A long-chain carbon chain nylon abrasion-resistant cable sheath and its preparation method

By modifying zirconium phosphate with long-chain amino compounds, using modified boron nitride and aramid fiber as a compound modifier, and combining various nylon materials with segmented temperature control processes, the wear resistance and mechanical properties of long-chain nylon cable sheaths under heavy-load friction and bending conditions were solved, achieving uniform stability and high wear resistance of the material.

CN123107344APending Publication Date: 2026-11-17GUANGZHOU ZHUJIANG CABLE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611182693.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-05
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing long-chain nylon cable sheaths are prone to peeling and powdering under heavy-load friction and repeated bending conditions, rapid decline in mechanical properties, and easy cracking. Furthermore, the inorganic fillers are unevenly dispersed and have poor interfacial compatibility, resulting in uneven wear resistance.

Method used

Long-chain amino compounds are used to modify zirconium phosphate, modified boron nitride and aramid fiber as modified wear-resistant additives to form a reinforcing system of lamellar filler lubrication and fiber toughening. Combined with nylon 12, nylon 1012 and nylon 1212 as matrix, long carbon chain nylon cable sheath is prepared by segmented temperature control process and graded mixing.

Benefits of technology

It significantly improves the wear resistance and mechanical properties of the cable sheath, enhances the interfacial bonding strength, and increases the service life and structural stability of the cable sheath.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention belongs to the field of nylon material technology, specifically relating to a long-chain nylon wear-resistant cable sheath and its preparation method. The long-chain nylon wear-resistant cable sheath provided by this invention comprises nylon, modified wear-resistant additives, plasticizers, chain extenders, antioxidants, and lubricants; the modified wear-resistant additives are long-chain amino compound-modified zirconium phosphate, modified boron nitride, and aramid fibers. This invention uses a compound system of long-chain amino-modified zirconium phosphate, modified boron nitride, and chopped aramid fibers as modified wear-resistant additives, significantly improving the wear resistance, durability, and structural stability of the material; through 11-aminoundecanoic acid intercalation modification of zirconium phosphate and in-situ coating of long-chain nylon with boron nitride, the defects of inorganic filler agglomeration and poor interfacial compatibility are thoroughly improved; using nylon 12, nylon 1012, and nylon 1212 as the long-chain nylon matrix, it balances low water absorption, high toughness, high hardness, and deformation resistance, achieving uniform and stable mechanical properties of the cable sheath.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nylon material technology, specifically relating to a long carbon chain nylon wear-resistant cable sheath and its preparation method. Background Technology

[0002] Cable sheaths are the core protective structure of cable products, primarily responsible for insulation, mechanical protection, weather resistance, and resistance to external corrosion. Their material properties directly determine the cable's service life, operational stability, and applicable application range. Currently, the mainstream cable sheath materials on the market are PVC, polyurethane, and short-chain nylon (PA6, PA66). Among them, short-chain nylon PA6 and PA66, due to their excellent mechanical strength and processing performance, have become commonly used modified base materials for cable sheaths. However, these short-chain polyamide materials have high amide group density and strong polarity in their molecular chains, resulting in inherent defects such as high water absorption and poor dimensional stability. After absorbing water, they are prone to volume expansion and increased internal stress, significantly reducing the sheath's wear resistance and bending resistance. Long-term use can easily lead to deformation, peeling, wear, and breakage, seriously affecting the safe operation of the cable.

[0003] Long-chain nylon, as a novel polyamide material, contains a long-chain alkyl structure with more than ten carbon atoms in its molecular structure, resulting in a significantly reduced density of amide groups. Compared to short-chain nylon, it possesses advantages such as low water absorption, high toughness, excellent low-temperature weather resistance, and dimensional stability, making it highly promising for applications in the field of wear-resistant protective materials. While some existing technologies have explored the application of long-chain nylon in cable sheaths, current long-chain nylon sheath formulations and preparation processes still exhibit significant technical shortcomings: pure long-chain nylon itself has limited wear resistance, and a single substrate is difficult to adapt to the harsh conditions of high-intensity, high-frequency friction; conventional modified systems suffer from uneven filler dispersion and poor interfacial compatibility, easily leading to uneven mechanical properties, decreased toughness, and problems such as sheath cracking and rapid degradation of wear resistance.

[0004] Chinese patent application CN122325971A discloses a nylon cable sheath material. The formulation includes nylon, plasticizer, modified wear-resistant agent, chain extender, antioxidant, light stabilizer, lubricant and other components. The nylon is one or more of nylon 1012, nylon 11, nylon 12 and nylon 1212. The modified wear-resistant agent is one or more of tin disulfide, zinc disulfide, molybdenum disulfide, graphite and silicon carbide that have been surface-hydroxylated. The hydroxylation modification method of the modified wear-resistant agent is: using a 10%-20% sodium hydroxide solution and heating for a short time at 50-80℃ to hydroxylate and modify the wear-resistant powder. However, in the scheme disclosed in the application document, strong alkali modification can only achieve weak hydroxyl activation on the powder surface, resulting in a low degree of modification. The interfacial bonding force between the powder and the nylon matrix is ​​only slightly improved, and powder is prone to falling off and peeling during friction, resulting in poor wear resistance and durability. Moreover, the modification process is a single chemical modification without coupling agent-assisted modification or ultrasonic dispersion treatment, making the powder extremely prone to agglomeration. The agglomeration of a small amount of added wear-resistant additives will form internal defects in the material, which will reduce the mechanical strength and wear resistance of the sheath. Summary of the Invention

[0005] In order to solve the technical problems of poor wear resistance and uneven mechanical properties in the prior art, the purpose of this invention is to provide a long carbon chain nylon wear-resistant cable sheath and its preparation method.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows:

[0007] A long-chain carbon nylon abrasion-resistant cable sheath comprises the following components in parts by weight: The composition includes 80-100 parts nylon, 4-10 parts modified wear-resistant additives, 8-13 parts plasticizer, 2-5 parts chain extender, 1-3 parts antioxidant, and 0.5-1.5 parts lubricant; the modified wear-resistant additives are long-chain amino compounds modified zirconium phosphate, modified boron nitride, and aramid fiber.

[0008] This invention employs a composite system of long-chain amino compounds modified zirconium phosphate, modified boron nitride, and aramid fibers as a modified wear-resistant additive to replace single inorganic wear-resistant fillers. Addressing the problems of peeling, powdering, rapid mechanical property degradation, and cracking in long-chain nylon cable sheaths under harsh conditions such as heavy-load friction and repeated bending, this invention forms a layered filler lubrication, wear resistance, and fiber toughening reinforcement system, effectively improving the wear resistance and mechanical properties of the nylon cable sheath. Furthermore, this invention adds plasticizers, chain extenders, antioxidants, and lubricants to the formula, which can effectively improve the flexibility of the cable sheath, strengthen interfacial bonding strength, and extend the service life of the cable sheath.

[0009] Furthermore, the modified wear-resistant additive is composed of long-chain amino compound modified zirconium phosphate, modified boron nitride and aramid fiber in a mass ratio of (10-15):(3-7):1; the average length of the aramid fiber is 0.2-1 mm.

[0010] This invention utilizes aramid fibers to form a three-dimensional network structure within the cable sheath. This network bears the shear stress transmitted from the friction surface, preventing the propagation of microcracks caused by wear, and improving structural integrity during scratching, tearing, and repeated bending. However, if the aramid fiber content exceeds the aforementioned range, fibers will float to the surface of the cable sheath, reducing the bending performance of small-diameter cables. Using aramid fibers within the aforementioned size range allows for uniform dispersion and interlocking within the matrix to form a dense micro-network. This effectively prevents the propagation of friction cracks, improves bending fatigue resistance, and is perfectly compatible with high-speed extrusion processes for cable sheaths, resulting in no die blockage, no agglomeration, and excellent molded appearance.

[0011] Further, the preparation method of the long-chain amino compound modified zirconium phosphate is as follows: zirconium oxychloride is added to deionized water, stirred and dissolved to prepare a zirconium oxychloride solution with a mass fraction of 10%-15%. Concentrated phosphoric acid solution is added dropwise under stirring, controlling the molar ratio of Zr / P to be 1:(6-8). After the addition is completed, the mixture is stirred for 30-60 min, allowed to stand, the supernatant is removed, and the mixture is washed to obtain zirconium phosphate gel. The zirconium phosphate gel is dispersed in concentrated phosphoric acid solution to form a suspension, heated to 95-105℃ and refluxed for 24 h. After cooling, the mixture is centrifuged to separate the solid crystals, which are then washed and dried to obtain α-zirconium phosphate crystal powder. The α-zirconium phosphate crystal powder is dispersed in an ethanol aqueous solution to form a dispersion with a mass concentration of 6%-10%. 11-aminoundecanoic acid is added, and the mixture is heated to 60-85℃ and stirred for 6-10 h. After filtration, washing, drying, and pulverization, long-chain amino compound modified zirconium phosphate is obtained.

[0012] This invention uses soluble zirconium salt and concentrated phosphoric acid as raw materials to prepare layered α-zirconium phosphate crystal powder via a reflux method. Then, 11-aminoundecanoic acid is used to intercalate and modify the α-zirconium phosphate crystals, increasing the interlayer spacing and enhancing its interlayer slip characteristics. When the cable sheath is subjected to friction and bending forces, the interlayer slip consumes frictional energy, improving the wear resistance of the cable sheath. α-Zirconium phosphate possesses a layered structure, high thermal stability, and electrical insulation. Intercalation with long-chain amino compounds and organic treatment of its surface reduce the agglomeration tendency of inorganic layers in long-chain nylon, improving the dispersibility of α-zirconium phosphate in the matrix. The amino group at one end of 11-aminoundecanoic acid can interact ionicly with the acidic sites on the zirconium phosphate layer, while its long methylene chain facilitates van der Waals interactions with the long-chain structure of the nylon matrix, significantly improving the bonding strength between α-zirconium phosphate and the nylon matrix interface.

[0013] Furthermore, in the preparation method of long-chain amino compound modified zirconium phosphate, the mass percentage of concentrated phosphoric acid solution is 85%, and the amount of 11-aminoundecanoic acid used is 15%-25% of the mass of α-zirconium phosphate crystal powder.

[0014] Further, the preparation method of the modified boron nitride is as follows: Boron nitride powder is dispersed in an aqueous sodium hydroxide solution, heated to 120-130℃ and reacted for 2-2.5 h, cooled, filtered, washed, and dried to obtain activated boron nitride; activated boron nitride is dispersed in anhydrous ethanol to prepare a suspension with a mass fraction of 8%-10%, γ-aminopropyltriethoxysilane is added, stirred evenly, heated to 70-80℃ and stirred for 1-2 h, centrifuged, washed, and dried to obtain amino-activated boron nitride; Nylon 12 is mixed with anhydrous ethanol, heated to 130-140℃ for swelling and pyrolysis for 2.5-3 h, amino-activated boron nitride is added, stirred evenly, heated to 120-130℃ and stirred for 2-3 h, cooled, filtered, dried, and pulverized to obtain modified boron nitride.

[0015] In this invention, boron nitride is activated by hydroxyl groups and modified at the interface with a silane coupling agent. Then, long-chain nylon oligomers are used to in-situ graft boron nitride onto the boron nitride particles, forming a nylon coating layer completely homologous to the matrix, thus improving the compatibility between boron nitride and the nylon matrix. Furthermore, boron nitride itself has a layered structure, which can form a low-shear slip layer on the friction surface of the sheath, reducing the coefficient of friction and adhesive wear, and improving the wear resistance of the sheath.

[0016] Furthermore, in the preparation method of modified boron nitride, the boron nitride has a particle size of 200-400 nm, the sodium hydroxide aqueous solution has a mass percentage of 15%-20%, the amount of γ-aminopropyltriethoxysilane is 5%-10% of the boron nitride powder mass, and the amount of nylon 12 is 3-5 times the boron nitride powder mass.

[0017] Furthermore, the nylon is composed of nylon 12, nylon 1012 and nylon 1212 in a mass ratio of (3-7):(2-5):1.

[0018] In this invention, nylon 12, nylon 1012 and nylon 1212 are used to form the nylon matrix. Nylon 12 is used to provide low water absorption, flexibility, low temperature resistance and extrusion processing performance; nylon 1012 is used to improve the strength, hardness and wear resistance of the sheath material; and nylon 1212 has high hardness, high wear resistance and high deformation resistance. The dual matrix composite makes up for the defects of low hardness and insufficient heavy-load wear resistance of nylon 12 alone, while retaining the advantages of low water absorption and high dimensional stability of long-chain nylon, thus achieving a balance between toughness and wear resistance.

[0019] Furthermore, the plasticizer is one or more of N-methylbenzenesulfonamide, N-butylbenzenesulfonamide, phthalate, and triphenyl phosphate; the chain extender is one of carbodiimide, oxazoline, and isocyanate; and the antioxidant is one or more of antioxidant 1010, antioxidant 1076, antioxidant 1098, 2,6-di-tert-butyl-4-methylphenol, and antioxidant 168.

[0020] Furthermore, the lubricant is one of polyethylene wax, calcium stearate, and silicone powder.

[0021] The present invention also provides a method for preparing the long carbon chain nylon abrasion-resistant cable sheath, comprising the following steps: S1: Dry the nylon at 80-90℃ for 4-5 hours, then add it together with the plasticizer and lubricant into a high-speed mixer and stir at low speed until uniform to obtain mixture I; S2: Add the modified wear-resistant agent, chain extender, and antioxidant to the mixture I obtained in step S1, heat to 90-100℃, stir evenly, and obtain mixture II; S3: The mixture II obtained in step S2 is fed into a twin-screw extruder and melt-extruded, water-cooled into strands, granulated, and dried using a segmented temperature-controlled process to obtain long-chain nylon granules; wherein the segmented temperature control is as follows: Zone 1 185-190℃, Zone 2 190-195℃, Zone 3 195-200℃, and die head 200-210℃, and the screw speed is 280-320 rpm; S4: The long carbon chain nylon granules obtained in step S3 are fed into a cable sheath extruder and extruded using a segmented constant temperature extrusion process: barrel zone 1 190-195℃, barrel zone 2 195-200℃, barrel zone 3 200-205℃, die temperature 205-210℃, screw speed 250-300rpm, constant temperature setting for 1-2 hours, cooling, and winding to obtain a long carbon chain nylon wear-resistant cable sheath.

[0022] This invention employs a segmented gradient temperature control and graded mixing process, which avoids the problems of uneven crystallization, high internal porosity, and decomposition and failure of additives in traditional processing processes. The product has good batch stability and is suitable for large-scale industrial production, combining technological innovation with mass production practicality.

[0023] Compared with the prior art, the long carbon chain nylon wear-resistant cable sheath and its preparation method provided by the present invention have the following technical advantages: (1) The present invention uses a composite system of long-chain amino-modified zirconium phosphate, modified boron nitride and short-cut aramid fiber as a modified wear-resistant additive, which significantly improves the wear resistance, durability and structural stability of the material; (2) The present invention thoroughly improves the defects of inorganic filler agglomeration and poor interfacial compatibility by intercalating zirconium phosphate with 11-aminoundecanoic acid and coating boron nitride in situ with long carbon chain nylon. (3) In this invention, Nylon 12, Nylon 1012 and Nylon 1212 are used as long carbon chain nylon matrix to take into account low water absorption, high toughness, high hardness and deformation resistance, so as to achieve uniform and stable mechanical properties of cable sheath. Detailed Implementation

[0024] The following description, in conjunction with embodiments, provides further details, but the present invention is not limited to these embodiments. Those skilled in the art can make various modifications based on the fundamental principles of the present invention, but such modifications are all within the scope of the invention as long as they do not depart from its basic principles.

[0025] Preparation Example 1 The preparation method of zirconium phosphate modified by long-chain amino compounds is as follows: 10g of zirconium oxychloride is added to deionized water and stirred to dissolve, thus preparing a 10% zirconium oxychloride solution. A concentrated phosphoric acid solution of 85% (w / w) is slowly added dropwise while stirring, controlling the Zr / P molar ratio to be 1:6. During the dropwise addition, a white flocculent amorphous zirconium phosphate gel gradually forms. After the addition is complete, stirring is continued for 30 minutes to ensure sufficient cross-linking reaction between zirconium oxychloride and phosphoric acid, obtaining a uniform and stable zirconium phosphate gel suspension. The suspension is allowed to settle, the supernatant is removed, and the gel precipitate is repeatedly washed with deionized water. Centrifugation was performed until the washing solution was neutral to remove residual chloride ions and excess phosphoric acid, yielding zirconium phosphate gel. The zirconium phosphate gel was dispersed in 60g of 85% concentrated phosphoric acid solution to form a suspension, heated to 95℃ and refluxed for 24h. After natural cooling to room temperature, the product system was centrifuged to collect the solid crystals, which were repeatedly washed with deionized water until the pH of the washing solution was neutral. The crystals were then dried at 70℃ to obtain α-zirconium phosphate crystal powder. 10g of α-zirconium phosphate crystal powder was dispersed in 60% aqueous ethanol solution to form a 6% dispersion. 1.5g of 11-aminoundecanoic acid was added, and the mixture was heated to 60℃ and stirred for 6h. After filtration, the mixture was washed twice with anhydrous ethanol and deionized water, respectively, and dried under vacuum at 70℃ for 10h. The mixture was then pulverized to obtain long-chain amino compound modified zirconium phosphate.

[0026] Preparation Example 2 The preparation method of zirconium phosphate modified by long-chain amino compounds is as follows: 15g of zirconium oxychloride is added to deionized water and stirred to dissolve, thus preparing a 15% zirconium oxychloride solution. A concentrated phosphoric acid solution of 85% (w / w) is slowly added dropwise while stirring, controlling the Zr / P molar ratio to be 1:8. During the dropwise addition, a white flocculent amorphous zirconium phosphate gel gradually forms. After the addition is complete, stirring is continued for 60 minutes to ensure sufficient cross-linking reaction between zirconium oxychloride and phosphoric acid, obtaining a uniform and stable zirconium phosphate gel suspension. The suspension is allowed to settle, the supernatant is removed, and the gel precipitate is repeatedly washed with deionized water and centrifuged. Separate the zirconium phosphate gel until the washing solution is neutral to remove residual chloride ions and excess phosphoric acid. Disperse the zirconium phosphate gel in 80g of 85% concentrated phosphoric acid solution to form a suspension. Heat the suspension to 105℃ and reflux for 24h. Cool the suspension to room temperature and centrifuge the product system. Collect the solid crystals and wash them repeatedly with deionized water until the pH of the washing solution is neutral. Dry the crystals at 80℃ to obtain α-zirconium phosphate crystal powder. Disperse 10g of α-zirconium phosphate crystal powder in 80% aqueous ethanol solution to form a 10% dispersion. Add 2.5g of 11-aminoundecanoic acid and heat the suspension to 85℃ and stir for 10h. Filter the suspension and wash it three times with anhydrous ethanol and deionized water, respectively. Dry the suspension under vacuum at 80℃ for 12h and pulverize the suspension to obtain long-chain amino compound modified zirconium phosphate.

[0027] Preparation Example 3 The preparation method of zirconium phosphate modified by long-chain amino compounds is as follows: 12g of zirconium oxychloride is added to deionized water and stirred to dissolve, thus preparing a 12% zirconium oxychloride solution. A concentrated phosphoric acid solution of 85% (w / w) is slowly added dropwise while stirring, controlling the Zr / P molar ratio to be 1:7. During the dropwise addition, a white flocculent amorphous zirconium phosphate gel gradually forms. After the addition is complete, stirring is continued for 40 minutes to ensure sufficient cross-linking reaction between zirconium oxychloride and phosphoric acid, obtaining a uniform and stable zirconium phosphate gel suspension. The suspension is allowed to settle, the supernatant is removed, and the gel precipitate is repeatedly washed with deionized water. Centrifugation was performed until the washing solution was neutral to remove residual chloride ions and excess phosphoric acid, yielding zirconium phosphate gel. The zirconium phosphate gel was dispersed in 65g of 85% concentrated phosphoric acid solution to form a suspension, heated to 100℃ and refluxed for 24h, then naturally cooled to room temperature. The product system was centrifuged to collect the solid crystals, which were repeatedly washed with deionized water until the pH of the washing solution was neutral, and dried at 75℃ to obtain α-zirconium phosphate crystal powder. 10g of α-zirconium phosphate crystal powder was dispersed in 70% ethanol aqueous solution to form a 7% dispersion, and 2g of 11-aminoundecanoic acid was added. The mixture was heated to 70℃ and stirred for 7.5h, filtered, washed three times with anhydrous ethanol and deionized water respectively, dried under vacuum at 75℃ for 11h, and pulverized to obtain long-chain amino compound modified zirconium phosphate.

[0028] Preparation Example 4 The preparation method of long-chain amino compound modified zirconium phosphate is as follows: 13.5g of zirconium oxychloride is added to deionized water and stirred to dissolve, preparing a 13% zirconium oxychloride solution. Under stirring, a 85% concentrated phosphoric acid solution is slowly added dropwise, controlling the Zr / P molar ratio to be 1:7.5. During the dropwise addition, a white flocculent amorphous zirconium phosphate gel gradually forms. After the addition is complete, stirring is continued for 50 minutes to ensure sufficient cross-linking reaction between zirconium oxychloride and phosphoric acid, obtaining a uniform and stable zirconium phosphate gel suspension. The suspension is allowed to settle, the supernatant is removed, and the gel precipitate is repeatedly washed with deionized water. Centrifugation was performed until the washing solution was neutral to remove residual chloride ions and excess phosphoric acid, yielding zirconium phosphate gel. The zirconium phosphate gel was dispersed in 72g of 85% concentrated phosphoric acid solution to form a suspension. The mixture was heated to 100℃ and refluxed for 24h. After natural cooling to room temperature, the product system was centrifuged, and the solid crystals were collected. The crystals were repeatedly washed with deionized water until the pH of the washing solution was neutral. The mixture was then dried at 75℃ to obtain α-zirconium phosphate crystal powder. 10g of α-zirconium phosphate crystal powder was dispersed in 70% aqueous ethanol solution to form an 8% dispersion. 2.2g of 11-aminoundecanoic acid was added, and the mixture was heated to 80℃ and stirred for 8h. The mixture was filtered, washed three times with anhydrous ethanol and deionized water, and dried under vacuum at 75℃ for 11h. The mixture was then pulverized to obtain long-chain amino compound modified zirconium phosphate.

[0029] Preparation Example 5 The preparation method of modified boron nitride is as follows: 20g of 200nm boron nitride powder is dispersed in a 15% sodium hydroxide aqueous solution at a solid-liquid mass ratio of 1:20. The mixture is heated to 120℃ and reacted for 2.5h to etch and activate the boron nitride sheets. After the reaction, the mixture is allowed to cool naturally, filtered, and the filter cake is repeatedly washed with deionized water until the washing liquid is neutral. The cake is then dried at 80℃ to obtain activated boron nitride. The activated boron nitride is dispersed in anhydrous ethanol to prepare an 8% suspension, and 1g of [unspecified substance] is added. γ-aminopropyltriethoxysilane was stirred until homogeneous and heated to 70°C for 2 hours to allow covalent grafting of γ-aminopropyltriethoxysilane with the hydroxyl groups on the surface of activated boron nitride, introducing active amino groups onto the surface of activated boron nitride. After the reaction, the mixture was centrifuged, washed twice with anhydrous ethanol, and dried at 80°C to obtain amino-activated boron nitride. 60g of nylon 12 was mixed with 500mL of anhydrous ethanol and heated to 130°C for swelling and pyrolysis for 2.5 hours. Amino-activated boron nitride was added, stirred until homogeneous, and then heated to 120°C for 3 hours to allow long-chain nylon to graft onto the surface of the boron nitride particles. After the reaction, the mixture was cooled to room temperature, filtered to collect the solid product, dried at 80°C, and pulverized to obtain modified boron nitride.

[0030] Preparation Example 6 The preparation method of modified boron nitride is as follows: 20g of 400nm boron nitride powder is dispersed in a 20% sodium hydroxide aqueous solution at a solid-liquid mass ratio of 1:20. The mixture is heated to 130℃ and reacted for 2 hours to etch and activate the boron nitride sheets. After the reaction, the mixture is allowed to cool naturally, filtered, and the filter cake is repeatedly washed with deionized water until the washing liquid is neutral. The cake is then dried at 80℃ to obtain activated boron nitride. The activated boron nitride is dispersed in anhydrous ethanol to prepare a 10% suspension, and 2g of [unspecified substance] is added. γ-aminopropyltriethoxysilane was stirred until homogeneous and heated to 80°C for 1 hour to allow covalent grafting of γ-aminopropyltriethoxysilane with the hydroxyl groups on the surface of activated boron nitride, introducing active amino groups onto the surface of activated boron nitride. After the reaction, the mixture was centrifuged, washed three times with anhydrous ethanol, and dried at 80°C to obtain amino-activated boron nitride. 100g of nylon 12 was mixed with 500mL of anhydrous ethanol and heated to 140°C for swelling and pyrolysis for 2.5 hours. Amino-activated boron nitride was added, stirred until homogeneous, and then heated to 130°C for 2 hours to allow long-chain nylon to graft onto the surface of boron nitride particles. After the reaction, the mixture was cooled to room temperature, filtered to collect the solid product, dried at 80°C, and pulverized to obtain modified boron nitride.

[0031] Preparation Example 7 The modified boron nitride was prepared as follows: 20g of 300nm boron nitride powder was dispersed in a 17% sodium hydroxide aqueous solution at a solid-liquid mass ratio of 1:20. The mixture was heated to 125℃ and reacted for 2.2h to etch and activate the boron nitride layers. After the reaction, the mixture was allowed to cool naturally, filtered, and the filter cake was repeatedly washed with deionized water until the washing liquid was neutral. The cake was then dried at 80℃ to obtain activated boron nitride. The activated boron nitride was dispersed in anhydrous ethanol to prepare a 9% suspension, and 1.5g of the solution was added. γ-aminopropyltriethoxysilane was stirred until homogeneous and heated to 75°C for 1.5 h to allow covalent grafting of γ-aminopropyltriethoxysilane with the hydroxyl groups on the surface of activated boron nitride, introducing active amino groups onto the surface of activated boron nitride. After the reaction, the mixture was centrifuged, washed three times with anhydrous ethanol, and dried at 80°C to obtain amino-activated boron nitride. 80 g of nylon 12 was mixed with 500 mL of anhydrous ethanol and heated to 135°C for swelling and pyrolysis for 2.8 h. Amino-activated boron nitride was added, stirred until homogeneous, and then heated to 125°C for 2.5 h to allow long-chain nylon to graft onto the surface of the boron nitride particles. After the reaction, the mixture was cooled to room temperature, filtered to collect the solid product, dried at 80°C, and pulverized to obtain modified boron nitride.

[0032] Preparation Example 8 The modified boron nitride was prepared as follows: 20g of 300nm boron nitride powder was dispersed in an 18% sodium hydroxide aqueous solution at a solid-liquid mass ratio of 1:20. The mixture was heated to 125℃ and reacted for 2.3h to etch and activate the boron nitride layers. After the reaction, the mixture was allowed to cool naturally, filtered, and the filter cake was repeatedly washed with deionized water until the washing liquid was neutral. The cake was then dried at 80℃ to obtain activated boron nitride. The activated boron nitride was dispersed in anhydrous ethanol to prepare a 9% suspension, and 1.7g of the solution was added. γ-aminopropyltriethoxysilane was stirred until homogeneous and heated to 75°C for 1.8 h to allow covalent grafting of γ-aminopropyltriethoxysilane with the hydroxyl groups on the surface of activated boron nitride, introducing active amino groups onto the surface of activated boron nitride. After the reaction, the mixture was centrifuged, washed three times with anhydrous ethanol, and dried at 80°C to obtain amino-activated boron nitride. 85 g of nylon 12 was mixed with 500 mL of anhydrous ethanol and heated to 135°C for swelling and pyrolysis for 2.8 h. Amino-activated boron nitride was added, stirred until homogeneous, and then heated to 125°C for 2.7 h to allow long-chain nylon to graft onto the surface of the boron nitride particles. After the reaction, the mixture was cooled to room temperature, filtered to collect the solid product, dried at 80°C, and pulverized to obtain modified boron nitride.

[0033] Example 1 A long-chain carbon nylon abrasion-resistant cable sheath comprises the following components in parts by weight: The mixture contained 80g of nylon, 10g of modified wear-resistant additive, 8g of N-methylbenzenesulfonamide, 2g of carbodiimide, 1g of antioxidant 1010, and 0.5g of polyethylene wax. The modified wear-resistant additive was composed of long-chain amino compound modified zirconium phosphate, modified boron nitride, and aramid fiber in a mass ratio of 10:3:1. The average length of the aramid fiber was 0.2mm. The long-chain amino compound modified zirconium phosphate was prepared in Preparation Example 1, and the modified boron nitride was prepared in Preparation Example 5. The nylon was composed of nylon 12, nylon 1012, and nylon 1212 in a mass ratio of 3:2:1.

[0034] The preparation method of long carbon chain nylon abrasion-resistant cable sheath is as follows: S1: Dry the nylon at 80℃ for 5 hours, then add it together with N-methylbenzenesulfonamide and polyethylene wax into a high-speed mixer and stir at low speed until uniform to obtain mixture I; S2: Add modified wear-resistant additive, carbodiimide, and antioxidant 1010 to the mixture I obtained in step S1, heat to 90°C, and stir evenly to obtain mixture II; S3: The mixture II obtained in step S2 is fed into a twin-screw extruder and melt-extruded, water-cooled into strands, granulated, and dried using a segmented temperature-controlled process to obtain long-chain nylon granules; wherein the segmented temperature control is: zone 1 185℃, zone 2 190℃, zone 3 195℃, die head 200℃, and the screw speed is 280 rpm. S4: The long carbon chain nylon granules obtained in step S3 are fed into a cable sheath extruder and extruded using a segmented constant temperature extrusion process: barrel zone 1 190℃, barrel zone 2 195℃, barrel zone 3 200℃, die temperature 205℃, screw speed 250rpm, constant temperature setting for 1 hour, cooling, and winding to obtain a long carbon chain nylon wear-resistant cable sheath.

[0035] Example 2 A long-chain carbon nylon abrasion-resistant cable sheath comprises the following components in parts by weight: The mixture contained 100g of nylon, 4g of modified wear-resistant agent, 13g of N-butylbenzenesulfonamide, 5g of oxazoline, 3g of antioxidant 1076, and 1.5g of calcium stearate. The modified wear-resistant agent was composed of long-chain amino compound modified zirconium phosphate, modified boron nitride, and aramid fiber in a mass ratio of 15:7:1. The average length of the aramid fiber was 1mm. The long-chain amino compound modified zirconium phosphate was prepared in Preparation Example 2, and the modified boron nitride was prepared in Preparation Example 6. The nylon was composed of nylon 12, nylon 1012, and nylon 1212 in a mass ratio of 7:5:1.

[0036] The preparation method of long carbon chain nylon abrasion-resistant cable sheath is as follows: S1: Dry the nylon at 90℃ for 4 hours, then add it together with N-butylbenzenesulfonamide and calcium stearate into a high-speed mixer and stir at low speed until uniform to obtain mixture I; S2: Add modified wear-resistant additive, oxazoline, and antioxidant 1076 to the mixture I obtained in step S1, heat to 100°C, stir evenly, and obtain mixture II; S3: The mixture II obtained in step S2 is fed into a twin-screw extruder and melt-extruded, water-cooled into strands, granulated, and dried using a segmented temperature-controlled process to obtain long-chain nylon granules; wherein the segmented temperature control is: zone 1 190℃, zone 2 195℃, zone 3 200℃, and die head 210℃, and the screw speed is 320 rpm. S4: The long carbon chain nylon granules obtained in step S3 are fed into a cable sheath extruder and extruded using a segmented constant temperature extrusion process: barrel zone 1 195℃, barrel zone 2 200℃, barrel zone 3 205℃, die temperature 210℃, screw speed 300rpm, constant temperature setting for 2 hours, cooling, and winding to obtain a long carbon chain nylon wear-resistant cable sheath.

[0037] Example 3 A long-chain carbon nylon abrasion-resistant cable sheath comprises the following components in parts by weight: The sample contained 90g of nylon, 6g of modified wear-resistant agent, 10g of phthalate, 4g of isocyanate, 2g of antioxidant 1098, and 1g of silicone powder. The modified wear-resistant agent was composed of long-chain amino compound modified zirconium phosphate, modified boron nitride, and aramid fiber in a mass ratio of 12:5:1. The average length of the aramid fiber was 0.6mm. The long-chain amino compound modified zirconium phosphate was prepared in Preparation Example 3, and the modified boron nitride was prepared in Preparation Example 7. The nylon was composed of nylon 12, nylon 1012, and nylon 1212 in a mass ratio of 5:4:1.

[0038] The preparation method of long carbon chain nylon abrasion-resistant cable sheath is as follows: S1: Dry the nylon at 85°C for 4.5 hours, then add it together with phthalate and silicone powder into a high-speed mixer and stir at low speed until uniform to obtain mixture I; S2: Add modified wear-resistant additive, isocyanate, and antioxidant 1098 to the mixture I obtained in step S1, heat to 95°C, and stir evenly to obtain mixture II; S3: The mixture II obtained in step S2 is fed into a twin-screw extruder and melt-extruded, water-cooled into strands, granulated, and dried using a segmented temperature-controlled process to obtain long-chain nylon granules; wherein the segmented temperature control is: zone 1 188℃, zone 2 193℃, zone 3 198℃, die head 205℃, and the screw speed is 300 rpm. S4: The long carbon chain nylon granules obtained in step S3 are fed into a cable sheath extruder and extruded using a segmented constant temperature extrusion process: barrel zone 1 193℃, barrel zone 2 198℃, barrel zone 3 203℃, die temperature 208℃, screw speed 280rpm, constant temperature setting for 1.7h, cooling, and winding to obtain a long carbon chain nylon wear-resistant cable sheath.

[0039] Example 4 A long-chain carbon nylon abrasion-resistant cable sheath comprises the following components in parts by weight: The mixture contained 93g of nylon, 9g of modified wear-resistant agent, 11g of triphenyl phosphate, 4g of carbodiimide, 2g of 2,6-di-tert-butyl-4-methylphenol, and 1.1g of polyethylene wax. The modified wear-resistant agent was composed of long-chain amino compound modified zirconium phosphate, modified boron nitride, and aramid fiber in a mass ratio of 13:6:1. The average length of the aramid fiber was 0.8mm. The long-chain amino compound modified zirconium phosphate was prepared in Preparation Example 4, and the modified boron nitride was prepared in Preparation Example 8. The nylon was composed of nylon 12, nylon 1012, and nylon 1212 in a mass ratio of 6:4:1.

[0040] The preparation method of the long carbon chain nylon wear-resistant cable sheath is the same as in Example 3.

[0041] Comparative Example 1 In this comparative example, the long-chain carbon chain nylon wear-resistant cable sheath and its preparation method are similar to those in Example 4. The difference between this comparative example and Example 4 is that in this comparative example, an equal amount of modified boron nitride is used instead of long-chain amino compound modified zirconium phosphate in the modified wear-resistant additive.

[0042] Comparative Example 2 In this comparative example, the long-chain carbon chain nylon wear-resistant cable sheath and its preparation method are similar to those in Example 4. The difference between this comparative example and Example 4 is that in this comparative example, an equal amount of α-zirconium phosphate crystal powder is used instead of long-chain amino compound modified zirconium phosphate in the modified wear-resistant additive.

[0043] Comparative Example 3 In this comparative example, the long carbon chain nylon wear-resistant cable sheath and its preparation method are similar to those in Example 4. The difference between this comparative example and Example 4 is that an equal amount of boron nitride is used instead of modified boron nitride in the modified wear-resistant additive.

[0044] Comparative Example 4 In this comparative example, the long carbon chain nylon wear-resistant cable sheath and its preparation method are similar to those in Example 4. The difference between this comparative example and Example 4 is that an equal amount of amino-activated boron nitride is used instead of modified boron nitride in the modified wear-resistant additive.

[0045] Comparative Example 5 In this comparative example, the long carbon chain nylon wear-resistant cable sheath and its preparation method are similar to those in Example 4. The difference between this comparative example and Example 4 is that the nylon used in this comparative example is nylon 12.

[0046] Test case Test samples: Long carbon chain nylon abrasion-resistant cable sheaths prepared in Examples 1-4 and Comparative Examples 1-5; Mechanical property testing: tensile properties are tested according to GB / T 1040.2-2022; impact properties are tested according to GB / T 1843-2008; bending properties are tested according to GB / T 9341-2008. Wear resistance test: The wear mass loss of the test sample is tested according to GB / T 5478-2019; The test results are shown in Table 1.

[0047] Table 1

[0048] As shown in Table 1, the long-chain nylon abrasion-resistant cable sheath provided by this invention has an elongation at break of 426%-467%, excellent flexibility, and can meet the requirements of repeated bending of cables. Its impact strength is 14.2-15.7 kJ·m. 2 It has a flexural strength of 33.4-36.5 MPa, moderate rigidity, wear mass loss of less than 10 mg, and excellent wear resistance.

[0049] This specific embodiment is merely an explanation of the present invention and not a limitation thereof. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but as long as they are within the scope of the claims of the present invention, they are protected by patent law.

Claims

1. A long-chain carbon chain nylon wear-resistant cable sheath, characterized in that, The components include the following parts by weight: The composition includes 80-100 parts nylon, 4-10 parts modified wear-resistant additives, 8-13 parts plasticizer, 2-5 parts chain extender, 1-3 parts antioxidant, and 0.5-1.5 parts lubricant; the modified wear-resistant additives are long-chain amino compounds modified zirconium phosphate, modified boron nitride, and aramid fiber.

2. The long carbon chain nylon abrasion-resistant cable sheath according to claim 1, characterized in that, The modified wear-resistant additive is composed of long-chain amino compound modified zirconium phosphate, modified boron nitride and aramid fiber in a mass ratio of (10-15):(3-7):1; the average length of the aramid fiber is 0.2-1 mm.

3. The long carbon chain nylon wear-resistant cable sheath according to claim 1, characterized in that, The preparation method of the long-chain amino compound modified zirconium phosphate is as follows: zirconium oxychloride is added to deionized water and stirred to dissolve, so as to prepare a zirconium oxychloride solution with a mass fraction of 10%-15%. Concentrated phosphoric acid solution is added dropwise under stirring, and the molar ratio of Zr / P is controlled to be 1:(6-8). After the addition is completed, the mixture is stirred for 30-60 min, allowed to stand, the supernatant is removed, and the mixture is washed to obtain zirconium phosphate gel. The zirconium phosphate gel is dispersed in concentrated phosphoric acid solution to form a suspension, heated to 95-105℃ and refluxed for 24 h. After cooling, the mixture is centrifuged to separate the solid crystals, which are then washed and dried to obtain α-zirconium phosphate crystal powder. The α-zirconium phosphate crystal powder is dispersed in an ethanol aqueous solution to form a dispersion with a mass concentration of 6%-10%. 11-aminoundecanoic acid is added, and the mixture is heated to 60-85℃ and stirred for 6-10 h. After filtration, washing, drying, and pulverization, long-chain amino compound modified zirconium phosphate is obtained.

4. The long carbon chain nylon wear-resistant cable sheath according to claim 3, characterized in that, In the preparation method of long-chain amino compound modified zirconium phosphate, the mass percentage of concentrated phosphoric acid solution is 85%, and the amount of 11-aminoundecanoic acid used is 15%-25% of the mass of α-zirconium phosphate crystal powder.

5. The long carbon chain nylon abrasion-resistant cable sheath according to claim 1, characterized in that, The modified boron nitride is prepared as follows: boron nitride powder is dispersed in an aqueous sodium hydroxide solution, heated to 120-130℃ and reacted for 2-2.5 hours, cooled, filtered, washed, and dried to obtain activated boron nitride; activated boron nitride is dispersed in anhydrous ethanol to prepare a suspension with a mass fraction of 8%-10%, γ-aminopropyltriethoxysilane is added, stirred evenly, heated to 70-80℃ and stirred for 1-2 hours, centrifuged, washed, and dried to obtain amino-activated boron nitride; nylon 12 is mixed with anhydrous ethanol, heated to 130-140℃ to swell and decompose for 2.5-3 hours, amino-activated boron nitride is added, stirred evenly, heated to 120-130℃ and stirred for 2-3 hours, cooled, filtered, dried, and pulverized to obtain modified boron nitride.

6. The long carbon chain nylon wear-resistant cable sheath according to claim 5, characterized in that, In the preparation method of modified boron nitride, the boron nitride has a particle size of 200-400 nm, the sodium hydroxide aqueous solution has a mass percentage of 15%-20%, the amount of γ-aminopropyltriethoxysilane is 5%-10% of the boron nitride powder mass, and the amount of nylon 12 is 3-5 times the boron nitride powder mass.

7. The long carbon chain nylon wear-resistant cable sheath according to claim 1, characterized in that, The nylon is composed of nylon 12, nylon 1012 and nylon 1212 in a mass ratio of (3-7):(2-5):

1.

8. The long carbon chain nylon abrasion-resistant cable sheath according to claim 1, characterized in that, The plasticizer is one or more of N-methylbenzenesulfonamide, N-butylbenzenesulfonamide, phthalate, and triphenyl phosphate; the chain extender is one of carbodiimide, oxazoline, and isocyanate; and the antioxidant is one or more of antioxidant 1010, antioxidant 1076, antioxidant 1098, 2,6-di-tert-butyl-4-methylphenol, and antioxidant 168.

9. The long carbon chain nylon wear-resistant cable sheath according to claim 1, characterized in that, The lubricant is one of polyethylene wax, calcium stearate, and silicone powder.

10. The method for preparing a long carbon chain nylon abrasion-resistant cable sheath according to any one of claims 1-9, characterized in that, Includes the following steps: S1: Dry the nylon at 80-90℃ for 4-5 hours, then add it together with the plasticizer and lubricant into a high-speed mixer and stir at low speed until uniform to obtain mixture I; S2: Add the modified wear-resistant agent, chain extender, and antioxidant to the mixture I obtained in step S1, heat to 90-100℃, stir evenly, and obtain mixture II; S3: The mixture II obtained in step S2 is fed into a twin-screw extruder and melt-extruded, water-cooled into strands, granulated, and dried using a segmented temperature-controlled process to obtain long-chain nylon granules. The segmented temperature control is as follows: Zone 1 185-190℃, Zone 2 190-195℃, Zone 3 195-200℃, Die head 200-210℃, and screw speed 280-320rpm. S4: The long carbon chain nylon granules obtained in step S3 are fed into a cable sheath extruder and extruded using a segmented constant temperature extrusion process: barrel zone 1 190-195℃, barrel zone 2 195-200℃, barrel zone 3 200-205℃, die temperature 205-210℃, screw speed 250-300rpm, constant temperature setting for 1-2 hours, cooling, and winding to obtain a long carbon chain nylon wear-resistant cable sheath.

Citation Information

Patent Citations

  • Nylon cable sheath material and preparation method thereof

    CN122325971A