials. Figure 6 A comparison chart of the heat distortion temperatures of different materials. Figure 7 This is a comparison of the surface roughness of 3D printed parts under a layer height of 0.2mm.

[0131] Figure 8 This is a schematic diagram showing the control of pore structure and the distribution of bubble size. Figure 8 (a) shows the relationship between porosity and density reduction rate under different carbon fiber contents. The green shaded area marks the optimal porosity range of 30% to 55%, and the red diamond-shaped line represents the optimal carbon fiber content of 10 wt%. Figure 8(b) shows a comparison of cell size distribution. The gray circular broken line indicates that the median cell size is about 50 μm without carbon fiber. The red diamond broken line indicates that after adding 10 wt% carbon fiber, the median cell size is refined to about 5 μm (about 10 times) through heterogeneous nucleation effect. The figure is further divided into three regions: micropores (< 10 μm), mesopores (10~100 μm), and macropores (> 100 μm).

[0132] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A foamed carbon fiber reinforced composite material consumable for 3D printing, characterized by, By weight percentage, it includes the following components; Thermoplastic matrix resin 72-85%; Short-cut carbon fiber 5-15%; Foaming agent 1-5%; Interface modifier 0.5-3%; Processing aids 0.5-5%; The thermoplastic matrix resin is selected from one or more of polylactic acid, polyethylene terephthalate-1,4-cyclohexanediol ester, or thermoplastic polyurethane. The length of the chopped carbon fiber is 100-200 μm; The foaming agent is selected from one or more of azodicarbonamide, 4,4'-oxobisbenzenesulfonylhydrazine, or expandable microspheres; The interface modifier is a silane coupling agent selected from γ-aminopropyltriethoxysilane or γ-glycidoxypropyltrimethoxysilane. The processing aids include lubricants, antioxidants, and dispersants.

2. The foamed carbon fiber reinforced composite material consumable for 3D printing according to claim 1, characterized in that, The thermoplastic matrix resin is polylactic acid having a relative molecular weight of 8 x 10 4 -1.5 x 10 5 a melt index of 5-15 g / 10 min under test conditions of 190°C / 2.16 kg.

3. The foamed carbon fiber reinforced composite material consumable for 3D printing according to claim 1, characterized by, The chopped carbon fibers have a length of 120-180 μm and a diameter of 5-7 μm.

4. The foamed carbon fiber reinforced composite material consumable for 3D printing according to claim 1, characterized by, The foaming agent is azodicarbonamide, with a particle size of 5-15 μm, a decomposition temperature of 140-220°C, and a gas generation rate of 220-250 mL / g.

5. The foamed carbon fiber reinforced composite material consumable for 3D printing according to claim 1, characterized in that, The foaming agent is an expandable microsphere with a shell made of thermoplastic acrylic copolymer and a core material made of isobutane. The initial expansion temperature is 140-180°C and the maximum expansion temperature is 180-220°C.

6. The foamed carbon fiber reinforced composite material consumable for 3D printing according to claim 1, characterized in that, The silane coupling agent is γ-aminopropyl triethoxysilane, which has a molecular weight of 221.37 and a density of 0.940-0.950 g / cm 3 .

7. The foamed carbon fiber reinforced composite material consumable for 3D printing according to claim 1, characterized in that, The lubricant is selected from one or more of zinc stearate, polyethylene wax, or ethylene bis-stearamide, and the dosage is 0.3-2%; the antioxidant is selected from one or more of antioxidant 1010, antioxidant 168, or antioxidant 1098, and the dosage is 0.1-1%; the dispersant is selected from one or more of stearic acid, titanate coupling agent, or aluminate coupling agent, and the dosage is 0.1-2%.

8. The foamed carbon fiber reinforced composite material consumable for 3D printing according to claim 1, characterized in that, The mass ratio of the foaming agent to the short-cut carbon fiber is 1:3 to 1:5 to refine the cell structure by using the carbon fiber as a heterogeneous nucleating agent in the foaming process, the average cell diameter is 5-15 μm, and the cell density is 1 x 10 8 -5 x 10 9 cm-3.

9. The foamed carbon fiber reinforced composite material consumable for 3D printing according to claim 1, characterized in that, The consumable has a filament diameter of 1.75±0.02mm or 2.85±0.02mm, an ellipticity of no more than 0.01mm, and a moisture content of no more than 0.02wt%, and is suitable for fused deposition modeling 3D printing.

10. The foamed carbon fiber reinforced composite material consumable for 3D printing according to claim 1, characterized in that, The consumable material has a density of 0.50-0.85 g / cm³, a tensile strength of 45-75 MPa, and a flexural modulus of 2.5-4.5 GPa.

11. A method for preparing a foamed carbon fiber reinforced composite material consumable for 3D printing as described in any one of claims 1-10, characterized in that, Includes the following steps: S1. Preparation of carbon fiber predispersed masterbatch: Short carbon fibers, a portion of thermoplastic matrix resin and dispersant are added into an internal mixer at a mass ratio of (5-15):(10-20):(0.1-1). The mixture is then internally mixed for 10-20 minutes at 160-180°C and 40-60 rpm to uniformly disperse the carbon fibers in the matrix resin. After crushing, carbon fiber predispersed masterbatch is obtained. S2: Twin-screw extrusion granulation—The remaining thermoplastic matrix resin, foaming agent, interface modifier, processing aid, and carbon fiber pre-dispersion masterbatch obtained in step S1 are added to a high-speed mixer according to the formula ratio and mixed for 5-10 minutes at a speed of 800-1200 rpm to obtain a premix; the premix is ​​fed into a twin-screw extruder and melt-extruded at a temperature of 160-220°C, a screw speed of 80-120 rpm, and a vacuum degree of -0.06 to -0.09 MPa. After water cooling and pelletizing, composite material granules are obtained. S3: Single-screw filament forming—The composite material granules obtained in step S2 are vacuum dried at 80-100°C for 4-8 hours to reduce the moisture content to below 0.02wt%; the dried granules are fed into a single-screw extruder and melt-extruded at a temperature of 180-210°C and a screw speed of 20-40rpm. The filaments are drawn out through a circular die with a diameter of 1.75mm or 2.85mm, cooled by a primary water bath at 20-30°C, followed by a secondary air cooling at room temperature, laser online diameter measurement, and traction winding to obtain the foamed carbon fiber reinforced composite material consumable for 3D printing.

12. A printing method using the foamed carbon fiber reinforced composite material consumable for 3D printing according to any one of claims 1-10, characterized in that, The process employs fused deposition modeling (FDM) with the following parameters: nozzle temperature 10-30°C higher than the initial decomposition or initial expansion temperature of the foaming agent; hot bed temperature 50-70°C; printing speed 30-50 mm / s; layer height 0.1-0.3 mm; extrusion ratio 0.4-0.6; filler density 15-40%; and annealing treatment at 60-100°C for 6-12 hours after printing. During printing, the cooling fan of the printing chamber is turned off or its speed is kept below 30% to maintain the melt temperature and pressure required for foaming.