A method for synergistic control of tensile defects in wide-width, ultra-thin stainless steel ribs during bright annealing
By employing methods such as furnace roller calibration, segmented annealing, idler roller optimization, and dynamic tension control, the defects of stretching and crescent creases in wide and ultra-thin stainless steel ribs were resolved, achieving efficient production and high yield.
Patent Information
- Application Number
- CN202611179481.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-05
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot effectively eliminate defects such as stretching and crescent-shaped creases in wide, ultra-thin stainless steel ribs, and have low production efficiency and yield.
A five-in-one collaborative control method is adopted, which includes unified furnace roller calibration, differentiated segmented annealing control, optimized idler roller layout, graded dynamic tension regulation, and graded emergency handling of defects. This method includes 9TV low-temperature transition process, low-speed cooling fan, reduction of the number of idlers, dynamic tension adjustment, and standardized emergency handling procedures.
It significantly reduces the incidence of tensile defects in ribs by 92%, improves unit production efficiency and yield, avoids frequent rewinding and speed reduction, and forms a closed-loop prevention and control system.
Smart Images

Figure CN123108274A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of bright continuous annealing process for stainless steel, and relates to a method for synergistic control of tensile defects in bright annealing of wide and ultra-thin stainless steel strips, applicable to wide and ultra-thin stainless steel strips with a thickness of 0.3mm and a width of 4F (1219mm). Background Technology
[0002] The length of the bright annealing furnace body and the arrangement of the burners are fixed, and their matching relationship with the process is as follows: 18TV corresponds to a maximum strip running speed of 60m / min, while the industry-standard wide and ultra-thin stainless steel usually uses 12TV, which corresponds to a running speed of 40m / min; the total length of the bright annealing unit inlet looper is 320m, the effective buffer capacity is taken as 80%, and the theoretical buffer time = 320m×80%÷40m / min=6.4min, which can only meet the basic operation window of conventional coil loading and changing.
[0003] Based on the "Process Design Specification for Bright Annealing Units of Stainless Steel", multiple published patents (CN113231479A, CN109097534B) and industry journal articles, the industry has long held two entrenched technical biases when processing 0.3mm×4F wide and extremely thin stainless steel rolls and handling abnormal operating conditions of the unit, relying solely on speed reduction.
[0004] I. TV segmentation bias
[0005] The industry-standard design specifications and factory-standard process TV (TV) are all based on a minimum value of 12, with no standardized design approach for a 9TV low-temperature transition process. Operators generally believe that simply reducing the speed can extend the looper buffer time and prevent strip breakage, ignoring that reducing the speed at the 12TV setting will extend the high-temperature holding time of the strip. The 0.3mm ultra-thin strip has coarse grains and significantly increased plasticity. Under the extrusion of the roller system and the effect of tension difference, the stretching defects of the ribs continue to worsen, forming a vicious cycle of "speed reduction - softening - defect aggravation". Those skilled in the art have no motivation to develop a matching low-temperature process with a TV lower than 12.
[0006] II. Cultivation bias in idler roller arrangement
[0007] The general design principle for thin plate looper and return channel is to add dense small idlers for multi-point support to prevent strip sagging. Industry technical upgrades and patent literature all follow this idea, generally ignoring the local point pressure contact of the strip caused by dense idlers, which induces rib stretching. There is no reverse optimization idea of actively reducing idlers and increasing the bread angle of strip rolls.
[0008] The existing process support system has multiple shortcomings: the furnace rollers lack a standardized calibration process with both ground coordinates and vertical lines, and roller system misalignment causes uneven stress on the plate shape; the inlet, outlet, and winding tensions use fixed values and cannot be dynamically adjusted according to the amount of looper stock; there is no standardized graded emergency handling process for ribs and crescent creases, and they rely solely on random temporary adjustments by operators.
[0009] According to the Chinese patent CN202110523716.X, "A Method for Reducing Plate Shape Defects in Dry Screws," a standard elongation rate is corrected using a 0.4±0.1mm thick steel strip of grade 430 steel, controlling the standard elongation rate at 0.25%±0.03%. For grade 430 steel, the temperature of the resistance heating zone in the vertical bright annealing furnace is controlled according to the process speed TV. When TV=15~18, the temperature is controlled at 940℃~990℃. The roll crown of the tempering and finishing line producing thin plates with a thickness of 0.37~0.68mm is 0.54~0.56mm, and the roll crown of the tempering and finishing line producing thin plates with a thickness of 0.68~0.88mm is 0.36~0.55mm. There is also a Chinese patent with patent number CN201810980198.2 entitled "Bright Annealing Process for Ultra-Thin Precision Stainless Steel Strip", which includes steps such as material selection and uncoiling, degreasing and cleaning, continuous annealing, cooling in the cooling section, and rewinding.
[0010] The two patents mentioned above only optimize the cooling fan and strip shape, and cannot solve the tensile defects of composite ribs in wide and thin materials. Therefore, existing technologies only adjust the speed or tension, which can only alleviate a single defect cause and cannot simultaneously eliminate the composite defects caused by the superposition of roller deviation, high temperature softening, idler roller extrusion, and tension imbalance. Summary of the Invention
[0011] The technical problem to be solved by the present invention is to provide a method for bright annealing to control the stretching defects of wide and ultra-thin stainless steel ribs, which can effectively eliminate defects such as rib stretching and crescent creases, and improve the production efficiency and yield of the unit.
[0012] The technical solution adopted by this invention to solve the above-mentioned technical problems is: a method for coordinated control of tensile defects in wide and ultra-thin stainless steel ribs during bright annealing, characterized by comprising the following steps:
[0013] 1) Unified calibration of furnace rolls: Stop the machine and empty the strip steel, correct the bouncing rolls based on the ground coordinates, calibrate the inlet sealing rolls and top rolls using the plumb line method, position the graphite rolls in the cooling section, and control the coaxial accuracy of the furnace rolls;
[0014] 2) Differentiated segmented annealing control: A 9TV low-temperature transition process is set up only for use during unit roll-up and roll-down and abnormal production conditions. Low-temperature annealing is matched with a low-speed cooling fan. When the unit is in stable production, 12~18TV is used to match the furnace temperature and cooling air volume. The inlet and outlet are adjusted in conjunction with the looper stock to adjust the operating speed and basic tension.
[0015] 3) Optimize the layout of idlers: reduce the number of exit loopers and return channel protective idlers, increase the roller spacing, and increase the contact wrap angle between the strip and the roller surface to avoid local point pressure and squeezing;
[0016] 4) Gradual dynamic tension control: The reference tension is increased at the beginning of winding and gradually reduced after winding is tight; the tension of the exit loop is adjusted in stages according to the amount of loop remaining.
[0017] 5) Defect classification and emergency handling: Gradient tension adjustment, differentiated control of cooling air volume, and standardized handling procedures for corrugated paper rolls are set up for indentation ribs and crescent creases respectively.
[0018] As an improvement, the coaxiality deviation of the furnace rollers in step 1) is ≤0.5mm.
[0019] Furthermore, the annealing temperature of the 9TV low-temperature transition process in step 2) is 1020±10℃, and the supporting segmented cooling fan runs at low speed. The fan speed can be adjusted with reference to the atmosphere temperature of the top roller, and the maximum temperature is controlled within 80℃.
[0020] When the unit is in stable production, the furnace temperature and cooling air volume are matched according to the 12~18TV range; the maximum operating speed of the inlet winding is limited, and the inlet tension is adjusted in conjunction with the looper stock and the strip deviation; the operating speed and basic tension of the outlet unwinding and paper changing are limited according to the looper stock.
[0021] Furthermore, the specific steps for inlet winding, outlet unwinding, and outlet paper changing are as follows:
[0022] Entrance roll-up operation
[0023] a. When the inlet is rolled up, the maximum process speed is controlled at 48m / min to prevent a sudden drop in process speed;
[0024] b. After the inlet welding is completed, the looper weight should be controlled within 60±2%, and the tension should be controlled according to L2. If the strip deviation in the inlet looper exceeds 40%, the inlet looper tension can be increased to 200±10%. L2 control is an L2 mathematical model that automatically calculates the "standard tension" based on the strip steel grade, thickness, and width. In the steel industry, it is usually called the Tension Set-up Model, or more specifically, the looper tension setting model / strip unit tension calculation model. It belongs to the process parameter setting model in the L2 level of the process control computer. Its main function is to convert the steel grade, specifications, and other information of the incoming material into the tension value required by the current production line (e.g., tension per unit area daN / mm). 2 (and then converted into total tension daN or percentage).
[0025] c. When increasing the looper amount before coiling, the looper tension can be increased to 150±10%; if the strip deviation within the looper still exceeds 40±2%, the looper tension can be further increased to 200±10%; if increasing the looper tension still cannot control the strip deviation, the looper amount should be reduced to 80±5%; at the same time, the process speed should be reduced for coiling and welding.
[0026] Export unloading operations
[0027] A. When the strip steel is fed into the furnace, the furnace temperature is controlled at 1020±10℃×6 zones, the process speed is controlled at 9TV, and the speeds of the six cooling fans are set to 1000±300 rpm, 1000±300 rpm, 1300±100 rpm, 1300±100 rpm, 1800±50 rpm, and 1800±50 rpm respectively.
[0028] B. Before unloading the coil at the exit, the exit looper should maintain a 3% tension; before the weld reaches the exit shear, the process speed should be reduced to 16±1m / min, and the tension of the exit looper should be controlled according to L2.
[0029] C. Before the exit winding is completed, the amount of the exit loop must be controlled within 30±1%;
[0030] D. If no indentation-like ribs appear at the outlet, the outlet loop tension is controlled according to the L2 setting; if indentation-like ribs appear, when the outlet loop amount is above 8±1%, the outlet loop tension can be increased by a maximum of 100±10 daN based on the L2 setting value.
[0031] E. The winding tension should be controlled between 2000 daN and 2200 daN;
[0032] Export paper changing operation
[0033] 1. Before the exit section stops, the tension of the exit loop is controlled according to the L2 set value;
[0034] 2. If an abnormality occurs during the paper changing process, reduce the process speed. Before the exit looper is pulled out, the exit looper must be controlled within 30±2%.
[0035] 3. After the paper is changed at the export site, if small ridges resembling indentations appear, refer to the export unloading operation requirements.
[0036] Furthermore, the number of protective idlers in step 3) is reduced from 21 to 10. The contact angle between the lifting strip and the roller surface is ≥5°.
[0037] Furthermore, in step 4), the initial tension during winding is increased to 1.3 to 1.5 times the reference tension, and then gradually reduced after winding. The tension of the exit loop is adjusted upwards in stages according to the loop stock, and gradually reduced after the defects are eliminated.
[0038] Furthermore, the specific process of step 5) is as follows: when indentation occurs, the pressure of the looper is adjusted according to the existing quantity gradient; if the adjustment is ineffective, the looper tension is reduced; when crescent creases occur, the cooling fan is used with differentiated air volume on both sides and the fan speed is interchanged; if the creases still cannot be eliminated, slow cooling is performed at low speed; when winding large-area ribs, the reference tension is increased and corrugated paper pad roll is used to eliminate defects.
[0039] Finally, when winding large-area reinforcing strips, the winding tension is increased to 1.5 to 1.8 times the base tension, and corrugated paper pads are used. The corrugated paper wraps the steel coil for no less than 2 turns.
[0040] Compared with existing technologies, the advantages of this invention are as follows: For the composite defects in 0.3mm, 4F wide, ultra-thin stainless steel ribs during stretching, a five-in-one collaborative control system is adopted, encompassing standardized furnace roll calibration, 9TV differentiated low-temperature annealing, optimized idler roll layout, graded dynamic tension, and graded emergency response to defects. Specifically, the 9TV low-temperature process addresses the root cause of strip softening, standardized furnace roll calibration eliminates roll system stress deviations, reducing idler rolls avoids localized extrusion, graded tension dynamically adapts to working conditions, and graded emergency response quickly handles sudden defects. These five modules mutually counterbalance and complement each other, forming a closed-loop control system. The multi-module coupling produces a non-linear quality improvement effect, reducing defects by up to 92%, far exceeding the theoretical expectation of 66% for single-process superposition, significantly reducing the incidence of rib stretching defects. The control method of this invention is scientifically and rationally designed, effectively eliminating defects such as rib stretching and crescent creases. Simultaneously, the unit does not require frequent rewinding or repeated speed reduction, significantly improving unit production efficiency and yield. Attached Figure Description
[0041] Figure 1 This is a schematic diagram of the overall structure of the No. 1 BA bright annealing unit's roller system, 320m inlet looper, and return channel provided in this embodiment of the invention.
[0042] Figure 2This is a bar chart comparing the number of coils with tensile defects in the reinforcing bars of seven control schemes provided in this embodiment of the invention; 1. Inlet looper, 2. Furnace inlet bouncing roller, 3. Furnace inlet sealing roller, 4. Furnace section, 5. Graphite roller, 6. Furnace top roller, 7. Outlet looper, 8. Return channel, 9. Small support roller, 10. Winding device. Detailed Implementation
[0043] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments.
[0044] A method for synergistic control of tensile defects in wide, ultra-thin stainless steel ribs during bright annealing includes the following steps: 1) Uniform calibration of furnace rolls: Stop the machine and empty the strip steel, calibrate the bouncing roll 2 based on the ground coordinates, calibrate the inlet sealing roll 3 and top roll 6 using the plumb line method, position the graphite roll 5 of the cooling section, and control the coaxial deviation of the furnace rolls to ≤0.5mm;
[0045] 2) Differentiated segmented annealing control: A 9TV low-temperature transition process is set up only for use during unit roll-up and roll-down and abnormal production conditions. Low-temperature annealing is matched with a low-speed cooling fan. When the unit is in stable production, 12~18TV is used to match the furnace temperature and cooling air volume. The inlet and outlet are adjusted in conjunction with the looper stock to adjust the operating speed and basic tension.
[0046] 3) Optimization of idler layout: Reduce the number of exit looper 7 and return channel 8 protective idlers 9 from the original 21 to 10, increase the roller spacing, improve the contact wrap angle between the strip and the roller surface, improve the contact wrap angle between the strip and the roller surface to ≥5°, and avoid local point pressure and squeezing;
[0047] 4) Gradual dynamic tension control: The reference tension is increased at the beginning of winding and gradually reduced after winding is tight; the tension of the exit loop is adjusted in stages according to the amount of loop remaining.
[0048] 5) Defect classification and emergency handling: Gradient tension adjustment, differentiated control of cooling air volume, and standardized handling procedures for corrugated paper rolls are set up for indentation ribs and crescent creases respectively.
[0049] In step 2), the annealing temperature of the 9TV low-temperature transition process is 1020±10℃, and the supporting segmented cooling fan runs at low speed. The fan speed can be adjusted with reference to the atmosphere temperature of the top roller, and the maximum temperature is controlled within 80℃.
[0050] When the unit is in stable production, the furnace temperature and cooling air volume are matched according to the 12~18TV range; the maximum operating speed of the inlet winding is limited, and the inlet tension is adjusted in conjunction with the looper stock and the strip deviation; the operating speed and basic tension of the outlet unwinding and paper changing are limited according to the looper stock.
[0051] The specific steps for inlet winding, outlet unwinding, and outlet paper changing are as follows:
[0052] Entrance roll-up operation
[0053] a. When the inlet is rolled up, the maximum process speed is controlled at 48m / min to prevent a sudden drop in process speed;
[0054] b. After the inlet welding is completed, the looper volume should be controlled within 60±2%, and the tension should be controlled according to L2. If the strip deviation in the inlet looper exceeds 40%, the inlet looper tension can be increased to 200±10%.
[0055] c. When increasing the looper amount before coiling, the looper tension can be increased to 150±10%; if the strip deviation within the looper still exceeds 40±2%, the looper tension can be further increased to 200±10%; if increasing the looper tension still cannot control the strip deviation, the looper amount should be reduced to 80±5%, and the process speed should be reduced for coiling and welding.
[0056] Export unloading operations
[0057] A. When the strip steel is fed into the furnace, the furnace temperature is controlled at 1020±10℃×6 zones, the process speed is controlled at 9TV, and the speeds of the six cooling fans are set to 1000±300 rpm, 1000±300 rpm, 1300±100 rpm, 1300±100 rpm, 1800±50 rpm, and 1800±50 rpm respectively.
[0058] B. Before unloading the coil at the exit, the exit looper should maintain a 3% tension; before the weld reaches the exit shear, the process speed should be reduced to 16±1m / min, and the tension of the exit looper should be controlled according to L2.
[0059] C. Before the exit winding is completed, the amount of the exit loop must be controlled within 30±1%;
[0060] D. If no indentation-like ribs appear at the outlet, the outlet loop tension is controlled according to the L2 setting; if indentation-like ribs appear, when the outlet loop amount is above 8±1%, the outlet loop tension can be increased by a maximum of 100±10 daN based on the L2 setting value.
[0061] E. The winding tension should be controlled between 2000 daN and 2200 daN;
[0062] Export paper changing operation
[0063] 1. Before the exit section stops, the tension of the exit loop is controlled according to the L2 set value;
[0064] 2. If an abnormality occurs during the paper changing process, reduce the process speed. Before the exit looper is pulled out, the exit looper must be controlled within 30±2%.
[0065] 3. After the paper is changed at the export site, if small ridges resembling indentations appear, refer to the export unloading operation requirements.
[0066] Step 4) Increase the tension at the initial winding stage to 1.3 to 1.5 times the reference tension, and gradually reduce it after winding. The tension of the exit loop is adjusted in stages according to the loop stock, and gradually reduced after the defects are eliminated.
[0067] Step 5) The specific process is as follows: When indentation occurs, adjust the pressure according to the looper's existing stock gradient. If the adjustment is ineffective, reduce the looper tension. When crescent creases occur, use the cooling fan with differentiated airflow on both sides and interchange the fan speeds. If the creases still cannot be eliminated, use slow cooling at low speed. When winding large-area ribs, increase the winding tension to 1.5 to 1.8 times the base tension and use corrugated paper pads. The corrugated paper should wrap the steel coil at least 2 times.
[0068] Example 1
[0069] 9TV Transition Process: Furnace temperature 1020℃, cooling fan speed matched to different levels; maximum inlet winding speed 48m / min; initial winding tension 1.3~1.5 times the reference tension, gradually decreasing after winding; outlet looper tension adjusted in 5 levels at 3% / 5% / 8% / 30% of remaining stock, and tension reduced by 100daN at a time after defect elimination; when large-area rib stretching occurs, winding tension is increased to 1.5~1.8 times the reference tension, with corrugated paper padding, and the corrugated paper wrapping the steel coil at least 2 turns.
[0070] Example 2
[0071] The return channel is 50m long. By reducing the number of idlers and increasing the gap between the rollers, the contact angle between the strip and the roller surface is increased to ≥5°, eliminating local point indentations.
[0072] The invention will be further illustrated below with seven comparative examples:
[0073] Unified testing standard: 0.3mm, 4F wide-width ultra-thin stainless steel, continuous stable production for 7 days, with an initial defective roll count of 38 rolls per group. Improvement data for each group are shown in Table 1.
[0074] Table 1
[0075]
[0076] A bar chart comparing the number of tensile defects in the reinforcing bars of seven control schemes is shown below. Figure 2 As shown, the nonlinear synergistic gain and the attenuation law of the missing module effect are intuitively displayed.
[0077] Table 2 shows the process-corresponding furnace temperatures and six-section cooling fan speeds for SUS304 steel grades 9TV / 12TV / 15TV / 18TV.
[0078]
[0079] Working mechanism
[0080] The stretching of 0.3mm, 4F wide ultra-thin stainless steel ribs is a complex defect induced by multiple factors. The four core causes are: uneven stress on the strip due to furnace roll installation misalignment, excessive softening of the strip at high temperature under 12TV low-speed conditions, local point pressure and extrusion by dense idler rolls, and the inability of the fixed tension to adapt to the real-time working conditions of the looper.
[0081] Single optimization can only eliminate a single cause of the defect, while the remaining three types of defect sources persist, resulting in limited improvement. The five modules of this invention mutually restrain and complement each other's shortcomings, forming a closed-loop prevention and control system: 9TV low-temperature process solves the root cause of strip steel softening, standardized furnace roll calibration eliminates roll system stress deviation, reducing the number of idler rolls avoids local extrusion, graded tension dynamically adapts to working conditions, and graded emergency rapid handling of sudden defects.
[0082] The reverse control experiment confirmed that omitting any one core module significantly reduced the defect improvement effect, proving that the five modules must be used in combination. Using any module alone cannot achieve a significant reduction in defects, and this is not a simple superposition of existing known methods.
[0083] Effect demonstration:
[0084] I. The theoretical maximum expected reduction: 21% + 27% + 18% = 66%. The actual defect reduction of this invention is 92%, which exceeds the theoretical value by 26 percentage points, resulting in nonlinear synergistic gain and achieving unexpected technical effects.
[0085] Second, overcoming the industry's technical bias of simply reducing speed, the 9TV low-temperature process significantly increases the operator's working time while meeting the 6.4min winding buffer time. In case of abnormalities, there is no need to reduce the process speed, thus eliminating the root cause of excessive speed reduction and softening of ultra-thin strips.
[0086] 3. The optimized layout of the idler rollers eliminates local pressure points on the strip, and the stretching defects of the looper and return channel ribs are basically eliminated; the graded dynamic tension is adapted to the unit's operating conditions in real time to avoid tension imbalance that induces stretching.
[0087] Fourth, the standardized graded emergency plan can quickly eliminate ribs and crescent creases, and prevent the scrapping of the entire coil of steel; the unit does not need to frequently rewind or repeatedly reduce speed, and the unit's production efficiency and yield are significantly improved at the same time. A single optimization method cannot achieve the same comprehensive benefits.
[0088] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for controlling bright annealing in conjunction with stretch defects of wide and very thin stainless steel bars, characterized by: Includes the following steps: 1) Unified calibration of furnace rolls: Stop the machine and empty the strip steel, correct the bouncing rolls based on the ground coordinates, calibrate the inlet sealing rolls and top rolls using the plumb line method, position the graphite rolls in the cooling section, and control the coaxial accuracy of the furnace rolls; 2) Differentiated segmented annealing control: A 9TV low-temperature transition process is set up only for use during unit roll-up and roll-down and abnormal production conditions. Low-temperature annealing is matched with a low-speed cooling fan. When the unit is in stable production, 12~18TV is used to match the furnace temperature and cooling air volume. The inlet and outlet are adjusted in conjunction with the looper stock to adjust the operating speed and basic tension. 3) Optimize the layout of idlers: reduce the number of exit loopers and return channel protective idlers, increase the roller spacing, and increase the contact angle between the strip and the roller surface to avoid local point pressure and squeezing; 4) Gradual dynamic tension control: Increase the reference tension at the beginning of winding, and gradually reduce it after winding. The tension of the exported looper is adjusted in stages according to the stock of loopers. 5) Defect classification and emergency handling: Gradient tension adjustment, differentiated control of cooling air volume, and standardized handling procedures for corrugated paper rolls are set up for indentation ribs and crescent creases respectively.
2. The method according to claim 1, wherein the method is characterized by: The coaxiality deviation of the furnace rollers in step 1) is ≤0.5mm.
3. The method according to claim 1, wherein the method is characterized by: The annealing temperature of the 9TV low-temperature transition process in step 2) is 1020±10℃, and the matching segmented cooling fan runs at low speed. The fan speed can be adjusted with reference to the atmosphere temperature of the top roller, and the maximum temperature is controlled within 80℃. When the unit is in stable production, the furnace temperature and cooling air volume are matched according to the 12~18TV range; the maximum operating speed of the inlet winding is limited, and the inlet tension is adjusted in conjunction with the looper stock and the strip deviation; the operating speed and basic tension of the outlet unwinding and paper changing are limited according to the looper stock.
4. The method according to claim 3, wherein the method is characterized by: The specific steps for inlet winding, outlet unwinding, and outlet paper changing are as follows: 4.1) Inlet roll-up operation a. When the inlet is rolled up, the maximum process speed is controlled at 48m / min to prevent a sudden drop in process speed; b. After the inlet welding is completed, the looper volume should be controlled within 60±2%, and the tension should be controlled according to L2. If the strip deviation in the inlet looper exceeds 40%, the inlet looper tension can be increased to 200±10%. c. When increasing the looper amount before coiling, the looper tension can be increased to 150±10%; if the strip deviation within the looper still exceeds 40±2%, the looper tension can be further increased to 200±10%; if increasing the looper tension still cannot control the strip deviation, the looper amount should be reduced to 80±5%, and the process speed should be reduced for coiling and welding. 4.2) Export unloading operation A. When the strip steel is fed into the furnace, the furnace temperature is controlled at 1020±10℃×6 zones, the process speed is controlled at 9TV, and the speeds of the six cooling fans are set to 1000±300 rpm, 1000±300 rpm, 1300±100 rpm, 1300±100 rpm, 1800±50 rpm, and 1800±50 rpm respectively. B. Before unloading the coil at the exit, the exit looper should maintain a 3% tension; before the weld reaches the exit shear, the process speed should be reduced to 16±1m / min, and the tension of the exit looper should be controlled according to L2. C. Before the exit winding is completed, the amount of the exit loop must be controlled within 30±1%; D. If no indentation-like ribs appear at the outlet, the outlet loop tension is controlled according to the L2 setting; if indentation-like ribs appear, when the outlet loop amount is above 8±1%, the outlet loop tension can be increased by a maximum of 100±10 daN based on the L2 setting value. E. The winding tension should be controlled between 2000 daN and 2200 daN; 4.3) Export paper changing operation 1. Before the exit section stops, the tension of the exit loop is controlled according to the L2 set value; 2. If an abnormality occurs during the paper changing process, reduce the process speed. Before the exit looper is pulled out, the exit looper must be controlled within 30±2%.
3. After the paper is changed at the export site, if small ridges resembling indentations appear, refer to the export unloading operation requirements.
5. The method for simultaneous control of stretcher strain bright annealing of wide and ultra-thin stainless steel bars according to claim 1, characterized in that: The number of protective rollers in step 3) is reduced from 21 to 10.
6. The method for simultaneous control of stretcher strain bright annealing of wide and ultra-thin stainless steel bars according to claim 1, characterized in that: In step 4), the initial tension during winding is increased to 1.3 to 1.5 times the reference tension, and then gradually reduced after winding. The tension of the exit loop is adjusted upwards in stages according to the amount of loop in stock, and gradually reduced after the defects are eliminated.
7. The method for simultaneous control of stretcher strain and bright annealing of wide and very thin stainless steel bars according to claim 1, characterized in that: The specific process of step 5) is as follows: When indentation occurs, adjust the pressure according to the looper's existing stock gradient. If the adjustment is ineffective, reduce the looper tension. When crescent creases occur, use the cooling fan with differentiated air volume on both sides and interchange the fan speed. If the problem still cannot be eliminated, use slow cooling at low speed. When winding large-area ribs, increase the reference tension and use corrugated paper pad roll to eliminate defects.
8. The method according to claim 7, wherein the method is characterized by: When winding large-area reinforcing strips, the winding tension is increased to 1.5 to 1.8 times the base tension, and corrugated paper pads are used. The corrugated paper wraps the steel coil for no less than 2 turns.
Citation Information
Patent Citations
Annealing process of filminess precision stainless steel with lucency
CN109097534A
Ultra-thin precision stainless steel strip bright annealing process
CN109097534B
Method for reducing plate type defects of dry type leveling machine
CN113231479A