A polycrystalline diamond polishing slurry and its efficient polishing method for ultra-smooth surfaces
By using a polishing slurry with specific components and a single-crystal silicon polishing pad at room temperature and pressure, atomic-level smooth surface polishing of polycrystalline diamond was achieved, solving the problems of low efficiency and high cost in existing technologies, making it suitable for industrial production in high-end fields.
Patent Information
- Application Number
- CN202611438193.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polycrystalline diamond polishing methods suffer from low polishing efficiency, poor surface quality, inability to achieve simultaneous oxidation of grains and grain boundaries, and high processing costs, making it difficult to meet the industrial mass production needs of high-end fields.
A polishing slurry with a composition of 0.1-10 wt% abrasive, 1-50 wt% oxidant, and 0.5-2 wt% dispersant is used. A single-crystal silicon polishing pad is used at room temperature and pressure. The strong oxidizing free radicals generated by the oxidant form Si-OC covalent bonds with the diamond surface. Combined with micro-cutting by the abrasive, chemical-mechanical synergistic polishing is achieved.
Atomic-level smooth surface polishing was achieved at room temperature and pressure, which significantly improved the material removal rate, reduced processing costs and equipment investment, and is suitable for the industrial mass production of large-size polycrystalline diamond wafers.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ultra-precision machining technology, specifically relating to a polycrystalline diamond polishing slurry and its efficient polishing method for ultra-smooth surfaces. This method is suitable for atomic-level planarization of semiconductor-grade polycrystalline diamond wafers and can be widely applied to the preparation of diamond substrates in high-end fields such as power devices and thermal management components, solving the technical challenges of large-scale, high-quality processing of polycrystalline diamond. Background Technology
[0002] Diamond, as the hardest known material in nature, possesses ultra-high thermal conductivity, excellent chemical stability, and superior semiconductor properties, making it irreplaceable in high-end fields such as next-generation power electronics, aerospace, and optical engineering. Polycrystalline diamond (PCD) can be fabricated at the large wafer level through chemical vapor deposition (CVD), solving the size limitation problem of single-crystal diamond. However, its high hardness, crystal anisotropy, and the presence of grain boundaries pose significant challenges to ultra-precision machining.
[0003] In existing polycrystalline diamond polishing methods, conventional liquid-phase polishing relies solely on mechanical cutting, resulting in low polishing efficiency and poor surface quality. It also fails to eliminate grain boundary steps and uneven removal caused by anisotropy. Grinding wheel mechanical polishing is simple and adaptable, compensating for the shortcomings of liquid-phase polishing. However, mechanical grinding easily leads to subsurface damage, and grinding wheels wear easily, requiring frequent dressing and exhibiting poor stability, limiting its application in high-precision machining. Plasma-assisted polishing (PAP) can achieve atomically smooth surfaces, but it relies on expensive vacuum plasma equipment, making the process complex and difficult to operate, hindering large-scale production. In contrast, chemical mechanical polishing (CMP), with its synergistic effect of chemical oxidation and mechanical grinding, can better balance processing efficiency and surface quality, and has become the most widely used and best-performing ultra-precision polishing technology. However, traditional CMP processes have poor chemical selectivity, failing to achieve simultaneous oxidation of grains and grain boundaries. This results in surface roughness that is difficult to achieve below the nanometer level, and low material removal efficiency, failing to meet the processing requirements of high-end diamond substrates.
[0004] Researchers often improve CMP processing efficiency and surface quality by adjusting the composition of polishing slurries, but these methods still have significant limitations. For example, CN202411841870.1 discloses a two-step zeta potential-controlled chemical mechanical polishing method for polycrystalline diamond, which performs mechanical rough polishing and fine polishing on polycrystalline diamond films, and then uses polishing slurries A and B to control the zeta potential to complete the chemical mechanical rough polishing and fine polishing. However, this method is lengthy, the process parameters are difficult to control precisely, and the polishing slurry formulation is complex and costly, resulting in insufficient overall process stability. CN202410901504.4 discloses a polishing slurry and polishing method for polycrystalline diamond, which uses large-particle-size diamond microparticles to rough grind polycrystalline diamond, and then uses a polishing slurry prepared with diamond microparticles, potassium permanganate, and water for CMP polishing. Although the surface roughness of the polished sample is less than 1 nm, the processing requires acid replenishment, the steps are cumbersome, the processing cycle is long, and the polishing efficiency is low, making it difficult to meet the needs of industrial mass production.
[0005] The numerous limitations of existing polishing methods severely restrict the promotion and application of polycrystalline diamond materials in high-end fields. Currently, the industry still lacks a highly efficient ultra-precision polishing technology that is simple to operate, low in cost, suitable for large-scale mass production, and can stably obtain grain boundary-free and atomically flat surfaces. In view of this, this application was developed. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of existing technologies and address numerous problems in current polycrystalline diamond processing by providing a polycrystalline diamond polishing slurry and a highly efficient polishing method for achieving ultra-smooth surfaces. This method fundamentally breaks through the limitations of simply optimizing the polishing slurry composition in CMP processes, achieving atomically smooth surfaces with high efficiency and low damage. The processing is carried out at room temperature and pressure, the polishing method has low equipment requirements, a simple polishing slurry composition, and strong parameter controllability, significantly reducing processing costs and meeting the industrial-scale mass production needs of 2-inch and larger polycrystalline diamond wafers.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: A polishing slurry, wherein the weight percentages of each component of the polishing slurry are as follows: 0.1-10 wt% abrasive, 1-50 wt% oxidant, 0.5-2 wt% dispersant, and the balance being deionized water; the oxidant is one of 28-30 wt% hydrogen peroxide, potassium permanganate, potassium ferrate, etc.; and the pH of the polishing slurry is 3-6.
[0008] Furthermore, the abrasive can be one or more of nanodiamond, cubic boron nitride, boron carbide, alumina, etc.; the abrasive particle size is 50-200 nm, the solid content is 0.1-10 wt%, and there is no obvious agglomeration phenomenon, which ensures the uniformity and non-damage of micro-cutting and avoids scratches and microcracks on the surface of polycrystalline diamond due to abrasive particle agglomeration.
[0009] More preferably, when the oxidant is 28-30 wt% hydrogen peroxide (H2O2), the addition amount is 10-50 wt%; as a source of active oxygen, it stably decomposes under pH=3-6 conditions to generate hydroxyl radicals (·OH), which are used to oxidize the surface of diamond and single crystal silicon, promoting the formation of Si-OC covalent bonds between the two; it can be replaced by one of potassium permanganate (KMnO4), potassium ferrate (K2FeO4), etc., and the addition amount is adjusted to 1-5 wt% after replacement.
[0010] Furthermore, the dispersant can be one or more of the following: polyacrylate, polycarboxylate, organophosphonate, high molecular weight nonionic dispersant, inorganic phosphate, etc. This includes, but is not limited to, sodium polyacrylate (PAAS), ammonium polyacrylate (PAANH4), polymethacrylate (PMAA), polyacrylate-acrylate copolymer salt, polyethylene glycol (PEG), sodium hexametaphosphate, sodium pyrophosphate, polyvinylpyrrolidone (PVP), aminotrimethylenephosphonic acid (ATMP), etc. The dispersant is added at an amount of 0.5-2 wt% to stabilize the suspension of nanodiamond powder in the polishing slurry, prevent abrasive particle agglomeration, and simultaneously improve the fluidity of the polishing slurry to ensure sufficient reaction at the polishing interface.
[0011] A method for high-efficiency polishing of polycrystalline diamond ultra-smooth surfaces using the polishing slurry involves selecting a monocrystalline silicon polishing pad. The strong oxidizing free radicals generated by the oxidant in the polishing slurry cause the monocrystalline silicon polishing pad to generate hydroxyl groups on the diamond surface and dehydrate to form Si-OC covalent bonds. Combined with the micro-cutting of abrasives in the polishing slurry to smooth and remove the surface, the method achieves high-efficiency and low-damage polishing of polycrystalline diamond.
[0012] Furthermore, the above-mentioned high-efficiency polishing method specifically includes the following steps: (1) Polishing solution preparation: Mix deionized water, dispersant and abrasive evenly, add oxidant and mix well, adjust pH to 3-6 using pH adjuster to obtain polishing solution; (2) Chemical-mechanical polishing: Polycrystalline diamond wafers with Ra≤50 nm are bonded to a single-crystal silicon polishing pad and polished at room temperature and pressure under set process parameters, with polishing fluid continuously supplied during the polishing process; (3) Post-processing: After polishing, the polished polycrystalline diamond sheet is cleaned to obtain the final product.
[0013] Furthermore, in step (1), the pH adjuster is dilute nitric acid or dilute sulfuric acid with a concentration of 1-5 mol / L.
[0014] Furthermore, in step (2), the single-crystal silicon polishing pad is a single-crystal silicon (100) polishing pad with a diameter ≥ 2 inches. For example, the diameter can be 152.4mm±1mm, 228.6mm±1mm, 304.8±1mm, 381±1mm, 457.2±1mm, etc.; the initial surface roughness Ra=0.8-1.5 μm, and the diameter ratio of the workpiece to the single-crystal silicon polishing pad is 1:3-1:5 (the polishing pad diameter is pre-selected according to 1:3).
[0015] Furthermore, in step (2), the process parameters for the chemical-mechanical polishing are: polishing pressure 300-1000 g / cm. 2 The polishing disc speed is 60-120 rpm, the workpiece speed is 10-20 rpm, the polishing fluid flow rate is 2-20 mL / min, and the temperature is 18-45℃.
[0016] As a preferred technical solution, the above-mentioned high-efficiency polishing method specifically includes the following steps: S1: Polishing fluid preparation: Deionized water, dispersant, and abrasive are mixed in a specific ratio and ultrasonically dispersed for 30-60 minutes until the abrasive is uniformly dispersed. An oxidant is added and stirred for 10-15 minutes until homogeneous. The pH value is adjusted to 3-6 using a pH adjuster and stirred for 10-15 minutes to obtain a stable polishing solution. Preferably, the pH adjuster in step S1 is dilute nitric acid or dilute sulfuric acid with a concentration of 1-5 mol / L, used to precisely adjust the pH value of the polishing solution to 3-6. This pH range effectively inhibits the rapid decomposition of hydrogen peroxide, extending the service life of the polishing solution. Simultaneously, this acidic range provides a suitable active environment for the oxidation reaction, significantly increasing the reaction rate and polishing efficiency, while avoiding excessive H⁺ attack caused by an overly acidic system, effectively inhibiting excessive oxidation and corrosion damage to the polycrystalline diamond surface, thus balancing oxidation efficiency and surface quality stability.
[0017] S2: Chemical-Mechanical Polishing like Figure 1As shown, the pre-processed polycrystalline diamond sheet 3 is placed in a limiting fixture for fixed constraint. A vacuum chuck 4 is used for adsorption, positioning, and limiting fixation, ensuring the workpiece is stably attached to the monocrystalline silicon polishing disk 2. The overall clamping is firm, and the force is uniform without deviation. The polishing surface is tightly attached to the monocrystalline silicon polishing disk 2, the polishing head 5 is lowered, the polishing process parameters are set, and the polishing machine turntable 1 is started. Polishing is performed at room temperature and pressure under the set process parameters. Polishing fluid 6 is continuously supplied during the polishing process to ensure full contact and reaction at the polishing interface, achieving a synergistic effect of chemical oxidation activation and mechanical cutting. Preferably, the surface roughness Ra of the polycrystalline diamond sheet in step S2 is ≤50 nm, and the diameter is ≥2 inches. The polishing pads used in step S2 are single-crystal silicon (100) polishing pads with diameters of 152.4 mm ± 1 mm, 228.6 mm ± 1 mm, 304.8 ± 1 mm, 381 ± 1 mm, and 457.2 ± 1 mm. The initial surface roughness Ra is 0.8-1.5 μm. The pad diameter is selected according to a 1:3 ratio between the workpiece and the single-crystal silicon polishing pad diameter to ensure uniformity of linear velocity and pressure across the entire surface, fully utilizing the Si-OC interfacial bonding and chemo-mechanical synergy. The polishing pad has a convexity of 10-15 μm and an initial surface roughness Ra of 0.8-1.5 μm, retaining appropriate micro-protrusions to facilitate the penetration of active oxygen in the polishing slurry and the occurrence of interfacial reactions. The polishing process parameters in step S2 are: polishing pressure 300-1000 g / cm³. 2 The polishing disc speed is 60-120 rpm, the workpiece speed is 10-20 rpm, the polishing fluid flow rate is 2-20 mL / min, and the temperature is 18-45℃.
[0018] S3: Post-processing: After polishing, the polycrystalline diamond sheet is cleaned sequentially with acetone, alcohol, and deionized water to remove residual abrasive particles, oxidation products, and organic matter from the surface. After cleaning, it is dried with nitrogen to obtain an atomically smooth polycrystalline diamond product.
[0019] This invention uses abrasives, oxidants, dispersants and other main ingredients to formulate a special polishing slurry. It selects a single-crystal silicon polishing pad and, under normal temperature and pressure conditions, reduces the C-C bond energy through chemical action. Combined with the synergistic effect of mechanical cutting, it achieves ultra-precision polishing of polycrystalline diamond.
[0020] Compared with the prior art, the present invention has the following advantages and beneficial effects: This invention uses a monocrystalline silicon disk as the core reaction carrier for a synergistic chemical-mechanical reaction, with oxidation activation and interfacial bonding as the core mechanisms. It utilizes strong oxidative free radicals generated by a liquid-phase oxidant to simultaneously activate the diamond substrate and the surface of the monocrystalline silicon polishing disk. This causes hydroxyl groups to form Si-OC covalent bonds between the monocrystalline silicon polishing disk and the diamond surface, which are then dehydrated. Combined with the micro-cutting action of abrasives, uniform and smooth material removal is achieved. This invention can obtain an atomically smooth surface with high efficiency and low damage, fundamentally breaking through the limitations of simply optimizing the composition of the polishing slurry. After polishing, the surface roughness of the polycrystalline diamond sheet Ra≤1 nm, with no obvious subsurface damage, can directly meet the requirements of semiconductor-grade applications.
[0021] Compared with traditional chemical mechanical polishing, the material removal rate of this invention is significantly improved, which can greatly shorten the processing cycle and improve production efficiency. The entire polishing process is carried out under normal temperature and pressure conditions, the process parameters are easy to control, and it can be adapted to the polishing of polycrystalline diamond wafers of 2 inches and above, with uniform and stable polishing effect.
[0022] This invention can be implemented directly on conventional polishing machines, reducing equipment investment by about 70%; the single-crystal silicon polishing pads experience mild wear, are reusable, and require no laser repair, significantly reducing equipment investment and maintenance costs; the polishing slurry has a simple composition, low cost, and good process stability, making it suitable for industrial mass production. Attached Figure Description
[0023] Figure 1 This is a schematic diagram of the polishing system of the present invention; in the figure, 1-polishing machine turntable; 2-monocrystalline silicon polishing disk; 3-polycrystalline diamond sheet; 4-vacuum chuck; 5-polishing head; 6-polishing fluid.
[0024] Figure 2 The image shows the AFM image of the processed sample from Example 1. Detailed Implementation
[0025] The present invention will be described in more detail below through specific embodiments, which are intended to illustrate the technical solutions of the present invention, rather than to limit it. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
[0026] This invention uses atomic force microscopy (AFM) to detect the surface roughness of a 10×10 μm area, weighs it using a precision electronic balance, and then calculates the material removal rate.
[0027] In the following embodiments, all raw materials used are commercially available products that can be directly purchased, or can be prepared using conventional techniques in the art. For example, the single-crystal silicon polishing disc (100) used was purchased from Zhengzhou Abrasives & Grinding Research Institute Co., Ltd., model ZZSM-Si-P-172, with diameters of 152.4mm±1mm, 228.6mm±1mm, 304.8±1mm, 381±1mm, and 457.2±1mm; the initial surface roughness Ra is approximately 1.0 μm, and the disc diameter is selected according to a workpiece to single-crystal silicon polishing disc diameter ratio of 1:3. The convexity of the polishing disc is approximately 15μm.
[0028] In the embodiments, the hydrogen peroxide used is hydrogen peroxide with a mass concentration of approximately 30%. Example 1
[0029] The object to be processed is a 2-inch polycrystalline diamond sheet with a thickness of 400 μm and a Ra value of 47 nm after pretreatment.
[0030] S1: Polishing fluid preparation Add 68 wt% deionized water to a beaker, add 1 wt% sodium polyacrylate dispersant, and stir to dissolve; add 1 wt% nano diamond powder with an abrasive particle size of 100 nm, and ultrasonically disperse for 45 min; slowly add 30 wt% hydrogen peroxide, and stir evenly; adjust the pH to 4.5 with 1 mol / L dilute nitric acid, and stir for 15 min to obtain a uniform and stable polishing solution.
[0031] S2: Chemical-Mechanical Polishing The polycrystalline diamond wafer to be processed is bonded to a monocrystalline silicon polishing pad, and polished using the monocrystalline silicon polishing pad and the aforementioned polishing slurry. The polishing slurry is continuously supplied during the polishing process. Specific parameters are: polishing pressure 740 g / cm². 2 The polishing disc rotated at 100 rpm, the workpiece rotated at 15 rpm, the polishing fluid flow rate was 3 mL / min, the polishing temperature was 25℃, and the polishing lasted for 15 hours.
[0032] S3: Post-processing After polishing, the polished polycrystalline diamond sheet is cleaned with acetone, alcohol, and deionized water in sequence. After cleaning, it is dried with nitrogen gas to obtain a finished polycrystalline diamond product with atomically smooth surface.
[0033] The surface roughness Ra was measured to be 0.63 nm using AFM, and the material removal rate was calculated to be 93 nm / h using a precision electronic balance.
[0034] Figure 2AFM images of the sample processed in Example 1 are presented, with a scanning range of 10.0 μm × 10.0 μm. The images show that the overall surface of the 2-inch polycrystalline diamond sheet after chemical-mechanical polishing (CMP) is relatively smooth, with a measured surface roughness Ra of 0.63 nm, achieving an atomic-level smoothness effect of Ra < 1 nm. Simultaneously, some faint processing textures are observed, without deep scratches, pits, or significant surface undulations. Combined with the process results, this demonstrates that the CMP scheme using a single-crystal silicon polishing pad in conjunction with this nanodiamond polishing slurry can achieve efficient removal of impurities from polycrystalline diamond sheets while obtaining a high-quality, ultra-smooth diamond surface. Example 2
[0035] The object to be processed is a 2-inch polycrystalline diamond sheet with a thickness of 400 μm and a Ra value of 45 nm after pretreatment.
[0036] S1: Polishing fluid preparation Add 95 wt% deionized water to a beaker, add 1 wt% sodium polyacrylate dispersant, and stir to dissolve; add 1 wt% nano diamond powder with an abrasive particle size of 100 nm, and ultrasonically disperse for 45 min; slowly add 3 wt% potassium permanganate, and stir until uniform; adjust the pH to 4.5 with 1 mol / L dilute nitric acid, and stir for 15 min to obtain a uniform and stable polishing solution.
[0037] S2: Chemical-Mechanical Polishing The polycrystalline diamond wafer to be processed is bonded to a monocrystalline silicon polishing pad, and polished using the monocrystalline silicon polishing pad and the aforementioned polishing slurry. The polishing slurry is continuously supplied during the polishing process. Specific parameters are: polishing pressure 740 g / cm². 2 The polishing disc rotated at 100 rpm, the workpiece rotated at 15 rpm, the polishing fluid flow rate was 3 mL / min, the polishing temperature was 25℃, and the polishing lasted for 15 hours.
[0038] S3: Post-processing After polishing, the polished polycrystalline diamond sheet is cleaned with acetone, alcohol, and deionized water in sequence. After cleaning, it is dried with nitrogen gas to obtain a finished polycrystalline diamond product with atomically smooth surface.
[0039] The surface roughness Ra was measured to be 0.77 nm using AFM, and the material removal rate was calculated to be 84 nm / h using a precision electronic balance. Example 3
[0040] The object to be processed is a 2-inch polycrystalline diamond sheet with a thickness of 400 μm and a Ra value of 48 nm after pretreatment.
[0041] S1: Polishing fluid preparation Add 68 wt% deionized water to a beaker, add 1 wt% sodium polyacrylate dispersant, and stir to dissolve; add 1 wt% cubic boron nitride powder with an abrasive particle size of 100 nm, and ultrasonically disperse for 45 min; slowly add 30 wt% hydrogen peroxide, and stir until uniform; adjust the pH to 4.5 with 1 mol / L dilute nitric acid, and stir for 15 min to obtain a uniform and stable polishing solution.
[0042] S2: Chemical-Mechanical Polishing The polycrystalline diamond wafer to be processed is bonded to a monocrystalline silicon polishing pad, and polished using the monocrystalline silicon polishing pad and the aforementioned polishing slurry. The polishing slurry is continuously supplied during the polishing process. Specific parameters are: polishing pressure 740 g / cm². 2 The polishing disc rotated at 100 rpm, the workpiece rotated at 15 rpm, the polishing fluid flow rate was 3 mL / min, the polishing temperature was 25℃, and the polishing lasted for 15 hours.
[0043] S3: Post-processing After polishing, the polished polycrystalline diamond sheet is cleaned with acetone, alcohol, and deionized water in sequence. After cleaning, it is dried with nitrogen gas to obtain a finished polycrystalline diamond product with atomically smooth surface.
[0044] The surface roughness Ra was measured to be 0.79 nm using AFM, and the material removal rate was calculated to be 73 nm / h using a precision electronic balance. Example 4
[0045] The object to be processed is a 2-inch polycrystalline diamond sheet with a thickness of 400 μm and a Ra value of 45 nm after pretreatment.
[0046] S1: Polishing fluid preparation Add 68 wt% deionized water to a beaker, add 1 wt% sodium polyacrylate dispersant, and stir to dissolve; then add 1 wt% nano diamond powder with an abrasive particle size of 50 nm, and ultrasonically disperse for 45 min; slowly add 30 wt% hydrogen peroxide, and stir evenly; adjust the pH to 4.5 with 1 mol / L dilute nitric acid, and stir for 15 min to obtain a uniform and stable polishing solution.
[0047] S2: Chemical-Mechanical Polishing The polycrystalline diamond wafer to be processed is bonded to a monocrystalline silicon polishing pad, and polished using the monocrystalline silicon polishing pad and the aforementioned polishing slurry. The polishing slurry is continuously supplied during the polishing process. Specific parameters are: polishing pressure 740 g / cm². 2 The polishing disc rotated at 100 rpm, the workpiece rotated at 15 rpm, the polishing fluid flow rate was 3 mL / min, the polishing temperature was 25℃, and the polishing lasted for 15 hours.
[0048] S3: Post-processing After polishing, the polished polycrystalline diamond sheet is cleaned with acetone, alcohol, and deionized water in sequence. After cleaning, it is dried with nitrogen gas to obtain a finished polycrystalline diamond product with atomically smooth surface.
[0049] The surface roughness Ra was measured to be 0.86 nm using AFM, and the material removal rate was calculated to be 76 nm / h using a precision electronic balance. Example 5
[0050] The object to be processed is a 2-inch polycrystalline diamond sheet with a thickness of 400 μm and a Ra value of 46 nm after pretreatment.
[0051] S1: Polishing fluid preparation Add 68 wt% deionized water to a beaker, add 1 wt% sodium polyacrylate dispersant, and stir to dissolve; then add 1 wt% nano diamond powder with an abrasive particle size of 200 nm, and ultrasonically disperse for 45 min; slowly add 30 wt% hydrogen peroxide, and stir evenly; adjust the pH to 4.5 with 1 mol / L dilute nitric acid, and stir for 15 min to obtain a uniform and stable polishing solution.
[0052] S2: Chemical-Mechanical Polishing The polycrystalline diamond wafer to be processed is bonded to a monocrystalline silicon polishing pad, and polished using the monocrystalline silicon polishing pad and the aforementioned polishing slurry. The polishing slurry is continuously supplied during the polishing process. Specific parameters are: polishing pressure 740 g / cm². 2 The polishing disc rotated at 100 rpm, the workpiece rotated at 15 rpm, the polishing fluid flow rate was 3 mL / min, the polishing temperature was 25℃, and the polishing lasted for 15 hours.
[0053] S3: Post-processing After polishing, the polished polycrystalline diamond sheet is cleaned with acetone, alcohol, and deionized water in sequence. After cleaning, it is dried with nitrogen gas to obtain a finished polycrystalline diamond product with atomically smooth surface.
[0054] The surface roughness Ra was measured to be 0.96 nm using AFM, and the material removal rate was calculated to be 90 nm / h using a precision electronic balance. Example 6
[0055] The object to be processed is a 4-inch polycrystalline diamond sheet with a thickness of 400 μm and a Ra value of 48 nm after pretreatment.
[0056] S1: Polishing fluid preparation Add 68 wt% deionized water to a beaker, add 1 wt% sodium polyacrylate dispersant, and stir to dissolve; add 1 wt% nano diamond powder with an abrasive particle size of 100 nm, and ultrasonically disperse for 45 min; slowly add 30 wt% hydrogen peroxide, and stir evenly; adjust the pH to 4.5 with 1 mol / L dilute nitric acid, and stir for 15 min to obtain a uniform and stable polishing solution.
[0057] S2: Chemical-Mechanical Polishing The polycrystalline diamond wafer to be processed is bonded to a monocrystalline silicon polishing pad, and polished using the monocrystalline silicon polishing pad and the aforementioned polishing slurry. The polishing slurry is continuously supplied during the polishing process. Specific parameters are: polishing pressure 320 g / cm². 2 The polishing disc rotated at 100 rpm, the workpiece rotated at 15 rpm, the polishing fluid flow rate was 3 mL / min, the polishing temperature was 25℃, and the polishing lasted for 15 hours.
[0058] S3: Post-processing After polishing, the polished polycrystalline diamond sheet is cleaned with acetone, alcohol, and deionized water in sequence. After cleaning, it is dried with nitrogen gas to obtain a finished polycrystalline diamond product with atomically smooth surface.
[0059] The surface roughness Ra was measured to be 0.72 nm using AFM, and the material removal rate was calculated to be 78 nm / h using a precision electronic balance.
[0060] Comparative Example 1
[0061] The object to be processed is a 2-inch polycrystalline diamond sheet with a thickness of 400 μm and a Ra value of 46 nm after pretreatment.
[0062] S1: Polishing fluid preparation Add 98 wt% deionized water to a beaker, add 1 wt% sodium polyacrylate dispersant, and stir to dissolve; then add 1 wt% nano diamond powder with an abrasive particle size of 100 nm, and ultrasonically disperse for 45 min; adjust the pH to 4.5 with 1 mol / L dilute nitric acid, and stir for 15 min to obtain a uniform and stable polishing solution.
[0063] S2: Chemical-Mechanical Polishing The polycrystalline diamond wafer to be processed is bonded to a monocrystalline silicon polishing pad, and polished using the monocrystalline silicon polishing pad and the aforementioned polishing slurry. The polishing slurry is continuously supplied during the polishing process. Specific parameters are: polishing pressure 740 g / cm². 2 The polishing disc rotated at 100 rpm, the workpiece rotated at 15 rpm, the polishing fluid flow rate was 3 mL / min, the polishing temperature was 25℃, and the polishing lasted for 15 hours.
[0064] S3: Post-processing After polishing, the polished polycrystalline diamond sheet is cleaned with acetone, alcohol, and deionized water in sequence. After cleaning, it is dried with nitrogen gas to obtain a finished polycrystalline diamond product with atomically smooth surface.
[0065] The test revealed obvious grain boundary steps on the surface of the polycrystalline diamond, with a surface roughness Ra=2.18 nm. The material removal rate was calculated to be only 33 nm / h using a precision electronic balance.
[0066] Comparative Example 2
[0067] The object to be processed is a 2-inch polycrystalline diamond sheet with a thickness of 400 μm and a Ra value of 47 nm after pretreatment.
[0068] S1: Polishing fluid preparation Add 68 wt% deionized water to a beaker, add 1 wt% sodium polyacrylate dispersant, and stir to dissolve; then add 1 wt% nano diamond powder with an abrasive particle size of 100 nm, and ultrasonically disperse for 45 min to ensure no agglomeration; slowly add 30 wt% hydrogen peroxide and stir evenly; adjust the pH to 4.5 with 1 mol / L dilute nitric acid and stir for 15 min to obtain a uniform and stable polishing solution.
[0069] S2: Chemical-Mechanical Polishing Polishing was performed using a cast iron disc and the aforementioned polishing slurry, with a continuous supply of the slurry throughout the process. Specific parameters included: polishing pressure 740 g / cm². 2 The polishing disc rotated at 100 rpm, the workpiece rotated at 15 rpm, the polishing fluid flow rate was 3 mL / min, the polishing temperature was 25℃, and the polishing lasted for 15 hours.
[0070] S3: Post-processing After polishing, the polished polycrystalline diamond sheet is cleaned with acetone, alcohol, and deionized water in sequence. After cleaning, it is dried with nitrogen gas to obtain a finished polycrystalline diamond product with atomically smooth surface.
[0071] The surface roughness of the polycrystalline diamond was measured to be Ra=2.85 nm using AFM, and the material removal rate was calculated to be 68 nm / h using a precision electronic balance.
[0072] Table 1. Measured roughness Ra and removal rate of polycrystalline diamond sheets after polishing in Examples 1-5 and Comparative Examples 1-2.
[0073] The results in Table 1 above demonstrate that the performance indicators of Examples 1-6 of this invention are comprehensively superior to those of Comparative Examples 1 and 2. The core reason lies in the fact that this invention constructs an "oxidation activation-interface bonding" system. It utilizes the active free radicals generated by the oxidant to bidirectionally activate the surface of the diamond and single-crystal silicon polishing pad, constructing a stable Si-OC covalent bond interface through hydroxyl dehydration condensation. Combined with micro-machining of the abrasive, it achieves precise coupling between chemical action and mechanical grinding, completing low-damage ultra-smooth surface polishing within 15 hours. In contrast, Comparative Examples 1 and 2, lacking a key oxidant or requiring a different suitable polishing pad, cannot construct an effective interface bonding system, losing the synergistic effect of chemical activation. They rely solely on a single mechanical grinding method, resulting in low removal rates, severe surface damage, and significantly limited overall polishing performance.
Claims
1. A polishing fluid, characterized in that, The polishing slurry comprises the following components by weight percentage: abrasive 0.1-10 wt%, oxidant 1-50 wt%, dispersant 0.5-2 wt%, with the balance being deionized water; the oxidant is one of 28-30 wt% hydrogen peroxide, potassium permanganate, or potassium ferrate; and the polishing slurry has a pH of 3-6.
2. The polishing slurry according to claim 1, characterized in that, The abrasive is one or more of nanodiamond, cubic boron nitride, boron carbide, and alumina; the particle size of the abrasive is 50-200 nm.
3. The polishing slurry according to claim 1, characterized in that, When the oxidant is 28-30 wt% hydrogen peroxide, the addition amount is 10-50 wt%; when the oxidant is potassium permanganate or potassium ferrate, the addition amount is 1-5 wt%.
4. The polishing slurry according to claim 1, characterized in that, The dispersant is one or more of the following: polyacrylate, polycarboxylate, organophosphonate, high molecular weight nonionic dispersant, and inorganic phosphate.
5. A method for efficient polishing of polycrystalline diamond ultra-smooth surfaces using the polishing slurry according to any one of claims 1 to 4, characterized in that, By selecting a monocrystalline silicon polishing pad, the strong oxidizing free radicals generated by the oxidant in the polishing slurry cause the monocrystalline silicon polishing pad to generate hydroxyl groups on the diamond surface and dehydrate to form Si-OC covalent bonds. Combined with the micro-cutting and smoothing removal of abrasives in the polishing slurry, high-efficiency and low-damage polishing of polycrystalline diamond is achieved.
6. The method according to claim 5, characterized in that, Includes the following steps: (1) Polishing solution preparation: Mix deionized water, dispersant and abrasive evenly, add oxidant and mix well, adjust pH to 3-6 using pH adjuster to obtain polishing solution; (2) Chemical-mechanical polishing: Polycrystalline diamond wafers with Ra≤50 nm are bonded to single-crystal silicon polishing pads and polished at room temperature and pressure under set process parameters, with polishing fluid continuously supplied during the polishing process; (3) Post-processing: After polishing, the polished polycrystalline diamond sheet is cleaned to obtain the final product.
7. The method according to claim 6, characterized in that, The pH adjuster is dilute nitric acid or dilute sulfuric acid with a concentration of 1-5 mol / L.
8. The method according to claim 6, characterized in that, The monocrystalline silicon polishing pad is a monocrystalline silicon (100) polishing pad with a diameter ≥ 2 inches and an initial surface roughness Ra = 0.8-1.5 μm. The diameter ratio of the workpiece to the monocrystalline silicon polishing pad is 1:3-1:
5.
9. The method according to claim 6, characterized in that, The process parameters for the chemical-mechanical polishing are: polishing pressure 300-1000 g / cm. 2 The polishing disc speed is 60-120 rpm, the workpiece speed is 10-20 rpm, the polishing fluid flow rate is 2-20 mL / min, and the temperature is 18-45℃.
Citation Information
Patent Citations
Polishing solution for polycrystalline diamond and polishing method
CN118638481A
A two-step zeta potential-controlled chemical mechanical polishing method for polycrystalline diamond
CN119609904B