A low-carbon, high-toughness fiber anti-loosening tile adhesive and its preparation method

By preparing low-carbon, high-toughness fiber anti-detachment tile adhesive, and utilizing modified carbon fibers and reactive reinforcing agents to form a cross-linked network, the problem of poor bonding performance of tile adhesive in low-temperature environments was solved, achieving an environmentally friendly and stable bonding effect.

CN123107553APending Publication Date: 2026-11-17佛山市德堡建材有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611610434.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing tile adhesives have poor bonding performance in low-temperature environments, which can easily lead to tile detachment, and they also have high carbon emissions, which is detrimental to environmental protection.

Method used

The preparation method of low-carbon, high-toughness fiber anti-detachment tile adhesive involves mixing components such as cement, limestone powder, quartz sand, mineral powder, microsilica powder, modified carbon fiber, and reactive reinforcing agent to form a cross-linked network with modified carbon fiber and reactive reinforcing agent, thereby improving bonding performance and toughness and enhancing low-temperature stability.

Benefits of technology

It effectively improves the bonding strength and freeze-thaw resistance of tile adhesive, prevents tiles from hollowing and falling off, reduces carbon emissions throughout the entire life cycle, and achieves environmental protection and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of tile adhesives, specifically to a low-carbon, high-toughness fiber-based anti-detachment tile adhesive and its preparation method. It addresses the problems of poor environmental performance, bonding performance, and low-temperature stability in existing tile adhesives, which easily lead to tile detachment. This tile adhesive uses rapid-hardening sulfoaluminate cement as the main cementitious component, and replaces part of the cement clinker with limestone powder, quartz sand, mineral powder, and microsilica powder, effectively reducing carbon emissions throughout its life cycle and contributing to environmental protection. The introduction of modified carbon fibers and reactive reinforcing agents into the system significantly improves the adhesive's bonding performance and toughness, enhances low-temperature stability and freeze-thaw resistance, effectively inhibits the propagation of freeze-thaw microcracks, and resists the adverse effects of external environmental changes, thereby endowing the tile adhesive with excellent long-term durability and structural stability, preventing tile hollowing and detachment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of tile adhesives, specifically to a low-carbon, high-toughness fiber anti-detachment tile adhesive and its preparation method. Background Technology

[0002] In the field of building decoration, ceramic tiles are a widely used decorative material, popular for their beauty and durability. Tile adhesive plays a key role in building decoration, mainly used to bond ceramic tiles or stone to increase their stability. Traditional tile adhesives mostly use organic or inorganic compounds as the main components, resulting in poor weather resistance and bonding strength. This leads to poor performance of existing tile adhesives in low-temperature environments, especially in cold regions or with temperature fluctuations. Over time, the bonding performance will gradually weaken, even causing tiles to fall off, greatly increasing safety hazards. Moreover, the over-reliance on silicate cement results in large carbon emissions throughout the entire life cycle, which is detrimental to environmental protection.

[0003] Therefore, the low-carbon, high-toughness fiber anti-detachment tile adhesive and its preparation method of the present invention are of great significance in the field of tile adhesives. Summary of the Invention

[0004] In order to overcome the above-mentioned technical problems, the purpose of this invention is to provide a low-carbon, high-toughness fiber anti-detachment tile adhesive and its preparation method, which solves the problems of poor environmental performance, bonding performance and low-temperature stability of existing tile adhesives, which easily cause tiles to fall off.

[0005] The objective of this invention can be achieved through the following technical solutions: In a first aspect, this application provides a low-carbon, high-toughness fiber anti-detachment tile adhesive, comprising the following components in parts by weight: 20-30 parts cement, 5-10 parts limestone powder, 75-85 parts quartz sand, 55-65 parts mineral powder, 10-15 parts microsilica, 4-8 parts modified carbon fiber, 3-6 parts reactive reinforcing agent, 0.5-1 part water-retaining agent, 0.5-1.5 parts water-reducing agent, and 2-4 parts powdered sodium silicate; The cement is a mixture of 42.5 grade rapid-hardening sulfoaluminate cement and P·O 42.5 ordinary Portland cement in a mass ratio of 8-12:12-18; the limestone powder has an average particle size of 400 mesh; the quartz sand is a mixture of quartz sand with average particle sizes of 70 mesh and 150 mesh in an equal mass ratio; the water-retaining agent is a mixture of hydroxypropyl methylcellulose ether and starch ether in a weight ratio of 0.3-0.5:0.1-0.3; the water-reducing agent is of type CP1701X; and the powdered sodium silicate has a modulus of 2.3.

[0006] In a preferred embodiment of the present invention, the reactive enhancer is prepared by the following steps: Step a1: Add polypropylene glycol to a reaction vessel and stir at 80-120 r / min for 1-2 h at 110-120℃ and vacuum degree -0.09MPa. Cool down to 60-65℃, purge with nitrogen for protection, add isophorone diisocyanate and dibutyltin dilaurate while stirring at 150-200 r / min, heat up to 80-85℃ and react for 2-3 h, cool naturally to 40-45℃, add aminosilane coupling agent, and stir at 150-200 r / min for 1-2 h to obtain modified polyurethane; Step a2: Add modified polyurethane and anhydrous ethyl acetate to a three-necked flask equipped with a stirrer and thermometer, and mix for 10-15 minutes to obtain a modified polyurethane solution; add fly ash to a mixer, and spray the modified polyurethane solution into the mixer in an atomized form at a speed of 800-1000 r / min with a spray pressure of 0.2-0.3 MPa, and mix for 30 minutes to obtain a slurry; transfer the slurry to a vacuum kneader, and perform desolvation and condensation treatment under the conditions of a jacket temperature of 60-80℃ and a vacuum degree of -0.09 MPa. During the treatment, water vapor is introduced into the kneader through a humidity generator to control the atmosphere dew point temperature at -5℃, the kneading speed at 30-50 r / min, and the treatment time is 2-3 hours. After the treatment is completed, remove the slurry and pulverize it to a particle size D90 < 50 μm using an air jet mill, and then sieve it through a 100-mesh sieve to obtain a reactive reinforcing agent.

[0007] In a preferred embodiment of the present invention, the ratio of polypropylene glycol, isophorone diisocyanate, dibutyltin dilaurate, and aminosilane coupling agent in step a1 is 40-50 mL: 11-14 mL: 0.1-0.2 mL: 8-10 mL; the polypropylene glycol is PPG2000; and the aminosilane coupling agent is JH-A112.

[0008] In a preferred embodiment of the present invention, the ratio of modified polyurethane, anhydrous ethyl acetate and fly ash in step a2 is 60-75 mL: 150-200 mL: 30-40 g; the fly ash is grade I fly ash.

[0009] In a preferred embodiment of the present invention, the modified carbon fiber is prepared by the following steps: Step b1: Place the carbon fiber in a muffle furnace and calcine it at 400-420℃ for 2-3 hours. Then, cool it with the furnace and add it along with acetone to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir the reaction at 25-30℃ and 300-400 r / min for 20-30 minutes. Then, raise the temperature to 50-60℃ and continue stirring for 3-5 hours. After the reaction is completed, cool the reaction product to room temperature, then centrifuge it. Wash the precipitate with distilled water 2-3 times and then place it in a vacuum drying oven and dry it at 70-80℃ for 2-3 hours to obtain pretreated carbon fiber. Step b2: Add the pretreated carbon fiber, ethanol, and deionized water to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Purge with nitrogen for protection and stir for 10-20 min at 25-30℃ and 300-400 r / min. Then add N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and ammonia water and continue stirring for 10-15 h at 70-80℃. After the reaction is complete, cool the reaction product to room temperature, centrifuge, wash the precipitate 2-3 times with distilled water, and then place it in a vacuum drying oven and dry at 40-50℃ for 5-6 h to obtain modified carbon fiber.

[0010] In a preferred embodiment of the present invention, the ratio of carbon fiber to acetone in step b1 is 2g:40-50mL; the carbon fiber is an alkali-resistant carbon fiber with a diameter of 14μm and a length of 12mm.

[0011] In a preferred embodiment of the present invention, the ratio of the amount of pretreated carbon fiber, ethanol, deionized water, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and ammonia in step b2 is 2g:90-95mL:10-15mL:1-7g:2-3mL; and the mass fraction of the ammonia is 20-25%.

[0012] Secondly, this application provides a method for preparing low-carbon, high-toughness fiber anti-detachment tile adhesive, comprising the following steps: Step 1: Weigh out the following components by weight: 20-30 parts cement, 5-10 parts limestone powder, 75-85 parts quartz sand, 55-65 parts mineral powder, 10-15 parts silica fume, 4-8 parts modified carbon fiber, 3-6 parts reactive reinforcing agent, 0.5-1 part water-retaining agent, 0.5-1.5 parts water-reducing agent, and 2-4 parts powdered sodium silicate. Step 2: Add cement, limestone powder, quartz sand, mineral powder, microsilica powder, modified carbon fiber, reactive reinforcing agent, water-retaining agent, water-reducing agent, and powdered sodium silicate into a conical double helix mixer, and mix and stir for 2-3 minutes at a speed of 80-120 r / min and 25℃ to obtain low-carbon, high-toughness fiber anti-detachment tile adhesive.

[0013] The beneficial effects of this invention are: This invention discloses a low-carbon, high-toughness fiber-based anti-detachment tile adhesive and its preparation method. The method involves uniformly mixing cement, limestone powder, quartz sand, mineral powder, microsilica powder, modified carbon fiber, reactive reinforcing agent, water-retaining agent, water-reducing agent, and powdered sodium silicate to obtain a solid powder-like low-carbon, high-toughness fiber-based anti-detachment tile adhesive. This adhesive can be applied by simply adding water and stirring. The adhesive uses rapid-hardening sulfoaluminate cement as the main cementitious component, and limestone powder, quartz sand, mineral powder, and microsilica powder replace part of the cement clinker, effectively reducing carbon emissions throughout its life cycle and contributing to environmental protection. The introduction of modified carbon fiber and reactive reinforcing agent significantly improves the adhesive's bonding performance and toughness, enhances low-temperature stability and freeze-thaw resistance, effectively inhibits the propagation of freeze-thaw microcracks, and resists the adverse effects of external environmental changes, thereby endowing the adhesive with excellent long-term durability and structural stability, preventing tile hollowing and detachment.

[0014] In the preparation of low-carbon, high-toughness fiber anti-detachment tile adhesive, modified carbon fiber was first prepared. Impurities on the carbon fiber surface were removed by calcination and acetone treatment to obtain pretreated carbon fiber. Then, surface grafting modification with N-(2-aminoethyl)-3-aminopropyltrimethoxysilane was performed to obtain modified carbon fiber with a surface rich in active amino groups. This modified carbon fiber exhibits excellent mechanical properties, effectively bridging cracks and transferring stress when the tile adhesive is under stress, resulting in significant reinforcement and toughening. The active groups introduced on its surface can chemically bond with components in the cementitious matrix, significantly improving the interfacial bonding strength between the fiber and the matrix, increasing tensile bond strength, ensuring the low-temperature stability of the tile adhesive, and achieving the anti-detachment effect.

[0015] In the preparation of low-carbon, high-toughness fiber-based anti-detachment tile adhesive, a reactive reinforcing agent was first prepared. A polyurethane prepolymer with terminal isocyanate was synthesized by reacting polypropylene glycol with isophorone diisocyanate. This prepolymer was then capped with an aminosilane coupling agent to obtain a silanized modified polyurethane. This modified polyurethane was loaded onto a fly ash carrier and subjected to vacuum desolventizing and moisture-induced condensation to obtain a solid powder of the reactive reinforcing agent. When this reinforcing agent is exposed to water and alkaline environments, the siloxane end groups undergo hydrolysis and condensation, forming a cross-linked polyurethane-siloxane hybrid network in the cementitious matrix. The soft segments in the polyurethane chain impart excellent flexibility and low-temperature deformation capability to the material, effectively absorbing temperature stress and freeze-thaw deformation. The fly ash carrier enables the solidification of liquid polymers into a powder and can also participate in alkali-activated hydration reactions, strengthening the interfacial transition zone between the reinforcing agent particles and the matrix. Through the synergistic effect of chemical bonding, flexible toughening, and interfacial strengthening, the bonding strength, lateral deformation capability, and low-temperature anti-detachment performance of the tile adhesive are improved. Detailed Implementation

[0016] To enable those skilled in the art to better understand the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0017] Example 1: This embodiment describes a method for preparing a low-carbon, high-toughness fiber-based anti-detachment tile adhesive, comprising the following steps: Step S1: Add 40 mL of polypropylene glycol PPG2000 to the reactor and stir at 80 r / min for 1 h at 110 °C and vacuum degree -0.09 MPa. Cool down to 60 °C, purge with nitrogen for protection, add 114 mL of isophorone diisocyanate and 0.1 mL of dibutyltin dilaurate while stirring at 150 r / min, heat up to 80 °C and react for 2 h, cool naturally to 40 °C, add 8 mL of aminosilane coupling agent JH-A112, and stir at 150 r / min for 1 h to obtain modified polyurethane; Step S2: Add 60 mL of modified polyurethane and 150 mL of anhydrous ethyl acetate to a three-necked flask equipped with a stirrer and thermometer, and mix for 10 min to obtain a modified polyurethane solution; add 30 g of primary fly ash to a mixer, and spray the modified polyurethane solution into the mixer in an atomized form at a speed of 800 r / min and a spray pressure of 0.2 MPa, and mix for 30 min to obtain a slurry; transfer the slurry to a vacuum kneader, and perform desolvation and condensation treatment under the conditions of a jacket temperature of 60℃ and a vacuum degree of -0.09 MPa. During the treatment, water vapor is introduced into the kneader through a humidity generator to control the atmosphere dew point temperature at -5℃, the kneading speed at 30 r / min, and the treatment time is 2 h. After the treatment is completed, the slurry is taken out and pulverized by an air jet mill to a particle size D90 < 50 μm, and then sieved through a 100-mesh sieve to obtain a reactive reinforcing agent; Step S3: Place 2g of carbon fiber in a muffle furnace and calcine it at 400℃ for 2 hours. Then, cool it with the furnace and add it along with 40mL of acetone to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Purge with nitrogen for protection and stir the reaction at 25℃ and a stirring rate of 300r / min for 20 minutes. Then, raise the temperature to 50℃ and continue stirring the reaction for 3 hours. After the reaction is completed, cool the reaction product to room temperature, centrifuge it, wash the precipitate twice with distilled water, and then place it in a vacuum drying oven and dry it at 70℃ for 2 hours to obtain pretreated carbon fiber. The carbon fiber is an alkali-resistant carbon fiber with a diameter of 14μm and a length of 12mm. Step S4: Add 2g of pretreated carbon fiber, 90mL of ethanol and 10mL of deionized water to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir for 10min at 25℃ and 300r / min. Then add 1g of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and 2mL of 20% ammonia water and heat to 70℃ and continue stirring for 10h. After the reaction is complete, cool the reaction product to room temperature, centrifuge, wash the precipitate twice with distilled water, and then place it in a vacuum drying oven and dry at 40℃ for 5h to obtain modified carbon fiber. Step S5: Weigh out 20 parts cement, 5 parts limestone powder, 75 parts quartz sand, 55 parts mineral powder, 10 parts silica fume, 4 parts modified carbon fiber, 3 parts reactive reinforcing agent, 0.5 parts water-retaining agent, 0.5 parts water-reducing agent, and 2 parts powdered sodium silicate according to the following weight ratios: The cement is a mixture of 42.5 grade rapid-hardening sulfoaluminate cement and P·O 42.5 ordinary Portland cement at a mass ratio of 8:12; the average particle size of the limestone powder is 400 mesh; the quartz sand is a mixture of quartz sand with average particle sizes of 70 mesh and 150 mesh at equal mass ratios; the water-retaining agent is a mixture of hydroxypropyl methylcellulose ether and starch ether at a weight ratio of 0.3:0.1; the water-reducing agent is of type CP1701X; the powdered sodium silicate is powdered sodium silicate with a modulus of 2.3. Step S6: Add cement, limestone powder, quartz sand, mineral powder, microsilica powder, modified carbon fiber, reactive reinforcing agent, water-retaining agent, water-reducing agent, and powdered sodium silicate into a conical double helix mixer and mix and stir for 2 minutes at a speed of 80 r / min and a temperature of 25°C to obtain low-carbon, high-toughness fiber anti-detachment tile adhesive.

[0018] Example 2: This embodiment describes a method for preparing a low-carbon, high-toughness fiber-based anti-detachment tile adhesive, comprising the following steps: Step S1: Add 45 mL of polypropylene glycol PPG2000 to the reactor and stir at 100 r / min for 1.5 h at 115 °C and vacuum degree -0.09 MPa. Cool down to 63 °C, purge with nitrogen, add 12.5 mL of isophorone diisocyanate and 0.15 mL of dibutyltin dilaurate while stirring at 175 r / min. Heat up to 83 °C and react for 2.5 h. Cool naturally to 43 °C, add 9 mL of aminosilane coupling agent JH-A112, and stir at 175 r / min for 1.5 h to obtain modified polyurethane. Step S2: Add 68 mL of modified polyurethane and 175 mL of anhydrous ethyl acetate to a three-necked flask equipped with a stirrer and thermometer, and mix for 13 min to obtain a modified polyurethane solution; add 35 g of primary fly ash to a mixer, and spray the modified polyurethane solution into the mixer in an atomized form at a speed of 900 r / min and a spray pressure of 0.3 MPa, and mix for 30 min to obtain a slurry; transfer the slurry to a vacuum kneader, and perform desolvation and condensation treatment under the conditions of a jacket temperature of 70℃ and a vacuum degree of -0.09 MPa. During the treatment, water vapor is introduced into the kneader through a humidity generator to control the atmosphere dew point temperature at -5℃, the kneading speed at 40 r / min, and the treatment time is 2.5 h. After the treatment is completed, remove the slurry, and pulverize it to a particle size D90 < 50 μm using an air jet mill. Then, sieve it through a 100-mesh sieve to obtain a reactive reinforcing agent; Step S3: Place 2g of carbon fiber in a muffle furnace and calcine it at 410℃ for 2.5h. Then, cool it with the furnace and add it along with 45mL of acetone to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Purge with nitrogen for protection and stir the reaction at 28℃ and a stirring rate of 350r / min for 25min. Then, raise the temperature to 55℃ and continue stirring the reaction for 4h. After the reaction is completed, cool the reaction product to room temperature, centrifuge it, wash the precipitate three times with distilled water, and then place it in a vacuum drying oven and dry it at 75℃ for 2.5h to obtain pretreated carbon fiber. The carbon fiber is an alkali-resistant carbon fiber with a diameter of 14μm and a length of 12mm. Step S4: Add 2g of pretreated carbon fiber, 93mL of ethanol and 13mL of deionized water to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir for 15min at 28℃ and 350r / min. Then add 4g of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and 2.5mL of 23% ammonia water and heat to 75℃ and continue stirring for 13h. After the reaction is complete, cool the reaction product to room temperature, centrifuge, wash the precipitate three times with distilled water, and then place it in a vacuum drying oven and dry at 45℃ for 5.5h to obtain modified carbon fiber. Step S5: Weigh out 25 parts cement, 8 parts limestone powder, 80 parts quartz sand, 60 parts mineral powder, 13 parts silica fume, 6 parts modified carbon fiber, 5 parts reactive reinforcing agent, 0.8 parts water-retaining agent, 1 part water-reducing agent, and 3 parts powdered sodium silicate according to the following weight ratios: The cement is a mixture of 42.5 grade rapid-hardening sulfoaluminate cement and P·O 42.5 ordinary Portland cement at a mass ratio of 10:15; the average particle size of the limestone powder is 400 mesh; the quartz sand is a mixture of quartz sand with average particle sizes of 70 mesh and 150 mesh at equal mass ratios; the water-retaining agent is a mixture of hydroxypropyl methylcellulose ether and starch ether at a weight ratio of 0.4:0.2; the water-reducing agent is CP1701X; the powdered sodium silicate is powdered sodium silicate with a modulus of 2.3. Step S6: Add cement, limestone powder, quartz sand, mineral powder, microsilica powder, modified carbon fiber, reactive reinforcing agent, water-retaining agent, water-reducing agent, and powdered sodium silicate into a conical double helix mixer and mix and stir for 2 minutes at a speed of 100 r / min and a temperature of 25°C to obtain low-carbon, high-toughness fiber anti-detachment tile adhesive.

[0019] Example 3: This embodiment describes a method for preparing a low-carbon, high-toughness fiber-based anti-detachment tile adhesive, comprising the following steps: Step S1: Add 50 mL of polypropylene glycol PPG2000 to the reactor and stir at 120 r / min for 2 h at 120 °C and vacuum degree -0.09 MPa. Cool down to 65 °C, purge with nitrogen for protection, add 14 mL of isophorone diisocyanate and 0.2 mL of dibutyltin dilaurate while stirring at 200 r / min, heat to 85 °C and react for 3 h, cool naturally to 45 °C, add 10 mL of aminosilane coupling agent JH-A112, and stir at 200 r / min for 2 h to obtain modified polyurethane; Step S2: Add 75 mL of modified polyurethane and 200 mL of anhydrous ethyl acetate to a three-necked flask equipped with a stirrer and thermometer, and mix for 15 min to obtain a modified polyurethane solution; add 40 g of primary fly ash to a mixer, and spray the modified polyurethane solution into the mixer in an atomized form at a speed of 1000 r / min and a spray pressure of 0.3 MPa, and mix for 30 min to obtain a slurry; transfer the slurry to a vacuum kneader, and perform desolvation and condensation treatment under the conditions of a jacket temperature of 80℃ and a vacuum degree of -0.09 MPa. During the treatment, water vapor is introduced into the kneader through a humidity generator to control the atmosphere dew point temperature at -5℃, the kneading speed at 50 r / min, and the treatment time is 3 h. After the treatment is completed, the slurry is taken out and pulverized by an air jet mill to a particle size D90 < 50 μm, and then sieved through a 100-mesh sieve to obtain a reactive reinforcing agent; Step S3: Place 2g of carbon fiber in a muffle furnace and calcine it at 420℃ for 3 hours. Then, cool it with the furnace and add it to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube with 50mL of acetone. Purge with nitrogen for protection and stir the reaction at 30℃ and a stirring rate of 400r / min for 30 minutes. Then, raise the temperature to 60℃ and continue stirring the reaction for 5 hours. After the reaction is completed, cool the reaction product to room temperature, centrifuge it, wash the precipitate three times with distilled water, and then place it in a vacuum drying oven and dry it at 80℃ for 3 hours to obtain pretreated carbon fiber. The carbon fiber is an alkali-resistant carbon fiber with a diameter of 14μm and a length of 12mm. Step S4: Add 2g of pretreated carbon fiber, 95mL of ethanol and 15mL of deionized water to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir for 20min at 30℃ and 400r / min. Then add 7g of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and 3mL of 25% ammonia water and heat to 80℃ and continue stirring for 15h. After the reaction is complete, cool the reaction product to room temperature, centrifuge, wash the precipitate three times with distilled water, and then place it in a vacuum drying oven and dry at 50℃ for 6h to obtain modified carbon fiber. Step S5: Weigh out 30 parts cement, 10 parts limestone powder, 85 parts quartz sand, 65 parts mineral powder, 15 parts silica fume, 8 parts modified carbon fiber, 6 parts reactive reinforcing agent, 1 part water-retaining agent, 1.5 parts water-reducing agent, and 4 parts powdered sodium silicate according to the following weight ratios: The cement is a mixture of 42.5 grade rapid-hardening sulfoaluminate cement and P·O 42.5 ordinary Portland cement at a mass ratio of 12:18; the average particle size of the limestone powder is 400 mesh; the quartz sand is a mixture of quartz sand with average particle sizes of 70 mesh and 150 mesh at equal mass ratios; the water-retaining agent is a mixture of hydroxypropyl methylcellulose ether and starch ether at a weight ratio of 0.5:0.3; the water-reducing agent is CP1701X; the powdered sodium silicate is powdered sodium silicate with a modulus of 2.3. Step S6: Add cement, limestone powder, quartz sand, mineral powder, microsilica powder, modified carbon fiber, reactive reinforcing agent, water-retaining agent, water-reducing agent, and powdered sodium silicate into a conical double helix mixer and mix for 3 minutes at a speed of 120 r / min and a temperature of 25°C to obtain low-carbon, high-toughness fiber anti-detachment tile adhesive.

[0020] Comparative Example 1: This comparative example illustrates a method for preparing a low-carbon, high-toughness fiber-based anti-detachment tile adhesive, comprising the following steps: Step S1: Weigh out 25 parts cement, 8 parts limestone powder, 80 parts quartz sand, 60 parts mineral powder, 13 parts silica fume, 0.8 parts water-retaining agent, 1 part water-reducing agent, and 3 parts powdered sodium silicate according to the following weight proportions: The cement is 42.5 grade rapid-hardening sulfoaluminate cement; the cement is a mixture of 42.5 grade rapid-hardening sulfoaluminate cement and P·O 42.5 ordinary Portland cement at a mass ratio of 10:15; the quartz sand is a mixture of quartz sand with an average particle size of 70 mesh and 150 mesh at an equal mass ratio; the water-retaining agent is a mixture of hydroxypropyl methylcellulose ether and starch ether at a weight proportion of 0.4:0.2; the water-reducing agent is of type CP1701X; the powdered sodium silicate is powdered sodium silicate with a modulus of 2.3. Step S2: Add cement, limestone powder, quartz sand, mineral powder, silica fume, water-retaining agent, water-reducing agent, and powdered sodium silicate into a conical double helix mixer and mix for 2 minutes at 100 r / min and 25℃ to obtain low-carbon, high-toughness fiber anti-detachment tile adhesive.

[0021] Comparative Example 2: This comparative example illustrates a method for preparing a low-carbon, high-toughness fiber-based anti-detachment tile adhesive, comprising the following steps: Step S1: Add 45 mL of polypropylene glycol PPG2000 to the reactor and stir at 100 r / min for 1.5 h at 115 °C and vacuum degree -0.09 MPa. Cool down to 63 °C, purge with nitrogen, add 12.5 mL of isophorone diisocyanate and 0.15 mL of dibutyltin dilaurate while stirring at 175 r / min. Heat up to 83 °C and react for 2.5 h. Cool naturally to 43 °C, add 9 mL of aminosilane coupling agent JH-A112, and stir at 175 r / min for 1.5 h to obtain modified polyurethane. Step S2: Add 68 mL of modified polyurethane and 175 mL of anhydrous ethyl acetate to a three-necked flask equipped with a stirrer and thermometer, and mix for 13 min to obtain a modified polyurethane solution; add 35 g of primary fly ash to a mixer, and spray the modified polyurethane solution into the mixer in an atomized form at a speed of 900 r / min and a spray pressure of 0.3 MPa, and mix for 30 min to obtain a slurry; transfer the slurry to a vacuum kneader, and perform desolvation and condensation treatment under the conditions of a jacket temperature of 70℃ and a vacuum degree of -0.09 MPa. During the treatment, water vapor is introduced into the kneader through a humidity generator to control the atmosphere dew point temperature at -5℃, the kneading speed at 40 r / min, and the treatment time is 2.5 h. After the treatment is completed, remove the slurry, and pulverize it to a particle size D90 < 50 μm using an air jet mill. Then, sieve it through a 100-mesh sieve to obtain a reactive reinforcing agent; Step S3: Weigh out 25 parts cement, 8 parts limestone powder, 80 parts quartz sand, 60 parts mineral powder, 13 parts silica fume, 5 parts reactive reinforcing agent, 0.8 parts water-retaining agent, 1 part water-reducing agent, and 3 parts powdered sodium silicate according to the following weight proportions: The cement is a mixture of 42.5 grade rapid-hardening sulfoaluminate cement and P·O 42.5 ordinary Portland cement at a mass ratio of 10:15; the average particle size of the limestone powder is 400 mesh; the quartz sand is a mixture of quartz sand with average particle sizes of 70 mesh and 150 mesh at equal mass proportions; the water-retaining agent is a mixture of hydroxypropyl methylcellulose ether and starch ether at a weight ratio of 0.4:0.2; the water-reducing agent is of type CP1701X; the powdered sodium silicate is powdered sodium silicate with a modulus of 2.3. Step S4: Add cement, limestone powder, quartz sand, mineral powder, silica fume, reactive reinforcing agent, water-retaining agent, water-reducing agent, and powdered sodium silicate into a conical double helix mixer and mix for 2 minutes at 100 r / min and 25℃ to obtain low-carbon, high-toughness fiber anti-detachment tile adhesive.

[0022] Comparative Example 3: This comparative example illustrates a method for preparing a low-carbon, high-toughness fiber-based anti-detachment tile adhesive, comprising the following steps: Step S1: Place 2g of carbon fiber in a muffle furnace and calcine at 410℃ for 2.5h. Then, cool the furnace and add it along with 45mL of acetone to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Purge with nitrogen for protection and stir at 28℃ and a stirring rate of 350r / min for 25min. Then, raise the temperature to 55℃ and continue stirring for 4h. After the reaction is complete, cool the reaction product to room temperature, centrifuge, wash the precipitate three times with distilled water, and then place it in a vacuum drying oven and dry at 75℃ for 2.5h to obtain pretreated carbon fiber. The carbon fiber is an alkali-resistant carbon fiber with a diameter of 14μm and a length of 12mm. Step S2: Add 2g of pretreated carbon fiber, 93mL of ethanol and 13mL of deionized water to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir for 15min at 28℃ and 350r / min. Then add 4g of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and 2.5mL of 23% ammonia water and heat to 75℃ and continue stirring for 13h. After the reaction is complete, cool the reaction product to room temperature, centrifuge, wash the precipitate three times with distilled water, and then place it in a vacuum drying oven and dry at 45℃ for 5.5h to obtain modified carbon fiber. Step S3: Weigh out 25 parts cement, 8 parts limestone powder, 80 parts quartz sand, 60 parts mineral powder, 13 parts silica fume, 6 parts modified carbon fiber, 0.8 parts water-retaining agent, 1 part water-reducing agent, and 3 parts powdered sodium silicate according to the following weight ratios: The cement is a mixture of 42.5 grade rapid-hardening sulfoaluminate cement and P·O 42.5 ordinary Portland cement at a mass ratio of 10:15; the average particle size of the limestone powder is 400 mesh; the quartz sand is a mixture of quartz sand with average particle sizes of 70 mesh and 150 mesh at equal mass ratios; the water-retaining agent is a mixture of hydroxypropyl methylcellulose ether and starch ether at a weight ratio of 0.4:0.2; the water-reducing agent is CP1701X; the powdered sodium silicate is powdered sodium silicate with a modulus of 2.3. Step S4: Add cement, limestone powder, quartz sand, mineral powder, microsilica powder, modified carbon fiber, water-retaining agent, water-reducing agent, and powdered sodium silicate into a conical double helix mixer and mix for 2 minutes at a speed of 100 r / min and a temperature of 25°C to obtain low-carbon, high-toughness fiber anti-detachment tile adhesive.

[0023] The low-carbon, high-toughness fiber anti-detachment tile adhesives prepared in Examples 1-3 and Comparative Examples 1-3 were mixed with water at a water-to-adhesive ratio of 3:1. Tensile bond strength and tensile bond strength after freeze-thaw cycles were tested according to JC / T 547-2017. The test results are shown in the table below. Comparing Examples 1-3 with Comparative Examples 1-3: In Example 1, the low dosage of reactive reinforcing agent and modified carbon fiber resulted in an overly sparse polyurethane-siloxane crosslinking network formed in the alkali-activated gel matrix, which could not effectively impart sufficient flexibility and low-temperature deformation capability to the material. The low dosage of modified carbon fiber made it difficult to form a dense three-dimensional bridging network within the matrix, and the fiber's role in inhibiting freeze-thaw microcracks and transferring stress was not fully realized, resulting in low bond strength and freeze-thaw resistance. In Example 2, the moderate dosage of reactive reinforcing agent and modified carbon fiber resulted in a synergistic effect between the flexible toughening of the reinforcing agent and the rigid crack resistance of the fiber, leading to improved bond strength and freeze-thaw resistance. The fusion retention capacity is relatively strong; in Example 3, the amount of reactive reinforcing agent and modified carbon fiber is relatively high; excessive reactive reinforcing agent hydrolyzes and condenses in the matrix to form an overly dense organic network, which, although enhancing flexibility, disrupts the overall continuity of the inorganic cementitious phase, weakening the density and rigid skeleton of the matrix itself; excessive modified carbon fiber is difficult to achieve complete and uniform dispersion during dry powder mixing and water addition, with some fibers forming local agglomeration, which in turn forms a weak interface in the matrix, causing stress concentration and microcrack initiation, thus reducing performance; comparing Example 2 with Comparative Example 1, it can be seen that: Comparative Example 1 did not add reactive reinforcing agent and modified carbon fiber, relying only on sulfur The alkali-activated pure inorganic cementitious system of aluminate cement-mineral powder-silica fume provides bonding strength. However, the hydration products of this system are brittle and lack the flexibility and low-temperature deformation capacity imparted by the organic polymer network. Furthermore, the matrix cannot form a fiber-bridged crack-resistant structure. Under the temperature stress and ice crystal expansion force generated by freeze-thaw cycles, microcracks rapidly propagate and penetrate, leading to a decrease in bond strength and a reduced strength retention rate after freeze-thaw cycles. Comparing Example 2 with Comparative Example 2, it can be seen that Comparative Example 2 introduces a reactive reinforcing agent and forms a polyurethane-siloxane crosslinked network, imparting certain flexibility and low-temperature toughening effects to the matrix. However, it lacks the synergistic reinforcement of modified carbon fibers, and no fibers are present in the matrix. The matrix forms a three-dimensional random bridging network, lacking effective bridging and stress transfer of fibers to crack tips, resulting in low original bond strength and post-freeze-thaw strength. Comparing Example 2 with Comparative Example 3, it can be seen that Comparative Example 3 only relies on the bridging and crack-resistant effect of modified carbon fibers and the chemical bonding of surface amino groups to improve the crack resistance of the matrix. No reactive reinforcing agent is introduced to provide a flexible polymer network. The pure inorganic matrix itself lacks toughness. Under the repeated temperature stress and deformation of freeze-thaw cycles, the rigid matrix lacks flexible components to buffer stress. Due to the difference in modulus, stress concentration and debonding failure easily occur at the fiber-matrix interface, resulting in a decrease in fiber toughening effect, bond strength, and post-freeze-thaw strength.

[0024] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0025] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in this application, they should all fall within the protection scope of the present invention.

Claims

1. A low-carbon, high-toughness fiber-based anti-detachment tile adhesive, characterized in that, Includes the following components by weight: 20-30 parts cement, 5-10 parts limestone powder, 75-85 parts quartz sand, 55-65 parts mineral powder, 10-15 parts microsilica, 4-8 parts modified carbon fiber, 3-6 parts reactive reinforcing agent, 0.5-1 part water-retaining agent, 0.5-1.5 parts water-reducing agent, and 2-4 parts powdered sodium silicate; The reactive enhancer is prepared by the following steps: Step a1: Dehydrate polypropylene glycol under vacuum, purge with nitrogen, add isophorone diisocyanate and dibutyltin dilaurate, heat to react, cool, add aminosilane coupling agent, stir to react, and obtain modified polyurethane. Step a2: Mix modified polyurethane and anhydrous ethyl acetate to obtain a modified polyurethane solution; add fly ash to a mixer, spray the modified polyurethane solution into the mixer in an atomized form using a nozzle, mix and stir to obtain a slurry; transfer the slurry to a vacuum kneader for desolventizing and condensation treatment, remove it, crush it in an air jet mill, and sieve it to obtain a reactive reinforcing agent.

2. The low-carbon, high-toughness fiber anti-detachment tile adhesive according to claim 1, characterized in that, The cement is a mixture of 42.5 grade rapid-hardening sulfoaluminate cement and P·O 42.5 ordinary silicate cement in a mass ratio of 8-12:12-18; the limestone powder has an average particle size of 400 mesh; the quartz sand is a mixture of quartz sand with average particle sizes of 70 mesh and 150 mesh in an equal mass ratio; the water-retaining agent is a mixture of hydroxypropyl methylcellulose ether and starch ether in a weight ratio of 0.3-0.5:0.1-0.3; the water-reducing agent is of type CP1701X; the powdered sodium silicate has a modulus of 2.

3.

3. The low-carbon, high-toughness fiber anti-detachment tile adhesive according to claim 1, characterized in that, In step a1, the ratio of polypropylene glycol, isophorone diisocyanate, dibutyltin dilaurate, and aminosilane coupling agent is 40-50 mL: 11-14 mL: 0.1-0.2 mL: 8-10 mL; the polypropylene glycol is PPG2000; and the aminosilane coupling agent is JH-A112.

4. The low-carbon, high-toughness fiber anti-detachment tile adhesive according to claim 1, characterized in that, The ratio of modified polyurethane, anhydrous ethyl acetate, and fly ash in step a2 is 60-75 mL: 150-200 mL: 30-40 g; the fly ash is grade I fly ash.

5. The low-carbon, high-toughness fiber anti-detachment tile adhesive according to claim 1, characterized in that, The modified carbon fiber is prepared by the following steps: Step b1: Calcine the carbon fiber, then cool it in the furnace and stir it with acetone. After the reaction is complete, cool the reaction product, then centrifuge it, wash and dry the precipitate to obtain pretreated carbon fiber. Step b2: The pretreated carbon fiber, ethanol and deionized water were stirred and reacted. Then N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and ammonia were added and the reaction was continued. After the reaction was completed, the reaction product was cooled, centrifuged, and the precipitate was washed and dried to obtain the modified carbon fiber.

6. The low-carbon, high-toughness fiber anti-detachment tile adhesive according to claim 5, characterized in that, In step b1, the ratio of carbon fiber to acetone is 2g:40-50mL; the carbon fiber is an alkali-resistant carbon fiber with a diameter of 14μm and a length of 12mm.

7. The low-carbon, high-toughness fiber anti-detachment tile adhesive according to claim 5, characterized in that, In step b2, the ratio of the pretreated carbon fiber, ethanol, deionized water, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and ammonia is 2g:90-95mL:10-15mL:1-7g:2-3mL; and the mass fraction of the ammonia is 20-25%.

8. A method for preparing low-carbon, high-toughness fiber anti-detachment tile adhesive as described in any one of claims 1-7, characterized in that, Includes the following steps: Step 1: Weigh out the following components by weight: 20-30 parts cement, 5-10 parts limestone powder, 75-85 parts quartz sand, 55-65 parts mineral powder, 10-15 parts silica fume, 4-8 parts modified carbon fiber, 3-6 parts reactive reinforcing agent, 0.5-1 part water-retaining agent, 0.5-1.5 parts water-reducing agent, and 2-4 parts powdered sodium silicate. Step 2: Mix cement, limestone powder, quartz sand, mineral powder, microsilica powder, modified carbon fiber, reactive reinforcing agent, water-retaining agent, water-reducing agent, and powdered sodium silicate to obtain low-carbon, high-toughness fiber anti-detachment tile adhesive.