A super weather-resistant fluorocarbon powder coating and its preparation method
By adding g-C3N4/TiO2 composite material to fluorocarbon powder coatings, the problem of gloss loss during long-term UV aging of fluorocarbon powder coatings is solved, achieving high weather resistance and gloss retention of the coating, which is suitable for high-end buildings and outdoor metal components.
Patent Information
- Application Number
- CN202611444430.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing fluorocarbon powder coatings gradually lose gloss and their gloss retention decrease during long-term outdoor UV aging. Existing modification methods are costly or complex, making it difficult to further improve weather resistance while maintaining good adhesion and mechanical properties.
By incorporating g-C3N4/TiO2 composite material into fluorocarbon powder coatings, the weather resistance and UV aging resistance of the coating are improved through their synergistic effect. Ultra-weather-resistant fluorocarbon powder coatings are prepared through uniform mixing, pulverization and extrusion processes.
It significantly improves the weather resistance and gloss retention of the coating, delays UV aging and gloss loss, has good coating adhesion, and has a simple preparation process, making it suitable for industrial production.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of powder coating technology, specifically relating to an ultra-weather-resistant fluorocarbon powder coating and its preparation method. Background Technology
[0002] Powder coatings use virtually no organic solvents during production, storage, transportation, and application. They exhibit low volatile organic compound (VOC) emissions, high raw material utilization, and convenient application, making them widely used in building materials, automotive parts, home appliances, furniture, and electronic components. They are a significant environmentally friendly alternative to traditional solvent-based coatings. Fluorocarbon powder coatings, in particular, possess excellent resistance to UV aging, chemical media, weathering, and staining due to the high C-F bond energy (approximately 485 kJ / mol) and strong electronegativity of fluorine atoms in fluorocarbon resin molecules. This makes them promising for applications in high-end building curtain walls, bridges, rail transportation, marine engineering, and outdoor metal components where long-term weather resistance is crucial.
[0003] Fluorocarbon resins used in coatings mainly include polyvinylidene fluoride (PVDF), vinyl fluoride-vinyl ether copolymer (FEVE), polyvinyl fluoride (PVF), and polytetrafluoroethylene (PTFE). Among them, PVDF is a thermoplastic fluoropolymer obtained by homopolymerization of vinylidene fluoride. Its CF bond energy is high and its polarizability is low, which endows the coating with excellent chemical stability and ultra-high weather resistance. FEVE is a hydroxyl-containing resin that can react with isocyanates to crosslink and cure, and the coating's weather resistance life can reach more than 30 years.
[0004] However, PVDF resin molecules lack reactive functional groups and are chemically inert, resulting in poor compatibility and adhesion with other resins such as acrylic resins and metal substrates. The inertness of PVDF leads to poor compatibility with other polymers and poor adhesion between the coating and metal substrates, thus limiting its application in fluorocarbon coatings. Functional modification through blending, filling, copolymerization, or chemical grafting is necessary. Introducing inorganic nanomaterials such as SiO2, Al2O3, TiO2, and ZnO into the PVDF matrix can improve its mechanical properties, thermal stability, and coating performance. Previous studies have used fluorocarbon resin as a matrix and compounded with functional fillers to prepare multifunctional fluorocarbon-based composite coatings with conductive, corrosion-resistant, and wear-resistant properties, further demonstrating that functional filler modification can expand the comprehensive performance of fluorocarbon coatings.
[0005] Despite this, existing fluorocarbon powder coatings still suffer from gradual gloss loss and decreased gloss retention during long-term outdoor UV aging. To achieve higher weather resistance, it is often necessary to increase the fluorocarbon resin content or employ more complex modification processes, leading to increased costs and process complexity. Conventional methods such as adding inorganic fillers like titanium dioxide or performing composite modifications have limited effectiveness in further improving the gloss retention and weather resistance of the coating under long-term UV aging. Therefore, how to further improve the weather resistance and delay UV aging gloss loss of fluorocarbon powder coatings while maintaining their good adhesion, mechanical properties, and environmental advantages remains a pressing technical problem to be solved in this field. Summary of the Invention
[0006] The purpose of this invention is to overcome the problems of significant gloss loss and insufficient gloss retention of fluorocarbon powder coatings after long-term ultraviolet aging in the prior art, and to provide an ultra-weather-resistant fluorocarbon powder coating and its preparation method.
[0007] To achieve the above objectives, the present invention provides the following technical solution: An ultra-weather-resistant fluorocarbon powder coating is characterized by comprising, by weight, the following components: 50 parts fluorocarbon resin, 20 parts acrylic resin, 10 parts barium sulfate, 1.0 part leveling agent, 1.0 part defoamer, 1.0 part dispersant, and 1-5 parts g-C3N4 / TiO2 composite material.
[0008] Furthermore, the fluorocarbon resin is a polyvinylidene fluoride resin, which is homopolymerized from vinylidene fluoride with a purity of not less than 99.99%.
[0009] Furthermore, the leveling agent is a polyether-modified organosilicon compound, BYK-320.
[0010] Furthermore, the defoamer is BYK-066N.
[0011] Furthermore, the dispersant is a silane coupling agent KH560.
[0012] Furthermore, the g-C3N4 / TiO2 composite material comprises 2 to 4 parts by weight.
[0013] Furthermore, the g-C3N4 nanosheets in the g-C3N4 / TiO2 composite material are prepared by the following method: 3 g of melamine and 9 g of NH4Cl are thoroughly mixed, transferred to a covered crucible, placed in a muffle furnace, heated to 550 ℃ at a heating rate of 5 ℃ / min and held for 4 h, and then cooled to room temperature to obtain g-C3N4 nanosheets.
[0014] Further, the g-C3N4 / TiO2 composite material was prepared by the following method: 2.5 g of g-C3N4 nanosheet powder was dispersed in deionized water and ultrasonically treated for 30 min to obtain a suspension; 1.2 mL of TiCl4 was slowly added to the suspension and placed in an ice-water bath; then 5 g of urea and 3.3 mL of sodium lactate were added, stirred for 30 min, and then transferred to a 60 mL reaction vessel and kept at 200 ℃ for 12 h; the precipitate was collected, washed with deionized water and ethanol, dried at 70 ℃, and then calcined at 450 ℃ for 1 h to obtain the g-C3N4 / TiO2 composite material.
[0015] The present invention also provides a method for preparing an ultra-weather-resistant fluorocarbon powder coating, comprising the following steps: uniformly mixing the raw materials of each component of the formula according to the formula ratio, and uniformly pulverizing them in a pulverizer; using a twin-screw extruder to mix and extrude the components; subsequently performing cryogenic pulverization and sieving to obtain the ultra-weather-resistant fluorocarbon powder coating.
[0016] Compared with the prior art, the present invention has the following advantages and beneficial effects: This invention significantly improves the weather resistance and UV aging resistance of the coating by adding g-C3N4 / TiO2 composite material to the fluorocarbon powder coating system and utilizing the synergistic effect of g-C3N4 and TiO2. The coating maintains a high gloss retention rate even after long-term UV irradiation. At the same time, the coating has good adhesion, a simple preparation process, and is environmentally friendly with no VOC emissions, making it suitable for industrial production and promising for applications in high-end buildings, outdoor metal components, and other fields. Detailed Implementation
[0017] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. The illustrative embodiments and descriptions of this invention are for illustrative purposes only and are not intended to limit the invention. The embodiments described below are some, but not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0018] In the following description, numerous specific details are set forth to provide a thorough understanding of the invention. However, it will be apparent to those skilled in the art that these specific details are not necessary to practice the invention. In other embodiments, well-known structures, materials, or methods are not specifically described to avoid obscuring the invention. Unless otherwise specified, the materials, instruments, and reagents used in the following embodiments are commercially available. Unless otherwise specified, the techniques used in the embodiments are conventional methods well known to those skilled in the art.
[0019] In the following examples and comparative examples, the fluorocarbon resin is PVDF resin, which is homopolymerized from vinylidene fluoride with a purity of not less than 99.99%; the leveling agent is polyether-modified organosilicon compound BYK-320; the defoamer is BYK-066N; and the dispersant is silane coupling agent KH560.
[0020] Preparation of g-C3N4 / TiO2 composite material: Preparation of g-C3N4 nanosheets: 3 g of melamine and 9 g of NH4Cl were thoroughly mixed and then transferred to a covered crucible. The crucible was placed in a muffle furnace and heated at 550 °C for 4 h at a heating rate of 5 °C / min. After cooling to room temperature, g-C3N4 nanosheets were obtained. 2.5 g of g-C3N4 nanosheets were dispersed in deionized water and sonicated for 30 min to obtain a uniform suspension. Then, 1.2 mL of TiCl4 was slowly added to the suspension, which was placed in an ice-water bath. Then, 5 g of urea and 3.3 mL of sodium lactate were added. After stirring the resulting solution for 30 min, it was transferred to a 60 mL Teflon reactor and kept at 200 °C for 12 h. After the solvothermal process, the precipitate was collected, washed several times with deionized water and ethanol, and dried at 70 °C. The precipitate was then heated at 450 °C. After calcination for 1 h, g-C3N4 / TiO2 composite material was obtained. Example
[0021] An ultra-weather-resistant fluorocarbon powder coating comprises, by weight: 50 parts fluorocarbon resin; 20 parts acrylic resin; 10 parts barium sulfate; 1.0 part leveling agent; 1.0 part defoamer; 1.0 part dispersant; and 1 part g-C3N4 / TiO2 composite material.
[0022] The preparation method of the ultra-weather-resistant fluorocarbon powder coating is as follows: the raw materials of each component of the formula are uniformly mixed according to the formula ratio, and uniformly crushed in a pulverizer. The components are then mixed and extruded using a twin-screw extruder, followed by cryogenic pulverization and sieving to obtain the desired powder coating. Example
[0023] An ultra-weather-resistant fluorocarbon powder coating comprises, by weight: 50 parts fluorocarbon resin; 20 parts acrylic resin; 10 parts barium sulfate; 1.0 part leveling agent; 1.0 part defoamer; 1.0 part dispersant; and 2 parts g-C3N4 / TiO2 composite material.
[0024] The preparation method of the ultra-weather-resistant fluorocarbon powder coating is as follows: the raw materials of each component of the formula are uniformly mixed according to the formula ratio, and uniformly crushed in a pulverizer. The components are then mixed and extruded using a twin-screw extruder, followed by cryogenic pulverization and sieving to obtain the desired powder coating. Example
[0025] An ultra-weather-resistant fluorocarbon powder coating comprises, by weight: 50 parts fluorocarbon resin; 20 parts acrylic resin; 10 parts barium sulfate; 1.0 part leveling agent; 1.0 part defoamer; 1.0 part dispersant; and 3 parts g-C3N4 / TiO2 composite material.
[0026] The preparation method of the ultra-weather-resistant fluorocarbon powder coating is as follows: the raw materials of each component of the formula are uniformly mixed according to the formula ratio, and uniformly crushed in a pulverizer. The components are then mixed and extruded using a twin-screw extruder, followed by cryogenic pulverization and sieving to obtain the desired powder coating. Example
[0027] An ultra-weather-resistant fluorocarbon powder coating comprises, by weight: 50 parts fluorocarbon resin; 20 parts acrylic resin; 10 parts barium sulfate; 1.0 part leveling agent; 1.0 part defoamer; 1.0 part dispersant; and 4 parts g-C3N4 / TiO2 composite material.
[0028] The preparation method of the ultra-weather-resistant fluorocarbon powder coating is as follows: the raw materials of each component of the formula are uniformly mixed according to the formula ratio, and uniformly crushed in a pulverizer. The components are then mixed and extruded using a twin-screw extruder, followed by cryogenic pulverization and sieving to obtain the desired powder coating. Example
[0029] An ultra-weather-resistant fluorocarbon powder coating comprises, by weight: 50 parts fluorocarbon resin; 20 parts acrylic resin; 10 parts barium sulfate; 1.0 part leveling agent; 1.0 part defoamer; 1.0 part dispersant; and 5 parts g-C3N4 / TiO2 composite material.
[0030] The preparation method of the ultra-weather-resistant fluorocarbon powder coating is as follows: the raw materials of each component of the formula are uniformly mixed according to the formula ratio, and uniformly crushed in a pulverizer. The components are then mixed and extruded using a twin-screw extruder, followed by cryogenic pulverization and sieving to obtain the desired powder coating.
[0031] Comparative Example 1 An ultra-weather-resistant fluorocarbon powder coating comprises, by weight: 50 parts fluorocarbon resin; 20 parts acrylic resin; 10 parts barium sulfate; 1.0 part leveling agent; 1.0 part defoamer; and 1.0 part dispersant.
[0032] The preparation method of the ultra-weather-resistant fluorocarbon powder coating is as follows: the raw materials of each component of the formula are uniformly mixed according to the formula ratio, and uniformly crushed in a pulverizer. The components are then mixed and extruded using a twin-screw extruder, followed by cryogenic pulverization and sieving to obtain the desired powder coating.
[0033] Comparative Example 2 An ultra-weather-resistant fluorocarbon powder coating comprises, by weight: 50 parts fluorocarbon resin; 20 parts acrylic resin; 10 parts barium sulfate; 1.0 part leveling agent; 1.0 part defoamer; 1.0 part dispersant; and 4 parts TiO2 composite material.
[0034] The preparation method of the ultra-weather-resistant fluorocarbon powder coating is as follows: the raw materials of each component of the formula are uniformly mixed according to the formula ratio, and uniformly crushed in a pulverizer. The components are then mixed and extruded using a twin-screw extruder, followed by cryogenic pulverization and sieving to obtain the desired powder coating.
[0035] The preparation method of the TiO2 composite material is as follows: 1.2 mL of TiCl4 was added to deionized water, and the suspension was placed in an ice-water bath. Then, 5 g of urea and 3.3 mL of sodium lactate were added. After stirring the resulting solution for 30 min, it was transferred to a 60 mL Teflon reactor and kept at 200 °C for 12 h. After the solvothermal process was completed, the precipitate was collected, washed several times with deionized water and ethanol, and dried at 70 °C. The precipitate was calcined at 450 °C for 1 h to obtain the TiO2 composite material.
[0036] Test Example 1: Using aluminum plates as the substrate, after pretreatment to eliminate the influence of other environmental factors, the products obtained in the examples or comparative examples were electrostatically sprayed onto the substrate surface, followed by curing at 200 ℃ for 15 min. The following coating tests were then conducted: adhesion was tested using the cross-cut adhesion test to observe coating peeling; in the B-lamp aging test, 24 consecutive irradiations were performed in 10-day cycles to obtain the aging degree of the coating under B-lamp irradiation, and the gloss level in each cycle was statistically analyzed to determine the aging characteristics of the experimental system. The test results are shown in Table 1.
[0037] Table 1 shows the coating performance test results of the examples and comparative examples.
[0038] Sample Adhesion test results gloss before aging / % Gloss after aging / % Example 1 Not detached 37.9 35.9 Example 2 Not detached 36.5 35.1 Example 3 Not detached 36.3 34.8 Example 4 Not detached 36.0 34.6 Example 5 Not detached 35.6 34.5 Comparative Example 1 Not detached 38.2 18.2 Comparative Example 2 Not detached 36.1 27.0 As shown in Table 1, the coatings of all examples and comparative examples exhibited good adhesion (no peeling). After aging under a B lamp, the gloss of the coatings in Examples 1-5 with the added g-C3N4 / TiO2 composite material decreased only slightly, remaining at 34.5%-35.9% after aging, with a gloss loss rate significantly lower than that of Comparative Example 1 and Comparative Example 2. These results demonstrate that by adding the g-C3N4 / TiO2 composite material to fluorocarbon powder coatings, this invention can significantly improve the weather resistance and gloss retention of the coating, and delay UV aging-induced gloss loss.
[0039] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A super weather-resistant fluorocarbon powder coating, characterized in that, By weight, it comprises the following components: 50 parts fluorocarbon resin, 20 parts acrylic resin, 10 parts barium sulfate, 1.0 part leveling agent, 1.0 part defoamer, 1.0 part dispersant, and 1 to 5 parts g-C3N4 / TiO2 composite material.
2. The ultra-weather-resistant fluorocarbon powder coating according to claim 1, characterized in that, The fluorocarbon resin is polyvinylidene fluoride resin, which is homopolymerized from vinylidene fluoride with a purity of not less than 99.99%.
3. The ultra-weather-resistant fluorocarbon powder coating according to claim 1, characterized in that, The leveling agent is a polyether-modified organosilicon compound, BYK-320.
4. The ultra-weather-resistant fluorocarbon powder coating according to claim 1, characterized in that, The defoamer is BYK-066N.
5. The ultra-weather-resistant fluorocarbon powder coating according to claim 1, characterized in that, The dispersant is silane coupling agent KH560.
6. The ultra-weather-resistant fluorocarbon powder coating according to claim 1, characterized in that, The g-C3N4 / TiO2 composite material is present in 2 to 4 parts by weight.
7. The ultra-weather-resistant fluorocarbon powder coating according to claim 1, characterized in that, The g-C3N4 nanosheets in the g-C3N4 / TiO2 composite material were prepared by the following method: 3 g of melamine and 9 g of NH4Cl were thoroughly mixed, transferred to a covered crucible, placed in a muffle furnace, heated to 550 ℃ at a heating rate of 5 ℃ / min and held for 4 h, and then cooled to room temperature to obtain g-C3N4 nanosheets.
8. The ultra-weather-resistant fluorocarbon powder coating according to claim 1, characterized in that, The g-C3N4 / TiO2 composite material was prepared by the following method: 2.5 g of g-C3N4 nanosheet powder was dispersed in deionized water and ultrasonically treated for 30 min to obtain a suspension; 1.2 mL of TiCl4 was slowly added to the suspension and placed in an ice-water bath; then 5 g of urea and 3.3 mL of sodium lactate were added, stirred for 30 min, and then transferred to a 60 mL reaction vessel and kept at 200 ℃ for 12 h; the precipitate was collected, washed with deionized water and ethanol, dried at 70 ℃, and then calcined at 450 ℃ for 1 h to obtain the g-C3N4 / TiO2 composite material.
9. A method for preparing the ultra-weather-resistant fluorocarbon powder coating as described in claim 1, characterized in that, The process includes the following steps: uniformly mixing the raw materials of each component of the formula according to the formula ratio, and uniformly pulverizing them in a pulverizer; The components are mixed and extruded using a twin-screw extruder; The coating is then subjected to cryogenic pulverization and sieving to obtain the ultra-weather-resistant fluorocarbon powder coating.