A high-performance polycrystalline silicon polishing slurry concentrate and its preparation method

By preparing a high-performance polycrystalline silicon polishing slurry concentrate, the problems of high gold impurity content, low polishing rate, and low selectivity in existing polycrystalline silicon polishing slurries are solved, thereby improving polishing efficiency and surface quality, and reducing particle residue and dish defects.

CN123107547APending Publication Date: 2026-11-17NINGBO PINGHENG ELECTRONICS MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611333529.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polycrystalline silicon polishing slurries have problems such as high gold impurity content, low polishing rate, low polycrystalline silicon/silicon oxide selectivity, residual particles on the wafer surface after polishing, and dish-shaped defects.

Method used

A high-performance polycrystalline silicon polishing slurry concentrate is used, which contains a specific ratio of silica abrasive, accelerator, protectant, preservative and pH adjuster. It is prepared through precise stirring and filtration processes, and after dilution, it is used for polycrystalline silicon polishing to optimize the polishing effect.

Benefits of technology

The polycrystalline silicon polishing rate was increased to 4800~6000 Å/min, the polycrystalline silicon/silicon oxide selectivity ratio was increased to 790~1500, the surface roughness after polishing was reduced to 0.5 nm, the particle residue was less than 10 particles, the dish-shaped depression was less than 350 Å, and the gold impurity content was less than 100 ppb.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107547A_ABST
    Figure CN123107547A_ABST
Patent Text Reader

Abstract

This invention provides a high-performance polycrystalline silicon polishing slurry concentrate and its preparation method. The polishing slurry concentrate comprises the following raw material components by mass fraction: 10-20 wt% silica abrasive, 0.1-5 wt% accelerator, 0.2-2 wt% protectant, 0.001-0.1 wt% preservative, with the balance being a pH adjuster and water. The pH adjuster adjusts the pH of the polishing slurry concentrate to 11-12. The accelerator is one or more of tetramethylammonium hydroxide, triethanolamine, or diethylenetriamine. The protectant is one or more of carboxymethyl cellulose, hydroxyethyl cellulose, or hydroxypropyl cellulose. The silica is in spherical particles with a particle size of 60-70 nm. The polishing slurry prepared by diluting this concentrate can significantly improve the polishing rate of polycrystalline silicon and increase the polycrystalline silicon / silicon oxide polishing selectivity while maintaining wafer surface quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of chemical mechanical polishing technology, and in particular to a high-performance polycrystalline silicon polishing slurry concentrate and its preparation method. Background Technology

[0002] Chemical mechanical polishing (CMP) is an ultra-smooth processing technology with low equipment requirements, low sensitivity to the composition and structural inhomogeneity of the material to be polished, and no adverse metallurgical state. It is highly practical and is currently the only effective means to achieve global ultra-precision planarization of large-size materials. The polishing slurry, which plays a decisive role, is composed of chemical additives such as oxidants, pH adjusters, corrosion inhibitors, surfactants, complexing agents, and chelating agents, mixed with abrasive grains in a specific ratio. It is generally believed that large abrasive grains grinding wafers during polishing can lead to excessive indentation depth and surface scratches, while small abrasive grains are difficult to achieve specific removal rate requirements. For example, Chinese patent (CN101652445B) discloses a method for preparing a chemical mechanical polishing slurry for polycrystalline silicon, which can effectively polish polycrystalline silicon films under alkaline conditions. The raw material composition of this polycrystalline silicon polishing slurry at room temperature includes: polyol nonionic surfactants, guanidine compounds, abrasive grains, and water. The polyol nonionic surfactant significantly reduces the removal rate of polycrystalline silicon without altering the removal rate of silica, thus significantly reducing the selectivity ratio of polycrystalline silicon to silica. Guanidine compounds also reduce the selectivity ratio of polycrystalline silicon to silica and have a pH-regulating effect, eliminating the need for conventional pH adjusters and greatly reducing metal ion contamination and environmental pollution. Therefore, this polishing solution can reduce the polishing rate of polycrystalline silicon.

[0003] However, the polycrystalline silicon polishing slurry described in the aforementioned patented technology cannot meet the requirements for controlling the removal rate of polycrystalline silicon thin films in practical applications. Furthermore, it cannot remain on the polycrystalline silicon layer after polishing, thus limiting its applicability to widespread use in polishing polycrystalline silicon thin films. Additionally, particles easily adhere to the wafer surface after polycrystalline silicon polishing, making cleaning difficult and leading to wafer scratches. Therefore, there is an urgent need to develop a polishing slurry with high grinding rate, high selectivity, low grinding roughness, low gold and impurity content, and minimal particle residue and dish-shaped defects on the wafer surface after polishing. Summary of the Invention

[0004] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a high-performance polycrystalline silicon polishing slurry concentrate and its preparation method, which solves the problems of high gold impurity content, low polycrystalline silicon polishing rate, low polycrystalline silicon / silicon oxide selectivity ratio during polishing, and residual particles and dish-shaped defects on the wafer surface after polishing in the prior art.

[0005] To achieve the above and other related objectives, the present invention provides a high-performance polycrystalline silicon polishing slurry concentrate and its preparation method.

[0006] The first aspect of this invention discloses a polycrystalline silicon polishing slurry concentrate, which comprises the following raw material components by mass fraction: 10-20 wt% silica abrasive, 0.1-5 wt% accelerator, 0.2-2 wt% protectant, 0.001-0.1 wt% preservative, and the balance being a pH adjuster and water. The pH adjuster adjusts the pH of the polishing slurry concentrate to 11-12. The accelerator is one or more of tetramethylammonium hydroxide, triethanolamine, or diethylenetriamine. The protectant is one or more of carboxymethyl cellulose, hydroxyethyl cellulose (HEC), or hydroxypropyl cellulose. The silica is in the form of spherical particles with a particle size of 60-70 nm, such as 60 nm, 62 nm, 64 nm, 66 nm, 68 nm, or 70 nm.

[0007] The mass fraction is calculated based on the total mass of the polishing slurry concentrate, and represents the percentage of each component in the total mass of the polishing slurry concentrate.

[0008] Considering polishing rate, surface effect, and production cost, preferably, the mass fraction of the silica abrasive is 12-18 wt%, such as 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, or 18 wt%. More preferably, the mass fraction of the silica abrasive is 15-18 wt%.

[0009] Considering polishing rate, surface effect, and production cost, preferably, the mass fraction of the accelerator is 0.1~5 wt%, such as 0.1 wt%, 0.5 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt%, or 5 wt%. More preferably, the mass fraction of the accelerator is 0.5~2%.

[0010] Preferably, the protective agent is one or more of carboxymethyl cellulose, hydroxyethyl cellulose (HEC), or hydroxypropyl cellulose. The protective agent is used to improve the polishing effect of the polishing slurry, reduce particle adhesion to the polished surface, and reduce scratches.

[0011] Preferably, the weight-average molecular weight of the protective agent is 400,000-600,000 Da. More preferably, the weight-average molecular weight of the carboxymethyl cellulose is approximately 400,000-500,000 Da, the weight-average molecular weight of the HEC is approximately 500,000-600,000 Da, and the weight-average molecular weight of the hydroxypropyl cellulose is approximately 400,000-600,000 Da. Even more preferably, the weight-average molecular weight of the HEC is 560,000 Da.

[0012] Considering polishing rate, surface effect and production cost, preferably, the mass fraction of the protective agent is 0.01~2wt%, such as 0.01wt%, 0.05wt%, 0.1wt%, 0.5wt%, 1wt%, 1.5wt% or 2wt%.

[0013] Preferably, the pH adjuster is one or more of a 25wt% tetramethylammonium hydroxide (TMAH) aqueous solution, ammonia, or piperazine hexahydrate.

[0014] Preferably, the pH of the polishing slurry concentrate is 11-12, such as 11, 11.2, 11.4, 11.6, 11.8, or 12. The pH of the polishing slurry concentrate is in an alkaline range, which helps maintain the stability of the components within the concentrate.

[0015] Preferably, the preservative is methylene bismorpholine (MBM) and / or BIT-20.

[0016] Preferably, the concentration of the preservative is 0.001~0.1wt%, such as 0.001wt%, 0.005wt%, 0.01wt%, 0.05wt%, or 0.1wt%. The preservative in the polishing slurry concentrate can inhibit and kill microorganisms, prevent pH shift and particle aggregation caused by microorganisms, and maintain the chemical stability of the polishing slurry concentrate during storage.

[0017] Preferably, the gold impurity content of the polishing slurry concentrate is <100 ppb. More preferably, the gold impurity content is 50~90 ppb, such as 50 ppb, 60 ppb, 70 ppb, 80 ppb, or 90 ppb.

[0018] The second aspect of the present invention discloses a polycrystalline silicon polishing slurry, wherein the polishing slurry is obtained by diluting the above-mentioned polishing slurry concentrate by 8 to 12 times.

[0019] For example, polishing slurry concentrate can be diluted with water by 8, 9, 10, 11 or 12 times to obtain polishing slurry.

[0020] Preferably, the polishing slurry obtained by diluting the above-mentioned concentrated polishing slurry 11 times exhibits a polishing rate of >4800 Å / min on polycrystalline silicon under the following conditions: polishing pressure of 1.5 pis, polishing speed of 63 / 57 rpm, polishing slurry flow rate of 285 ml / min, and temperature of 42°C. More preferably, the polishing rate of the polishing slurry on polycrystalline silicon is 5000~6000 Å / min.

[0021] Preferably, the polishing slurry obtained by diluting the above-mentioned concentrated polishing slurry 11 times exhibits a polishing rate of <7 Å / min on silicon oxide under the following conditions: polishing pressure of 1.5 pis, polishing speed of 63 / 57 rpm, polishing slurry flow rate of 285 ml / min, and temperature of 42°C. More preferably, the polishing rate of the polishing slurry on silicon oxide is 1~7 Å / min.

[0022] Preferably, the polishing slurry obtained by diluting the above-mentioned polishing slurry concentrate by 11 times has a polishing rate selectivity ratio of >790 for polycrystalline silicon / silicon oxide. More preferably, the selectivity ratio is 790~1500, such as 790, 800, 900, 1000, 1100, 1200, 1300, 1400 or 1500.

[0023] More preferably, the polishing slurry obtained by diluting the above-mentioned polishing slurry concentrate by 11 times has a polishing rate selectivity ratio of >950 for polycrystalline silicon / silicon oxide, and even more preferably, the selectivity ratio is 950~1500.

[0024] Preferably, the polishing slurry obtained by diluting the above-mentioned concentrated polishing slurry 11 times, under the conditions of polishing pressure of 1.5 pis, polishing speed of 63 / 57 rpm, polishing slurry flow rate of 285 ml / min, and temperature of 42°C, has a surface roughness Ra ≤ 0.5 nm after polishing. More preferably, the surface roughness Ra is 0.1~0.5 nm, such as 0.1 nm, 0.2 nm, 0.3 nm, 0.4 nm, or 0.5 nm.

[0025] Preferably, the polishing slurry obtained by diluting the above-mentioned concentrated polishing slurry 11 times, under the conditions of polishing pressure of 1.5 pis, polishing speed of 63 / 57 rpm, polishing slurry flow rate of 285 ml / min, and temperature of 42°C, has a residual particle count of 1 to 10 particles on the polished surface after polishing, such as 1, 2, 4, 6, 8, or 10 particles.

[0026] Preferably, the polishing slurry obtained by diluting the above-mentioned concentrated polishing slurry 11 times, under the conditions of polishing pressure of 1.5 pis, polishing speed of 63 / 57 rpm, polishing slurry flow rate of 285 ml / min, and temperature of 42°C, has a disc-shaped indentation amount of <350 Å on the polished surface after polishing. More preferably, the disc-shaped indentation amount is 150~350 Å, such as 150 Å, 200 Å, 250 Å, 300 Å, or 350 Å.

[0027] The third aspect of this invention discloses a method for preparing the above-mentioned polishing slurry concentrate, the method comprising: mixing and stirring silica abrasive, accelerator, protectant, preservative, pH adjuster and water evenly, and filtering to obtain the polishing slurry concentrate.

[0028] To ensure a more stable polishing slurry concentrate with better polishing rate and dispersibility, the protective agent is preferably added after pH adjustment. The protective agent is stable under alkaline conditions; therefore, pH adjustment is necessary before adding the protective agent.

[0029] Preferably, the stirring speed is 40~100 r / min, such as 40 r / min, 50 r / min, 60 r / min, 70 r / min, 80 r / min, 90 r / min or 100 r / min.

[0030] Preferably, stirring should continue for 15-30 minutes after each component is added, such as 15 min, 20 min, 25 min, or 30 min. Thorough stirring after each component addition ensures that each component is fully mixed and prevents agglomeration caused by adding all components at once.

[0031] Preferably, the filtration involves sequentially filtering the polishing slurry concentrate using a three-stage filter cartridge and a primary filter cartridge used in the filling line. More preferably, the dimensions of the three-stage filter cartridges are 2~5μm, 0.8~1.8μm, and 0.4~0.6μm, respectively; and the pore size of the primary filter cartridge used in the filling line is 0.1~0.3μm.

[0032] The fourth aspect of the present invention discloses the application of the above-mentioned polycrystalline silicon polishing slurry concentrate after dilution as a polycrystalline silicon polishing slurry.

[0033] Preferably, the application includes any one or more of the following:

[0034] 1) Improve the polishing rate of polycrystalline silicon;

[0035] 2) Improve the polysilicon / silicon oxide polishing rate selectivity ratio;

[0036] 3) Improve the surface quality of polycrystalline silicon after polishing.

[0037] More preferably, improving the surface quality of polycrystalline silicon after polishing includes one or more of reducing the surface roughness, reducing surface particle residue, or reducing the amount of dish-shaped depressions.

[0038] Preferably, the polishing slurry increases the polishing rate to 4800~6000 Å / min in polycrystalline silicon polishing, such as 4800 Å / min, 5000 Å / min, 5500 Å / min or 6000 Å / min.

[0039] Preferably, the polishing rate of the polishing slurry on silicon oxide is 1~7 Å / min.

[0040] Preferably, the polishing rate selectivity of the polishing slurry for polycrystalline silicon / silicon oxide is increased to 790~1500, such as 790, 800, 850, 900, 1000, 1100, 1200, 1300, 1400 or 1500.

[0041] Preferably, the polishing rate selectivity of the polishing slurry for polycrystalline silicon / silicon oxide is increased to 950~1500, such as 950, 1000, 1100, 1200, 1300, 1400 or 1500.

[0042] Preferably, the application includes controlling the amount of residual particles on the surface of the polycrystalline silicon wafer after polishing to be 1 to 10 particles.

[0043] Preferably, the application includes controlling the surface roughness of the polycrystalline silicon wafer to be reduced to 0.1~0.5 nm after polishing.

[0044] Preferably, the application includes controlling the amount of dish-shaped depressions on the surface of the polished polycrystalline silicon wafer to be 150~350 Å.

[0045] As described above, the high-performance polycrystalline silicon polishing slurry concentrate and its preparation method of the present invention have the following beneficial effects:

[0046] 1) The polishing slurry concentrate of this invention has a low gold and impurity content, with a total gold and impurity content of less than or equal to 100 ppb.

[0047] 2) The polishing slurry of the present invention has a polishing rate of more than 4800 Å / min for polycrystalline silicon and a polycrystalline silicon / silicon oxide polishing rate selectivity ratio of more than 790. During grinding, polycrystalline silicon can be ground quickly, reducing the silicon oxide removal rate.

[0048] 3) The polishing slurry of the present invention has an overall surface roughness Ra of less than or equal to 0.5 nm, a dish-shaped indentation amount of less than 350 Å, and a low amount of residual particles on the polished surface, with a residual number of less than or equal to 10 particles, which greatly reduces the number of scratches. Attached Figure Description

[0049] Figure 1 The polishing rate of a polycrystalline silicon wafer along the diameter direction after dilution of the polishing slurry concentrate prepared in Example 1 of this application. Detailed Implementation The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.

[0050] It should be noted that the process equipment or apparatus not specifically mentioned in the following embodiments are all conventional equipment or apparatus in the art.

[0051] Furthermore, it should be understood that the existence of other method steps before or after the combined steps, or the insertion of other method steps between these explicitly mentioned steps, does not preclude the presence of other method steps before or after the combined steps, unless otherwise stated. It should also be understood that the combined connection relationship between one or more devices / apparatus mentioned in this invention does not preclude the existence of other devices / apparatus before or after the combined devices / apparatus, or the insertion of other devices / apparatus between these explicitly mentioned devices / apparatus. Moreover, unless otherwise stated, the numbering of each method step is merely a convenient tool for identifying each method step, and not for limiting the order of the method steps or defining the scope of the invention. Changes or adjustments to their relative relationships, without substantially altering the technical content, should also be considered within the scope of the invention.

[0052] Before further describing specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terminology used in the embodiments of the present invention is for describing specific embodiments and not for limiting the scope of protection of the present invention; in the specification and claims of the present invention, unless otherwise expressly stated in the text, the singular forms "a", "an" and "this" include the plural forms.

[0053] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise stated in the present invention, both endpoints of each numerical range and any value between the two endpoints may be selected. Unless otherwise defined, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art. In addition to the specific methods, apparatus, and materials used in the embodiments, based on the knowledge of the prior art possessed by one of ordinary skill in the art and the description of this invention, any prior art methods, apparatus, and materials similar to or equivalent to those described, apparatus, and materials in the embodiments of this invention may be used to implement the present invention.

[0054] In the following embodiments of the present invention, the silica abrasive added is silica sol, and the mass fraction of silica abrasive in the silica sol is 30 wt%.

[0055] Example 1

[0056] This embodiment 1 provides a specific polishing slurry concentrate. Based on the total mass of the polishing slurry concentrate, its specific composition is as follows: 17.5 wt% silica abrasive, 1 wt% diethylenetriamine (accelerator), 0.4 wt% hydroxyethyl cellulose (HEC) (protectant), 0.005 wt% preservative (BIT-20), and the balance being pH adjuster (piperazine hexahydrate) and water. The silica abrasive is spherical with a particle size of 60-70 nm, and the weight-average molecular weight of HEC is 560,000 Da.

[0057] The specific preparation method is as follows:

[0058] 1) Add water and pH adjuster to the reactor, turn on the stirrer, adjust the pH to 11.5, and stir for 30 minutes at a speed of 50±1 r / min;

[0059] 2) Add the protective agent, keep the rotation speed constant, and stir for 15 ± 1 min.

[0060] 3) Add the accelerator, keep the speed constant, and stir for 15 ± 1 min.

[0061] 4) Add silica abrasive, keep the rotation speed constant, and stir for 30±2 min.

[0062] 5) Add preservative, keep the speed constant, and stir for 30±1 min.

[0063] 6) After the above polishing slurry concentrate is filtered through a three-stage filter element (3μm+1μm+0.5μm), it is then filtered through a first-stage filter element (0.3μm) on the bottling line and bottled to obtain the polishing slurry concentrate.

[0064] Examples 2-3

[0065] The difference between Examples 2 and 3 and Example 1 lies in the silica content in the polishing slurry concentrate. In Example 2, the silica content is 12 wt%, and in Example 3, the silica content is 18 wt%. The remaining components and preparation methods are the same as in Example 1.

[0066] Comparative Examples 1-2

[0067] The difference between Comparative Examples 1 and 2 and Example 1 is the content of silicon dioxide. The silicon dioxide content in Comparative Example 1 is 5 wt%, and the silicon dioxide content in Comparative Example 2 is 25 wt%. The other components and preparation methods are the same as those in Example 1.

[0068] Comparative Examples 3-4

[0069] The difference between Comparative Examples 3 and 4 and Example 1 is that the pH of the polishing slurry concentrate is different. The pH of the polishing slurry concentrate in Comparative Example 3 is 10, and the pH of the polishing slurry concentrate in Comparative Example 4 is 13. The other components and preparation methods are the same as those in Example 1.

[0070] Examples 4-6

[0071] The difference between Examples 4-6 and Example 1 lies in the composition and content of the accelerator. In Example 4, the accelerator is diethylenetriamine with a content of 0.5 wt%. In Example 5, the accelerator is diethylenetriamine with a content of 5 wt%. In Example 6, the accelerator is triethanolamine with a content of 1 wt%. The remaining components and preparation methods are the same as in Example 1.

[0072] Comparative Examples 5-6

[0073] The difference between Comparative Examples 5 and 6 and Example 1 lies in the composition and content of the accelerator. No accelerator was added in Comparative Example 5, while the accelerator in Comparative Example 6 was diethylenetriamine with a content of 6 wt%. The remaining components and preparation methods were the same as in Example 1.

[0074] Examples 7-9

[0075] The difference between Examples 7-9 and Example 1 lies in the composition and content of the protective agent. In Example 7, the protective agent is HEC with a content of 0.2 wt%. In Example 8, the protective agent is HEC with a content of 1.5 wt%. In Example 9, the protective agent is carboxymethyl cellulose with a weight average molecular weight of 500,000 Da and a content of 0.4 wt%. The remaining components and preparation methods are the same as in Example 1.

[0076] Comparative Examples 7-8

[0077] The difference between Comparative Examples 7 and 8 and Example 1 lies in the composition and content of the protective agent. No protective agent was added in Comparative Example 7, while the protective agent in Comparative Example 8 was HEC with a content of 2.5 wt%. The remaining components and preparation methods were the same as in Example 1.

[0078] Comparative Examples 9-10

[0079] The difference between Comparative Examples 9 and 10 and Example 1 lies in the type and particle size of the silica abrasive. In Comparative Example 9, the silica abrasive is curved and the particle size is 60-70 nm. In Comparative Example 10, the silica abrasive is spherical and the particle size is 100-120 nm. The remaining components and preparation methods are the same as in Example 1.

[0080] Comparative Examples 11-13

[0081] The difference between Comparative Examples 11-13 and Example 1 lies in the product filtration process. Comparative Example 11 does not use a three-stage filter cartridge, Comparative Example 12 does not use a first-stage filter cartridge for the filling line, and Comparative Example 13 does not use filtration. The remaining components and preparation methods are the same as in Example 1.

[0082] The formulation composition of the polishing slurry concentrate in Examples 1-9 and Comparative Examples 1-13 is shown in Table 1.

[0083] Table 1. Composition of Polishing Slurry Concentrate Formulation in Examples

[0084]

[0085] Table 1 continues.

[0086]

[0087] Test section

[0088] The performance of the polishing slurry concentrates prepared in the above embodiments and comparative examples of this application was tested. Polishing performance was tested after the polishing slurry concentrates were placed for one day following preparation. The polishing slurry concentrates were diluted with deionized water at a mass ratio of 1:10 and mixed thoroughly before polishing tests (1 part by mass of polishing slurry concentrate + 10 parts by mass of water). The process conditions for polishing 12-inch poly wafers and 12-inch oxide wafers are as follows:

[0089] Polishing equipment: Horizon

[0090] Polishing targets: 12-inch poly wafer (polycrystalline silicon wafer), 12-inch oxide wafer (silicon oxide wafer)

[0091] Polishing pad: WH6060

[0092] Polishing pressure: 1.5 psi

[0093] Polishing speed: 63 / 57 rpm

[0094] Grinding slurry flow rate: 285 mL / min

[0095] Polishing temperature: 42℃

[0096] Polishing time: 60s

[0097] 1) The polishing rate was measured using a KLA non-metallic film thickness gauge (F50). Specifically, the thickness of the 12-inch poly wafer and the 12-inch oxide wafer were measured before and after polishing. The polishing rate was calculated by dividing the thickness difference before and after polishing by the polishing time. The results are shown in Table 2.

[0098] 2) Surface roughness Ra test: The 12-inch poly wafer was tested using an atomic force microscope. The test area at each location was 10μm×10μm. The roughness at 3 locations was taken and the average value was calculated. The results are shown in Table 2.

[0099] 3) Surface particle residue: The polished 12-inch poly wafer was tested using a laser microscope to detect and count particle residue. Three samples were taken for testing, and the result is the average of the particle residue from the three tests. The results are shown in Table 2.

[0100] 4) Metal content: The concentration of metal ions in the polishing slurry was detected using an Agilent 7900 ICP-MS system.

[0101] 5) Disk-shaped defects: A Dektak XTL step profiler was used to test a 12-inch poly wafer.

[0102] Measurement principle: The diamond probe of the profilometer is pressed against the sample surface with constant pressure and scans at a uniform speed to acquire the longitudinal height profile curve in real time. The dish-shaped depression is characterized by an arc-shaped profile with high reference planes on both sides and low central area. By fitting the sample to effectively flatten the reference plane, the vertical height difference between the reference plane and the lowest point of the depression is calculated, which is the amount of dish-shaped depression.

[0103] Standardized measurement operation procedures:

[0104] ① Alignment and leveling: Move the stage along the X and Y axes to position the scanning start point on a flat reference area on one side of the sample, and confirm that the probe is vertically aligned with the surface to be measured without tilting or offset.

[0105] ② Probe placement: Start the automatic probe placement program, slowly lower the probe, and lock the initial position after the software shows that the probe is in normal contact with the surface and the contact signal is stable.

[0106] ③ Formal Scan: After confirming that the parameters are correct, start the scan and observe the contour curve throughout the process. If any abnormalities such as sudden changes, jump points, or broken lines occur, immediately pause and terminate the scan, check for problems with the sample and equipment, and then retest.

[0107] ④ Multi-point repeated testing: The same depression area to be tested is scanned 3 times in parallel; 3 measuring points are selected at different symmetrical positions of the sample to obtain a total of 9 sets of valid contour data, and outliers are eliminated.

[0108] ⑤ Lifting and returning the probe to its original position: After a single scan is completed, the probe is automatically lifted to a safe height. After all tests are completed, the stage and probe are reset to the original position of the equipment.

[0109] The polishing slurry concentrate prepared in Example 1 was diluted 11 times, and the polishing rate was measured and calculated at different locations on the surface of a 12-inch poly wafer after polishing. Figure 1 As shown, Figure 1 The vertical axis represents the polycrystalline silicon polishing rate, and the horizontal axis represents the distance moved in opposite directions from the wafer center. Figure 1 It can be seen that the polishing rate is different along the wafer diameter direction. The average polishing rate is calculated and recorded in Table 2. The other polishing rates are calculated in the same way.

[0110] Table 2. Performance test results of polishing slurry prepared after dilution of polishing slurry concentrate.

[0111]

[0112] As shown in Table 2, the polishing rates of polycrystalline silicon prepared in Examples 1-9 of this application after dilution of the polycrystalline silicon polishing slurry concentrate are all >5000 Å / min, the polishing rate of silicon oxide is <7 Å / min, the selectivity ratio of polycrystalline silicon to silicon oxide in the polishing slurry is >790, the surface roughness is ≤0.5 nm, the residual amount of surface particles is ≤10, the amount of dish-shaped depressions is <350 Å, and the total gold impurity content of the polishing slurry is <100 ppb.

[0113] As can be seen from Table 2 of the various examples and comparative examples: the polishing slurries prepared in Examples 1-3 showed an increase in the polishing rate of polycrystalline silicon with the increase of silicon dioxide, and an increase in the polishing rate selectivity ratio of polycrystalline silicon to silicon dioxide. However, the amount of dish-shaped depressions and the content of gold impurities also increased slightly, and the surface roughness and surface particle residue did not change much. Combined with Comparative Example 2, it was found that when the silicon dioxide solid content increased to 25%, the polishing rate of silicon dioxide by the polishing slurry increased significantly, but the polishing rate of polycrystalline silicon did not increase much, resulting in a significant decrease in the selectivity ratio, a significant increase in surface roughness and the amount of dish-shaped depressions, and a decrease in polishing quality. The concentrated polishing slurries in Examples 1 and Comparative Examples 3-4 had different pH values. When the pH was too low, the polishing rate of polycrystalline silicon decreased significantly. When the pH was too high (13), the polishing rate of silicon dioxide increased significantly, the polycrystalline silicon / silicon dioxide selectivity ratio decreased, and the amount of dish-shaped depressions increased after polishing, resulting in a decrease in polishing quality.

[0114] In Examples 1, 4-6, and Comparative Examples 5-6, the accelerator content varied. Increasing the accelerator content significantly increased the polishing rate of polycrystalline silicon. The polishing rate of silicon oxide remained unchanged when the accelerator content varied from 0 to 1 wt%. Compared to Example 1, in Example 5, with the accelerator increased to 5 wt%, the silicon oxide polishing rate increased to 7 Å / min, while the polycrystalline silicon polishing rate only increased from 5502 Å / min to 5567 Å / min, resulting in a significant decrease in the polycrystalline silicon / silicon oxide selectivity ratio to 795. In Comparative Example 5, without the addition of an accelerator, the polycrystalline silicon polishing rate decreased significantly. Compared to Example 5, in Comparative Example 6, with the accelerator content increased to 6 wt%, the polycrystalline silicon polishing rate did not increase, but the silicon dioxide polishing rate increased significantly, resulting in a decrease in the selectivity ratio to 617 and excessive dish-shaped indentation after polishing. In Example 6, triethanolamine was used as the accelerator; although the polycrystalline silicon polishing rate was only 4856 Å / min, the selectivity was high, resulting in only 273 dish-shaped indentations after polishing. The overall polishing quality was good. In Examples 1, 7-9, and Comparative Examples 7-8, the content of the protective agent varied. As the protective agent content increased, the amount of polished disc-shaped depressions gradually decreased, but the overall polishing rate of polycrystalline silicon showed a downward trend, while the polishing rate of silicon dioxide did not change significantly, leading to a gradual decrease in selectivity. Comparative Example 7 showed that without adding a protective agent, the particle residue after polishing was >10000, and the disc-shaped defects were obvious. Comparative Example 8 showed that when the amount of protective agent added was too high, the polycrystalline silicon polishing rate was only 4460 Å / min, and the gold impurity content exceeded 100 ppb. Examples 1 and Comparative Examples 9-10 used different silicon dioxide abrasives. Comparative Example 9 used a curved type, which led to a significant increase in polishing particle residue and surface roughness, resulting in a decrease in polishing quality. Comparative Example 10 used silicon dioxide with a particle size of 100-120 nm, resulting in the same polishing surface roughness, but with increased particle residue and disc-shaped depressions, and a decrease in polishing quality. Comparative Examples 11-13 used different filtration methods. In Comparative Example 11, a 0.3μm canister filter was used directly without a three-stage filter, which caused the canister filter to become clogged, wasting time and filter cartridges. The repeated replacement of filter cartridges led to an increase in gold impurities. With only three-stage filtration or no filtration at all, the amount of residual particles and disc-shaped depressions on the surface of the polishing liquid was too large, and the polishing quality did not meet the standards.

[0115] In summary, the total gold impurity content of the polycrystalline silicon polishing slurry concentrate prepared by this invention is <100ppb, the polishing rate of the polycrystalline silicon after dilution of the concentrate is >5000 Å / min, the polishing rate of silicon oxide is <7 Å / min, the selectivity ratio of polycrystalline silicon to silicon oxide in the polishing slurry is >790, the surface roughness of the polycrystalline silicon wafer after polishing is ≤0.5nm, the residual amount of surface particles is ≤10, and the amount of dish-shaped depressions is <350 Å.

[0116] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any form or substance. It should be noted that those skilled in the art can make various improvements and additions without departing from the method of the present invention, and these improvements and additions should also be considered within the scope of protection of the present invention. Any modifications, alterations, and equivalent changes made by those skilled in the art based on the above-disclosed technical content without departing from the spirit and scope of the present invention are equivalent embodiments of the present invention. Furthermore, any modifications, alterations, and evolutions made to the above embodiments based on the essential technology of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A polycrystalline silicon polishing slurry concentrate, characterized in that, The polishing slurry concentrate comprises the following raw material components by mass fraction: 10-20 wt% silica abrasive, 0.1-5 wt% accelerator, 0.2-2 wt% protectant, 0.001-0.1 wt% preservative, with the balance being pH adjuster and water. The pH adjuster adjusts the pH of the polishing slurry concentrate to 11-12. The accelerator is one or more of tetramethylammonium hydroxide, triethanolamine, or diethylenetriamine. The protectant is one or more of carboxymethyl cellulose, hydroxyethyl cellulose, or hydroxypropyl cellulose. The silica is in spherical particles with a particle size of 60-70 nm.

2. The polycrystalline silicon polishing slurry concentrate according to claim 1, characterized in that, The weight-average molecular weight of the protective agent is 400,000-600,000 Da; And / or, the preservative is methylene bismorpholine and / or BIT-20.

3. The polycrystalline silicon polishing slurry concentrate according to claim 1, characterized in that, The pH adjuster is one or more of a 25wt% tetramethylammonium hydroxide aqueous solution, ammonia, or piperazine hexahydrate.

4. A polycrystalline silicon polishing slurry, characterized in that, It is obtained by diluting the polishing slurry concentrate according to any one of claims 1-3 by 8-12 times.

5. A method for preparing a polycrystalline silicon polishing slurry concentrate as described in any one of claims 1 to 3, characterized in that, The preparation method includes: mixing and stirring silica abrasive, accelerator, protectant, preservative, pH adjuster and water evenly, and filtering to obtain the polishing fluid concentrate.

6. The preparation method according to claim 5, characterized in that, The protective agent is added after pH adjustment.

7. The preparation method according to claim 5, characterized in that, The stirring speed is 40~100 r / min; And / or, after each component is added, stirring should continue for 15 to 30 minutes; And / or, the filtration is to sequentially filter the polishing slurry concentrate using a three-stage filter cartridge and a primary filter cartridge in the filling line.

8. The preparation method according to claim 7, characterized in that, The dimensions of the three-stage filter elements are 2~5μm, 0.8~1.8μm, and 0.4~0.6μm, respectively. And / or, the size of the primary filter element of the filling line is 0.1~0.3μm.

9. The application of the polycrystalline silicon polishing slurry concentrate according to any one of claims 1 to 3, after dilution, as a polycrystalline silicon polishing slurry.

10. The application according to claim 9, characterized in that, The applications include any one or more of the following: 1) Improve the polishing rate of polycrystalline silicon; 2) Improve the polysilicon / silicon oxide polishing selectivity ratio; 3) Improve the surface quality of polycrystalline silicon after polishing.

Citation Information

Patent Citations

  • Chemical mechanical polishing liquid for polycrystalline silicon

    CN101652445B