A rapid electromagnetic induction heating process before forging and its optimization method for large-diameter precipitation-strengthened martensitic stainless steel
By employing a three-stage electromagnetic induction heating process and optimization methods, the problems of high energy consumption and low efficiency in the pre-forging heat treatment of large-diameter precipitation-strengthened martensitic stainless steel have been solved, achieving rapid and uniform heating and grain refinement, thus ensuring high strength, toughness, and uniform microstructure of the forgings.
Patent Information
- Application Number
- CN202611468577.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing heat treatment methods for large-diameter precipitation-strengthened martensitic stainless steel before forging are energy-intensive, have low production efficiency, and lack systematic means of matching heating process parameters, resulting in performance that is difficult to meet requirements and poor process adaptability.
A three-stage heating electromagnetic induction heating process is adopted, which is combined with finite element software simulation and physical experiment cross-verification to optimize electrical parameters and auxiliary temperature uniformity measures. Rapid and uniform heating is achieved through slide rail conveying, robotic arm material handling and powder rolling platform lubrication, and the mold entry temperature is optimized.
It significantly shortens heating time, achieves grain refinement and homogenization, improves production efficiency, ensures high strength and toughness and uniform microstructure of forgings, avoids the formation of high-temperature ferrite, and improves forging quality.
Smart Images

Figure CN123108244A_ABST
Abstract
Description
[0001] This invention relates to the field of metallic materials technology, and in particular to a rapid electromagnetic induction heating process before forging and its optimization method for large-diameter precipitation-strengthened martensitic stainless steel. Background Technology
[0002] Precipitation-strengthened martensitic stainless steel is widely used in aerospace, energy and chemical industries, and high-end equipment manufacturing due to its high strength, high toughness, and good corrosion resistance. This type of material typically requires preheating before forging to improve its plasticity, reduce deformation resistance, and lay the foundation for subsequent forging microstructure and performance control. However, preheating of large-diameter precipitation-strengthened martensitic stainless steel has long faced numerous challenges. Large-diameter precipitation-strengthened martensitic stainless steel is defined as precipitation-strengthened martensitic stainless steel billets with a diameter or cross-sectional size of 150-250 mm. In industrial practice, traditional heat treatment furnaces such as resistance furnaces or gas furnaces are commonly used for heating. Due to the low thermal conductivity of this type of material, traditional furnace heating methods must employ a "slow heating + long holding time" process strategy to avoid hot cracking of large cross-section billets due to excessive internal and external temperature differences. This heating method typically requires several hours or even longer to heat the billet to the temperature range required for forging. Not only is it energy-intensive and inefficient, but more importantly, the long heating and holding process can easily lead to excessive coarsening of austenite grains, which then form a genetic structure during subsequent cooling. This coarse grain structure is inherited into the final forging, severely deteriorating the mechanical properties and service reliability of the forging.
[0003] In recent years, electromagnetic induction heating technology has attracted attention due to its advantages such as fast heating speed, high thermal efficiency, and ease of automation control. Existing research shows that rapid heating can achieve fine or even ultra-fine grains in steel. However, existing induction heating methods are mainly designed for small-sized parts or surface quenching applications. For large-diameter precipitation-strengthened martensitic stainless steel, there is a lack of systematic methods combining physical experiments and numerical simulations, making it difficult to quickly match optimal heating process parameters and resulting in poor process adaptability. Therefore, developing a rapid electromagnetic induction heating method before forging that can achieve rapid and uniform heating and effectively refine grains for large-diameter precipitation-strengthened martensitic stainless steel has significant engineering value and urgent application needs. Summary of the Invention
[0004] In view of the above, the present invention aims to provide a rapid electromagnetic induction heating process and its optimization method for pre-forging of large-diameter precipitation-strengthened martensitic stainless steel, in order to solve the defects of high energy consumption, low production efficiency and difficulty in meeting performance requirements of existing pre-forging heat treatment of large-diameter precipitation-strengthened martensitic stainless steel. At the same time, it is difficult to quickly match the optimal heating process parameters and the process adaptability is poor for large-diameter precipitation-strengthened martensitic stainless steel forgings of different specifications due to the lack of systematic means combining physical experiments and numerical simulation.
[0005] The objective of this invention is mainly achieved through the following technical solutions: On one hand, the present invention provides a rapid electromagnetic induction heating process before forging for large-diameter precipitation-strengthened martensitic stainless steel, comprising: Includes three-stage heating: First stage heating: When the billet temperature is lower than the Curie point temperature, induction heating is performed at a frequency of 800-1000Hz and an input power of 30-50KW. Second stage heating: When the surface temperature of the billet reaches the Curie point, switch the input frequency to 100-500Hz and the input power to 80-140KW until the surface temperature of the billet reaches the target temperature of 1100±20℃. The third stage is temperature equalization: when the surface of the billet reaches the target temperature of 1100±20℃, increase the input power to 140-180kw, heat to the furnace exit temperature of 1150±20℃, hold for heat and then remove from the furnace.
[0006] Furthermore, the diameter of the blank is 150-300mm.
[0007] Furthermore, the total heating time for the three-stage heating process is 2.5-3.5 hours. The first stage lasts 1-1.5 hours, the second stage lasts 1-1.5 hours, and the third stage lasts 0.5-0.6 hours.
[0008] Furthermore, auxiliary temperature equalization measures are also included: the steel billet is heated, and according to the measured temperature equalization, a special heat preservation cover is placed at the upper port of the induction heating furnace, a high-temperature resistant fiber sealing ring is installed at the lower port, and an insulation sleeve is added to the outside.
[0009] Furthermore, it also includes optimizing the mold entry process: through the automated process of slide rail conveying, robotic arm material handling, powder rolling platform lubrication, and robotic arm mold entry, the total time from the end of heating to the entry of the billet into the forging mold is reduced to less than 2 minutes.
[0010] Furthermore, the martensitic stainless steel treated by electromagnetic induction heating process does not contain high-temperature ferrite when it enters the forging mold.
[0011] On the other hand, the present invention also provides an optimized method for a rapid electromagnetic induction heating process before forging of large-diameter precipitation-strengthened martensitic stainless steel, specifically including the following steps: Step 1: Simulate the transient temperature field. Using finite element software, numerical simulation of the transient temperature field of the billet during electromagnetic induction heating is performed in a two-dimensional axisymmetric model. Step 2: Physical heating experiment and model cross-validation and correction. The billet is electromagnetically induction heated in an induction furnace. During the process, temperature change data is collected in real time through a data acquisition system and compared with the simulation results in Step 1 to correct the model. Step 3: Simulate and optimize electrical parameters. Based on the corrected model, with the maximum temperature difference of billet ≤10℃, target furnace exit temperature 1150±20℃, and total heating time ≤5h as optimization targets, the three-stage heating electrical parameters and holding time are obtained. Step 4: Auxiliary temperature equalization measures. Using the electrical parameters and holding time obtained in Step 3, heat the steel billet. Based on the measured temperature equalization, place a special heat preservation cover on the upper port of the induction heating furnace, install a high-temperature resistant fiber sealing ring on the lower port, and add an insulation sleeve around the outside. Step 5: Optimize the mold entry temperature. After heating is completed, the billet is transferred to the mold through an automated transfer system. The mold entry temperature T0 and transfer time Δt during the transfer process are collected to deduce the reasonable furnace exit temperature and adjust the input power and time of the third stage of heating in Step 3.
[0012] Furthermore, in step 1, the transient study includes the following steps: S101. A two-dimensional axisymmetric simulation model is established using the induction heating module of finite element software. The computational domain of the model includes: the billet as the object to be heated, the induction coil that generates the alternating magnetic field, the cooling water used to cool the coil, the furnace wall that forms the boundary of the furnace body, and the air that fills the remaining space. S102. Add material properties to the model, inputting parameter values for martensitic stainless steel within the temperature range of 20℃ to 1200℃, including magnetic permeability, electrical conductivity, Young's modulus, Poisson's ratio, density, specific heat capacity, coefficient of linear expansion, and thermal conductivity; among which, magnetic permeability, electrical conductivity, Young's modulus, and Poisson's ratio are calculated based on the chemical composition of martensitic stainless steel using metal material phase diagram calculation and performance simulation software; density, specific heat capacity, coefficient of linear expansion, and thermal conductivity are measured data; dielectric constant is set to 1; S103. Set the coil model, and set the structural and electrical parameters of the induction coil. The structural parameters include the number of coil turns, inner diameter, and pitch, all of which are preset values consistent with the actual induction heating furnace. The electrical parameters include the current frequency of 500-1500Hz and the output power of 10-200 kW. S104. Set the heat transfer of the model, including convection and radiation between the billet and the air inside the furnace, and convection and heat transfer between the furnace wall and the air inside and outside the furnace; apply heat transfer boundary conditions to the model, including convective heat transfer between the billet surface and the furnace atmosphere, and radiative heat transfer between the billet surface and the furnace wall; set the initial temperature of the billet and the outside to 25°C and the pressure to 1 atmosphere. S105. Mesh the model. Create a triangular mesh for the blank model. Add a "boundary layer mesh" to the workpiece surface. Set the number of layers to 5, the stretch factor to 1.6, and the core mesh size to 2-3mm. S106. Perform simulated heating with a heating time of 1-5 hours, a step size of 0.1 hours, and a heating temperature of 1150℃ as the heating target. Use a high current frequency of 800-1000 Hz and a low input power of 30-50 kW as the input conditions to numerically simulate the transient temperature field of the billet during the electromagnetic induction heating process and obtain the transient temperature field distribution of the billet during the heating process.
[0013] Furthermore, in step 2, the physical heating and model correction include the following steps: S201, Physical Heating Experiment Martensitic stainless steel billets of the same specifications as those in the simulation model were used. The heating experiment was conducted using the same current and input power as the electromagnetic induction heating in step 1 when simulating the transient temperature field. The heating furnace used was a semiconductor frequency conversion induction heating furnace. Armored S-type thermocouples are installed radially at the end and middle sections of the billet, respectively, on the surface and in the core, to record the temperature change data at each measuring point in real time. This data is used to correct the model and to determine the Curie transformation temperature range of the billet. S202, Modified Numerical Model Permeability correction: Based on the actual temperature measurement curve, the Curie temperature point is obtained, and the permeability above this temperature is corrected to 1; Parameter fine-tuning: After completing the permeability correction, the resistivity, dielectric constant, mesh generation, and heat transfer coefficient of the model are adjusted to make the temperature close to the measured data and control the difference between the measured temperature and the actual temperature within an acceptable range of 20℃.
[0014] Furthermore, in step 3, the optimal electrical parameters are obtained by cross-validation between the final heating effect and the heating target.
[0015] Further, in step 5, optimizing the mold entry temperature includes the following steps: S501, Slide rail conveying: After the billet reaches the target forging temperature of 1150±20℃ through electromagnetic induction heating, the induction power is cut off, the billet is lowered to the furnace, and then the slide rail drive motor is started; the slide rail carrying the billet moves the billet from under the furnace to the forging press at a certain speed until the billet completely leaves the coil and reaches the robotic arm picking station located on the discharge side of the induction heating furnace. S502, Robotic Arm Material Handling and Powder Rolling: The first robotic arm grips one end of the billet, lifts it from the slide rail, and transfers it to the powder rolling platform located adjacent to the workstation. This platform has a V-groove structure, with a layer of S-Glass powder with a particle size of 100-200 mesh and a thickness of about 3-5 mm pre-laid inside the groove. The bottom of the platform is driven by a servo motor to rotate at a certain speed. The robotic arm places the billet on the rotating platform, and the billet rotates in place for a certain period of time under the drive of the platform, so that the glass powder is evenly adhered to the entire cylindrical surface. The surface of the platform is coated with an anti-stick coating to prevent the glass powder from sticking at high temperatures. S503, Robotic arm loading into the mold: After rotation stops, the same robotic arm picks up the blank again and transfers it to the center of the lower mold of the opened forging mold, where it is positioned by the locating pin inside the mold; then the mold closes and forging begins.
[0016] S504. Further optimize heating parameters: Based on the measured data such as the temperature before mold entry and transfer time in steps S501-S503, deduce the reasonable furnace exit temperature, finely adjust the input power and time of the third stage in step 3, optimize the mold entry temperature, ensure high grain size [4.1] and uniform grain size before forging, and completely eliminate high temperature ferrite. Furthermore, in step 5, the total time Δt from the start of step S501 to the completion of step S503 does not exceed a preset threshold T, where T≤60 seconds.
[0017] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects: 1. Through three-stage rapid electromagnetic induction heating, the microstructure inheritance of martensitic stainless steel is effectively broken, achieving grain refinement and homogenization. The rapid heating process enables austenitization to be completed in a short time, significantly increasing the nucleation rate and the initial austenite grain size. At the same time, due to the extremely short high-temperature residence time, grain coarsening and microstructure inheritance are interrupted, resulting in smaller and more uniform austenite grain size in the billet after heating, laying the microstructure foundation for the high strength and toughness of the final forging.
[0018] 2. Strictly control the frequency, power, and time of the three stages. The first stage ensures a low power density to avoid instantaneous overheating of the surface layer, allowing time for heat to conduct to the inner layer and ensuring a gentle preheating temperature rise. The second stage reduces the frequency to increase the penetration depth and simultaneously increases the power, allowing heat to propel into the core with a greater heat flux density. The time is controlled to ensure that the grains do not coarsen excessively. The third stage increases the power, using high power to shorten the overall heating time and prevent excessive grain growth caused by prolonged high temperature. At the same time, the time is controlled to ensure that the billet does not overheat, preventing the formation of high-temperature ferrite. The temperature of any part of the billet is controlled to not exceed the high-temperature ferrite formation temperature throughout the process, ultimately achieving a pre-forging grain size of 2-3.
[0019] 3. This invention determines the optimal heating parameters that meet multiple objectives through cross-validation and correction using physical experiments and simulations, avoiding the extensive experimental costs of traditional trial-and-error methods. The optimized core-to-surface temperature difference of large-diameter billets is only 10℃, far superior to the over 30℃ of conventional electromagnetic induction heating methods, resulting in a more uniform temperature distribution within the billet's internal gradient space. Simultaneously, it significantly shortens the heating time in conventional heat treatment furnaces, reducing the total heating time by more than 70% compared to traditional resistance furnaces. Furthermore, it allows for pre-forging temperature feedback to adjust heating parameters, ultimately achieving effective control over the billet's grain size and laying the microstructural foundation for the high strength and toughness of the final forging.
[0020] 4. Optimizing mold entry temperature through efficient integration of induction rapid heating and forging processes. This invention, through automated processes of slide rail conveying, robotic arm material handling, powder rolling platform lubrication, and robotic arm mold entry, reduces the total time from the end of heating to the entry of the billet into the forging mold to less than 2 minutes, significantly better than the traditional overhead crane hoisting + manual application of glass powder (usually taking more than 15 minutes). This design effectively avoids grain coarsening caused by prolonged residence of fine-grained structures at high temperatures, thus securing the grain refinement effect obtained by induction rapid heating.
[0021] 5. Uniform and controllable lubrication, improving forging quality. The powder rolling platform rotates to ensure that the glass powder adheres evenly to the surface of the billet, avoiding problems such as uneven thickness and missed coating caused by manual application. At the same time, this "post-powder rolling" process avoids excessive reaction between the glass powder and the substrate due to prolonged high-temperature melting during the induction heating stage, ensuring lubrication effect without damaging the surface quality of the material.
[0022] 6. Secondary optimization ensures stable grain size and high uniformity of the workpiece before forging (grain size grade difference less than 1 grade), with no high-temperature ferrite. The third-stage heating process is precisely controlled. Based on measured data such as pre-drilling temperature and transfer time, the optimal furnace exit temperature is further improved. The input power and time of the third stage are fine-tuned to optimize the mold entry temperature and ensure high grain size before forging.
[0023] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description
[0024] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.
[0025] Figure 1 This is a flowchart illustrating the overall technical route of the method of the present invention.
[0026] Figure 2 This is a temperature curve of the billet cross section under segmented variable power induction heating conditions.
[0027] Figure 3 This is a schematic diagram of the sealing scheme for the furnace bottom and furnace opening of an electromagnetic induction heating furnace.
[0028] Figure 4 This is a schematic diagram of the position of the attached pair.
[0029] Figure 5 The image shows the grain size before extrusion after being placed in the mold in Example 3 of this invention.
[0030] Figure 6 Comparison photos of grain size before extrusion after entering the mold, for example 1, using the traditional method.
[0031] Figure label: 1. Top seal; 2. Billet; 3. Induction furnace; 4. Bottom seal; 5. Support column (movable up and down for furnace entry and exit); 6. Encasing. Detailed Implementation
[0032] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.
[0033] This invention provides a rapid electromagnetic induction heating process before forging for large-diameter precipitation-strengthened martensitic stainless steel, comprising: Includes three-stage heating: First stage heating: When the billet temperature is lower than the Curie point temperature, induction heating is performed at a frequency of 800-1000Hz and an input power of 30-50KW. Second stage heating: When the surface temperature of the billet reaches the Curie point, switch the input frequency to 100-500Hz and the input power to 80-140KW until the surface temperature of the billet reaches the target temperature of 1100±20℃. The third stage is temperature equalization: when the surface of the billet reaches the target temperature of 1100±20℃, increase the input power to 140-180kw, heat to the furnace exit temperature of 1150±20℃, hold for heat and then remove from the furnace.
[0034] It should be noted that the three-stage rapid electromagnetic induction heating effectively breaks down the microstructure inheritance of martensitic stainless steel, achieving grain refinement and homogenization. The rapid heating process allows austenitization to be completed in a short time, significantly increasing the nucleation rate and the initial austenite grain size. At the same time, due to the extremely short high-temperature residence time, grain coarsening and microstructure inheritance are interrupted, resulting in smaller and more uniform austenite grains in the billet after heating, laying the microstructure foundation for the high strength and toughness of the final forging.
[0035] Specifically, the diameter of the blank is 150-300mm.
[0036] Specifically, the total heating time for the three-stage heating process is 2.5-3.5 hours.
[0037] First stage (preheating stage): The billet temperature is below the Curie point, the material is ferromagnetic, and the induced current is concentrated on the surface. A frequency of 800–1000 Hz and a power of 30–50 kW are used. At this stage, the magnetic current penetration depth is shallow, and the low power density avoids instantaneous overheating of the surface, allowing time for heat to conduct to the inner layers, achieving a gentle preheating temperature rise. This stage is maintained for 1–1.5 hours and ends when the surface temperature reaches the Curie point.
[0038] The second stage (heating stage): Once the surface temperature reaches the Curie point, the material loses its magnetism and its equivalent resistance increases, allowing induction heating to penetrate deeper. Therefore, the frequency is switched to 100–500 Hz (reducing the frequency to increase penetration depth), and the power is simultaneously increased to 80–140 kW, allowing heat to propel into the core with a higher heat flux density until the surface temperature reaches the target of 1100±20℃. This stage is maintained for 1–1.5 hours, ensuring that the grain size does not become excessively coarsened through rapid heating.
[0039] The third stage (uniform temperature unloading stage): After the surface temperature reaches 1100±20℃, the power is increased to 140–180 kW. After the temperature reaches the unloading temperature of 1150±20℃, the material is briefly held at this temperature before unloading to achieve uniform surface and core temperature. This stage is maintained for 0.5–0.6 hours. The high power is used to shorten the overall heating time and prevent excessive grain growth caused by prolonged high temperature, achieving a pre-forging grain size of 1–3. At the same time, the time is controlled to ensure that the billet does not overheat and to prevent the formation of high-temperature ferrite.
[0040] Specifically, auxiliary temperature equalization measures are also included: the steel billet is heated, and according to the actual temperature equalization, a special heat preservation cover is placed at the upper port of the induction heating furnace, a high-temperature resistant fiber sealing ring is installed at the lower port, and an insulation sleeve is added to the outside.
[0041] It should be noted that by placing a dedicated heat-insulating cover at the upper port of the induction heating furnace, installing a high-temperature resistant fiber sealing ring at the lower port, and adding an outer heat-insulating sleeve, the overall temperature of the forging is more uniform, resulting in finer grain size after temperature homogenization. The auxiliary temperature homogenization structure effectively ensures the grain refinement effect of the heat treatment process and is one of the important technical means of this invention.
[0042] Specifically, this also includes optimizing the mold-entry process: through the automated process of slide rail conveying, robotic arm material handling, powder rolling platform lubrication, and robotic arm mold entry, the total time from the end of heating to the entry of the billet into the forging mold is reduced to less than 2 minutes.
[0043] Specifically, the martensitic stainless steel treated with electromagnetic induction heating does not contain high-temperature ferrite when it enters the forging mold. It should be noted that during forging, the presence of high-temperature ferrite can cause uneven deformation and stress concentration at the two-phase interface, easily leading to crack initiation and forging failure. This invention, through precise control of the third-stage heating process, combined with an auxiliary temperature equalization structure and optimized mold-feeding device, further ensures that the forging does not contain high-temperature ferrite before forging.
[0044] This invention provides an optimized method for a rapid electromagnetic induction heating process before forging of large-diameter precipitation-strengthened martensitic stainless steel. It includes: Step 1: Simulate the transient temperature field. Using finite element software, numerical simulations are performed on the transient temperature field of the billet during electromagnetic induction heating in a two-dimensional axisymmetric model.
[0045] Step 2: Cross-validation and correction of physical heating experiments and model. The billet is electromagnetically induction heated in an induction furnace. Temperature change data is collected in real time through a data acquisition system and compared with the simulation results from Step 1 to correct the model. Special attention should be paid to the change in the billet's magnetic permeability with temperature.
[0046] Step 3: Simulate and optimize electrical parameters. Based on the corrected model, with the optimization objectives of maximum billet temperature difference ≤10℃, target furnace exit temperature 1150±20℃, and total heating time ≤5h (heating + holding), the electrical parameters are optimized to obtain the three-stage heating electrical parameters.
[0047] Step 4: Auxiliary temperature equalization measures. Using the electrical parameters simulated in Step 3, the steel billet is heated. Based on whether the measured temperature equalization meets the heating requirements, a special heat preservation cover is placed at the upper port of the induction heating furnace, a high-temperature resistant fiber sealing ring is installed at the lower port, and an insulation sleeve is added to the outside to reduce the escape of hot gas from the furnace. Ultimately, the goal of achieving a longitudinal temperature difference of ≤10℃ between the end and middle sections of the billet is achieved.
[0048] Step 5: Optimize mold entry temperature. After heating is complete, the billet is transferred to the mold via an automated transfer system, and the mold entry temperature T0 and transfer time Δt during the transfer process are collected and fed back to Step 3 for optimization of heating parameters.
[0049] Specifically, in step 1 above, the transient study includes the following steps: S101. A simulation model is established using the induction heating module of finite element software. Given that both the billet and the coil have axisymmetric structures, a two-dimensional axisymmetric model is established to save computation time. The computational domain of the model includes: the billet being heated, the induction coil generating the alternating magnetic field, the cooling water used to cool the coil, the furnace wall forming the furnace boundary, and the air filling the remaining space. The induction copper coil is hollow, with cooling water flowing through the center. The furnace body is a cylindrical tube.
[0050] S102. Add material properties to the model. Input the permeability, conductivity, dielectric constant, density, specific heat capacity, coefficient of linear expansion, thermal conductivity, Young's modulus, and Poisson's ratio of 15-5PH stainless steel as a function of temperature within the temperature range of 20℃ to 1200℃. The permeability, conductivity, Young's modulus, and Poisson's ratio are calculated using metal material phase diagram calculation and performance simulation software based on the chemical composition of 15-5PH stainless steel. Density, specific heat capacity, coefficient of linear expansion, and thermal conductivity are measured data; all input are numerical points corresponding to a series of different temperatures. Set the dielectric constant to 1. Define the material properties of other components (such as coils, furnace walls, etc.) in the conventional way.
[0051] S103. Set the coil model. Set the structural and electrical parameters of the induction coil. The structural parameters include the number of coil turns, inner diameter, and pitch, all of which are preset values consistent with the actual induction heating furnace. The electrical parameters include the current frequency of 500~1500Hz and the output power of 10~200 kW.
[0052] S104. Set the heat transfer parameters for the model. This includes convection and radiation between the billet and the air inside the furnace, as well as convection and heat transfer between the furnace wall and the air inside and outside the furnace. Apply heat transfer boundary conditions to the model based on the convection and radiation patterns between the billet and the air inside the furnace. Specifically, this includes convective heat transfer between the cylindrical surface and upper and lower surfaces of the billet and the furnace atmosphere (using the software's built-in natural convection mode for the heat transfer coefficient), and radiative heat transfer between the billet surface and the furnace wall (surface emissivity α = 0.7). Set the initial temperature of the billet and the outside environment to 25°C and the pressure to 1 atmosphere.
[0053] S105. Mesh the model. Perform triangular meshing on the blank model, add a "boundary layer mesh" to the workpiece surface, set the number of layers to 5, the stretch factor to 1.6, and the core mesh size to 2~3mm.
[0054] S106. Simulated heating is performed. The heating time is 1-5 hours with a step size of 0.1 hours, and the heating temperature is 1150℃ as the heating target. Considering the risk of thermal cracking due to excessive temperature difference between the core and the surface, as well as the requirements of through-heating, melting, and heat treatment in heavy industrial scenarios, the coil adopts high current frequency (800-1000 Hz) and low input power (30-50kW) as input conditions to numerically simulate the transient temperature field of the billet during the electromagnetic induction heating process, and the transient temperature field distribution of the billet during the heating process is obtained from the simulation.
[0055] Specifically, step 2 above includes the following steps: S201, Physical Heating Experiment To verify the accuracy of the numerical model established in step 1, a physical heating experiment was conducted in this embodiment. The experiment used 15-5PH stainless steel billets of the same specifications as the simulation model (200mm diameter, 400mm length), and employed the same current and input power as S106 for the heating experiment. To ensure the heat penetration capability of the large forgings, a semiconductor frequency conversion induction heating furnace was used, with a maximum frequency of 1kHz and a maximum output power of 750kW. This furnace can also be adjusted according to the actual steel billet composition and size.
[0056] To comprehensively acquire temperature field information of the billet, armored S-type thermocouples were installed radially at the end and middle sections of the billet, at the surface and core, respectively, for a total of four measuring points. During the heating process, the temperature change data of each measuring point was recorded in real time through a data acquisition system for subsequent model correction. Simultaneously, the Curie transformation temperature range of the billet was determined.
[0057] S202, Modify the numerical model.
[0058] The measured temperature rise curves at each measuring point were compared with the numerical simulation results from step 1. A significant deviation was found between the initial model predictions and the measured data, especially at the measuring points in the core of the billet, where the difference between the measured temperature and the model prediction exceeded acceptable limits. Analysis suggests that the main reason is that the initial model did not accurately reflect the rapid change in magnetic permeability of 15-5PH stainless steel near the Curie temperature.
[0059] Therefore, the model is modified as follows: Permeability correction: Based on the actual temperature measurement curve, the Curie temperature point (the region where the heating rate suddenly drops) is obtained, and the permeability above this temperature is corrected to 1.
[0060] Parameter fine-tuning: After completing the permeability correction, the resistivity, dielectric constant, mesh generation, and heat transfer coefficient of the model are adjusted to make the temperature close to the measured data and control the difference between the measured temperature and the actual temperature within an acceptable range of 20℃.
[0061] Specifically, in step 3 above, based on the modified numerical simulation model and the change of the magnetic permeability of the billet with temperature, the frequency, input power, and holding time are adjusted.
[0062] Based on the above strategies, continue to adjust the heating input power, frequency, and time, observe whether the final heating effect is closest to the heating target, and finally determine the appropriate induction heating input power, frequency, and time.
[0063] It should be noted that simulations revealed a sharp drop in heating efficiency after reaching the Curie point, and the billet underwent excessively long heating times, leading to a significant increase in the temperature difference between the surface and core. The surface was overheated while the core had not yet reached the required temperature. Through model correction steps, particularly the correction of the magnetic permeability to 1, and fine-tuning of key parameters such as resistivity, dielectric constant, mesh generation, and heat transfer coefficient, the simulation process was further optimized. This effectively improved the accuracy of the simulation, reduced the time and cost of 5-10 physical verifications, shortened the R&D cycle by approximately one month, and provided a foundation for subsequent experimental cross-validation and calibration accuracy.
[0064] Simulation results show that a three-stage power input heating strategy can achieve rapid heating and uniform internal and external temperatures. In the initial stage, 50kW is maintained for 80 minutes to raise the temperature to the Curie transition temperature (approximately 720℃). In the middle stage, 130kW is maintained for 50 minutes to raise the surface temperature to 1100℃. In the final stage, 150kW is maintained for 20 minutes to uniformly raise the temperature to 1150℃. At this point, the maximum radial temperature difference of the billet is 10℃, and the maximum longitudinal temperature difference is 30℃, with the upper end being hotter than the lower end.
[0065] Specifically, in step 4 above, the actual heating was carried out according to the optimized scheme of steps 1-4. The total heating time for the billet to reach the forging temperature of 1150±20℃ and achieve uniform temperature was measured to be 3 hours, which is 80% shorter than the traditional resistance furnace heating time of about 15 hours. Metallographic analysis results show that the austenite grain size of the billet cross section after heating reaches grade 2-3, while the grain size of the comparative sample treated by traditional furnace heating is only grade 0-00.
[0066] Specifically, in step 5 above, the measured data is fed back to step 3 to optimize the mold entry temperature, including the following steps: S501, Slide Rail Conveying: After the billet reaches the target forging temperature of 1150±20℃ through electromagnetic induction heating, the induction power is cut off, the billet is lowered to the furnace, and then the slide rail drive motor is started. The slide rail carrying the billet moves the billet from under the furnace towards the forging press at a certain speed until the billet completely leaves the coil and reaches the robotic arm picking station located on the discharge side of the induction heating furnace.
[0067] S502. Robotic Arm Material Handling and Powder Rolling: The first robotic arm grips one end of the billet, lifts it from the slide rail, and transfers it to a powder rolling platform located adjacent to the workstation. This platform has a V-groove structure, with a layer of S-Glass powder with a particle size of 100-200 mesh, approximately 3-5 mm thick, pre-laid inside the groove. The bottom of the platform is driven by a servo motor, rotating at a certain speed. The robotic arm places the billet on the rotating platform, and the billet rotates in place for a certain period of time under the platform's influence, allowing the glass powder to adhere evenly to the entire cylindrical surface. The platform surface is coated with an anti-stick coating to prevent the glass powder from sticking together at high temperatures.
[0068] S503, Robotic Arm Insertion into the Die: After rotation stops, the same robotic arm picks up the billet again and transfers it to the center of the lower die of the opened forging mold, where it is positioned by the locating pin inside the mold. The mold then closes, and forging begins.
[0069] S504. Further optimize heating parameters: Based on the measured data such as the temperature before mold entry and transfer time in steps S501-S503, deduce a reasonable furnace exit temperature, fine-tune the input power and time in the third stage of step 3, optimize the mold entry temperature, and ensure high grain size before forging.
[0070] The transfer time Δt and the mold entry temperature T0 are recorded. The total time Δt from the start of step S501 to the completion of step S503 does not exceed the preset threshold T. This threshold T is calculated by combining the numerical simulation model in step one with the temperature drop curve of the billet in air. Usually, T≤60 seconds, to ensure that the surface temperature T0 of the billet when it enters the mold is not lower than the lower limit of the target forging temperature.
[0071] Record the oven exit temperature as T1, and the mold entry temperature after transfer as T0. Then, the temperature drop during the transfer process is ΔT = T1 - T0. If the ideal mold entry temperature is T2, then the ideal oven exit temperature is T2 + ΔT.
[0072] By optimizing the mold entry temperature, on the one hand, the effectiveness of the simulation and experimental optimization results can be improved, and the optimal induction heating process for large-diameter precipitation hardening stainless steel can be obtained; on the other hand, it can further ensure that the grain size of the forging before forging is greater than level 1, the overall grain size difference of the billet is less than level 2, and it is completely free of high-temperature ferrite, thereby ensuring the mechanical properties and microstructure of the forging after forging.
[0073] Specifically, the samples forged after steps 1-5, after further performance heat treatment, exhibit the following characteristics in the steel billet: grain size ≥ 6, tensile strength ≥ 1100 MPa, yield strength ≥ 1050 MPa, elongation after fracture ≥ 13%, and reduction of area ≥ 60%. The surface hardness uniformity is good, with a difference within 20 HB. It does not contain high-temperature ferrite. Optimization using the same method on billets with diameters of 150 mm and 300 mm yields different optimal parameter combinations, demonstrating the good universality of the optimization method of this invention.
[0074] To more clearly describe the present invention, the following embodiments and comparative examples are provided for further illustration.
[0075] Example 1 Using a 15-5PH precipitation-hardening martensitic stainless steel round bar billet with a diameter of Φ200mm and a length of 400mm as the experimental object, the method of the present invention was implemented according to the following steps: First stage heating: When the billet temperature is lower than the Curie point temperature, induction heating is performed at a frequency of 800Hz and an input power of 50KW. The skin effect is mainly used to quickly heat the surface of the billet at a higher frequency and transfer heat to the inside. Second stage heating: When the surface temperature of the billet reaches the Curie point temperature of 720℃, the input frequency is switched to 100Hz and the input power is 100KW. Taking advantage of the characteristic that the penetration depth increases significantly after the magnetic permeability of the billet drops sharply, the internal heating rate of the billet is increased, the internal and external temperature difference is reduced, until the surface temperature of the billet reaches the target furnace exit temperature of 1100℃.
[0076] The third stage is temperature equalization: when the surface of the billet reaches the target temperature of 1100℃, the input power is increased to 150kw, and the billet is heated to 1150℃ before being taken out of the furnace.
[0077] Grain size is grade 1-3. Grade 1 has coarser grains on the upper surface, while Grade 3 has lower temperatures or shorter holding times in the lower part and core. It contains no high-temperature ferrite at all.
[0078] Example 2 In addition to the same three-stage temperature equalization process as in Example 1, a special heat-insulating cover is placed at the upper port of the induction heating furnace, a high-temperature resistant fiber sealing ring is installed at the lower port, and an insulation sleeve is added to the outside to reduce the escape of hot gas from the furnace chamber, ultimately achieving the goal of a longitudinal temperature difference of ≤10℃ between the end and middle sections of the billet.
[0079] With a grain size of 2-3, the overall temperature is more uniform, resulting in a relatively finer and more uniform grain size. Specifically, the surface is grade 2 and the core is grade 3, completely free of high-temperature ferrite.
[0080] Example 3 Using a 15-5PH precipitation-hardening martensitic stainless steel round bar billet with a diameter of Φ250mm and a length of 400mm as the experimental object, the method of the present invention was implemented according to the following steps: Step 1: Simulate the transient temperature field.
[0081] S101. A two-dimensional axisymmetric simulation model is established using the induction heating module of finite element software. The computational domain of the model includes: the billet being heated, the induction coil that generates the alternating magnetic field, the cooling water used to cool the coil, the furnace wall that forms the boundary of the furnace body, and the air filling the remaining space.
[0082] S102. Add material properties to the model. Input the magnetic permeability, electrical conductivity, dielectric constant, density, specific heat capacity, coefficient of linear expansion, thermal conductivity, Young's modulus, and Poisson's ratio of 15-5PH stainless steel as a function of temperature in the temperature range of 20℃ to 1200℃.
[0083] The permeability, conductivity, Young's modulus, and Poisson's ratio were calculated using phase diagram calculation and performance simulation software based on the chemical composition of 15-5PH stainless steel. Density, specific heat capacity, coefficient of linear expansion, and thermal conductivity were measured data, all input as a series of discrete temperature-value points. The dielectric constant was set to 1. The material properties of other components (such as coils and furnace walls) were defined in a conventional manner.
[0084] S103. Set the coil model. Set the structural and electrical parameters of the induction coil. The structural parameters are: 15 coil turns, 0.3 cm inner diameter, and 1.5 cm pitch. The electrical parameters are: current frequency 1 kHz and output power 40 kW.
[0085] S104. Set the heat transfer parameters for the model. This includes convection and radiation between the billet and the furnace air, and convection and heat transfer between the furnace wall and the air inside and outside the furnace. Apply heat transfer boundary conditions to the model, including convective heat transfer between the billet surface and the furnace atmosphere (heat transfer coefficient using the software's built-in natural convection mode) and radiative heat transfer between the billet surface and the furnace wall (surface emissivity α = 0.7). Set the initial temperature of the billet and the outside environment to 25°C and the pressure to 1 atmosphere.
[0086] S105. Mesh the model. Perform triangular meshing on the blank model, add a "boundary layer mesh" to the workpiece surface, set the number of layers to 5, the stretch factor to 1.6, and the core mesh size to 2~3mm.
[0087] S106, S106, simulated heating. With a heating time of 1-5h, a step size of 0.1h, and a heating temperature of 1150℃ as the heating target, and a current frequency of 1kHz and an input power of 40kW as the input conditions, the transient temperature field of the billet during the electromagnetic induction heating process is numerically simulated, and the transient temperature field distribution of the billet during the heating process is obtained.
[0088] Step 2: Physical heating experiment and model correction.
[0089] S201, Physical Heating Experiment To verify the accuracy of the numerical model established in step 1, a physical heating experiment was conducted in this embodiment. The experiment used 15-5PH stainless steel billet of the same specifications as the simulation model (Φ200mm×400mm), and the heating experiment was carried out at a current frequency of 1kHz and an input power of 40kW.
[0090] To comprehensively acquire information about the billet temperature field, four sheathed S-type thermocouples were installed radially at the end and middle sections of the billet, one on the surface and the other at the core. During heating, the temperature changes at each measuring point were recorded in real time using a data acquisition system, which was then used to correct the model. Simultaneously, the Curie transformation temperature range of the billet was determined, providing experimental basis for the next three-stage simulation.
[0091] S202, Modify the numerical model.
[0092] The measured temperature rise curves at each measuring point were compared with the numerical simulation results from step 1. A significant deviation was found between the initial model predictions and the measured data, especially at the measuring points in the core of the billet, where the difference between the measured temperature and the model prediction exceeded acceptable limits. Analysis suggests that the main reason is that the initial model did not accurately reflect the rapid change in magnetic permeability of 15-5PH stainless steel near the Curie temperature.
[0093] Therefore, the model is modified as follows: Permeability correction: Based on the actual temperature measurement curve, the Curie temperature point (the area where the heating rate suddenly drops, approximately 720℃) is obtained, and the permeability above this temperature is corrected to 1.
[0094] Parameter fine-tuning: After completing the permeability correction, the resistivity, dielectric constant, mesh generation, and heat transfer coefficient of the model are adjusted to make the temperature close to the measured data and control the difference between the measured temperature and the actual temperature within an acceptable range of 20℃.
[0095] Step 3: Simulate and optimize electrical parameters. The electrical parameters are optimized with the following objectives: maximum billet temperature difference ≤10℃, target furnace exit temperature 1150±20℃, and total heating time ≤5h (heating + holding). Based on the corrected numerical simulation model and the change in billet magnetic permeability with temperature, the design involves adjusting the frequency and input power in three stages to simulate the heating process.
[0096] Based on the above strategies, the heating input power, frequency, and time are fine-tuned, the final heating effect is observed, and the appropriate induction heating input power, frequency, and time are finally determined.
[0097] Simulation results show that the three-stage power input heating strategy can achieve rapid heating and uniform internal and external temperatures. In the initial stage, 50kW is maintained for 80 minutes to raise the temperature to the Curie transition temperature of approximately 720℃. In the middle stage, 130kW is maintained for 50 minutes to raise the surface temperature to 1100℃. In the later stage, 150kW is maintained for 20 minutes to uniformly raise the temperature to 1150℃. The maximum temperature difference in the radial direction of the billet is 10℃, and the temperature at the upper end is about 30℃ higher than that at the lower end.
[0098] Step 4: Auxiliary temperature equalization measures. Using the electrical parameters simulated in Step 3, heating is performed, and the measured temperature equalization is recorded. A special heat-insulating cover is placed at the upper port of the induction heating furnace, and a high-temperature resistant fiber sealing ring is installed at the lower port. An insulation sleeve is added around the outside, made of refractory insulation cotton, with a sleeve thickness of about 5-10mm. This reduces the escape of hot gas from the furnace chamber, further reducing the longitudinal temperature gradient at the ends and middle sections of the billet by about 30%.
[0099] Following the optimized scheme in steps 1-4, the actual heating time for the billet to reach the forging temperature of 1150±20℃ and achieve uniform temperature was measured to be 3 hours, which is 80% shorter than the approximately 15 hours required for traditional resistance furnace heating. Metallographic analysis results show that the austenite grain size of the billet cross-section after heating reaches grade 2-3, while the grain size of the comparative sample treated by traditional furnace heating is only grade 0-00.
[0100] Step 5: Optimize the mold inlet temperature.
[0101] S501, Slide Rail Conveying: After the billet reaches the target forging temperature of 1150±20℃ through electromagnetic induction heating, the induction power is cut off, the billet is lowered to the outlet of the furnace, and then the slide rail drive motor is started. The slide rail carrying the billet moves the billet from under the furnace towards the forging press at a speed of about 0.2 m / s. After about 10 seconds, the billet completely leaves the coil and arrives at the robotic arm picking station located on the outlet side of the induction heating furnace.
[0102] S502. Robotic Arm Material Handling and Powder Rolling: The first robotic arm grips one end of the billet, lifts it from the slide rail, and transfers it to a powder rolling platform located adjacent to the workstation. This platform has a V-groove structure, with a layer of S-Glass powder with a particle size of 100-200 mesh, approximately 3-5 mm thick, pre-laid inside the groove. The bottom of the platform is driven by a servo motor, rotating at a speed of 20 rpm. The robotic arm places the billet on the rotating platform, and the billet rotates in place for approximately 10 seconds under the platform's influence, allowing the glass powder to adhere evenly to the entire cylindrical surface. The platform surface is coated with an anti-stick coating to prevent the glass powder from sticking together at high temperatures.
[0103] S503, Robotic Arm Insertion into the Die: After rotation stops, the same robotic arm picks up the billet again and transfers it to the center of the lower die of the opened forging mold, where it is positioned by the locating pin inside the mold. The mold then closes, and forging begins.
[0104] S504. Further optimize heating parameters: Based on the measured data such as the temperature before mold entry and transfer time in steps S501-S503, deduce a reasonable exit temperature, and fine-tune the input power and time of the third stage of heating parameters to form adaptive control.
[0105] The entire process, from heating to blank placement in the mold, was timed and displayed, taking approximately 2 minutes in total. This included 20 seconds for unloading, approximately 10 seconds for slide rail transfer, approximately 40 seconds for robotic transfer and powder rolling, and approximately 50 seconds for secondary transfer and mold placement. The measured surface temperature of the blank upon mold placement was 1130~1150℃, still within the recommended forging window temperature of 1050~1150℃ for precipitation-strengthened martensitic stainless steel. The pre-forging blank had a grain size of 2-3 grades and high overall uniformity.
[0106] It is important to note that since the temperature difference after electromagnetic induction heating is mainly reflected in the upper end surface being hotter than the lower end surface, the blank is rotated up and down before being placed into the mold, so that the hotter part comes into contact with the mold, thereby further homogenizing the temperature difference.
[0107] Metallographic analysis of the billet after the above complete process showed that its austenite grain size remained at level 2-3, which was basically consistent with that at the end of heating, indicating that the transfer and powder rolling process within 2 minutes did not cause obvious grain coarsening.
[0108] Compared with the traditional process of using overhead cranes to transport glass and manually applying glass powder, the above transfer process optimizes the mold entry temperature, effectively locks in the fine-grained structure obtained by induction rapid heating, and provides an optimization direction for adjusting the induction heating parameters.
[0109] Among them, after electromagnetic induction heating, forging, and performance heat treatment, the overall grain size level of the prototype is above level 7, which indicates that the pre-forging heating method of the present invention significantly refines the austenite grains and effectively inhibits the inheritance of microstructure.
[0110] Comparative Example 1 A conventional pit-type resistance furnace was used to heat 15-5PH billets of the same specifications as in Example 1. The heating temperature was set at 1150℃, the heating rate was about 100℃ / h, the heating time was 10h, and the temperature was uniformized for 5h after heating for 10h. The total heating time was about 15h.
[0111] Among them, after heating for 10 hours, there is a significant temperature difference between the center and the surface of the billet. This is because the heat treatment furnace relies on thermal radiation and heat conduction, and the heating of the core of large billets is severely delayed. After 4 hours of uniform temperature, the internal and external temperatures are uniform, but at this time the surface has been held at 1150℃ for 4 hours, resulting in coarser austenite grains on the surface, with obvious mixed crystals and hereditary microstructure.
[0112] After subsequent forging, the grains of this batch of forgings were coarser, and the uniformity of grain size was significantly lower than that of the forgings obtained in Example 1, which did not meet the product technical requirements.
[0113] Comparative Example 2 The same optimization method as in Example 3 was adopted, but instead of using automated slide rails and a powder rolling platform, an overhead crane was used to hoist and apply glass powder on the ground, and then an operator was used to clamp the blank onto the mold.
[0114] The results showed that it took about 15 minutes from the end of heating to the time of mold insertion. When the billet was inserted into the mold, the surface temperature had dropped to below 1000℃, which was lower than the lower limit of the forging window (1050℃), resulting in surface cracks during extrusion. Metallographic analysis showed that the austenite grains had coarsened to about 0-00 grade.
[0115] After subsequent forging, the grain size is grade 1-2.
[0116] Comparative Example 3 No model correction was used; otherwise, it was the same as in Example 3.
[0117] The excessive temperature difference between the top and bottom of the billet resulted in poor uniformity of grain size. The upper part, with its excessively high temperature, had a grain size of 0-1 grade, while the lower part, with its lower temperature, had a grain size of 3-4 grade. This temperature unevenness affected the uniformity of the overall microstructure and properties during subsequent forging / extrusion deformation. The lower part, with its excessively low temperature, exhibited surface cracking during extrusion.
[0118] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A pre-forging rapid electromagnetic induction heating process for large diameter precipitation strengthened martensitic stainless steel, characterized in that, Includes three-stage heating: First stage heating: When the billet temperature is lower than the Curie point temperature, induction heating is performed at a frequency of 800-1000Hz and an input power of 30-50KW. Second stage heating: When the surface temperature of the billet reaches the Curie point temperature, switch the input frequency to 100-500Hz and the input power to 80-140KW until the surface temperature of the billet reaches the target temperature of 1100±20℃. The third stage is temperature equalization: when the surface of the billet reaches the target temperature of 1100±20℃, increase the input power to 140-180kw, heat to the furnace exit temperature of 1150±20℃, hold for heat and then remove from the furnace.
2. The process according to claim 1, characterized in that, The diameter of the blank is 150-300mm.
3. The process according to claim 1, characterized in that, The total heating time for the three-stage heating process is 2.5-3.5 hours.
4. The process according to claim 1, characterized in that, It also includes auxiliary temperature equalization measures: heating the steel billet, placing a special heat preservation cover at the upper port of the induction heating furnace according to the actual temperature equalization, installing a high-temperature resistant fiber sealing ring at the lower port, and adding an insulation sleeve around the outside.
5. The process according to claim 4, characterized in that, Martensitic stainless steel treated with electromagnetic induction heating does not contain high-temperature ferrite before being forged into the forging die.
6. An optimized method for a rapid electromagnetic induction heating process before forging of large-diameter precipitation-strengthened martensitic stainless steel according to claim 1, characterized in that, Specifically, the following steps are included: Step 1: Simulate the transient temperature field. Using finite element software, numerical simulation of the transient temperature field of the billet during electromagnetic induction heating is performed in a two-dimensional axisymmetric model. Step 2: Physical heating experiment and model cross-validation and correction. The billet is electromagnetically induction heated in an induction furnace. During the process, temperature change data is collected in real time through a data acquisition system and compared with the simulation results in Step 1 to correct the model. Step 3: Simulate and optimize electrical parameters. Based on the corrected model, with the maximum temperature difference of billet ≤10℃, target furnace exit temperature 1150±20℃, and total heating time ≤5h as optimization targets, the three-stage heating electrical parameters and holding time are obtained. Step 4: Auxiliary temperature equalization measures. Using the electrical parameters and holding time obtained in Step 3, heat the steel billet. Based on the measured temperature equalization, place a special heat preservation cover on the upper port of the induction heating furnace, install a high-temperature resistant fiber sealing ring on the lower port, and add an insulation sleeve around the outside. Step 5: Optimize the mold entry temperature. After heating is completed, the billet is transferred to the mold through an automated transfer system. The mold entry temperature T0 and transfer time Δt during the transfer process are collected to deduce the reasonable furnace exit temperature and adjust the input power and time of the third stage of heating in Step 3.
7. The optimization method according to claim 6, characterized in that, In step 1, the transient study includes the following steps: S101. A two-dimensional axisymmetric simulation model is established using the induction heating module of finite element software. The computational domain of the model includes: the billet as the object to be heated, the induction coil that generates the alternating magnetic field, the cooling water used to cool the coil, the furnace wall that forms the boundary of the furnace body, and the air that fills the remaining space. S102. Add material properties to the model, inputting parameter values for martensitic stainless steel within the temperature range of 20℃ to 1200℃, including magnetic permeability, electrical conductivity, Young's modulus, Poisson's ratio, density, specific heat capacity, coefficient of linear expansion, and thermal conductivity; among which, magnetic permeability, electrical conductivity, Young's modulus, and Poisson's ratio are calculated based on the chemical composition of martensitic stainless steel using metal material phase diagram calculation and performance simulation software; density, specific heat capacity, coefficient of linear expansion, and thermal conductivity are measured data; dielectric constant is set to 1; S103. Set the coil model, and set the structural and electrical parameters of the induction coil. The structural parameters include the number of coil turns, inner diameter, and pitch, all of which are preset values consistent with the actual induction heating furnace. The electrical parameters include current frequency of 500~1500 Hz and output power of 10~200 kW. S104. Set the heat transfer of the model, including convection and radiation between the billet and the air inside the furnace, and convection and heat transfer between the furnace wall and the air inside and outside the furnace; apply heat transfer boundary conditions to the model, including convective heat transfer between the billet surface and the furnace atmosphere, and radiative heat transfer between the billet surface and the furnace wall; set the initial temperature of the billet and the outside to 25°C and the pressure to 1 atmosphere. S105. Mesh the model. Create a triangular mesh for the blank model. Add a "boundary layer mesh" to the workpiece surface. Set the number of layers to 5, the stretch factor to 1.6, and the core mesh size to 2~3mm. S106. Perform simulated heating with a heating time of 1-5 hours, a step size of 0.1 hours, and a heating temperature of 1150℃ as the heating target. Use a high current frequency of 800-1000 Hz and a low input power of 30-50 kW as the input conditions to numerically simulate the transient temperature field of the billet during the electromagnetic induction heating process and obtain the transient temperature field distribution of the billet during the heating process.
8. The optimization method according to claim 7, characterized in that, Step 2, the physical heating and model correction, includes the following steps: S201, Physical Heating Experiment Martensitic stainless steel billets of the same specifications as those in the simulation model were used. The heating experiment was conducted using the same current and input power as the electromagnetic induction heating in step 1 when simulating the transient temperature field. The heating furnace used was a semiconductor frequency conversion induction heating furnace. Armored S-type thermocouples are installed radially at the end and middle sections of the billet, respectively, on the surface and in the core, to record the temperature change data at each measuring point in real time. This data is used to correct the model and to determine the Curie transformation temperature range of the billet. S202, Modified Numerical Model Permeability correction: Based on the actual temperature measurement curve, the Curie temperature is obtained, and the permeability above this temperature is corrected to 1; Parameter fine-tuning: After completing the permeability correction, the resistivity, dielectric constant, mesh generation, and heat transfer coefficient of the model are adjusted to make the temperature close to the measured data and control the difference between the measured temperature and the actual temperature within an acceptable range of 20℃.
9. The optimization method according to claim 6, characterized in that, Step 5, optimizing the mold entry temperature, includes the following steps: S501, Slide rail conveying: After the billet reaches the target forging temperature of 1150±20℃ through electromagnetic induction heating, the induction power is cut off, the billet is lowered to the furnace, and then the slide rail drive motor is started; the slide rail carrying the billet moves the billet from under the furnace to the forging press at a certain speed until the billet completely leaves the coil and reaches the robotic arm picking station located on the discharge side of the induction heating furnace. S502, Robotic Arm Material Handling and Powder Rolling: The first robotic arm grips one end of the billet, lifts it from the slide rail, and transfers it to the powder rolling platform located adjacent to the workstation. This platform has a V-groove structure, with a layer of S-Glass powder with a particle size of 100~200 mesh and a thickness of 3~5 mm pre-laid inside the groove. The bottom of the platform is driven by a servo motor to rotate at a certain speed. The robotic arm places the billet on the rotating platform, and the billet rotates in place for a certain period of time under the drive of the platform, so that the glass powder is evenly adhered to the entire cylindrical surface. The surface of the platform is coated with an anti-stick coating to prevent the glass powder from sticking at high temperatures. S503, Robotic Arm Entering the Die: After rotation stops, the same robotic arm picks up the billet again and transfers it to the center of the lower die of the opened forging die, where it is positioned by the locating pin inside the die; then the die closes and forging begins; S504. Further optimize heating parameters: Based on the measured data such as the temperature before mold entry and transfer time in steps S501-S503, deduce a reasonable furnace exit temperature, fine-tune the input power and time in the third stage of step 3, optimize the mold entry temperature, ensure high grain size and uniformity before forging, and completely eliminate high-temperature ferrite.
10. The optimization method according to claim 9, characterized in that, In step 5, the total time Δt from the start of step S501 to the completion of step S503 does not exceed the preset threshold T, where T≤60 seconds.