A high-toughness HIC-resistant HBW550 grade wear-resistant steel plate and its preparation method

HBW550 grade wear-resistant steel plates are prepared by converter smelting and precision-controlled rolling process, which solves the problem of hydrogen-induced cracking of steel plates in high sulfur and low temperature environments in the existing technology. It achieves a balance of high hardness, low temperature toughness and resistance to hydrogen-induced cracking, and is suitable for complex working conditions.

CN123108255APending Publication Date: 2026-11-17SHANDONG IRON & STEEL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611394346.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing HBW550 grade wear-resistant steel plates are prone to hydrogen-induced cracking in environments containing hydrogen sulfide and at low temperatures. They also lack low-temperature toughness and cannot meet the requirements of complex working conditions such as high-sulfur mines and oil and gas fields containing hydrogen sulfide. Furthermore, traditional processes cannot simultaneously achieve a balance between hardness, toughness, and resistance to hydrogen-induced cracking.

Method used

By employing converter smelting + LF refining + RH vacuum treatment, controlling the steel composition and rolling process, and combining light reduction, full argon protection, two-stage controlled rolling and heat treatment, HBW550 grade wear-resistant steel plate with excellent resistance to hydrogen-induced cracking was prepared.

Benefits of technology

The prepared steel plate exhibits HBW550 grade high hardness, excellent low-temperature toughness and resistance to hydrogen-induced cracking under high sulfur, humid and low temperature environments, making it suitable for heavy-load wear conditions and improving the service safety and service life of equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a high-toughness HBW550 grade wear-resistant steel plate with HIC resistance and its preparation method. The chemical composition of the steel plate is: C: 0.28~0.35%, Si: 0.10~0.50%, Mn: 0.20~1.0%, P≤0.010%, S≤0.0010%, Nb: 0.010~0.040%, V: 0.030~0.060%, Ti≤0.010%, Cr: 0.60~ The composition of the steel plate is as follows: 2.0%, Mo: 0.10~0.50%, Ni: 0.20~0.80%, Cu: 0.10~0.30%, B: 0.001~0.003%, Ca: 0.0010~0.0040%, Al: 0.020~0.080%, N≤0.0040%, O≤0.0020%, H≤0.00015%. The preparation method includes smelting, continuous casting, slab heating, rolling, and heat treatment. The wear-resistant steel plate of this invention possesses both HBW550 grade high hardness and wear resistance, excellent low-temperature toughness, and exhibits excellent resistance to HIC (High-Intensity Concentration Increasing).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of high-strength wear-resistant steel, specifically relating to a high-toughness HBW550 grade wear-resistant steel plate with HIC resistance and its preparation method. Background Technology

[0002] With the technological iteration and increasing scale of equipment in industries such as mining equipment, construction machinery, coal transportation, and oil and gas field construction, the service conditions for key wear-resistant components in heavy-duty equipment are becoming increasingly stringent. The industry's technical requirements for the hardness grade, wear resistance stability, and overall service performance of wear-resistant steel plates are rising year by year. Traditional low- and medium-hardness wear-resistant steels can no longer meet the design requirements of equipment with high wear, long service life, and high safety. HBW550 grade high-hardness wear-resistant steel plates, with their higher matrix hardness and superior resistance to abrasive wear, will gradually become the preferred material for high-end heavy-duty wear-resistant equipment, and market demand will increase significantly year by year, with application scenarios continuously expanding.

[0003] Given the actual operating conditions in high-sulfur mines and hydrogen sulfide-containing oil and gas fields, conventional HBW550 grade wear-resistant steel plates currently exhibit significant performance shortcomings. In hydrogen sulfide-containing, humid, and acidic operating environments, conventional HBW550 grade steel plates are prone to hydrogen-induced cracking (HIC) defects. Hydrogen atoms penetrate into the steel's crystal lattice, triggering the initiation and propagation of microcracks, ultimately leading to component cracking and failure. Their resistance to HIC is extremely poor, failing to meet the requirements for wear-resistant equipment in oil and gas applications and the humid and corrosive conditions of underground mines. Furthermore, HBW550 grade wear-resistant steel plates produced using traditional manufacturing processes lack sufficient low-temperature toughness. In extremely cold environments at -20℃ and below, their impact energy decreases significantly, resulting in a very high risk of brittle fracture, severely limiting their application in cold northern regions and in low-temperature outdoor heavy-duty equipment. Furthermore, existing wear-resistant steels, in pursuit of hardness and wear resistance, generally suffer from problems such as unreasonable alloy ratios, coarse grains, high levels of inclusions, and poor microstructure uniformity, making it impossible to simultaneously achieve wear resistance, low-temperature toughness, and resistance to HIC corrosion. Conventional processes struggle to achieve a synergistic match of high-strength wear resistance, low-temperature toughening, and resistance to hydrogen-induced cracking, and the performance stability of steel plates during mass production is poor, with low yield rates, making them unsuitable for the complex and harsh working conditions of high sulfur content, humidity, low temperature, and heavy-load wear. The industry urgently needs a wear-resistant steel plate and its matching manufacturing process that combines HBW550 standard hardness, ultra-high and low temperature toughness, and excellent HIC resistance. However, relevant literature and the latest publicly available patent technology search results show that a wear-resistant steel plate possessing HBW550 hardness, ultra-high and low temperature toughness, and excellent HIC resistance remains a gap in the existing technological system.

[0004] Therefore, developing a wear-resistant steel plate with a hardness of HBW550, excellent resistance to hydrogen-induced cracking, and high toughness at low temperatures, along with its supporting preparation method, is of great engineering application value for addressing the shortcomings of existing technologies, adapting to the upgrading trend of high-end wear-resistant steel, expanding the applicable range of material working conditions, and improving the service safety and service life of heavy-duty wear-resistant equipment. Summary of the Invention

[0005] To address the aforementioned technical problems in the prior art, this invention provides a high-toughness HBW550 grade wear-resistant steel plate with HIC resistance and its preparation method. This wear-resistant steel plate possesses excellent HIC resistance and low-temperature impact toughness. Its Brinell hardness (HBW) value, an indicator of wear resistance, reaches the HBW550 grade. It is suitable for heavy-load wear conditions in environments with hydrogen sulfide, high humidity, and low temperature, such as high-sulfur mines and hydrogen sulfide-containing oil and gas fields, meeting the stringent requirements of equipment for material hardness, toughness, and HIC resistance.

[0006] In a first aspect of the present invention, the method for preparing HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate includes the following steps: (1) Smelting: The steel is smelted in a converter + refined by LF + vacuum treated by RH. The chemical composition of the molten steel is controlled by weight percentage as follows: C: 0.28~0.35%, Si: 0.10~0.50%, Mn: 0.20~1.0%, P≤0.010%, S≤0.0010%, Nb: 0.010~0.040%, V: 0.030~0.060%, Ti≤0.010%, Cr: 0.60~2.0%, Mo: 0.10~0.50%, Ni: 0.20~0.80%, Cu: 0.10~0.30%, B: 0.001~0.003%, Ca: 0.0010~0.0040%, Al: 0.020~0.080%. N≤0.0040%, O≤0.0020%, H≤0.00015%, with the remainder being Fe and unavoidable impurities; (2) Continuous casting: Argon gas and protective slag are used for casting throughout the process, and the continuous casting slab is slowly cooled for more than 48 hours after it leaves the line; (3) Slab heating: The heating temperature is controlled at 1200~1230℃, the heating time is controlled at 8~10min / cm based on the slab thickness, and the heat soaking time is controlled at ≥40min; (4) Rolling: The slab is rolled into steel plate using a two-stage controlled rolling process. In the rough rolling stage, the high-penetration mode fully recrystallized zone controlled rolling is carried out at ≥1000℃, and in the finish rolling stage, the strain accumulation controlled rolling is carried out in the non-recrystallized zone at an initial rolling temperature of 900~970℃. (5) Heat treatment: Heat the steel plate to 920~930℃, and control the holding time according to the thickness of the steel plate at 1.0~2.0min / mm. After the holding time is completed, quench to room temperature and then temper at 160~200℃.

[0007] Furthermore, in the smelting process, the molten iron is pre-desulfurized before converter smelting to control the weight percentage content of sulfur in the molten iron to within 0.0012%.

[0008] Furthermore, in the smelting step, the weight percentage ratio of Ca to S in the molten steel is controlled to be [Ca] / [S] = 2.0~3.5, the weight percentage ratio of Ca to Al is controlled to be [Ca] / [Al] = 0.05~0.07, the weight percentage ratio of Mn to Si is controlled to be [Mn] / [Si] = 3.5~5.5, and the weight percentage ratio of Mn to S is controlled to be [Mn] / [S] ≥ 200.

[0009] Furthermore, in the continuous casting process, a light reduction process is used, with the light reduction amount controlled at 5~6mm, the billet pulling speed controlled at 1.0~1.3m / min, and the superheat of the molten steel controlled at ≤20℃.

[0010] Furthermore, in the roughing stage of the rolling process, the initial rolling temperature is controlled at ≥1050℃, the final rolling temperature is controlled at ≥1000℃, and the cumulative reduction rate is controlled at >50%. In addition, the reduction rate of each pass in the roughing stage is distributed according to the principle of increasing with each pass, and the reduction rate of each pass in the last 3 passes is controlled at >16%. The thickness of the intermediate billet to be heated is controlled at 2.5 to 5.0 times the thickness of the finished steel plate. In the finishing stage of the rolling process, the initial rolling temperature is controlled at 900 to 960℃, the final rolling temperature is controlled at 840 to 860℃, and the cumulative reduction rate is controlled at >60%. In addition, the reduction rate of each pass in the finishing stage is distributed according to the principle of decreasing with each pass.

[0011] In a second aspect of the invention, the chemical composition of the provided HIC-resistant high-toughness HBW550 grade wear-resistant steel plate, by weight percentage, is as follows: C: 0.28~0.35%, Si: 0.10~0.50%, Mn: 0.20~1.0%, P≤0.010%, S≤0.0010%, Nb: 0.010~0.040%, V: 0.030~0.060%, Ti≤0.010%, Cr: 0.60~2.0%, Mo: 0.10~0.50%, Ni: 0.20~0.80%, Cu: 0.10~0.30%, B: 0.001~0.003%, Ca: 0.0010~0.0040%, Al: 0.020~0.080%. N≤0.0040%, O≤0.0020%, H≤0.00015%, with the remainder being Fe and unavoidable impurities.

[0012] Furthermore, in the HIC-resistant high-toughness HBW550 wear-resistant steel plate, the weight percentage ratio of Ca to S is controlled to be [Ca] / [S] = 2.0~3.5, the weight percentage ratio of Ca to Al is controlled to be [Ca] / [Al] = 0.05~0.07, the weight percentage ratio of Mn to Si is controlled to be [Mn] / [Si] = 3.5~5.5, and the weight percentage ratio of Mn to S is controlled to be [Mn] / [S] ≥ 200.

[0013] Furthermore, the carbon equivalent (CEV) of the HIC-resistant high-toughness HBW550 grade wear-resistant steel plate is CEV≤0.75%, and the corrosion resistance index (I) is I>6.0%.

[0014] Furthermore, the near-surface Brinell hardness of the HIC-resistant high-toughness HBW550 grade wear-resistant steel plate is HBW520~570, the core Brinell hardness is ≥HBW480, the thickness gradient Brinell hardness is ≥HBW500, and the yield strength R... p0.2 ≥1200MPa, tensile strength R m ≥1600MPa, elongation after fracture A 50 ≥8%, Charpy V-notch impact energy KV2≥35J at -40℃, Charpy V-notch impact energy KV2≥27J at -50℃, crack length ratio CLR≤10%, crack thickness ratio CTR≤3%, crack sensitivity ratio CSR≤1%.

[0015] The method for preparing HIC-resistant high-toughness HBW550 grade wear-resistant steel plates of the present invention is simple and easy to operate, suitable for large-scale industrial production. The prepared HIC-resistant high-toughness HBW550 grade wear-resistant steel plates combine the high hardness and wear resistance of HBW550 grade, excellent low-temperature toughness, and other characteristics, while exhibiting excellent HIC resistance. Its mechanical properties meet the following requirements: near-surface Brinell hardness HBW520~570, core Brinell hardness ≥HBW480, thickness gradient Brinell hardness ≥HBW500; yield strength R p0.2 ≥1200MPa, tensile strength R m ≥1600MPa, elongation after fracture A 50≥8%, Charpy V-notch impact energy (transverse / longitudinal) KV2≥35J at -40℃, Charpy V-notch impact energy (transverse / longitudinal) KV2≥27J at -50℃; its HIC resistance meets the NACE TM0284-2016 standard A solution test requirements, crack length ratio CLR≤10%, crack thickness ratio CTR≤3%, crack sensitivity rate CSR≤1%, solving the industry pain point that traditional wear-resistant steel cannot simultaneously achieve hardness, toughness, and corrosion cracking resistance. It perfectly meets the multiple requirements of complex service conditions such as high sulfur humidity, low temperature, and heavy-load wear. It has very important engineering application value for solving the shortcomings of existing technologies, adapting to the upgrading trend of high-end wear-resistant steel, expanding the application range of materials, and improving the service safety and service life of heavy-duty wear-resistant equipment. Detailed Implementation

[0016] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0017] The method for preparing HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate provided by this invention includes the following steps: (1) Smelting: Converter smelting is adopted, and double slag operation is used during smelting to reduce P content; through LF refining + RH vacuum treatment, harmful gases such as O, H, N and S content are reduced. The chemical composition of the molten steel prepared by smelting is controlled by weight percentage as follows: C: 0.28~0.35%, Si: 0.10~0.50%, Mn: 0.20~1.0%, P≤0.010%, S≤0.0010%, Nb: 0.010~0.040%, V: 0.030~0.060%, Ti≤0.010%, Cr: 0.60~2.0%, Mo: 0.10~0.50%, Ni: 0.20~0.80%, Cu: 0.10~0.30%, B: 0.001~0.003%, Ca: 0.0010~0.0040%, Al: 0.020~0.080%. N≤0.0040%, O≤0.0020%, H≤0.00015%, with the remainder being Fe and unavoidable impurities.

[0018] (2) Continuous casting: Argon gas and protective slag are used for casting throughout the process. The light reduction process is combined with the light reduction amount controlled at 5~6mm and the billet pulling speed controlled at 1.0~1.3m / min. The control of the first and second cooling processes in the continuous casting process is strengthened, and the continuous casting slab is slowly cooled for more than 48 hours after leaving the line.

[0019] (3) Slab heating: Strictly control the atmosphere in the heating furnace, adopt micro-positive pressure control, control the heating temperature at 1200~1230℃, control the heating time based on the slab thickness at 8~10min / cm, and control the heat soaking time at ≥40min to ensure that the steel billet is heated evenly and thoroughly.

[0020] (4) Rolling: The slab is rolled into steel plate using a two-stage controlled rolling process. In the rough rolling stage, the high-penetration mode fully recrystallized zone controlled rolling is carried out at ≥1000℃, and in the finish rolling stage, the strain accumulation controlled rolling is carried out in the non-recrystallized zone at an initial rolling temperature of 900~970℃.

[0021] (5) Heat treatment: After shot blasting, the steel plate is heated to 920~930℃. The holding time is controlled according to the thickness of the steel plate at 1.0~2.0min / mm. After the holding time is completed, the plate is quenched to room temperature and then tempered at 160~200℃.

[0022] Preferably, in the smelting step, the molten iron is pre-desulfurized before converter smelting to control the weight percentage content of S in the molten iron to within 0.0012%.

[0023] Preferably, in the smelting step, the content ratio of Ca to S in the molten steel prepared by smelting (the ratio of weight percentage content, i.e., weight ratio) is controlled at [Ca] / [S] = 2.0~3.5, the content ratio of Ca to Al (the ratio of weight percentage content, i.e., weight ratio) is controlled at [Ca] / [Al] = 0.05~0.07, the content ratio of Mn to Si (the ratio of weight percentage content, i.e., weight ratio) is controlled at [Mn] / [Si] = 3.5~5.5, and the content ratio of Mn to S (the ratio of weight percentage content, i.e., weight ratio) is controlled at [Mn] / [S] ≥ 200, so as to fully complete the modification of inclusions, optimize the morphology of deoxidation products, realize the spheroidization modification of sulfides, reduce the enrichment of large-size inclusions, and weaken the tendency of manganese element interdendritic segregation. Thus, the level of segregation and banded structure is reduced from the smelting source, while ensuring the stability of the steel's resistance to hydrogen-induced cracking.

[0024] Preferably, in the continuous casting step, the superheat of the molten steel is controlled to be ≤20°C.

[0025] Preferably, in the roughing stage of the rolling process, the initial rolling temperature is controlled at ≥1050℃, the final rolling temperature is controlled at ≥1000℃, the cumulative reduction rate is controlled at >50%, and the reduction rate of each pass in the roughing stage is distributed according to the progressively increasing distribution, with the reduction rate of each of the last 3 passes controlled at >16%.

[0026] Preferably, in the roughing stage of the rolling process, the thickness of the intermediate billet to be heated is controlled to be 2.5 to 5.0 times the thickness of the finished steel plate.

[0027] Preferably, in the finishing rolling stage of the rolling process, the initial rolling temperature is controlled at 900~960℃, the final rolling temperature is controlled at 840~860℃, the cumulative reduction rate is controlled at >60%, and the reduction rate of each pass in the finishing rolling stage is distributed according to the decreasing distribution of each pass to ensure the flatness of the steel plate.

[0028] Preferably, in the rolling step, the rolled steel plate is water-cooled to 610°C using ACC.

[0029] Preferably, in the heat treatment step, the quenching adopts the "low roller speed + large water volume" mode to fully ensure the hardenability of the steel plate, and the roller speed of the quenching machine is controlled to be ≤4.0m / min.

[0030] The chemical composition (by weight percentage) of the HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate prepared by the above-described preparation method of the present invention is as follows: C: 0.28~0.35%, Si: 0.10~0.50%, Mn: 0.20~1.0%, P≤0.010%, S≤0.0010%, Nb: 0.010~0.040%, V: 0.030~0.060%, Ti≤0.010%, Cr: 0.60~2.0%, Mo: 0.10~0.50%, Ni: 0.20~0.80%, Cu: 0.10~0.30%, B: 0.001~0.003%, Ca: 0.0010~0.0040%, Al: 0.020~0.080%. N≤0.0040%, O≤0.0020%, H≤0.00015%, with the remainder being Fe and unavoidable impurities.

[0031] Preferably, in the HIC-resistant high-toughness HBW550 wear-resistant steel plate, the content ratio of Ca to S (weight percentage ratio, i.e., weight ratio) is controlled to [Ca] / [S] = 2.0~3.5, the content ratio of Ca to Al (weight percentage ratio, i.e., weight ratio) is controlled to [Ca] / [Al] = 0.05~0.07, the content ratio of Mn to Si (weight percentage ratio, i.e., weight ratio) is controlled to [Mn] / [Si] = 3.5~5.5, and the content ratio of Mn to S (weight percentage ratio, i.e., weight ratio) is controlled to [Mn] / [S] ≥ 200, so as to fully complete the modification of inclusions. The corresponding effects and technical benefits are: optimizing the morphology of deoxidation products, realizing spheroidization modification of sulfides, reducing the enrichment of large-size inclusions, and weakening the tendency of manganese element interdendritic segregation, thereby reducing the level of segregation and banded structure from the smelting source, while ensuring the stability of the steel's resistance to hydrogen-induced cracking.

[0032] Preferably, the carbon equivalent (CEV) of the HIC-resistant high-toughness HBW550 grade wear-resistant steel plate is controlled to be CEV≤0.75%, where CEV=[C]+[Mn] / 6+([Cr]+[V]+[Mo]) / 5+([Ni]+[Cu]) / 15, and the unit is %. [C], [Mn], [Cr], [V], [Mo], [Ni], and [Cu] refer to the weight percentage content of C, Mn, Cr, V, Mo, Ni, and Cu, respectively.

[0033] Preferably, the corrosion resistance index I of the HIC-resistant high-toughness HBW550 grade wear-resistant steel plate is controlled to be I > 6.0%, where I (%) = 26.01 × [Cu] + 3.88 × [Ni] + 1.20 × [Cr] + 1.49 × [Si] + 17.28 × [P] - 7.29 × [Cu] × [Ni] - 9.10 × [Ni] × [P] - 33.39 × [Cu] 2 The units are %, and [Cu], [Ni], [Cr], [Si], and [P] refer to the weight percentage content of Cu, Ni, Cr, Si, and P, respectively.

[0034] Preferably, the HIC-resistant high-toughness HBW550 grade wear-resistant steel plate has a microstructure mainly composed of tempered martensite, with the original austenite grain size controlled at level 6 to 9.

[0035] Preferably, the mechanical properties of the HIC-resistant high-toughness HBW550 grade wear-resistant steel plate meet the following requirements: near-surface Brinell hardness HBW520~570, core Brinell hardness ≥HBW480, thickness gradient Brinell hardness ≥HBW500; yield strength R p0.2 ≥1200MPa, tensile strength R m ≥1600MPa, elongation after fracture A 50 ≥8%, Charpy V-notch impact energy (lateral / longitudinal) KV2≥35J at -40℃, Charpy V-notch impact energy (lateral / longitudinal) KV2≥27J at -50℃.

[0036] Preferably, the HIC resistance of the HIC-resistant high-toughness HBW550 grade wear-resistant steel plate meets the requirements of the NACE TM0284-2016 standard A solution test: crack length ratio CLR≤10%, crack thickness ratio CTR≤3%, and crack sensitivity ratio CSR≤1%.

[0037] The following detailed description of the HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate and its preparation method are illustrated with specific embodiments of the present invention.

[0038] Example 1 The chemical composition of the HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate in Example 1 is controlled by weight percentage as follows: C: 0.30%, Si: 0.15%, Mn: 0.60%, P: 0.008%, S: 0.001%, Ni: 0.53%, Nb: 0.025%, V: 0.040%, Ti: 0.005%, Cr: 0.95%, Mo: 0.32%, Cu: 0.21%, Al: 0.062%, B: 0.0021%, Ca: 0.0033%, H: 0.00011%, N: 0.0032%, with the remainder being Fe and unavoidable impurities.

[0039] The carbon equivalent (CEV) of the HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate in Example 1 is: CEV = [C] + [Mn] / 6 + ([Cr] + [V] + [Mo]) / 5 + ([Ni] + [Cu]) / 15 = 0.71%, and the corrosion resistance index (I) is: I = 26.01 × [Cu] + 3.88 × [Ni] + 1.20 × [Cr] + 1.49 × [Si] + 17.28 × [P] - 7.29 × [Cu] × [Ni] - 9.10 × [Ni] × [P] - 33.39 × [Cu] 2 =6.70%.

[0040] The specific implementation process of the preparation method of HIC-resistant high-toughness HBW550 grade wear-resistant steel plate in Example 1 is as follows: (1) Hot metal pretreatment: The KR mechanical stirring method is used to desulfurize the hot metal and control the weight percentage content of S in the hot metal to ≤0.001%.

[0041] (2) Smelting: The steel is produced by smelting in a converter + refining in LF + vacuum treatment in RH. The chemical composition of the steel is controlled by weight percentage as follows: C: 0.30%, Si: 0.15%, Mn: 0.60%, P: 0.008%, S: 0.001%, Ni: 0.53%, Nb: 0.025%, V: 0.040%, Ti: 0.005%, Cr: 0.95%, Mo: 0.32%, Cu: 0.21%, Al: 0.062%, B: 0.0021%, Ca: 0.0033%, H: 0.00011%, N: 0.0032%, with the remainder being Fe and unavoidable impurities.

[0042] (3) Continuous casting: Argon gas and protective slag are used for the entire casting process. The superheat is controlled to be ≤20℃. The continuous casting slab is slowly cooled for more than 48 hours after it is removed from the line. The dimensions (thickness × width × length) of the continuous casting slab are 250mm × 1800mm × 3600mm.

[0043] (4) Slab heating: The heating temperature is controlled at 1212℃, the heating time is controlled at 225~250min, and the heat soaking time is controlled at ≥40min to ensure that the steel billet is heated evenly and thoroughly.

[0044] (5) Rolling: The slab is rolled into a steel plate with a thickness of 10 mm by a two-stage controlled rolling process with two stands. The roughing rolling start temperature is 1158℃, the roughing rolling finish temperature is 1085℃, and the intermediate slab thickness is 50.0 mm. The finishing rolling start temperature is 930℃, and the finishing rolling finish temperature is 847℃.

[0045] (6) Heat treatment: Heat the steel plate to 920°C, hold for 10-20 minutes, quench to room temperature, and then temper at 190°C.

[0046] Example 2 The chemical composition of the HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate in Example 2 is controlled by weight percentage as follows: C: 0.31%, Si: 0.14%, Mn: 0.55%, P: 0.009%, S: 0.001%, Ni: 0.58%, Nb: 0.030%, V: 0.045%, Ti: 0.004%, Cr: 0.87%, Mo: 0.28%, Cu: 0.20%, Al: 0.060%, B: 0.0020%, Ca: 0.0031%, H: 0.00012%, N: 0.0031%, with the remainder being Fe and unavoidable impurities.

[0047] The carbon equivalent (CEV) of the HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate in Example 2 is: CEV = [C] + [Mn] / 6 + ([Cr] + [V] + [Mo]) / 5 + ([Ni] + [Cu]) / 15 = 0.69%, and the corrosion resistance index (I) is: I = 26.01 × [Cu] + 3.88 × [Ni] + 1.20 × [Cr] + 1.49 × [Si] + 17.28 × [P] - 7.29 × [Cu] × [Ni] - 9.10 × [Ni] × [P] - 33.39 × [Cu] 2 =6.20% The specific implementation process of the preparation method of HIC-resistant high-toughness HBW550 grade wear-resistant steel plate in Example 2 is as follows: (1) Hot metal pretreatment: The KR mechanical stirring method is used to desulfurize the hot metal and control the weight percentage content of S in the hot metal to ≤0.001%.

[0048] (2) Smelting: The steel is produced by smelting in a converter + refining in LF + vacuum treatment in RH. The chemical composition of the steel is controlled by weight percentage as follows: C: 0.31%, Si: 0.14%, Mn: 0.55%, P: 0.009%, S: 0.001%, Ni: 0.58%, Nb: 0.030%, V: 0.045%, Ti: 0.004%, Cr: 0.87%, Mo: 0.28%, Cu: 0.20%, Al: 0.060%, B: 0.0020%, Ca: 0.0031%, H: 0.00012%, N: 0.0031%, with the remainder being Fe and unavoidable impurities.

[0049] (3) Continuous casting: Argon gas and protective slag are used for the entire casting process. The superheat is controlled to be ≤20℃. The continuous casting slab is slowly cooled for more than 48 hours after it is removed from the line. The dimensions (thickness × width × length) of the continuous casting slab are 250mm × 1800mm × 3600mm.

[0050] (4) Slab heating: The heating temperature is controlled at 1219℃, the heating time is controlled at 200~250min, and the heat soaking time is controlled at ≥40min to ensure that the steel billet is heated evenly and thoroughly.

[0051] (5) Rolling: The slab is rolled into a steel plate with a thickness of 30 mm by a two-stage controlled rolling process with two stands. The roughing rolling start temperature is 1152℃, the roughing rolling finish temperature is 1087℃, and the intermediate slab thickness is 105.0 mm. The finishing rolling start temperature is 910℃, and the finishing rolling finish temperature is 842℃.

[0052] (6) Heat treatment: Heat the steel plate to 930°C, hold for 30-60 minutes, quench to room temperature, and then temper at 200°C.

[0053] Example 3 The chemical composition of the HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate in Example 3 is controlled by weight percentage as follows: C: 0.32%, Si: 0.16%, Mn: 0.72%, P: 0.007%, S: 0.001%, Ni: 0.62%, Nb: 0.022%, V: 0.041%, Ti: 0.006%, Cr: 0.90%, Mo: 0.33%, Cu: 0.23%, Al: 0.058%, B: 0.0023%, Ca: 0.0030%, H: 0.00011%, N: 0.0030%, with the remainder being Fe and unavoidable impurities.

[0054] The carbon equivalent (CEV) of the HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate in Example 3 is: CEV = [C] + [Mn] / 6 + ([Cr] + [V] + [Mo]) / 5 + ([Ni] + [Cu]) / 15 = 0.75%. The corrosion resistance index I = 26.01 × [Cu] + 3.88 × [Ni] + 1.20 × [Cr] + 1.49 × [Si] + 17.28 × [P] - 7.29 × [Cu] × [Ni] - 9.10 × [Ni] × [P] - 33.39 × [Cu] 2 =6.98%.

[0055] The specific implementation process of the preparation method of HIC-resistant high-toughness HBW550 grade wear-resistant steel plate in Example 3 is as follows: (1) Hot metal pretreatment: The KR mechanical stirring method is used to desulfurize the hot metal and control the weight percentage content of S in the hot metal to ≤0.001%.

[0056] (2) Smelting: The steel is produced by smelting in a converter + refining in LF + vacuum treatment in RH. The chemical composition of the steel is controlled by weight percentage as follows: C: 0.32%, Si: 0.16%, Mn: 0.72%, P: 0.007%, S: 0.001%, Ni: 0.62%, Nb: 0.022%, V: 0.041%, Ti: 0.006%, Cr: 0.90%, Mo: 0.33%, Cu: 0.23%, Al: 0.058%, B: 0.0023%, Ca: 0.0030%, H: 0.00011%, N: 0.0030%, with the remainder being Fe and unavoidable impurities.

[0057] (3) Continuous casting: Argon gas and protective slag are used for the entire casting process. The superheat is controlled to be ≤20℃. The continuous casting slab is slowly cooled for more than 48 hours after it is removed from the line. The dimensions (thickness × width × length) of the continuous casting slab are 250mm × 1800mm × 3600mm.

[0058] (4) Slab heating: The heating temperature is controlled at 1215℃, the heating time is controlled at 200~250min, and the heat soaking time is controlled at ≥40min to ensure that the steel billet is heated evenly and thoroughly.

[0059] (5) Rolling: The slab is rolled into a steel plate with a thickness of 50 mm by a two-stage controlled rolling process with two stands. The roughing rolling start temperature is 1153℃, the roughing rolling finish temperature is 1088℃, and the intermediate slab thickness is 130.0 mm. The finishing rolling start temperature is 900℃, and the finishing rolling finish temperature is 844℃.

[0060] (6) Heat treatment: Heat the steel plate to 930°C, hold for 50-100 minutes, quench to room temperature, and then temper at 200°C.

[0061] The mechanical properties and HIC resistance of the HIC-resistant high-toughness HBW550 grade wear-resistant steel plates prepared using Examples 1-3 of this invention were tested and verified. The test results are shown in Tables 1, 2, and 3 below: Table 1. Brinell hardness / room temperature tensile properties of the HIC-resistant high-toughness HBW550 grade wear-resistant steel plate of the present invention.

[0062] Table 2. Low-temperature Charpy impact properties of the HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate of the present invention.

[0063] Table 3. HIC resistance properties of the high-toughness HBW550 grade wear-resistant steel plate of the present invention.

[0064] The hardness test conducted on the HIC-resistant high-toughness HBW550 grade wear-resistant steel plate of the present invention was based on GB-T231.1-2018 "Metallic Materials - Brinell Hardness Test - Part 1: Test Method"; the yield strength, tensile strength, and elongation tests were based on GB / T228-2002 "Metallic Materials - Tensile Test at Room Temperature"; the impact energy test was based on GB / T229-2007 "Metallic Materials - Charpy Pendulum Impact Test Method"; and the HIC resistance test was based on NACE TM0284-2016 "NACE TM0284-2016 Evaluation of Hydrogen-Induced Cracking Resistance of Pipeline and Pressure Vessel Steels", using solution A (saturated H2S, pH≈2.7), and the test time was 96 hours.

[0065] As can be seen from the data in the table above, the preparation method of the HIC-resistant high-toughness HBW550 grade wear-resistant steel plate of the present invention is simple and easy to operate. The HIC-resistant high-toughness HBW550 grade wear-resistant steel plate produced has the characteristics of high hardness and wear resistance of HBW550 grade, excellent low temperature toughness, etc., and at the same time exhibits excellent HIC resistance performance. It is suitable for large-scale industrial production and perfectly meets the multiple requirements of complex service conditions such as high sulfur humidity, low temperature, and heavy load wear.

[0066] Compared with the prior art, the HIC-resistant high-toughness HBW550 grade wear-resistant steel plate and its preparation method of the present invention have the following advantages and beneficial effects: (1) The steel plate adopts a suitable CEV+Cr / Mo / Ni / Cu alloying + Nb / V / Al composite microalloying composition design, and high-penetration rolling to achieve homogenization of the microstructure in the thickness direction of the steel plate; offline quenching + tempering heat treatment to obtain a microstructure dominated by tempered martensite with suitable grain size, so that the steel plate has both the high hardness and wear resistance of HBW550 grade, excellent low temperature toughness and anti-HIC performance, and uniform microstructure in the thickness direction. This solves the industry pain point that the hardness, toughness and corrosion cracking resistance of traditional wear-resistant steel cannot be taken into account at the same time, and perfectly meets the multiple requirements of complex service conditions such as high sulfur humidity, low temperature and heavy load wear. At the same time, the service life is increased by more than 40% compared with traditional HBW550 steel plate.

[0067] (2) Through composition optimization and precise control of the whole process, the steel plate’s excellent resistance to hydrogen-induced cracking is guaranteed in all aspects; the content of harmful impurities is strictly limited, and the steel cleanliness is improved by pre-desulfurization and double refining processes, eliminating the source of crack initiation from the source; the ratio of various metallurgical elements is reasonably controlled to achieve spheroidization modification of sulfides, improve the segregation and banded structure of the billet, and block the crack propagation path; with the aid of controlled rolling and quenching + low temperature tempering processes, a dense and uniform tempered martensite structure is formed, which inhibits hydrogen atom aggregation and crack extension, so that the steel plate meets the standard high-level resistance to HIC and can be used in harsh acidic conditions.

[0068] (3) The whole process is mature, the process is closely connected, the parameters are precisely controlled, and the production stability and repeatability are good; the performance uniformity of the through plate is high, which is suitable for large-scale industrial production and has extremely high industrialization and promotion value.

[0069] (4) It breaks through the limitation that traditional HBW550 grade wear-resistant steel plates are only suitable for normal temperature dry wear conditions. It can be widely used in high-end and complex working conditions such as bucket teeth, scrapers, and conveying pipelines of excavators in high-sulfur mines in low-temperature and cold regions, wear-resistant equipment with sulfur corrosion in the oil and gas industry, and heavy-duty wear-resistant components in ports. It has strong market adaptability.

[0070] It should be noted that, unless otherwise specified, the terms used herein have the meanings commonly understood by those skilled in the art. Furthermore, when a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum. Additionally, when multiple ranges are provided to describe features, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0071] It should also be noted that, in this document, the term "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, such that an article or device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such an article or device.

[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit them. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the present invention.

Claims

1. A method for preparing HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate, characterized in that, Includes the following steps: (1) Smelting: The steel is smelted in a converter + refined by LF + vacuum treated by RH. The chemical composition of the molten steel is controlled by weight percentage as follows: C: 0.28~0.35%, Si: 0.10~0.50%, Mn: 0.20~1.0%, P≤0.010%, S≤0.0010%, Nb: 0.010~0.040%, V: 0.030~0.060%, Ti≤0.010%, Cr: 0.60~2.0%, Mo: 0.10~0.50%, Ni: 0.20~0.80%, Cu: 0.10~0.30%, B: 0.001~0.003%, Ca: 0.0010~0.0040%, Al: 0.020~0.080%. N≤0.0040%, O≤0.0020%, H≤0.00015%, with the remainder being Fe and unavoidable impurities; (2) Continuous casting: Argon gas and protective slag are used for the entire casting process, and the continuous casting slab is slowly cooled for more than 48 hours after it leaves the line; (3) Slab heating: The heating temperature is controlled at 1200~1230℃, the heating time is controlled at 8~10min / cm based on the slab thickness, and the heat soaking time is controlled at ≥40min; (4) Rolling: The slab is rolled into steel plate using a two-stage controlled rolling process. In the rough rolling stage, the high-penetration mode fully recrystallized zone controlled rolling is carried out at ≥1000℃, and in the finish rolling stage, the strain accumulation controlled rolling is carried out in the non-recrystallized zone at an initial rolling temperature of 900~970℃. (5) Heat treatment: Heat the steel plate to 920~930℃, and control the holding time according to the thickness of the steel plate at 1.0~2.0min / mm. After the holding time is completed, quench to room temperature and then temper at 160~200℃.

2. The method for preparing HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate according to claim 1, characterized in that, In the smelting process, the molten iron is pre-desulfurized before converter smelting to control the weight percentage content of sulfur in the molten iron to within 0.0012%.

3. The method for preparing HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate according to claim 2, characterized in that, In the smelting process, the weight percentage ratio of Ca to S in the molten steel is controlled at [Ca] / [S] = 2.0~3.5, the weight percentage ratio of Ca to Al is controlled at [Ca] / [Al] = 0.05~0.07, the weight percentage ratio of Mn to Si is controlled at [Mn] / [Si] = 3.5~5.5, and the weight percentage ratio of Mn to S is controlled at [Mn] / [S] ≥ 200.

4. The method for preparing HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate according to claim 1, characterized in that, In the continuous casting process, a light reduction process is used, with the light reduction amount controlled at 5~6mm, the billet pulling speed controlled at 1.0~1.3m / min, and the superheat of the molten steel controlled at ≤20℃.

5. The method for preparing HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate according to claim 1, characterized in that, In the roughing stage of the rolling process, the initial rolling temperature is controlled at ≥1050℃, the final rolling temperature is controlled at ≥1000℃, and the cumulative reduction rate is controlled at >50%. Furthermore, the reduction rate of each pass in the roughing stage is distributed according to the principle of increasing with each pass, and the reduction rate of each pass in the last 3 passes is controlled at >16%. The thickness of the intermediate billet to be heated is controlled at 2.5 to 5.0 times the thickness of the finished steel plate. In the finishing stage of the rolling process, the initial rolling temperature is controlled at 900 to 960℃, the final rolling temperature is controlled at 840 to 860℃, and the cumulative reduction rate is controlled at >60%. Furthermore, the reduction rate of each pass in the finishing stage is distributed according to the principle of decreasing with each pass.

6. A high-toughness HBW550 grade wear-resistant steel plate with HIC resistance, characterized in that, The chemical composition of the HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate, by weight percentage, is as follows: C: 0.28~0.35%, Si: 0.10~0.50%, Mn: 0.20~1.0%, P≤0.010%, S≤0.0010%, Nb: 0.010~0.040%, V: 0.030~0.060%, Ti≤0.010%, Cr: 0.60~2.0%, Mo: 0.10~0.50%, Ni: 0.20~0.80%, Cu: 0.10~0.30%, B: 0.001~0.003%, Ca: 0.0010~0.0040%, Al: 0.020~0.080%, N≤0.0040%, O≤0.0020%, H≤0.00015%, with the remainder being Fe and unavoidable impurities.

7. The HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate according to claim 6, characterized in that, The weight percentage ratio of Ca to S in the HIC-resistant high-toughness HBW550 wear-resistant steel plate is controlled at [Ca] / [S] = 2.0~3.5, the weight percentage ratio of Ca to Al is controlled at [Ca] / [Al] = 0.05~0.07, the weight percentage ratio of Mn to Si is controlled at [Mn] / [Si] = 3.5~5.5, and the weight percentage ratio of Mn to S is controlled at [Mn] / [S] ≥ 200.

8. The HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate according to claim 6, characterized in that, The HIC-resistant high-toughness HBW550 grade wear-resistant steel plate has a carbon equivalent (CEV) of ≤0.75% and a corrosion resistance index (I) of >6.0%.

9. The HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate according to claim 6, characterized in that, The near-surface Brinell hardness of the HIC-resistant, high-toughness HBW550 grade wear-resistant steel plate is HBW520~570, the core Brinell hardness is ≥HBW480, the thickness gradient Brinell hardness is ≥HBW500, and the yield strength R... p0.2 ≥1200MPa, tensile strength R m ≥1600MPa, elongation after fracture A 50 ≥8%, Charpy V-notch impact energy KV2≥35J at -40℃, Charpy V-notch impact energy KV2≥27J at -50℃, crack length ratio CLR≤10%, crack thickness ratio CTR≤3%, crack sensitivity ratio CSR≤1%.

Citation Information

Patent Citations

  • Cutting tool for the continuous machining of metals and the method of making same

    CA1000040A