Low VOC waterborne epoxy floor paint
By introducing a hyperbranched polyurethane-modified waterborne epoxy curing agent containing disulfide bonds into waterborne epoxy floor coatings, the problems of high VOC, microcrack propagation, and insufficient toughness of waterborne epoxy floor coatings have been solved, achieving the effects of low VOC, high toughness, and self-healing.
Patent Information
- Application Number
- CN202611589957.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing waterborne epoxy floor coatings suffer from problems such as high VOC content, easy expansion of microcracks that cannot be repaired on their own, and difficulty in achieving both toughness and hardness. These issues have not been effectively addressed, especially in scenarios requiring high filler content and high wear resistance.
A polyamine adduct containing disulfide bonds was prepared by using N,N-bis(acryloyl)cysteine and butyl glycidyl ether-terminated tetraethylenepentamine. Combined with hyperbranched polyurethane-modified epoxy resin, a hyperbranched polyurethane-modified waterborne epoxy curing agent containing disulfide bonds was prepared. The disulfide bonds were covalently fixed in the epoxy crosslinking network, and self-healing was achieved by the dynamic exchange reaction of disulfide bonds. The agent was also toughened by the flexible polyether segments and intramolecular cavities of the hyperbranched polyurethane.
This water-based epoxy floor coating achieves low VOC and self-healing functions, possesses high toughness and wear resistance, and its micro-crack self-healing efficiency can reach 72% to 91%, making it suitable for indoor flooring scenarios subject to frequent impact and wear.
Smart Images

Figure CN123107501A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of floor coating technology, specifically to a low-VOC waterborne epoxy floor coating. Background Technology
[0002] Epoxy resin floor coatings are widely used in industrial plants, underground garages, warehouses, hospitals, and other places due to their excellent adhesion, abrasion resistance, chemical corrosion resistance, and decorative properties. Traditional epoxy floor coatings are mainly solvent-based, containing a large amount of volatile organic compounds (VOCs), which emit harmful gases during construction, endangering human health and causing environmental pollution. With increasingly stringent environmental regulations, the development of low-VOC waterborne epoxy floor coatings has become an industry trend.
[0003] However, water-based epoxy floor coatings still have the following shortcomings: First, after the epoxy resin cures, the cross-linking density is high and the internal stress is large, resulting in a brittle coating that is prone to microcracks when subjected to external impacts or temperature changes during use. Second, once microcracks are formed, they will continue to expand under the influence of environmental factors, leading to a decrease in coating adhesion and loss of protective performance, ultimately requiring complete renovation and incurring high maintenance costs. Third, existing toughening modification methods (such as adding elastomers and flexible segments) often come at the cost of sacrificing hardness, wear resistance, and heat resistance.
[0004] To address the problem of microcracks, self-healing epoxy coatings have become a research hotspot. Introducing dynamic covalent bonds (such as disulfide bonds and Diels-Alder bonds) into polymer networks and utilizing the reversible exchange reaction of these dynamic bonds to achieve self-healing is the main technical route for intrinsic self-healing materials. Among these, the disulfide bond (-SS-) has a low bond energy (approximately 214–273 kJ / mol) and can undergo dynamic exchange under mild conditions, making it an ideal dynamic bond for constructing self-healing polymers.
[0005] In the prior art, CN116970327A discloses a thermally initiated self-healing epoxy resin coating. This coating uses bisphenol A type epoxy resin as the main component and dithiodic acids (such as 3,3'-dithiodipropionic acid, 4,4'-dithiodibutyric acid, etc.) as crosslinking agents. Under the action of a catalyst, the coating reacts to generate an epoxy coating containing dynamic disulfide bonds. This coating can achieve self-healing at high temperatures of 50–80℃, with a fracture strength repair efficiency of up to 95%. However, this technical solution has the following shortcomings: First, the reaction system uses organic solvents such as N,N-dimethylformamide, dimethyl sulfoxide, and propylene glycol methyl ether, which are solvent-based systems with high VOC content, failing to meet environmental protection requirements. Second, the disulfide bonds are introduced through the reaction of the carboxyl group of the dithiodic acid with the epoxy group, requiring quaternary ammonium salts or phosphine catalysts, making the process complex.
[0006] To overcome the shortcomings of solvent-based systems, CN113292926B discloses a water-based self-healing epoxy anti-corrosion coating. This coating incorporates mercapto-terminated polysulfide rubber into modified epoxy resin and epoxy emulsifier, distributing disulfide bonds within the resin particles and at the particle fusion interface. It also uses γ-mercaptopropyltrimethoxysilane-modified zinc phosphate as an anti-rust pigment. The mercapto groups on the zinc phosphate surface provide a thiolate medium, reducing the activation energy of disulfide bond rearrangement and achieving self-healing. While this technical solution achieves water-based application and self-healing, it still has the following shortcomings: First, disulfide bonds are only introduced into the modified epoxy resin and epoxy emulsifier, and the curing agent still uses commercially available ordinary water-based epoxy curing agents (such as Huntsman Aradur 38-1, Dow WB 8001, etc.). The curing agent itself does not have self-healing function, and the disulfide bonds are unevenly distributed in the crosslinking network after curing, limiting the self-healing efficiency. Second, room temperature self-healing highly depends on the addition of mercapto-modified zinc phosphate as a medium, resulting in a complex system composition. Furthermore, free thiols have an odor problem, and the introduction of mercapto may also affect the weather resistance and storage stability of the coating. Third, disulfide bonds are introduced through a mercapto-epoxy ring-opening reaction, requiring catalysts such as triethylamine or boron trifluoride ether. The reaction temperature is 60°C, and the reaction time is as long as 8 hours, resulting in low production efficiency. Fourth, this technical solution is designed for metal corrosion protection scenarios and has not optimized the formulation for the high filler and high wear resistance requirements of floor coatings.
[0007] On the other hand, hyperbranched polymers exhibit unique advantages in polymer modification due to their highly branched three-dimensional structure, numerous active end groups, and intramolecular cavities. Introducing hyperbranched polyurethane (HBPU) into waterborne epoxy curing agents can simultaneously achieve toughening and emulsification functions, significantly improving the impact strength and water dispersion stability of the coating. However, existing hyperbranched polyurethane-modified waterborne epoxy curing agents only focus on toughening and emulsification properties, without introducing dynamic covalent bonds, lacking self-healing capabilities, and failing to solve the fundamental problem of microcrack propagation in floor coatings.
[0008] In summary, the existing technology lacks a waterborne epoxy floor coating that simultaneously possesses the following characteristics: (1) water as the dispersion medium, resulting in low VOC content; (2) disulfide bonds are introduced into the curing agent molecular structure, allowing self-healing functional units to be uniformly distributed in the crosslinking network; (3) self-healing is achieved solely through the dynamic exchange of disulfide bonds without relying on external thiol media; (4) it integrates the toughening function of hyperbranched polyurethane, balancing toughness and hardness; and (5) it features a filler and additive system optimized for floor coating applications. Therefore, developing a self-healing, low-VOC waterborne epoxy floor coating containing disulfide bonds has significant application value and technical importance. Summary of the Invention
[0009] The purpose of this invention is to provide a low-VOC waterborne epoxy floor coating. A polyamine adduct containing disulfide bonds is prepared by Michael addition of N,N-bis(acryloyl)cysteine (CBA) and butyl glycidyl ether mono-terminated tetraethylenepentamine (TEPA-660a). This adduct is used as the curing agent amine component and reacted with hyperbranched polyurethane-modified epoxy resin (HBPU-EP) to prepare a hyperbranched polyurethane-modified waterborne epoxy curing agent containing disulfide bonds. This allows the disulfide bonds to be covalently fixed in the epoxy crosslinking network. The dynamic exchange reaction of disulfide bonds in the glassy state enables self-repair of microcracks. Simultaneously, the flexible polyether segments and intramolecular cavities of the hyperbranched polyurethane achieve toughening. Ultimately, a waterborne epoxy floor coating with low VOC, high toughness, wear resistance, and self-repairing functions is obtained, solving the technical problems of existing waterborne epoxy floor coatings being brittle, prone to microcrack propagation, and unable to self-repair.
[0010] This invention is achieved through the following technical solution: This invention provides a low-VOC waterborne epoxy floor coating, which is a two-component system comprising component A and component B, wherein the mixing mass ratio of component A to component B is 1 to 3:1.
[0011] The component A, by weight, comprises: 30-50 parts of waterborne epoxy resin emulsion, 30-55 parts of filler, 3-10 parts of pigment, 1-5 parts of additives, and 5-15 parts of deionized water.
[0012] Component B is a water-based epoxy curing agent, which is a hyperbranched polyurethane-modified water-based epoxy curing agent containing disulfide bonds. Its solid content is 40% to 60%, its particle size is 30 to 80 nm, and its viscosity at 25°C is 1500 to 3000 mPa∙s.
[0013] The waterborne epoxy curing agent contains dynamic disulfide bonds (-SS-) in its molecular structure, with a disulfide bond content of 0.05 to 0.3 mmol / g. After curing, the disulfide bonds are covalently fixed in the epoxy crosslinking network and can undergo dynamic exchange reactions, giving the coating microcracks self-healing properties.
[0014] Preferably, the aqueous epoxy resin emulsion is an aqueous dispersion of bisphenol A type epoxy resin, including one or two of bisphenol A type epoxy resin E-44 and bisphenol A type epoxy resin E-51, with a solid content of 40% to 60%.
[0015] Preferably, the filler is one or more of the following: quartz sand, quartz powder, heavy calcium carbonate, talc powder, barium sulfate, and mica powder. The particle size of the filler is 325-1500 mesh (D50 is 10-45 μm).
[0016] Preferably, the pigment is one or more of titanium dioxide, iron oxide red, iron oxide yellow, iron oxide black, ultramarine, and phthalocyanine blue.
[0017] Preferably, the additive is a combination of wetting and dispersing agents, defoamers, leveling agents, and thixotropic agents; The wetting and dispersing agent is a polyacrylate or a polycarboxylate; specifically, it includes one or more of sodium polyacrylate, ammonium polyacrylate, potassium polyacrylate, sodium polycarboxylate, ammonium polycarboxylate, acrylic acid-maleic anhydride copolymer salt, and polyether-modified polycarboxylate.
[0018] The defoamer is a mineral oil or an organosilicon; specifically, it includes one or more of the following: liquid paraffin, white oil, modified mineral oil, aluminum stearate, calcium stearate, polydimethylsiloxane, polyether-modified polysiloxane, fluorinated polysiloxane, organosilicon emulsion, and silicone-containing polyether.
[0019] The leveling agent is a polyether-modified siloxane; specifically, it includes one or more of polyether-modified polydimethylsiloxane, polyether-modified methylalkylsiloxane, polyester-modified polysiloxane, polyether-polyester co-modified polysiloxane, alkyl-polyether co-modified polysiloxane, and polyether-modified polysiloxane containing reactive groups; the polyether segment is a polyoxyethylene segment, a polyoxypropylene segment, or a polyoxyethylene-polyoxypropylene copolymer segment.
[0020] The thixotropic agent is fumed silica or bentonite; specifically, it is one or more of hydrophilic fumed silica, hydrophobic fumed silica, sodium-based bentonite, calcium-based bentonite, and organically modified bentonite; the hydrophobic fumed silica is fumed silica surface-treated with dimethyldichlorosilane, hexamethyldisilazane, polydimethylsiloxane, or octylsilane, with a specific surface area of 100–400 m². 2 / g; The organically modified bentonite is bentonite modified with quaternary ammonium salt.
[0021] The preparation method of the hyperbranched polyurethane-modified waterborne epoxy curing agent containing disulfide bonds includes the following steps: Step 1: Hyperbranched polyurethane modified epoxy resin (HBPU-EP) S1. Preparation of hyperbranched polyurethane core: Isophorone diisocyanate (IPDI) and dimethylolpropionic acid (DMPA) were dissolved in N,N-dimethylformamide (DMF) and reacted at 80–90 °C for 1–2 h. Then, the temperature was lowered to -5–0 °C in an ice-salt bath, and a DMF solution of diethanolamine (DEOA) was added dropwise. After the addition was completed in 2 h, the reaction was continued for 0.5 h. Subsequently, dibutyltin dilaurate (DBTDL) was added as a catalyst, and the temperature was raised to 55–65 °C and maintained for 1.5–2.5 h. Finally, the hyperbranched polyurethane core was obtained by separation, purification, and drying. A typical reaction route is as follows: ; The ratio of isophorone diisocyanate (IPDI) to dimethylolpropionic acid (DMPA) is 5 to 7:1, calculated by molar ratio.
[0022] The amount of diethanolamine (DEOA) used, on a molar ratio basis, is 0.8 to 1.2:1, preferably 0.9 to 1.1:1.
[0023] The amount of dibutyltin dilaurate (DBTDL) used is 0.03% to 0.15% of the total mass of IPDI and DMPA.
[0024] The amounts of N,N-dimethylformamide (DMF) used are as follows: the amount of DMF used to dissolve IPDI and DMPA is 1.5 to 3 times the total mass of IPDI and DMPA; the amount of DMF used to dissolve DEOA is 2 to 4 times the mass of DEOA.
[0025] S2. Preparation of hyperbranched polyurethane (HBPU): Polyether diol N210 (Mn=1000) and IPDI were reacted at 80-90℃ for 2h to obtain a linear polyurethane prepolymer; then, the temperature was lowered to 60℃, DMPA, 1,4-butanediol (BDO) and DBTDL were added, and the temperature was raised to 80-90℃ to continue the reaction for 2h; the hyperbranched polyurethane core obtained in S1 was added, and the reaction was carried out at 80-90℃ for another 2h, so that the -NCO of the linear polyurethane prepolymer reacted with the hydroxyl / amine groups on the hyperbranched polyurethane core, and the linear PU was grafted onto the hyperbranched core to obtain HBPU.
[0026] The amount of polyether diol N210 used is 1.0 to 2.0 times the mass of IPDI, preferably 1.3 to 1.7 times.
[0027] The amounts of DMPA, 1,4-butanediol (BDO), and DBTDL are 8%–18%, 2%–7%, and 0.1%–0.6% of the mass of IPDI, respectively.
[0028] The amount of the hyperbranched polyurethane core is 25% to 50% of the mass of IPDI, preferably 30% to 45%.
[0029] S3. Preparation of hyperbranched polyurethane modified epoxy resin (HBPU-EP): The HBPU obtained in S2 is reacted with epoxy resin at 90-100℃ for 2-3 hours, so that the -NCO end group on the HBPU structure reacts with the hydroxyl group on the epoxy resin structure to form urethane bond, and HBPU is grafted onto the epoxy resin molecule to obtain HBPU-EP. The epoxy resin includes one or two of bisphenol A type epoxy resin E-44 and bisphenol A type epoxy resin E-51, preferably bisphenol A type epoxy resin E-44.
[0030] The amount of epoxy resin used is 40% to 120% of the mass of the hyperbranched polyurethane, preferably 60% to 110%.
[0031] Step 2: Preparation of polyamine adducts containing disulfide bonds In a reaction vessel, butyl glycidyl ether (660a) was added dropwise to tetraethylenepentamine (TEPA), and the reaction was carried out at 65–75 °C for 3 h to generate the single-terminated product TEPA-660a. Subsequently, a dimethylformamide (DMF) solution of N,N-bis(acryloyl)cysteine (CBA) was added dropwise at a rate of 20–30 drops / min. The reaction was carried out at 30–40 °C for 2–4 h. The acrylamide double bond of CBA underwent a azeotropic Michael addition with the amine hydrogen of TEPA-660a, and the double bond opened to form a β-aminoamide structure, introducing a disulfide bond into the polyamine molecule to obtain a polyamine adduct containing a disulfide bond. The reaction route is shown below: ; Preferably, the molar ratio of butyl glycidyl ether (660a) to tetraethylenepentamine (TEPA) is 0.8 to 1:1, with TEPA in excess or in equal molar amounts to avoid over-capping which could affect the polyamine activity.
[0032] Preferably, the molar ratio of TEPA-660a to CBA is 3 to 10:1. The excess of TEPA-660a ensures that both double bonds of CBA react to form a symmetrical structure of TEPA-660a-CBA-TEPA-660a, thus avoiding gelation. The concentration of the dimethylformamide (DMF) solution of N,N-bis(acryloyl)cysteine (CBA) is 0.1 to 0.5 g / mL, preferably 0.2 to 0.3 g / mL (i.e., a mass fraction of about 15% to 30%).
[0033] Step 3: Preparation of hyperbranched polyurethane-modified waterborne epoxy curing agent containing disulfide bonds In a reaction vessel, the HBPU-EP obtained in step one was dissolved in propylene glycol methyl ether. The polyamine adduct containing disulfide bonds obtained in step two was slowly added dropwise at 40–50°C, with the dropping rate controlled at 30–40 drops / min. The reaction was allowed to proceed for 2–3 hours after the addition was complete. Subsequently, the temperature was lowered to below 60°C, and glacial acetic acid was added dropwise to adjust the pH of the system to 7.0 ± 0.5, so that the amine matrix was protonated to form an ammonium salt, which imparts hydrophilicity. The propylene glycol methyl ether solvent was removed by vacuum distillation at 50–60°C and a vacuum degree of -0.090 to -0.095 MPa. Then, deionized water was added dropwise at 50–60 drops / min and stirred at 8000–10000 rpm to emulsify the mixture, thereby obtaining a hyperbranched polyurethane modified waterborne epoxy curing agent containing disulfide bonds.
[0034] The active amine hydrogen in the polyamine adduct containing disulfide bonds undergoes ring-opening addition with the epoxy group of HBPU-EP, incorporating the amine component containing disulfide bonds into the curing agent molecule and endowing the material with self-healing properties.
[0035] The aforementioned low-VOC waterborne epoxy floor coatings can be applied to floor coatings in industrial plants, underground garages, parking lots, warehouses, logistics centers, hospitals, schools, office buildings, laboratories, and cleanrooms. They are especially suitable for indoor flooring scenarios with strict VOC emission requirements, frequent impact and wear, and sensitive maintenance costs.
[0036] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention uses water as the dispersion medium. The co-solvent is recovered by vacuum distillation during the preparation of the curing agent. The VOC content of the final product is less than 50g / L, which meets environmental protection requirements. It is suitable for construction in indoor enclosed spaces and overcomes the defect of high VOC emissions in traditional solvent-based epoxy coatings.
[0037] 2. This invention introduces disulfide bonds into the curing agent amine component. After curing into a film, the disulfide bonds are covalently bonded to the epoxy crosslinking network. By utilizing the thermally induced dynamic exchange characteristics of disulfide bonds, microcracks can be self-repaired after being stimulated at 65°C without the need to introduce external repair media. This solves the problem of the harsh repair conditions and dependence on external repair reagents of existing self-healing coatings. Under the condition of heat preservation at 65°C for 2 hours, the microcrack repair efficiency can reach 72% to 91%.
[0038] 3. This invention uses hyperbranched polyurethane-modified epoxy resin (HBPU-EP). HBPU has flexible polyether segments and intramolecular cavities, which form a sea-island phase separation structure after curing, effectively dissipating impact energy. The impact strength of the coating film can reach 9.7–12.6 kJ / m. 2 While significantly improving the toughness of the coating, it can maintain H~2H pencil hardness and good wear resistance, solving the technical problem that existing self-healing epoxy coatings are difficult to balance in terms of both strength and toughness and have insufficient toughness. Attached Figure Description
[0039] Figure 1 This is a schematic diagram of the waterborne epoxy crosslinking network containing disulfide bonds and dynamic covalent bonds according to the present invention; Figure 2 The bar charts show the impact strength, tensile strength, VOC content, elongation at break, and self-healing efficiency of the coating films obtained in Examples 1-3 and Comparative Examples 1-3. Detailed Implementation
[0040] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0041] Unless otherwise specified, the experimental methods in the following embodiments are conventional methods, performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions.
[0042] Unless otherwise specified, all materials and reagents used in the following examples are commercially available.
[0043] Example 1
[0044] A low-VOC waterborne epoxy floor coating, wherein the waterborne epoxy floor coating is a two-component system, including component A and component B, wherein the mixing mass ratio of component A to component B is 2:1.
[0045] Specifically, component A, by weight, comprises 42 parts of waterborne bisphenol A type epoxy resin E-44 emulsion (50% solid content); 22 parts of filler, 16 parts of heavy calcium carbonate (600 mesh), and 6 parts of barium sulfate (1000 mesh); 5 parts of pigment, rutile titanium dioxide R-930; 2 parts of additives, sodium polyacrylate dispersant, 0.5 parts of polydimethylsiloxane defoamer, 0.3 parts of polyether-modified methylalkylsiloxane leveling agent, and 0.2 parts of fumed silica thixotropic agent; and 6 parts of deionized water.
[0046] Component B is a water-based epoxy curing agent, which is a hyperbranched polyurethane-modified water-based epoxy curing agent containing disulfide bonds, and is prepared through the following steps: Step 1: Hyperbranched polyurethane modified epoxy resin (HBPU-EP) S1. Preparation of hyperbranched polyurethane core: 110.0 g of isophorone diisocyanate (IPDI) and 10.2 g of dimethylolpropionic acid (DMPA) were added to a reaction vessel, and 200 g of N,N-dimethylformamide (DMF) was added to dissolve them. The mixture was heated to 85 °C under nitrogen protection and stirred for 1.5 h. Then, the system was cooled to -2 °C through an ice-salt bath. 50.0 g of diethanolamine (DEOA) was dissolved in 120 g of DMF to obtain a DEOA solution, which was added to the reaction vessel dropwise at 40 drops / min for 2 h. The reaction was then continued at this temperature for 0.5 h. Subsequently, 0.06 g of dibutyltin dilaurate (DBTDL) was added, and the mixture was heated to 60 °C and kept at this temperature for 2 h. After the reaction was completed, the precipitate was collected, filtered, and vacuum dried to obtain the hyperbranched polyurethane core.
[0047] S2. Preparation of hyperbranched polyurethane (HBPU): 40g of polyether diol N210 (Mn=1000) and 28g of IPDI were added to a reaction vessel and reacted at 85℃ for 2h to obtain a linear polyurethane prepolymer; then, the temperature was lowered to 60℃, and 3.2g of DMPA, 1.2g of 1,4-butanediol (BDO) and 0.12g of DBTDL were added, and the temperature was raised to 85℃ to continue the reaction for 2h; 14.0g of the hyperbranched polyurethane core obtained in S1 was added, and the reaction was maintained at 85℃ for another 2h to obtain HBPU.
[0048] S3. Preparation of hyperbranched polyurethane modified epoxy resin (HBPU-EP): 60g of bisphenol A type epoxy resin E-44 was added to the reaction vessel of S2, and the temperature was raised to 95℃ and kept at the temperature for 2.5h. The -NCO at the end of HBPU and the hydroxyl group on the epoxy resin underwent an urethane reaction to obtain HBPU-EP.
[0049] Step 2: Preparation of polyamine adducts containing disulfide bonds 45.0 g of tetraethylenepentamine (TEPA) was added to a reaction vessel and stirred until the temperature reached 70 °C. 28.4 g of butyl glycidyl ether (660a) was added dropwise at 35 drops / min. After the addition was complete, the reaction was maintained at 70 °C for 3 h to obtain a single-terminated polyamine TEPA-660a. Subsequently, 6.0 g of N,N-bis(acryloyl)cysteine (CBA) was dissolved in 25 g of DMF to prepare a solution. The solution was added dropwise to the TEPA-660a system at 20 drops / min at 35 °C. After the addition was complete, the reaction was maintained at 3 h, and Michael addition was performed to obtain a polyamine adduct containing disulfide bonds.
[0050] Step 3: Preparation of hyperbranched polyurethane-modified waterborne epoxy curing agent containing disulfide bonds 146.4g of [material] was placed in the reaction vessel. HBPU-EP was dissolved in 75g of propylene glycol methyl ether and stirred at 45℃. 79.2g of the polyamine adduct containing disulfide bonds, prepared in step two, was added dropwise at 30 drops / min. After the addition was complete, the reaction was maintained at this temperature for 2.5h. The reaction system was then cooled to 50℃, and glacial acetic acid was added dropwise to adjust the pH to 7.0, causing the amine matrix to protonate and form an ammonium salt. Subsequently, the temperature was controlled at 55℃, and propylene glycol methyl ether was removed by vacuum distillation under a vacuum of -0.090MPa. Then, deionized water was added dropwise at 50 drops / min at 55℃, and emulsification was carried out by high-speed stirring at 8500rpm. After emulsification, the mixture was filtered to obtain a hyperbranched polyurethane-modified waterborne epoxy curing agent containing disulfide bonds. The hyperbranched polyurethane-modified waterborne epoxy curing agent containing disulfide bonds had a solid content of 48.2%, a particle size of 30–80nm, a viscosity of 1520mPa∙s, and a disulfide bond content of 0.08mmol / g.
[0051] The preparation process of the low-VOC waterborne epoxy floor paint is as follows: Deionized water, dispersant, and defoamer are added to a dispersion tank and stirred at a low speed of 300 rpm until homogeneous; filler and titanium dioxide are added sequentially, and the mixture is dispersed at a high speed of 2500 rpm for 30 minutes, with the fineness measured to be ≤40μm; then the speed is reduced to 800 rpm, and waterborne bisphenol A type epoxy resin E-44 emulsion, leveling agent, and thixotropic agent are added and stirred for 15 minutes; the mixture is filtered to obtain component A of the floor paint; subsequently, component A is mixed with the hyperbranched polyurethane modified waterborne epoxy curing agent containing disulfide bonds prepared in the above steps at a mass ratio of 2:1, stirred evenly, and then a film is formed. The film is cured at room temperature (25℃) for 7 days, and various performance tests are conducted.
[0052] Example 2
[0053] The difference from Example 1 is that the amount of N,N-bis(acryloyl)cysteine (CBA) added in step two was changed from 6.0g to 12.0g; the other steps remained unchanged, and the mass of the solid product containing disulfide bonds was 85.0g. In step three, 85.0 g of the polyamine adduct containing disulfide bonds prepared in step two was added dropwise at 30 drops / min. The remaining steps remained unchanged to obtain a hyperbranched polyurethane modified waterborne epoxy curing agent containing disulfide bonds. The hyperbranched polyurethane modified waterborne epoxy curing agent containing disulfide bonds had a solid content of 47.6%, a particle size of 30-80 nm, a viscosity of 1680 mPa∙s, and a disulfide bond content of 0.16 mmol / g.
[0054] The proportions of other raw materials, all process operating conditions, formulation of component A, and mass ratio of component A / B are exactly the same as in Example 1.
[0055] Example 3
[0056] The difference from Example 1 is that the amount of N,N-bis(acryloyl)cysteine (CBA) added in step two was changed from 6.0g to 18.0g; the other steps remained unchanged, and the mass of the solid product containing disulfide bonds was 91.1g. In step three, 91.1 g of the polyamine adduct containing disulfide bonds prepared in step two was added dropwise at a rate of 30 drops / min. The remaining steps remained unchanged to obtain a hyperbranched polyurethane-modified waterborne epoxy curing agent containing disulfide bonds. The hyperbranched polyurethane-modified waterborne epoxy curing agent containing disulfide bonds had a solid content of 48.5%, a particle size of 30-80 nm, a viscosity of 2130 mPa∙s, and a disulfide bond content of 0.26 mmol / g.
[0057] The proportions of other raw materials, all process operating conditions, formulation of component A, and mass ratio of component A / B are exactly the same as in Example 1.
[0058] Comparative Example 1 A low-VOC waterborne epoxy floor coating is disclosed, comprising a two-component system including component A and component B. Specifically, component A, by weight, comprises: 42 parts of waterborne bisphenol A type epoxy resin E-44 emulsion (50% solid content); 22 parts of filler (800 mesh), 16 parts of heavy calcium carbonate (600 mesh), and 6 parts of barium sulfate (1000 mesh); 5 parts of pigment (rutile titanium dioxide R-930); 2 parts of additives (sodium polyacrylate dispersant), 0.5 parts of polydimethylsiloxane defoamer, 0.3 parts of polyether-modified methylalkylsiloxane leveling agent, and 0.2 parts of fumed silica thixotropic agent); and 6 parts of deionized water.
[0059] The B component is a commercially available water-based epoxy polyamine curing agent (Huntsman Aradur 38-1, AHEW≈150g / eq, solid content 79%~81%). 100 parts by weight of the above-mentioned component A are mixed with 7.0 parts by weight of component B (Huntsman Aradur 38-1) so that the active hydrogen equivalent provided by the curing agent is equivalent to the active hydrogen addition level in the system of Example 1. The remaining raw material ratios, all process operations, and curing conditions are the same as in Example 1.
[0060] Comparative Example 2 A low-VOC waterborne epoxy floor coating differs from Example 1 in that: component B is a waterborne epoxy curing agent modified only by hyperbranched polyurethane (HBPU) and free of disulfide bonds; that is, the amount of N,N-bis(acryloyl)cystamine (CBA) in step two is 0, as detailed below: Step 2: Preparation of polyamine adducts containing disulfide bonds 45.0 g of tetraethylenepentamine (TEPA) was added to a reaction vessel and stirred until the temperature reached 70 °C. 28.4 g of butyl glycidyl ether (660a) was added dropwise at a rate of 30–40 drops / min. After the addition was complete, the reaction was maintained at 70 °C for 3 h to obtain a single-terminated polyamine TEPA-660a. Subsequently, 0 g of N,N-bis(acryloyl)cysteine (CBA) was dissolved in 25 g of DMF to prepare a solution. The solution was added dropwise to the TEPA-660a system at a rate of 20 drops / min at 35 °C. After the addition was complete, the reaction was maintained at 3 h to obtain a polyamine adduct.
[0061] Step 3: Preparation of hyperbranched polyurethane-modified waterborne epoxy curing agent In a reaction vessel, 146.4 g of HBPU-EP was dissolved in 75 g of propylene glycol methyl ether and stirred at 45 °C. 73.0 g of the polyamine adduct prepared in step two was added dropwise at 30 drops / min, and the reaction was maintained at this temperature for 2.5 h. The reaction system was then cooled to 50 °C, and glacial acetic acid was added dropwise to adjust the pH to 7.0 ± 0.5, causing the amine matrix to protonate and form an ammonium salt. Subsequently, the temperature was controlled at 55 °C, and propylene glycol methyl ether was removed by vacuum distillation under a vacuum of -0.090 MPa. Then, deionized water was added dropwise at 50 drops / min at 55 °C, and emulsification was carried out by high-speed stirring at 8500 rpm. After emulsification, the mixture was filtered to obtain a hyperbranched polyurethane-modified waterborne epoxy curing agent. The hyperbranched polyurethane-modified waterborne epoxy curing agent had a solid content of 48.0%, a particle size of 30–80 nm, a viscosity of 1380 mPa∙s, and a disulfide bond content of 0 mmol / g.
[0062] The proportions of other raw materials, all process operating conditions, formulation of component A, and mass ratio of component A / B are exactly the same as in Example 1.
[0063] Comparative Example 3 A low-VOC waterborne epoxy floor coating differs from Example 1 in that: component B is a waterborne epoxy curing agent containing only disulfide bonds without modification by hyperbranched polyurethane (HBPU); that is, it does not include the synthesis step of hyperbranched polyurethane-modified epoxy resin (HBPU-EP); the polyamine adduct containing disulfide bonds prepared in Example 1 is directly used as the curing agent matrix, specifically: 79.2 g of a polyamine adduct containing disulfide bonds was dissolved in 75 g of propylene glycol methyl ether and stirred at 45 °C until dissolved. The temperature was lowered to 50 °C, and glacial acetic acid was added dropwise to adjust the pH of the system to 7.0, causing the amine matrix to protonate and form an ammonium salt. The solvent was removed by vacuum distillation at -0.090 MPa under controlled temperature of 55 °C. Deionized water was added dropwise at 50 drops / min at 55 °C, and the mixture was emulsified by high-speed stirring at 8500 rpm and filtered to obtain a waterborne epoxy curing agent containing only disulfide bonds and without the HBPU flexible structure. The waterborne epoxy curing agent without the HBPU flexible structure had a solid content of 48.1%, a particle size of 30–80 nm, a viscosity of 1315 mPa∙s, and a disulfide bond content of 0.08 mmol / g.
[0064] The proportions of other raw materials, all process operating conditions, formulation of component A, and mass ratio of component A / B are exactly the same as in Example 1.
[0065] The following performance tests were performed on Examples 1-3 and Comparative Examples 1-3 described above: (1) VOC content: The relevant tests were conducted in accordance with GB / T 23986.2-2023 "Determination of volatile organic compounds (VOC) and / or semi-volatile organic compounds (SVOC) content in paints and varnishes - Part 2: Gas chromatography".
[0066] (2) Self-healing efficiency (%): The paint film was subjected to cross-cut damage using a cross-cutting instrument, with the scratches penetrating the paint film to the substrate surface; the damaged sample was placed in an oven at normal pressure and kept at 65℃ for 2 hours for repair; the impact strength of the original paint film and the repaired paint film were measured respectively, and the self-healing efficiency was calculated according to the following formula: .
[0067] (3) Impact strength (kJ / m) 2 The relevant tests were conducted in accordance with GB / T 1732-2020 "Test Method for Impact Resistance of Coating Film".
[0068] (4) Pencil hardness: The relevant tests were conducted in accordance with GB / T 6739-2022 "Determination of paint film hardness by pencil method for paints and varnishes".
[0069] (5) Abrasion resistance (g): According to GB / T 1768-2006 "Determination of abrasion resistance of paints and varnishes by rotating rubber grinding wheel", record the mass of abrasion loss of the sample.
[0070] (6) Tensile strength (MPa) and elongation at break (%): According to GB / T 1040.1-2018 "Determination of tensile properties of plastics", the paint film was made into a standard type II specimen for testing.
[0071] The test results are recorded in Table 1.
[0072] Table 1. Summary of performance data for Examples 1-3 and Comparative Examples 1-3
[0073] This invention also introduces HBPU flexible segments and disulfide dynamic covalent bonds to form an aqueous epoxy crosslinking network containing disulfide dynamic covalent bonds, as shown in the relevant schematic diagram. Figure 1 As shown, under low VOC conditions, the coating film possesses both excellent mechanical strength and good self-healing properties.
[0074] Based on the test results in Table 1 Figure 2 It can be seen that as the amount of CBA added increases, the self-healing efficiency of the coating film continuously improves, the elongation at break increases, while the tensile strength, impact strength, and hardness decrease slightly. Comparative Example 1 uses a commercial curing agent, resulting in a coating film with high hardness but high brittleness, no obvious self-healing effect, and relatively high VOC. Comparative Example 2 only introduces HBPU, which improves the toughness of the coating film, but lacks disulfide bonds and has almost no self-healing ability. Comparative Example 3 only introduces disulfide bonds, which, although possessing high self-healing efficiency, has insufficient toughness due to the lack of a flexible HBPU matrix. In summary, this invention utilizes the synergistic effect of flexible HBPU segments and dynamic covalent bonds of disulfide bonds to obtain a waterborne epoxy floor coating film that simultaneously possesses low VOC, high toughness, and excellent self-healing effect.
[0075] It should be noted that the specific implementation methods described above provide a detailed explanation of the technical solution and application results of the present invention. The above embodiments are only the most preferred embodiments and are not intended to limit the present invention. Modifications or equivalent substitutions made by those skilled in the art within the core theoretical scope of the present invention should all fall within the protection scope of the present invention.
Claims
1. A low VOC waterborne epoxy floor paint, characterized by, The water-based epoxy floor coating is a two-component system, including component A and component B; Component A includes an aqueous epoxy resin emulsion, fillers, pigments, additives, and deionized water; The B component is a disulfide-bonded hyperbranched polyurethane-modified waterborne epoxy curing agent, which is prepared by reacting a disulfide-bonded polyamine adduct with a hyperbranched polyurethane-modified epoxy resin. The polyamine adduct containing disulfide bonds is prepared by Michael addition reaction of N,N-bis(acryloyl)cysteine and butyl glycidyl ether monoterminated tetraethylenepentamine. The molecular structure of the hyperbranched polyurethane modified waterborne epoxy curing agent containing disulfide bonds contains dynamic disulfide bonds.
2. The low VOC waterborne epoxy floor paint according to claim 1, characterized in that, The mixing mass ratio of component A to component B is 1 to 3:
1.
3. The low VOC waterborne epoxy floor paint according to claim 1, characterized in that, The component A, by weight, comprises: 30-50 parts of waterborne epoxy resin emulsion, 30-55 parts of filler, 3-10 parts of pigment, 1-5 parts of additives, and 5-15 parts of deionized water.
4. The low VOC waterborne epoxy floor paint according to claim 1, characterized in that, The aqueous epoxy resin emulsion is an aqueous dispersion of bisphenol A type epoxy resin, wherein the bisphenol A type epoxy resin is one or both of bisphenol A type epoxy resin E-44 and bisphenol A type epoxy resin E-51.
5. The low-VOC waterborne epoxy floor coating according to claim 1, characterized in that, The filler is one or more of the following: quartz sand, quartz powder, heavy calcium carbonate, talc powder, barium sulfate, and mica powder, and the particle size of the filler is 325-1500 mesh. The pigment is one or more of titanium dioxide, iron oxide red, iron oxide yellow, iron oxide black, ultramarine, and phthalocyanine blue; The additives are a combination of wetting and dispersing agents, defoamers, leveling agents, and thixotropic agents.
6. The low-VOC waterborne epoxy floor coating according to claim 1, characterized in that, The superbranched polyurethane modified waterborne epoxy curing agent containing disulfide bonds has a solid content of 40%–60%, a particle size of 30–80 nm, a viscosity of 1500–3000 mPa∙s at 25°C, and a disulfide bond content of 0.05–0.3 mmol / g.
7. The low-VOC waterborne epoxy floor coating according to claim 1, characterized in that, The hyperbranched polyurethane modified epoxy resin is prepared by reacting hyperbranched polyurethane with epoxy resin. The amount of epoxy resin used is 40% to 120% of the mass of hyperbranched polyurethane. The epoxy resin is one or two of bisphenol A type epoxy resin E-44 and bisphenol A type epoxy resin E-51.
8. The low-VOC waterborne epoxy floor coating according to claim 1, characterized in that, The molar ratio of the butyl glycidyl ether monocapped tetraethylenepentamine to N,N-bis(acryloyl)cystamine is 3 to 10:
1.
9. The low-VOC waterborne epoxy floor coating according to claim 8, characterized in that, The preparation method of the hyperbranched polyurethane-modified waterborne epoxy curing agent containing disulfide bonds includes the following steps: Step 1: React hyperbranched polyurethane with epoxy resin to obtain hyperbranched polyurethane modified epoxy resin. Step 2: React butyl glycidyl ether with tetraethylenepentamine to obtain butyl glycidyl ether mono-terminated tetraethylenepentamine; then perform a Michael addition reaction between N,N-bis(acryloyl)cysteine and the butyl glycidyl ether mono-terminated tetraethylenepentamine to obtain a polyamine adduct containing disulfide bonds. Step 3: Add the polyamine adduct containing disulfide bonds dropwise to the propylene glycol methyl ether solution of hyperbranched polyurethane modified epoxy resin, and let the reaction proceed for 2-3 hours after the addition is complete; adjust the pH of the system to 7.0±0.5 with glacial acetic acid, remove the solvent by vacuum distillation, and emulsify with water to obtain the waterborne epoxy curing agent containing disulfide bonds modified by hyperbranched polyurethane.
10. The low-VOC waterborne epoxy floor coating according to claim 9, characterized in that, In step one, the preparation steps of the hyperbranched polyurethane-modified epoxy resin include: S1. Isophorone diisocyanate, dimethylolpropionic acid and diethanolamine are reacted to prepare hyperbranched polyurethane core; S2. A linear polyurethane prepolymer is prepared by reacting polyether diol with isophorone diisocyanate, and then reacted with the hyperbranched polyurethane core to obtain hyperbranched polyurethane. S3. React the hyperbranched polyurethane with epoxy resin to obtain hyperbranched polyurethane modified epoxy resin; In step two, the Michael addition reaction temperature is 30–40°C and the reaction time is 2–4 hours. In step three, the dropping rate is 30-40 drops / minute, the vacuum distillation temperature is 50-60℃, and the vacuum degree is -0.090 to -0.095 MPa.
Citation Information
Patent Citations
A water-based self-healing epoxy anti-corrosion coating and its preparation method
CN113292926B
Thermal-initiation self-repairing epoxy resin coating as well as preparation method and application thereof
CN116970327A