A method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium extraction waste from spodumene.
By using low-temperature roasting mixed with ammonium sulfate, organophosphorus extractants, and alkaline leaching-hydrolysis precipitation, the problem of low separation efficiency of rubidium, cesium, tantalum, and niobium in lithium extraction waste residue from spodumene was solved, achieving efficient and pure metal recovery.
Patent Information
- Application Number
- CN202611396269.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot effectively separate valuable metals such as rubidium, cesium, tantalum, and niobium from lithium extraction waste from spodumene, and also suffer from problems such as equipment scaling, low extraction efficiency, and low recovery rate.
By employing a low-temperature roasting and ammonium sulfate mixture, combined with a neutral organophosphorus extractant and an alkaline leaching-hydrolysis precipitation method, rubidium, cesium, tantalum, and niobium can be separated in stages, avoiding the shortcomings of traditional methods.
It achieves efficient recovery of rubidium, cesium, tantalum and niobium, improves concentrate grade and recovery rate, avoids equipment scaling and impurity exchange problems, and obtains high-purity products.
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal recycling technology, and more specifically, to a method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium spodumene extraction waste. Background Technology
[0002] Lithium extraction waste from spodumene contains valuable metals such as rubidium, cesium, tantalum, and niobium. However, the high-temperature roasting during the lithium extraction process causes the formation of a large amount of amorphous glassy phase in the waste, with tantalum and niobium minerals densely encapsulated in the glassy phase. This phase characteristic makes it impossible for traditional physical separation methods (magnetic separation, gravity separation) to liberate the tantalum and niobium minerals, resulting in low concentrate grade and recovery rate.
[0003] Existing lithium slag valuable metal recovery technologies have the following shortcomings: First, the roasting and activation step often uses a compound system of ammonium sulfate and sodium sulfate, and the introduced sodium ions are prone to react with silicate ions in subsequent wet processes to form calcium silicate scale, leading to equipment scaling and blockage. Second, if acidic phosphorus extractants are used for rubidium and cesium extraction, their cation exchange mechanism is prone to exchange with impurities such as calcium, magnesium, and iron in the leachate, causing emulsification or a third phase, affecting phase separation and extraction efficiency. Third, for tantalum and niobium recovery, physical sorting routes have reached their limit due to the limitation of glass phase encapsulation, while direct strong acid or strong alkali leaching has problems such as severe equipment corrosion and large co-dissolved impurities.
[0004] Currently, there is no process that can achieve efficient, step-by-step separation of rubidium, cesium, tantalum, and niobium by synergistic process steps, taking into account the aforementioned characteristics of lithium slag. Summary of the Invention
[0005] The purpose of this invention is to provide a method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium spodumene extraction waste. The method is simple to operate, operates under mild conditions, and can recover valuable metals from lithium slag with high grade and high recovery rate.
[0006] The embodiments of the present invention are implemented as follows: A method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium extraction waste from spodumene includes: S1. Lithium extraction waste residue from spodumene is mixed with ammonium sulfate and then roasted at low temperature. The roasted product is then leached in water to obtain a leachate containing rubidium and cesium and a leachate residue containing tantalum and niobium. S2. The leachate is extracted by contacting it with a neutral organophosphorus extractant to obtain a loaded organic phase; the loaded organic phase is then back-extracted with an acidic solution to obtain a rubidium-cesium mixture; the rubidium-cesium mixture is separated and purified to obtain high-purity rubidium salt and / or cesium salt products. S3. The leaching residue is subjected to alkaline leaching, followed by hydrolysis and precipitation to obtain tantalum-niobium concentrate.
[0007] The beneficial effects of the embodiments of the present invention are: This invention provides a method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium spodumene extraction waste. The method involves low-temperature roasting of the lithium spodumene extraction waste using ammonium sulfate alone, avoiding the calcium silicate scaling problem caused by the introduction of sodium ions into the compound system. Water leaching achieves preliminary separation of rubidium and cesium from tantalum and niobium. A neutral organophosphorus extractant is used for extraction and back-extraction of the leachate, utilizing ion-pair coordination mechanisms to avoid emulsification and third-phase problems caused by the exchange of impurities such as calcium, magnesium, and iron with acidic extractants. This method is suitable for high-silicon and high-impurity systems, and high-purity rubidium and cesium salts are obtained after purification. The leachate residue is then subjected to alkaline leaching and hydrolysis precipitation, chemically dissolving the glassy phase encapsulating tantalum and niobium, releasing and enriching them. This method overcomes the grade ceiling caused by the glassy phase encapsulation in physical sorting, achieving efficient cascade recovery of rubidium, cesium, tantalum, and niobium. Detailed Implementation
[0008] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0009] The following is a detailed description of a method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium spodumene extraction waste residue according to an embodiment of the present invention.
[0010] A method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium extraction waste from spodumene includes: S1. Lithium extraction waste residue from spodumene is mixed with ammonium sulfate and then roasted at low temperature. The roasted product is then leached in water to obtain a leachate containing rubidium and cesium and a leachate residue containing tantalum and niobium.
[0011] S2. The leachate is extracted by contacting it with a neutral organophosphorus extractant to obtain a loaded organic phase; the loaded organic phase is then back-extracted with an acidic solution to obtain a rubidium-cesium mixture; the rubidium-cesium mixture is separated and purified to obtain high-purity rubidium salt and / or cesium salt products.
[0012] S3. The leaching residue is subjected to alkaline leaching, followed by hydrolysis and precipitation to obtain tantalum-niobium concentrate.
[0013] Lithium extraction waste from spodumene contains valuable metals such as rubidium, cesium, tantalum, and niobium. However, the high-temperature roasting during the lithium extraction process causes the formation of a large amount of amorphous glassy phase in the waste, with tantalum and niobium minerals densely encapsulated in the glassy phase. This phase characteristic makes it impossible for traditional physical separation methods (magnetic separation, gravity separation) to liberate the tantalum and niobium minerals, resulting in low concentrate grade and recovery rate.
[0014] This invention first distinguishes itself from existing compound salt systems by using ammonium sulfate alone for low-temperature roasting, avoiding the calcium silicate scaling problem in subsequent extraction processes caused by the introduction of foreign metal ions such as sodium ions, while also reducing the cost of roasting aids. Subsequently, solvent extraction is performed using a neutral organophosphorus extractant, utilizing ion-pair coordination mechanisms to co-extract rubidium and cesium in a high-ionic-strength medium. This avoids the emulsification or third-phase formation problems caused by cation exchange between acidic extractants and impurities such as calcium, magnesium, and iron, making it particularly suitable for lithium slag leachate systems with high silica and high impurity content. Finally, a chemical pathway of alkaline leaching-hydrolysis precipitation replaces physical sorting, fundamentally dissolving the glassy phase and aluminosilicates encapsulating tantalum and niobium, allowing tantalum and niobium to redefine and enrich, overcoming the grade and recovery rate limitations caused by mineral intergrowth in physical sorting. These three steps form a complete tiered separation process, achieving synergistic and efficient recovery of rubidium, cesium, and tantalum and niobium from lithium slag.
[0015] Further, in step S1, the lithium extraction waste residue from spodumene is mixed with ammonium sulfate solution at a mass-to-volume ratio of 1:(2~4), and the mass-to-volume concentration of the ammonium sulfate solution is 20%~40%. This ratio ensures uniform contact between the waste residue and the roasting aid, and sufficient sulfation conversion of rubidium and cesium. It also avoids increased material viscosity, difficulties in mass transfer, or reagent waste caused by excessive ammonium sulfate, allowing the roasting reaction to proceed in a suitable liquid-solid system and providing stable feed conditions for subsequent water leaching and extraction processes.
[0016] Optionally, in step S1, the low-temperature roasting temperature is 200~350℃, and the roasting time is 30~180min. This temperature range is considered low-temperature roasting, which can selectively destroy the aluminosilicate framework to induce rubidium-cesium sulfation, while avoiding phase transformation or sintering of tantalum-niobium minerals caused by high temperatures. At the same time, the lower roasting temperature is beneficial for energy conservation, emission reduction, and reducing equipment wear.
[0017] Furthermore, in step S1, the liquid-to-solid volume ratio of water to the calcined product during water leaching is (2~6):1, the leaching temperature is 60~95℃, and the leaching time is 30~120min. This range ensures sufficient dissolution of rubidium and cesium sulfate and efficient liquid-solid separation, while preventing excessive leaching of impurity elements that would increase the subsequent extraction load. This maintains a suitable volume and ionic strength in the leachate, creating favorable conditions for the extraction process.
[0018] Further, in step S2, a neutral organophosphorus extractant is dissolved in an inert diluent to form an organic phase. The inert diluent is kerosene. The neutral organophosphorus extractant is selected from at least one of tributyl phosphate, trialkylphosphine oxide, and trioctylphosphine oxide. These extractants exhibit excellent ion-pair coordination ability and selectivity for rubidium and cesium under high ionic strength. Kerosene, as a diluent, can effectively adjust the viscosity and density of the organic phase, avoiding the formation of a third phase or emulsification in the extraction system. It is particularly suitable for treating lithium slag leachate with high silicon content.
[0019] Optionally, in step S2, the extraction ratio of O / A is (1:6) to (1:2), and the extraction temperature is 20 to 60°C. This ratio range ensures the single-stage extraction rate of rubidium and cesium while avoiding increased costs due to excessively large organic phase volume or incomplete extraction due to excessively small ratio. At the same time, this temperature range reduces the emulsification tendency of the extraction system and ensures rapid stratification of the two phases.
[0020] Furthermore, the neutral organophosphorus extractant is tributyl phosphate, with a volume fraction of 10%–60% in kerosene. Tributyl phosphate has been proven to offer the most balanced extraction selectivity and loading capacity for rubidium and cesium through practical experience. Optionally, the acidic solution used for back-extraction is 0.5–3 mol / L hydrochloric acid. This concentration range effectively back-extracts rubidium and cesium from the loaded organic phase to the aqueous phase while avoiding excessive acid concentration that could lead to extractant degradation or equipment corrosion. The resulting rubidium-cesium mixture has a moderate acidity, facilitating subsequent ion exchange purification.
[0021] Optionally, in step S2, the separation and purification are performed using ion exchange, and the ion exchange resin is selected from either a strongly acidic cation exchange resin or a chelating resin. These two resins have highly selective adsorption capacity for rubidium and cesium ions, effectively removing impurity cations such as potassium, sodium, calcium, and magnesium from the leachate, thereby obtaining high-purity rubidium salts and / or cesium salts with a purity ≥99.5%, thus increasing the economic added value of the entire process.
[0022] Furthermore, in step S3, the leaching agent used for alkaline leaching is a sodium hydroxide solution with a concentration of 3–8 mol / L, the leaching temperature is 150–220 °C, the pressure is 1.0–3.0 MPa, and the leaching time is 60–180 min. This range of conditions covers the operating range that can effectively dissolve the glassy phase and aluminosilicate. The combination of pressure and temperature ensures that the alkaline leaching reaction is carried out under subcritical conditions, enhancing the attack ability of OH- on silicon-oxygen bonds and aluminum-oxygen bonds, allowing tantalum and niobium to be fully released from the encapsulated phase, while avoiding the dramatic increase in equipment costs caused by supercritical conditions.
[0023] Further, in step S3, the specific operation of hydrolysis precipitation is as follows: the slurry after alkaline leaching is cooled to room temperature, the pH is adjusted to 8-11, and after stirring and aging for 30-120 minutes, solid-liquid separation is performed to obtain tantalum-niobium concentrate. By limiting the specific operation of hydrolysis precipitation and controlling the cooling rate and pH value, tantalum-niobium is promoted to uniformly nucleate and grow crystals in the form of (Ta,Nb)₂O₅·nH₂O. The aging process further promotes the agglomeration and sedimentation of fine particles, improves the filtration performance and crystallinity of the hydrolysis products, thereby facilitating the acquisition of tantalum-niobium concentrate with a grade ≥60% and simplifying subsequent solid-liquid separation operations.
[0024] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0025] Example 1
[0026] This embodiment provides a method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium extraction waste from spodumene. The raw material is lithium extraction waste from a lithium extraction plant using the sulfuric acid process, and its main components are as follows (mass percentage): SiO2 62.3%, Al2O3 21.5%, Fe2O3 3.2%, Na2O 2.8%, K2O 1.5%, Ta2O5 0.018%, Nb2O5 0.015%, Rb2O 0.12%, Cs2O 0.08%, with the remainder being loss on ignition.
[0027] The specific steps are as follows: S1. Calcination and activation: The lithium extraction waste residue from spodumene is crushed to a density of over 85% at -200 mesh, and mixed evenly with a 30% ammonium sulfate solution at a solid-liquid mass-to-volume ratio of 1:3. The mixture is then calcined at 250°C for 90 minutes. The calcined product is then added to water at a liquid-to-solid mass-to-volume ratio of 4:1 and leached at 90°C for 60 minutes. The leaching solution containing rubidium and cesium and the leaching residue containing tantalum and niobium are obtained by filtration.
[0028] S2. Rubidium and Cesium Extraction and Separation: The leachate was contacted with a kerosene solution containing 40% (volume fraction) TBP as the organic phase for extraction. The extraction ratio O / A = 1:4, the extraction temperature was 40℃, and the mixture was shaken for 15 min. After phase separation, a loaded organic phase was obtained. The loaded organic phase was back-extracted with 1 mol / L hydrochloric acid to obtain a rubidium and cesium mixture. The mixture was separated and purified by a strong acid cation exchange resin to obtain rubidium carbonate and cesium carbonate products with a purity ≥99.5%.
[0029] S3. Tantalum-Niobium Concentrate Recovery: The leaching residue containing tantalum and niobium obtained from S1 is leached with 5 mol / L NaOH solution at 180℃ and 2.0 MPa for 120 min. After cooling to room temperature, the pH is adjusted to 9, stirred and aged for 60 min, filtered, washed and dried to obtain tantalum-niobium concentrate product.
[0030] Test results: The total mass percentage of (Ta, Nb)₂O₅ in the tantalum-niobium concentrate was 63.5%, and the total recovery rate of tantalum and niobium was 86.2%.
[0031] Example 2
[0032] This embodiment provides a method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium spodumene extraction waste, using the same raw materials as in Example 1.
[0033] The specific steps are as follows: S1. Calcination and activation: The waste residue is mixed with a 25% ammonium sulfate solution at a solid-liquid ratio of 1:3.5 and calcined at 280℃ for 120 min; the water leaching solution has a solid-liquid ratio of 5:1, a leaching temperature of 80℃, and a leaching time of 90 min. The leachate and leaching residue are obtained by filtration.
[0034] S2. Rubidium and cesium extraction and separation: The leachate is contacted with an organic phase of kerosene containing 30% TBP for extraction, with an O / A ratio of 1:3 and a temperature of 35°C. Back-extraction is performed using 2 mol / L hydrochloric acid, and the product is purified by chelating resin to obtain high-purity rubidium and cesium salts.
[0035] S3. Tantalum-niobium concentrate recovery: The leaching residue was leached with 4 mol / L NaOH solution at 160℃ and 1.5 MPa for 150 min. After cooling, the pH was adjusted to 10 and aged for 90 min. The solid and liquid were separated to obtain tantalum-niobium concentrate.
[0036] Test results: The total mass percentage of (Ta, Nb)₂O₅ in the tantalum-niobium concentrate was 61.8%, and the total recovery rate of tantalum and niobium was 83.5%.
[0037] Example 3
[0038] This embodiment provides a method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium spodumene extraction waste, using the same raw materials as in Example 1.
[0039] The specific steps are as follows: S1. Calcination and activation: The waste residue is mixed with a 40% ammonium sulfate solution at a mass-to-volume ratio of 1:2 and calcined at 300℃ for 120 min. During water leaching, the liquid-to-solid volume ratio of water to the calcined product is 6:1, the leaching temperature is 80℃, and the leaching time is 90 min, yielding leachate and leaching residue.
[0040] S2. Rubidium and cesium extraction and separation: The leachate was contacted with a 50% TBP-kerosene solution for extraction. The extraction ratio O / A = 1:2, the temperature was 50℃, and the time was 30 min. The acidic solution used for back-extraction was 2 mol / L hydrochloric acid. The purification was the same as in Example 1, and high-purity rubidium salt and cesium salt with a purity ≥99.5% were obtained.
[0041] S3: Tantalum-Niobium Concentrate Recovery: The alkaline leaching agent used is a 6 mol / L sodium hydroxide solution, the leaching temperature is 200℃, the pressure is 2.5 MPa, and the leaching time is 150 min. The specific operation of hydrolysis precipitation is as follows: the slurry after alkaline leaching is cooled to room temperature, the pH is adjusted to 9, and after stirring and aging for 90 min, solid-liquid separation is performed to obtain tantalum-niobium concentrate.
[0042] Test results: The total mass percentage of (Ta, Nb)₂O₅ in the concentrate was 62.3%, and the total recovery rate of tantalum and niobium was 85.7%.
[0043] Comparative Example 1 This comparative example provides a method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium spodumene extraction waste, using the same raw materials as in Example 1. The difference in operating steps compared to Example 1 is: The roasting and activation steps are omitted. The waste residue is directly crushed to -200 mesh with a proportion of ≥85%, and the tailings are discarded by strong magnetic separation (magnetic field strength 1.2T). The magnetic concentrate is then subjected to shaking table gravity separation (stroke 12mm, stroke 300 times / min, transverse slope 3°) to obtain tantalum-niobium concentrate.
[0044] In lithium slag, because tantalum and niobium are encapsulated by a glassy phase, conventional mechanical crushing cannot break the inclusions to allow the tantalum and niobium particles to separate independently. As a result, gravity separation and magnetic separation cannot effectively capture pure tantalum and niobium particles, and the concentrate contains a large amount of silicate gangue. After testing, the tantalum and niobium concentrate has a Ta2O5 grade of 20.87%, a Nb2O5 grade of 16.24%, and a total (Ta,Nb)2O5 grade of 36.11%; the Ta2O5 recovery rate is 54.21%, and the Nb2O5 recovery rate is 52.39%.
[0045] Comparative Example 2 This comparative example provides a method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium spodumene extraction waste, using the same raw materials as in Example 1. The difference in operating steps compared to Example 1 is: The waste residue was mixed with a compound solution consisting of ammonium sulfate and sodium sulfate (ammonium sulfate concentration 20%, sodium sulfate concentration 10%, mass to volume ratio 1:3), and calcined at 250°C for 90 min. The subsequent water leaching, extraction, alkaline leaching and hydrolysis precipitation steps were the same as in Example 1.
[0046] Testing revealed that the introduction of sodium ions into the compound system caused silicate and calcium ions in the solution to combine and form calcium silicate (CaSiO3) colloids during the water leaching and extraction processes. This resulted in severe emulsification during extraction, with the two-phase separation time exceeding 2 hours and an organic phase loss of approximately 15%. Simultaneously, significant scaling occurred on the inner wall of the alkaline leaching equipment. The final tantalum-niobium concentrate had a combined (Ta, Nb)₂O₅ content of 48.3%, and a total tantalum-niobium recovery rate of 72.5%. This indicates that the introduction of exogenous sodium ions triggers the formation of calcium silicate colloids, leading to emulsification, scaling, and a decrease in the tantalum-niobium enrichment effect in subsequent processes.
[0047] Comparative Example 3 This comparative example provides a method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium spodumene extraction waste, using the same raw materials as in Example 1. The difference in operating steps compared to Example 1 is: In step S2, the leachate is extracted by contacting it with a 30% (v / v) P204 (di(2-ethylhexyl) phosphate)-kerosene solution, with a ratio of O / A = 1:4 and a temperature of 40°C.
[0048] Testing revealed that P204, being an acidic phosphorus extractant, extracts through a cation exchange mechanism, reacting with a large amount of Ca in the leachate. 2+ Mg 2+ Fe 3+ When impurities undergo exchange reactions, the extractant consumption is high, a third phase appears in the organic phase, and phase separation is difficult. The single-stage extraction rate of rubidium and cesium is only 65%. After back-extraction and purification, the purity of the rubidium and cesium salts obtained is 98.2%, which does not meet the high-purity product requirement (≥99.5%). This indicates that acidic extractants are easily affected by impurities when treating high-silicon, high-impurity lithium slag leachates, and cannot simultaneously achieve both extraction rate and product purity.
[0049] In summary, this invention discloses a method for the cascade recovery of rubidium, cesium, and tantalum-niobium concentrates from lithium spodumene extraction waste. It utilizes ammonium sulfate alone for low-temperature roasting of the lithium spodumene extraction waste, avoiding the calcium silicate scaling problem caused by the introduction of sodium ions into the compound system. Water leaching achieves preliminary separation of rubidium and cesium from tantalum and niobium. A neutral organophosphorus extractant is used for extraction and back-extraction of the leachate, utilizing ion-pair coordination mechanisms to avoid emulsification and third-phase problems caused by the exchange of impurities such as calcium, magnesium, and iron with acidic extractants. This method is suitable for high-silicon and high-impurity systems, and high-purity rubidium and cesium salts are obtained after purification. The leachate residue undergoes alkaline leaching and hydrolysis precipitation, chemically dissolving the glassy phase encapsulating tantalum and niobium, releasing and enriching them. This method overcomes the grade ceiling caused by the glassy phase encapsulation in physical sorting, achieving efficient cascade recovery of rubidium, cesium, tantalum, and niobium.
[0050] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for stepwise recovery of rubidium, cesium and tantalum-niobium concentrates from lithium extraction waste residue of spodumene, characterized in that, include: S1. The lithium extraction waste residue from spodumene is mixed with ammonium sulfate and then roasted at low temperature. The roasted product is then leached in water to obtain a leachate containing rubidium and cesium and a leachate residue containing tantalum and niobium. S2. The leachate is extracted by contacting it with a neutral organophosphorus extractant to obtain a loaded organic phase; the loaded organic phase is then back-extracted with an acidic solution to obtain a rubidium-cesium mixture; the rubidium-cesium mixture is separated and purified to obtain high-purity rubidium salt and / or cesium salt products. S3. The leaching residue is subjected to alkaline leaching, followed by hydrolysis and precipitation to obtain tantalum-niobium concentrate.
2. The method of claim 1, wherein, In step S1, lithium extraction waste residue from spodumene is mixed with ammonium sulfate solution at a mass-to-volume ratio of 1:(2~4), and the mass-to-volume concentration of the ammonium sulfate solution is 20%~40%.
3. The method of claim 1, wherein, In step S1, the low-temperature calcination temperature is 200~350℃, and the calcination time is 30~180min.
4. The method of claim 1, wherein, In step S1, the liquid-to-solid volume ratio of water to the roasted product during water leaching is (2~6):1, the leaching temperature is 60~95℃, and the leaching time is 30~120min.
5. The method of claim 1, wherein, In step S2, the neutral organophosphorus extractant is dissolved in an inert diluent to form an organic phase, wherein the inert diluent is kerosene; the neutral organophosphorus extractant is selected from at least one of tributyl phosphate, trialkylphosphine oxide, and trioctylphosphine oxide.
6. The method according to claim 5, characterized in that, In step S2, the extraction ratio O / A is (1:6) to (1:2), and the extraction temperature is 20 to 60°C.
7. The method according to claim 6, characterized in that, The neutral organophosphorus extractant is tributyl phosphate, with a volume fraction of 10% to 60% in kerosene; the acidic solution used for back-extraction is 0.5 to 3 mol / L hydrochloric acid.
8. The method according to claim 1, characterized in that, In step S2, the separation and purification are performed using ion exchange, and the resin used for ion exchange is selected from either a strong acid cation exchange resin or a chelating resin.
9. The method according to claim 1, characterized in that, In step S3, the leaching agent used in the alkaline leaching is a sodium hydroxide solution with a concentration of 3~8 mol / L, a leaching temperature of 150~220℃, a pressure of 1.0~3.0 MPa, and a leaching time of 60~180 min.
10. The method according to claim 1, characterized in that, In step S3, the specific operation of hydrolysis precipitation is as follows: cool the slurry after alkaline leaching to room temperature, adjust the pH to 8~11, stir and age for 30~120 minutes, and then perform solid-liquid separation to obtain tantalum-niobium concentrate.