A method for neutralizing Ni-containing gravel under high pressure acid leaching slurry
By combining heat treatment modification of Ni-containing gravel in laterite nickel ore with limestone neutralizing agent, the problems of low nickel extraction efficiency and high residual acid treatment cost in high-pressure acid leaching process are solved, realizing efficient nickel recovery and cascade utilization of resources. It is suitable for capacity expansion and renovation of laterite nickel ore hydrometallurgical plants.
Patent Information
- Application Number
- CN202611261143.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
In existing high-pressure acid leaching processes, the extraction efficiency of valuable metals such as nickel and cobalt in laterite nickel ore is low, and the cost of treating residual sulfuric acid is high, wasting the remaining leaching value of the high-pressure acid leaching slurry.
Ni-containing gravel is pretreated by heat treatment modification, combined with limestone neutralizing agent, and then neutralized and leached by high-pressure acid leaching slurry. The pH value and temperature at the end of the reaction are controlled to achieve efficient recovery of nickel.
It improves the nickel leaching rate, reduces production costs, and takes into account both the cascade utilization of resources and process compatibility, making it suitable for capacity expansion and renovation of laterite nickel ore hydrometallurgical plants.
Smart Images

Figure CN123108313A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of hydrometallurgy, specifically relating to a method for neutralizing Ni-containing gravel under high-pressure acid leaching slurry. Background Technology
[0002] High-pressure acid leaching (HPAL) is one of the core technologies for extracting valuable metals such as nickel and cobalt from laterite nickel ore. This process typically uses a dilute sulfuric acid solution to break down the mineral lattice of the ore under high temperature (approximately 250℃-270℃) and high pressure conditions, allowing nickel and cobalt to be selectively dissolved.
[0003] However, due to limitations in chemical equilibrium and kinetic factors, the slurry produced by the HPAL process typically contains a large amount of residual sulfuric acid (approximately 38-47 g / L). To meet the requirements of subsequent solid-liquid separation and solution purification processes, this residual acid must be neutralized to increase its pH and reduce its concentration.
[0004] The current mainstream treatment process uses a large amount of limestone to consume residual acid, thereby increasing the pH of the leachate to meet the requirements of subsequent processes, prevent corrosion of downstream equipment, and reduce construction costs. While this neutralization method effectively consumes residual acid, it wastes the remaining leaching value of the high-pressure acid leaching pulp.
[0005] The Ni-containing gravel used in this application is mainly composed of serpentine, with a content of up to 80%. Mg in Ni-containing gravel is relatively easy to leach and can be leached at pH < 2; while Fe and Al can only be leached at lower pH environments; Ni, along with Fe, is uniformly interspersed within the gravel and cannot be enriched by physical means, but can only be gradually released through the leaching of Mg and Al.
[0006] In view of this, this application proposes a method for neutralizing high-pressure acid leaching slurry with Ni-containing gravel based on actual production processes and considering the properties of Ni-containing gravel itself, so as to efficiently recover the Ni element therein; while taking into account production needs, it adapts to production and ensures that the pH of the leachate meets the requirements of subsequent production processes. Summary of the Invention
[0007] To address the technical problems existing in the prior art, the present invention provides a method for neutralizing Ni-containing gravel under high-pressure acid leaching slurry.
[0008] To achieve the above objectives, the present invention adopts the following technical solution: A method for neutralizing high-pressure acid leaching slurry from Ni-containing gravel includes the following steps: (1) Raw material pretreatment: The Ni-bearing gravel mined from the bottom of the laterite nickel mine is crushed and dry-ground to reduce the gravel particle size to less than 2 mm. (2) Heat treatment modification: A certain proportion of limestone is added to the gravel obtained in step (1), and after mixing, it is sent to a rotary kiln for heat treatment to obtain a modified gravel neutralizer. (3) Pulping and Grading: The gravel neutralizer obtained in step (2) is slurried with water and wet-milled. The milled gravel slurry is sent to a hydrocyclone for gravity separation and classification, and overflow slurry with solid particle size less than 74 μm is collected. (4) Thickening pulping: The overflow slurry obtained from the top discharge of the hydrocyclone is sent to a thickener for thickening to obtain gravel neutralized slurry; (5) Neutralization and leaching: The gravel neutralization slurry obtained in step (4) is fed into the high-pressure acid leaching slurry for reaction. The residual acid in the high-pressure acid leaching slurry is used to neutralize and leach the gravel. The pH value, temperature and reaction time at the end of the reaction are controlled. After the leaching is completed, the neutralized leaching slurry is obtained.
[0009] In step (2), the limestone content accounts for 1%-3% of the dry mass of the gravel.
[0010] The heat treatment process in step (2) is carried out in a non-inert atmosphere, the heat treatment temperature is set at 800℃-1000℃, and the time is controlled at 30min-120min.
[0011] In step (2), the heat treatment temperature is set to 915℃ and the time is set to 45min.
[0012] In step (3), the coarse particles from the hydrocyclone underflow are returned to the wet grinding process for further processing, in order to control the solid particle size of the hydrocyclone slurry to be less than 74 μm.
[0013] The low-slag overflow obtained in step (3) is added to the gravel slurry to maintain the concentration of the gravel slurry at 25%-35%, the leaching pH at 1.6-2.0, and the leaching time at 60min-120min; the Ni content in the gravel slurry is maintained at 0.6%-0.8%, and the Al content is maintained at 0.6%-0.8%.
[0014] In step (4), the concentration of the gravel neutralized slurry obtained at the bottom of the thickener is controlled at 25%-35%, and the overflow return water is sent to the pulping and wet grinding section of step (3).
[0015] In step (5), the pH value at the end of the neutralization leaching reaction is controlled at 1.4-1.6, the leaching temperature is controlled at 70℃-80℃, and the leaching time is controlled at 1h-2h.
[0016] In step (5), the neutralization leaching time is set to 2 hours, the pH is set to 1.6, and the leaching temperature is set to 80°C.
[0017] The neutralized leaching slurry obtained in step (5) is sent to a thickener for countercurrent washing, and after washing, it is sent to the subsequent supporting production process.
[0018] The beneficial effects of this invention are as follows: (1) This application realizes the tiered utilization of resources. This application transforms Ni-containing gravel, which was originally considered "high acid consumption waste," into "neutralized raw material." The residual acid from the HPAL slurry is used to leach nickel from the gravel for recovery. This process does not consume additional concentrated sulfuric acid or increase wastewater discharge, greatly reducing production costs and improving the overall recovery rate of mineral resources. (2) The leaching efficiency is significantly improved by "heat treatment modification". This application addresses the characteristics of serpentine's dense crystal structure and slow leaching at room temperature by specifying a heat treatment process of 800℃-1000℃. Experiments have shown that this temperature range can promote the dehydroxylation of serpentine, destroy its crystal structure, and significantly improve its reactivity in the subsequent neutralization leaching process, increasing the nickel leaching rate from 57.21% in the untreated case to over 75%. (3) Control the pH range to avoid iron precipitation and coating. This application specifies that the endpoint pH value of neutralization leaching should be controlled between 1.4 and 1.6; if the pH is too high (>2.0), the Fe in the high-pressure acid leaching pulp will be affected. 3+ It will hydrolyze to generate Fe(OH)3 colloid, which coats the surface of unreacted gravel, forming a "passivation layer" that hinders further leaching of nickel from the inside; if the pH is too low, the neutralization effect will not meet the standard; this application controls the pH to effectively utilize the residual acid and inhibit the hydrolysis and precipitation of iron, thus ensuring the smooth progress of the neutralization and leaching reaction. (4) It has strong process compatibility and is easy to implement in industrial applications. The Ni-bearing gravel used in this application comes from the gravel layer at the bottom of the laterite nickel mine. The raw material is easy to mine, and the method disclosed in this application does not require large-scale modification of the existing HPAL production line. After crushing, heat treatment and pulping, the Ni-bearing gravel can be directly pumped into the HPAL slurry for reaction. The process is short and easy to operate, and it is suitable for capacity expansion and efficiency improvement of laterite nickel ore hydrometallurgical plants. Attached Figure Description
[0019] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation
[0020] The present invention will be further described below with reference to specific embodiments.
[0021] like Figure 1 As shown, a method for neutralizing Ni-containing gravel under high-pressure acid leaching slurry includes the following steps: (1) Raw material pretreatment: The Ni-bearing gravel mined from the bottom of the laterite nickel mine is crushed and dry-ground to reduce the gravel particle size to less than 2 mm. (2) Heat treatment modification: A certain proportion of limestone (CaCO3) is added to the gravel obtained in step (1), and after mixing, it is sent to a rotary kiln for heat treatment to obtain a modified gravel neutralizer. (3) Pulping and Grading: The gravel neutralizer obtained in step (2) is slurried with water and wet-milled. The milled gravel slurry is sent to a hydrocyclone for gravity separation and classification, and overflow slurry with solid particle size less than 74 μm is collected. (4) Thickening pulping: The overflow slurry obtained from the top discharge of the hydrocyclone is sent to a thickener for thickening to obtain gravel neutralized slurry; (5) Neutralization and leaching: The gravel neutralization slurry obtained in step (4) is fed into the high-pressure acid leaching slurry for reaction. The residual acid in the high-pressure acid leaching slurry is used to neutralize and leach the gravel. The pH value, temperature and reaction time at the end of the reaction are controlled. After the leaching is completed, the neutralized leaching slurry is obtained.
[0022] In step (2), the limestone content accounts for 1%-3% of the dry mass of the gravel; the heat treatment process is carried out in a non-inert atmosphere (no special atmosphere is required), the heat treatment temperature is set at 800℃-1000℃, and the time is controlled at 30min-120min. Preferably, the heat treatment temperature in step (2) is set at 915℃ and the time is set at 45min, which can achieve a better treatment effect; further increasing the temperature and extending the holding time can improve the leaching efficiency of the subsequent neutralization leaching section and shorten the required reaction time, but the effect on improving the Ni leaching rate is limited; the actual heat treatment temperature and time are adjusted according to the reaction time of the neutralization leaching section.
[0023] In step (3), the coarse particles from the hydrocyclone underflow are returned to the wet grinding process for reprocessing to control the solid particle size of the hydrocyclone slurry to be less than 74 μm. The resulting low-slag overflow is added to the gravel slurry to maintain the gravel slurry concentration at 25%-35%, the leaching pH at 1.6-2.0, and the leaching time at 60 min-120 min. The Ni content and Al content in the gravel slurry are maintained at 0.6%-0.8% and 0.6%-0.8%, respectively.
[0024] In step (4), the concentration of the gravel neutralized slurry obtained at the bottom of the thickener is controlled at 25%-35%, and the overflow return water is sent to the pulping and wet grinding section in step (3).
[0025] In step (5), the final pH value of the neutralization leaching reaction is controlled at 1.4-1.6, the leaching temperature is controlled at 70℃-80℃, and the leaching time is controlled at 1h-2h. During the gravel neutralization leaching process, Mg, an easily leached element in the gravel slurry, preferentially consumes acid for leaching and gradually releases SiO2 during the leaching process; under high temperature and high acid conditions, SiO2 will slowly transform into insoluble H2SiO3 and adhere to the gravel surface. When the neutralization leaching pH > 2, Fe in the high-pressure acid leaching slurry 3+ It will gradually settle into Fe(OH)₂ 3, It coats the surface of gravel, reduces neutralization efficiency, increases the solids content of the leaching system, and increases the load on subsequent washing processes.
[0026] Preferably, in step (5), the neutralization leaching time is set to 2 hours, the pH is set to 1.6, and the leaching temperature is set to 80°C. This achieves the desired effect of quickly neutralizing the high-pressure acid leaching slurry while obtaining a high Ni leaching rate.
[0027] The neutralized leaching slurry obtained in step (5) is sent to a thickener for countercurrent washing. After washing, it is sent to subsequent supporting production processes (such as iron and aluminum removal processes). Example 1:
[0028] A method for neutralizing Ni-containing gravel under high pressure acid leaching slurry (see...) Figure 1 The specific steps are as follows: (1) Take samples from the bottom of the laterite nickel ore excavation pit, at a depth of 30cm-50cm, to obtain Ni-containing gravel; (2) Grind and dry the Ni-containing gravel, and pass the dry gravel residue through a 2mm sieve to remove the material on the sieve; (3) Take 99g of dry gravel residue, add 1g of CaCO3 powder to it, and mix thoroughly; (4) Place the above-mentioned dry gravel residue in a corundum crucible (with a lid), and send it into a muffle furnace for heat treatment. Heat it to 815°C and keep it at that temperature for 1 hour. After the heat treatment is completed, take out the material and let it cool naturally to room temperature to obtain treated gravel powder. (5) Grind the treated gravel powder and pass it through a 200-mesh sieve. Take the material passing through the sieve as a gravel neutralizing agent. (6) Take 30g of gravel neutralizing agent and add it to 500ml of high-pressure acid leaching solution. Neutralize and leach at 70℃ for 60min. (7) After the neutralization leaching is completed, the neutralization leaching system is filtered to obtain neutralization leaching residue and neutralization leaching solution; (8) The neutralization leaching system was filtered, and the resulting neutralization leaching residue was washed and dried. The leaching rate of each element was analyzed.
[0029] After data normalization and analysis, the Ni content in the Ni-bearing gravel sample was 0.74%.
[0030] The resulting neutralized leaching residue had a dry weight of 24.35 g, a residue rate of 81.2%, and a Ni content of 0.271%. The leaching rates of Mg, Fe, Al, and Ni were 46.73%, 2.21%, 8.16%, and 70.27%, respectively. The pH of the neutralized leachate was 1.44.
[0031] It was observed that under these conditions, the leaching rate of Ni element in Ni-containing gravel reached over 70%, and the pH of the neutralized leachate rose to 1.44. This indicates that this method can adjust the pH of the high-pressure acid leaching solution and successfully utilize the leaching capacity of the residual acid to recover Ni element from Ni-containing gravel, thus creating economic value. Example 2:
[0032] A method for neutralizing Ni-containing gravel under high pressure acid leaching slurry (see...) Figure 1 The specific steps are as follows: (1) Take samples from the bottom of the laterite nickel ore excavation pit, at a depth of 30cm-50cm, to obtain Ni-containing gravel; (2) Grind and dry the Ni-containing gravel, and pass the dry gravel residue through a 2mm sieve to remove the material on the sieve; (3) Take 99g of dry gravel residue, add 1g of CaCO3 powder to it, and mix thoroughly; (4) Place the above-mentioned dry gravel residue in a corundum crucible (with a lid), and send it into a muffle furnace for heat treatment. Heat it to 915°C and hold it for 45 minutes. After the heat treatment is completed, take out the material and let it cool naturally to room temperature to obtain treated gravel powder. (5) Grind the treated gravel powder and pass it through a 200-mesh sieve. Take the material passing through the sieve as a gravel neutralizing agent. (6) Take 30g of gravel neutralizing agent and add it to 500ml of high-pressure acid leaching solution. Neutralize and leach at 80℃ for 60min. (7) After the neutralization leaching is completed, the neutralization leaching system is filtered to obtain neutralization leaching residue and neutralization leaching solution; (8) The neutralization leaching system was filtered, and the resulting neutralization leaching residue was washed and dried. The leaching rate of each element was analyzed.
[0033] After data processing and analysis, the Ni content in the Ni-bearing gravel sample was found to be 0.73%.
[0034] The resulting neutralized leaching residue had a dry weight of 23.95 g, a residue rate of 79.8%, and a Ni content of 0.227%. The leaching rates of Mg, Fe, Al, and Ni were 48.34%, 2.17%, 8.26%, and 75.34%, respectively. The pH of the neutralized leachate was 1.58.
[0035] It was observed that, compared with "Example 1", after increasing the heat treatment temperature of Ni-containing gravel (815℃→915℃), although the heat treatment time was reduced (1h→45min), the leaching rate of Ni element in the prepared neutralized slurry reached 75%, and the pH of the neutralized leachate increased to 1.58.
[0036] In summary, the heat treatment temperature directly affects the leaching efficiency of Ni-containing gravel during the neutralization leaching stage. This is because the heat treatment temperature directly affects the leaching efficiency of serpentine [Mg6(Si4O3)2]. 10 The degree of decomposition of [(OH)8] affects the leaching effect of gravel. According to system experiments, a heat treatment temperature of 915℃ and a heat treatment time of 45min can achieve a high neutralization leaching effect. Further increasing the heat treatment temperature and extending the heat treatment time has little effect on the Ni leaching rate and the pH of the neutralized leachate.
[0037] Therefore, this method can adjust the pH of the high-pressure acid leaching solution and successfully utilize the leaching capacity of the residual acid to recover Ni element from Ni-containing gravel, thus creating economic value.
[0038] Comparative Example 1: The specific steps for direct leaching of Ni-containing gravel are as follows: (1) Take samples from the bottom of the laterite nickel ore excavation pit, at a depth of 30cm-50cm, to obtain Ni-containing gravel; (2) Grind and dry the Ni-containing gravel, take the dry gravel residue and pass it through a 200-mesh sieve, and retain the material passing through the sieve; (3) Take the high-pressure acid leaching system of laterite nickel ore and filter it, and take 500ml of acid leaching solution; (4) Heat the acid leaching solution in a water bath to 80°C, then add 30g of dry gravel residue and keep it warm for leaching for 120min; (5) After leaching is completed, filter the leaching system and wash and dry the resulting leaching residue.
[0039] After data normalization and analysis, the Ni content in the Ni-bearing gravel sample was 0.74%.
[0040] The resulting leaching residue had a dry weight of 24.37 g, a residue rate of 81.24%, a Ni element content of 0.39%, and a Ni element leaching rate of 57.21%. It was observed that, while maintaining the same amount of high-pressure acid leaching solution and gravel dry weight during the leaching process, the Ni element leaching yield from direct leaching was lower. This is because at higher leaching temperatures (90℃), the Si element [Mg6(Si4O] in serpentine... 10 During the leaching process of Mg, Si is continuously released. Under prolonged conditions of high acidity and high temperature, Si gradually appears in the form of silicic acid and adheres to the surface of solid particles, significantly affecting the leaching reaction rate.
[0041] This application proposes a method for neutralizing Ni-bearing gravel in high-pressure acid leaching slurry, based on the utilization of the residual leaching capacity of the slurry and taking into account actual production processes. According to the geological genesis of laterite nickel ore, the ore layer is generally divided into a limonite layer, a transition layer, a residual ore layer, and a gravel-bearing residual layer from top to bottom. The gravel-bearing residual layer is called the gravel layer. The main metallic element in the gravel layer is Mg, and its main component is serpentine [Mg6(Si4O3)2]. 10 [(OH)8], accounting for 80%; of which Ni element content is about 0.8%. Due to its high Mg and high acid consumption characteristics, although it cannot be used as a raw material in the high-pressure acid leaching system, it can be used as a neutralizing agent to neutralize the residual acid in the high-pressure acid leaching slurry. By utilizing the residual leaching capacity of the residual acid, Ni element in Ni-containing gravel can be recovered, thereby obtaining certain economic benefits.
[0042] However, the main component of Ni-bearing gravel is serpentine [Mg6(Si4O]]. 10 Ni-containing gravel ((OH)8) consumes a lot of acid but leaches slowly, so it needs to be treated to change its properties and improve production efficiency. This application heat-treats Ni-containing gravel to promote partial thermal decomposition, improve leaching efficiency, quickly neutralize the residual acid in the high-pressure acid leaching pulp, recover the Ni element in the gravel, and make full use of the residual value of the high-pressure leaching residual acid.
[0043] Comparative Example 2: The leaching process for Ni-containing gravel after low-temperature treatment (800℃) is as follows: (1) Take samples from the bottom of the laterite nickel ore excavation pit, at a depth of 30cm-50cm, to obtain Ni-containing gravel; (2) Grind and dry the Ni-containing gravel, and pass the dry gravel residue through a 2mm sieve to remove the material on the sieve; (3) Take 99g of dry gravel residue, add 1g of CaCO3 powder to it, and mix thoroughly; (4) Place the above-mentioned dry gravel residue in a corundum crucible (with a lid), and send it into a muffle furnace for heat treatment. Heat it to 800°C and keep it at that temperature for 45 minutes. After the heat treatment is completed, take out the material and let it cool naturally to room temperature to obtain treated gravel powder. (5) Grind the treated gravel powder and pass it through a 200-mesh sieve. Take the material passing through the sieve as a gravel neutralizing agent. (6) Take 30g of gravel neutralizing agent and add it to 500ml of high-pressure acid leaching solution. Neutralize and leach at 80℃ for 60min. (7) After the neutralization leaching is completed, the neutralization leaching system is filtered to obtain neutralization leaching residue and neutralization leaching solution; (8) The neutralization leaching system was filtered, and the resulting neutralization leaching residue was washed and dried. The leaching rate of each element was analyzed.
[0044] After data processing and analysis, the Ni content in the Ni-bearing gravel sample was found to be 0.73%.
[0045] The resulting neutralized leaching residue had a dry weight of 26.71 g, a residue rate of 89.0%, and a Ni content of 0.317%. The leaching rates of Mg, Fe, Al, and Ni were 41.43%, 1.82%, 7.82%, and 61.2%, respectively. The pH of the neutralized leaching solution was 1.32.
[0046] It was observed that, with the same amount of gravel residue, compared with "Example 2", the Al leaching rate remained basically unchanged, while the Ni and Mg leaching rates decreased significantly. The Ni leaching rate decreased from 75.34% to 61.2%, but was still higher than the 57.21% of "Comparative Example 1".
[0047] This indicates that heat treatment temperature is an important factor affecting the leaching rate of nickel-containing gravel. When the heat treatment temperature is 800℃, it begins to provide a positive driving force for gravel leaching.
[0048] Comparative Example 3: The leaching process for Ni-containing gravel after high-temperature treatment (1180℃) is as follows: (1) Take samples from the bottom of the laterite nickel ore excavation pit, at a depth of 30cm-50cm, to obtain Ni-containing gravel; (2) Grind and dry the Ni-containing gravel, and pass the dry gravel residue through a 2mm sieve to remove the material on the sieve; (3) Take 99g of dry gravel residue, add 1g of CaCO3 powder to it, and mix thoroughly; (4) Place the above-mentioned dry gravel residue in a corundum crucible (with a lid), and send it into a muffle furnace for heat treatment. Heat it to 1180°C and hold it for 45 minutes. After the heat treatment is completed, take out the material and let it cool naturally to room temperature to obtain treated gravel powder. (5) Grind the treated gravel powder and pass it through a 200-mesh sieve. Take the material passing through the sieve as a gravel neutralizing agent. (6) Take 30g of gravel neutralizing agent and add it to 500ml of high-pressure acid leaching solution. Neutralize and leach at 80℃ for 60min. (7) After the neutralization leaching is completed, the neutralization leaching system is filtered to obtain neutralization leaching residue and neutralization leaching solution; (8) The neutralization leaching system was filtered, and the resulting neutralization leaching residue was washed and dried. The leaching rate of each element was analyzed.
[0049] After data processing and analysis, the Ni content in the Ni-bearing gravel sample was found to be 0.73%.
[0050] The resulting neutralized leaching residue had a dry weight of 22.56 g, a residue rate of 75.2%, and a Ni content of 0.218%. The leaching rates of Mg, Fe, Al, and Ni were 50.27%, 2.32%, 9.15%, and 77.6%, respectively. The pH of the neutralized leaching solution was 1.61.
[0051] Compared with the Ni leaching rate of 75.34% in "Example 2", increasing the heat treatment temperature has a limited effect on improving the Ni leaching rate. Considering the cost of heat treatment temperature control and rotary kiln construction, it is not recommended to blindly increase the heat treatment temperature.
[0052] In summary, this application significantly improves the performance of Ni-containing gravel as a neutralizing agent in high-pressure acid leaching slurry by introducing a heat treatment process to modify it. Comparison of experimental results between direct leaching and heat treatment at different temperatures shows that untreated Ni-containing gravel exhibits a slow leaching reaction due to its stable serpentine structure and is easily affected by silica encapsulation, resulting in a low Ni leaching rate (57.21%). However, after heat treatment at 800℃-1180℃, the reactivity of the gravel is activated to varying degrees. Specifically, under the process conditions of 915℃ and holding for 45 minutes (Example 2), a high-efficiency leaching rate of 75.34% of Ni can be achieved with lower thermal energy costs, and the pH of the neutralized leachate increases to 1.58, which is superior to the treatment effects at 815℃ and 800℃. Although further increasing the temperature to 1180℃ can slightly increase the leaching rate to 77.6%, its marginal benefit diminishes considering the cost of temperature control and equipment construction. Therefore, this method successfully recovered valuable metals from Ni-containing gravel by utilizing the leaching capacity of residual acid, achieving both economical resource utilization and maximizing process benefits while effectively adjusting the slurry pH.
[0053] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions, and variations can be made to these embodiments, or they can be used directly or indirectly, without departing from the principles and spirit of the invention. In other related technical fields, the scope of the invention is defined by the appended claims and their equivalents, and they are similarly included within the scope of patent protection of the invention.
Claims
1. A method for neutralizing high-pressure acid leaching slurry from Ni-containing gravel, characterized in that, Includes the following steps: (1) Raw material pretreatment: The Ni-bearing gravel mined from the bottom of the laterite nickel mine is crushed and dry-ground to reduce the gravel particle size to less than 2 mm. (2) Heat treatment modification: A certain proportion of limestone is added to the gravel obtained in step (1), and after mixing, it is sent to a rotary kiln for heat treatment to obtain a modified gravel neutralizer. (3) Pulping and Grading: The gravel neutralizer obtained in step (2) is slurried with water and wet-milled. The milled gravel slurry is sent to a hydrocyclone for gravity separation and classification, and overflow slurry with solid particle size less than 74 μm is collected. (4) Thickening pulping: The overflow slurry obtained from the top discharge of the hydrocyclone is sent to a thickener for thickening to obtain gravel neutralized slurry; (5) Neutralization and leaching: The gravel neutralization slurry obtained in step (4) is fed into the high-pressure acid leaching slurry for reaction. The residual acid in the high-pressure acid leaching slurry is used to neutralize and leach the gravel. The pH value, temperature and reaction time at the end of the reaction are controlled. After the leaching is completed, the neutralized leaching slurry is obtained.
2. The method for neutralizing high-pressure acid leaching slurry containing Ni gravel as described in claim 1, characterized in that: In step (2), the limestone content accounts for 1%-3% of the dry mass of the gravel.
3. The method for neutralizing high-pressure acid leaching slurry containing Ni gravel as described in claim 1, characterized in that: The heat treatment process in step (2) is carried out in a non-inert atmosphere, the heat treatment temperature is set at 800℃-1000℃, and the time is controlled at 30min-120min.
4. The method for neutralizing high-pressure acid leaching slurry containing Ni gravel as described in claim 3, characterized in that: In step (2), the heat treatment temperature is set to 915℃ and the time is set to 45min.
5. The method for neutralizing high-pressure acid leaching slurry from Ni-containing gravel as described in claim 1, characterized in that: In step (3), the coarse particles from the hydrocyclone underflow are returned to the wet grinding process for further processing, in order to control the solid particle size of the hydrocyclone slurry to be less than 74 μm.
6. The method for neutralizing high-pressure acid leaching slurry containing Ni gravel as described in claim 5, characterized in that: The low-slag overflow obtained in step (3) is added to the gravel slurry to maintain the gravel slurry concentration at 25%-35%, the leaching pH at 1.6-2.0, and the leaching time at 60min-120min; the Ni content in the gravel slurry is maintained at 0.6%-0.8%, and the Al content is maintained at 0.6%-0.8%.
7. The method for neutralizing high-pressure acid leaching slurry containing Ni gravel as described in claim 1, characterized in that: In step (4), the concentration of the gravel neutralized slurry obtained at the bottom of the thickener is controlled at 25%-35%, and the overflow return water is sent to the pulping and wet grinding section of step (3).
8. The method for neutralizing high-pressure acid leaching slurry containing Ni gravel as described in claim 1, characterized in that: In step (5), the pH value at the end of the neutralization leaching reaction is controlled at 1.4-1.6, the leaching temperature is controlled at 70℃-80℃, and the leaching time is controlled at 1h-2h.
9. The method for neutralizing high-pressure acid leaching slurry from Ni-containing gravel as described in claim 8, characterized in that: In step (5), the neutralization leaching time is set to 2 hours, the pH is set to 1.6, and the leaching temperature is set to 80°C.
10. The method for neutralizing high-pressure acid leaching slurry from Ni-containing gravel as described in claim 1, characterized in that: The neutralized leaching slurry obtained in step (5) is sent to a thickener for countercurrent washing, and after washing, it is sent to the subsequent supporting production process.