A method for melting and processing brazable cast aluminum alloys with reduced inclusion content
By employing techniques such as raw material pretreatment, layered composite flux refining, and online synchronous degassing and stirring, the problem of balancing brazable performance and high-strength mechanical properties in die-cast aluminum alloys has been solved. This has resulted in improved aluminum liquid cleanliness and increased production efficiency, meeting the standardized baseline requirements of high-end customers.
Patent Information
- Application Number
- CN202611262665.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing die-cast aluminum alloys struggle to balance brazability and high-strength mechanical properties. They also suffer from insufficient control over the cleanliness of molten aluminum, excessive inclusions and dissolved hydrogen, numerous casting defects, poor smelting temperature control accuracy, low production efficiency and resource utilization, poor batch consistency, and an inability to meet the standardized baseline requirements of high-end customers.
The process employs a multi-stage synergistic approach, including raw material pretreatment, layered composite flux refining, online synchronous degassing and stirring, and constant temperature settling. This process involves steps such as raw material sandblasting to remove oxide scale, gradient heating melting, composite flux refining, online integrated degassing and electromagnetic stirring, and inert protection transfer, to ensure the cleanliness and compositional stability of the molten aluminum.
It significantly reduces inclusions and hydrogen content, improves the tensile and yield mechanical properties of materials, meets brazing requirements, improves production efficiency and material consistency, reduces casting defects, and enhances melting temperature control accuracy and resource utilization.
Smart Images

Figure CN123108335A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloy melting, casting and processing technology, specifically to a brazable casting aluminum alloy melting and processing method that reduces inclusion content. Background Technology
[0002] Cast aluminum alloys refer to aluminum-silicon or aluminum-magnesium cast base materials that are suitable for die casting and metal mold casting processes, have good fluidity, and are suitable for the one-piece molding of complex structural parts. Brazing is the ability of the filler metal to uniformly wet the surface of the base material after the casting is formed, under the specified brazing temperature and flux system, to form a high-strength brazing seam without any false welds, which meets the brazing baseline of the lead-ahead and the brazing access standards of Huawei 2116H products.
[0003] For example, patent CN1958818A discloses a method for smelting cast aluminum alloys. The key technical points are: after pure aluminum is melted in a crucible, pure silicon is added when the temperature of the aluminum melt reaches 690-720℃. When the temperature of the aluminum-silicon melt reaches 700-730℃, a refining and modifying agent prepared by adding 10kg of NaNO3, 13kg of BaCl2, 10kg of NaF, 13kg of Na3AlF6, 21kg of K2TiF6, 6kg of KBF4, 13kg of NaCl, and 10kg of C powder is added. The agent is pressed into the aluminum melt using a salt-immersing spoon, 100-150mm from the bottom of the crucible. This method for smelting cast alloys can achieve refining, modification, and refining in one step, shortening the operation time, reducing iron gain during alloy smelting, improving the quality of aluminum alloys, and reducing environmental pollution.
[0004] For example, patent CN110438378A discloses a method for melting and casting 2-series aluminum alloys, comprising the following components by mass percentage: Si: ≤0.4%, Fe: ≤0.35%, Cu: 2.4~2.65%, Mn: 0.4~0.55%, Mg: 0.3~0.55%, Cr: ≤0.1%, Ni: ≤0.05%, Zn: ≤0.15%, Ti: 0.02~0.1%, Bi: 0.55~0.7%, with individual impurities ≤0.05%, and total... The alloy contains ≤0.15% aluminum alloy and the balance is Al. After smelting, refining, degassing, slag removal, and casting, a semi-continuous casting process is used to cast the alloy. The casting temperature is controlled at 670℃~690℃, the casting speed is 32~35mm / min, and the single-branch water flow rate is 100~120L / min. This yields a 2-series aluminum alloy ingot. The aluminum alloy round ingots produced by this invention's 2-series aluminum alloy smelting and casting method have fewer defects, improved material properties and yield, reduced energy consumption, and lower production costs, resulting in good economic benefits.
[0005] However, existing die-cast aluminum alloys cannot simultaneously achieve both brazing performance and high-strength mechanical properties, making them unsuitable for the baseline requirements of high-end equipment in multiple fields. Furthermore, traditional smelting processes lack sufficient control over the cleanliness of molten aluminum, resulting in excessive inclusions and dissolved hydrogen, numerous casting defects, and severe degradation of mechanical properties. In addition, the smelting temperature control accuracy is poor, and there is no online integrated degassing and stirring equipment, leading to low production efficiency and resource utilization. The lack of online closed-loop composition fine-tuning processes results in poor batch consistency of products, failing to meet the standardized baseline indicators of high-end customers. Moreover, there is no inertial protection design in the die-casting transfer and forming process, making the results of the front-end purification process prone to failure.
[0006] To address the aforementioned issues, there is an urgent need for innovative designs based on existing methods. Summary of the Invention
[0007] The purpose of this invention is to provide a method for melting and processing brazable cast aluminum alloys to reduce inclusion content, thereby solving the problems in the prior art where existing die-cast aluminum alloys cannot simultaneously achieve brazability and high-strength mechanical properties, cannot meet the baseline requirements of high-end equipment in multiple fields, and have insufficient control over the cleanliness of molten aluminum in traditional melting processes, resulting in excessive inclusions and dissolved hydrogen, numerous casting defects, severe degradation of mechanical properties, poor temperature control accuracy during melting, lack of online integrated degassing and stirring equipment, low production efficiency and resource utilization, lack of online closed-loop composition fine-tuning process, poor batch consistency of products, inability to meet the standardized baseline indicators of high-end customers, lack of inertial protection design in the die-casting transfer and forming process, and easy failure of the results of the front-end purification process.
[0008] To achieve the above objectives, the present invention provides the following technical solution: a method for melting and processing brazable cast aluminum alloys to reduce inclusion content, comprising the following steps:
[0009] S1: Raw material ratio pre-control, the raw materials are sandblasted to remove oxide scale and preheated to remove moisture, and the materials are prepared separately according to two types of base materials: DC05 brazable cast aluminum alloy and HJ-09B high-strength cast aluminum alloy. The content of impurity elements is strictly limited to reduce the original inclusions from the source.
[0010] S2: Gradient heating melting, the aluminum material is heated and melted in three stages in a closed melting furnace: low temperature, medium temperature and high temperature. Argon gas is introduced throughout the process to isolate the air, so as to melt the aluminum material gently, suppress secondary oxidation and gas absorption during the melting process, and avoid the generation of a large number of new fine alumina inclusions.
[0011] S3: Composite flux layered refining. After the aluminum liquid is completely melted, the bottom layer of coarse refining flux and the top layer of covering refining flux are added in sequence. After bottom blowing argon gas stirring, the mixture is allowed to stand and remove slag to remove large-sized inclusions and free hydrogen.
[0012] S4: Online integrated degassing and electromagnetic stirring, used for deep and fine purification. The aluminum liquid is passed into the online processing unit with integrated rotary rotor degassing and low-frequency electromagnetic stirring, and the fine dispersed impurities and dissolved hydrogen in the aluminum liquid that cannot be removed in S3 are removed simultaneously.
[0013] S5: Precise constant temperature static setting allows the composite inclusions after S4 agglomeration to completely settle due to gravity, thoroughly separating the aluminum liquid from the impurities.
[0014] S6: Real-time online composition fine-tuning, direct-reading spectral online detection of aluminum liquid elements, addition of alloying elements for two types of substrates and short-term stirring and settling to control cross-batch composition deviation;
[0015] S7: Inert protection transfer die casting. The aluminum liquid is transferred to the die casting station under the protection of argon atmosphere. The flow channel is protected against oxidation to suppress the generation of new inclusions and pores during the transfer process.
[0016] Preferably, the gradient temperature rise in S2 is as follows: when the room temperature rises to 420℃, the heating rate is 45℃ / h; when the room temperature rises to 650℃, the heating rate is 60℃ / h; and when the room temperature rises to 720-730℃, the heating rate is 30℃ / h.
[0017] Preferably, in S3, the bottom crude refining flux is NaCl, NaF and cryolite, and they are mixed in a mass ratio of 5:3:2; the surface refining flux is KCl mixed with trace amounts of rare earth chlorides; the bottom refining argon bottom blowing stirring time is 8 min, and the initial standing time after refining is 12 min.
[0018] Preferably, in the online processing unit of S4, a mixture of argon and trace amounts of chlorine gas is introduced into the rotating rotor, wherein the rotor speed is 280 r / min; the low-frequency electromagnetic stirring current is 250 A; the online synchronous processing time is 15 min; and the processing temperature is maintained at 710-720℃.
[0019] Preferably, the constant temperature in S5 is 715℃, the static time is 22min, and the temperature fluctuation of the furnace body throughout the process is ≤±8℃.
[0020] Preferably, the DC05 brazable cast aluminum alloy in S1 is used for structural components of Huawei communication equipment and structural components of new energy vehicles; the HJ-09B high-strength cast aluminum alloy is used for load-bearing components of low-altitude economic aircraft.
[0021] Preferably, the maximum operating temperature of the sealed melting furnace is 730℃, and the temperature control accuracy of the entire process is stable at ±8℃. The online processing unit needs to integrate the dual functions of rotary degassing and electromagnetic synchronous stirring.
[0022] Preferably, the specific steps of S1 are as follows:
[0023] S11: Base material classification and preparation, with two sets of formulas for precise batching to distinguish the two target alloys. The raw material components and impurity limits are defined separately and stored separately to prevent mixing. The main materials, intermediate alloys, and remelted materials of the two alloys are stored and labeled separately to prevent mixing of different alloy raw materials and avoid the aluminum liquid composition exceeding the standard, brazing, and strength performance failure in the later stage.
[0024] S12: Raw material surface pretreatment to remove the original alumina skin, reduce the amount of smelting inclusions, remove oil, mold release agents and other organic contaminants, and inhibit hydrogen and gas production;
[0025] S13: Low-temperature preheating of raw materials is used to remove adsorbed water vapor, completely eliminate water vapor, and block the core reactions of hydrogen production and alumina production in molten aluminum.
[0026] S14: Batching and metering verification, zoned feeding to isolate two alloys, used for high-precision weighing control, and stabilizing the basic composition of molten aluminum.
[0027] Preferably, the specific steps of S3 are as follows:
[0028] S31: Bottom roughing and refining operation, used to remove large particles of refractory slag and large pieces of alumina inclusions;
[0029] S32: Surface rare earth coating refining, used to agglomerate fine inclusions, adsorb and dissolve hydrogen, and prevent secondary oxidation;
[0030] S33: Initial long-term static stratification to complete slag-aluminum separation;
[0031] S34: Thoroughly remove floating scum and bottom sediment to complete the S3 process.
[0032] Preferably, the specific steps of S6 are as follows:
[0033] S61: Stable aluminum liquid conditions, online sampling and testing preparation, used to balance the temperature and composition of aluminum liquid, ensuring the authenticity and reliability of test data;
[0034] S62: Online spectral sampling distinguishes substrates and determines compositional deviations, enabling full-coverage detection of key elements and complete understanding of the composition and state of molten aluminum.
[0035] S63: Targeted and precise replenishment of intermediate alloy raw materials, targeted replenishment of materials according to the base material, precise replenishment of the alloy elements required for performance, feeding through the closed feeding channel on the furnace side without opening the main furnace door, adding alloy in small amounts multiple times to avoid local alloy concentration surges and segregation, while argon protection throughout the process to prevent air intrusion and impurity generation.
[0036] S64: Low-speed short-time stirring ensures uniform alloy composition. The added intermediate alloy will briefly gather near the feeding port. Low-intensity electromagnetic stirring allows alloying elements to diffuse evenly in the molten aluminum, ensuring consistent composition throughout the entire furnace of molten aluminum.
[0037] S65: Secondary settling and re-inspection to ensure consistent batch composition. Short-term settling allows trace amounts of fine slag stirred up by stirring to settle again, restoring the high purity of the molten aluminum and preventing impurities from flowing into the die-casting process with the molten aluminum.
[0038] Compared with the prior art, the beneficial effects of the present invention are:
[0039] 1. It can effectively reduce inclusions and hydrogen content. Through raw material pretreatment, layered composite flux refining, online synchronous degassing and stirring, and constant temperature settling multi-stage synergy, the hydrogen content of aluminum liquid can be effectively reduced, the removal rate of fine inclusions can be improved, the porosity and shrinkage defects of castings can be reduced, and the tensile and yield mechanical properties of materials can be significantly improved.
[0040] 2. Overcoming the bottleneck of non-brazing of die-cast aluminum, by pre-controlling the composition of DC05 aluminum alloy raw materials and using low-temperature gradient melting process, the ratio of silicon and iron elements was balanced, the formation of dense oxide film during brazing was suppressed, and the requirements of the baseline brazing capability of the Outlook die-casting and the baseline capability of Huawei 2116H were fully met, thus realizing reliable brazing of die-cast aluminum alloys.
[0041] 3. Through online real-time spectral detection and micro-alloy fine-tuning processes, the compositional fluctuations across batches can be minimized, ensuring stable material performance in mass production and significantly reducing product defect rates.
[0042] 4. Through the integrated continuous process of melting, refining, degassing and stirring and fine-tuning of composition, there is no need for multiple furnace transfer and standing, which shortens the production cycle. Argon atmosphere protection reduces the oxidation and burn-off of aluminum liquid, thus improving the effective utilization rate of aluminum raw materials.
[0043] 5. With a stable temperature control accuracy of ±8℃ throughout the entire process, the maximum melting temperature can reach 730℃. The temperature fluctuation is small, which reduces the problems of aluminum liquid oxidation and gas absorption caused by sudden temperature changes, and further inhibits the formation of new inclusions. Attached Figure Description
[0044] Figure 1 This is a schematic diagram of the overall method flow of the present invention.
[0045] Figure 2 This is a schematic diagram of step 1 of the present invention;
[0046] Figure 3 This is a schematic diagram of step 3 of the present invention;
[0047] Figure 4 This is a schematic diagram of step 6 of the present invention. Detailed Implementation
[0048] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0049] This application provides a method for melting and processing brazable cast aluminum alloys to reduce inclusion content. To better understand the above technical solution, it will be described in detail below with reference to the accompanying drawings and specific embodiments. Figures 1-4 As shown in this embodiment of the present application, a method for melting and processing brazable cast aluminum alloy to reduce inclusion content includes the following steps:
[0050] S1: Raw material ratio pre-control, the raw materials are sandblasted to remove oxide scale and preheated to remove moisture, and the materials are prepared separately according to two types of base materials: DC05 brazable cast aluminum alloy and HJ-09B high-strength cast aluminum alloy. The content of impurity elements is strictly limited to reduce the original inclusions from the source.
[0051] It should be noted that in this application, DC05 brazable cast aluminum alloy is used for structural components of Huawei communication equipment and structural components of new energy vehicles, while HJ-09B high-strength cast aluminum alloy is used for load-bearing components of low-altitude economic aircraft. The specific steps are as follows:
[0052] S11: Base material classification and preparation, with two sets of formulas for precise batching to distinguish the two target alloys. The raw material components and impurity limits are defined separately and stored separately to prevent mixing. The main materials, intermediate alloys, and remelted materials of the two alloys are stored and labeled separately to prevent mixing of different alloy raw materials and avoid the aluminum liquid composition exceeding the standard, brazing, and strength performance failure in the later stage.
[0053] S12: Raw material surface pretreatment to remove the original alumina skin, reduce the amount of smelting inclusions, remove oil, mold release agents and other organic contaminants, and inhibit hydrogen and gas production;
[0054] S13: Low-temperature preheating of raw materials is used to remove adsorbed water vapor, completely eliminate water vapor, and block the core reactions of hydrogen production and alumina production in molten aluminum.
[0055] S14: Batching and metering verification, zoned feeding to isolate two alloys, used for high-precision weighing control, and to stabilize the basic composition of molten aluminum;
[0056] In practical implementation, the two target alloys are first distinguished, and the raw material components and impurity limits are defined separately. They are then stored separately to prevent mixing. The DC05 brazable cast aluminum alloy batching system uses 99.7% high-purity primary aluminum ingots as its base material. The alloy additives include trace amounts of metallic silicon, pure magnesium, high-purity copper, and titanium-aluminum refining agents. The impurity limits are strictly controlled: Fe ≤ 0.12%, total Pb+Sn content ≤ 0.01%, and Ca ≤ 0.005%. A key constraint in the proportioning is a strictly low total silicon content to avoid the formation of high-purity silicon during brazing. A dense, non-wetting oxide film meets brazing baseline requirements; the base materials of the HJ-09B high-strength cast aluminum alloy batching system are high-purity aluminum ingots and clean first-grade aluminum remelting materials; alloy additives include: metallic manganese, zirconium-aluminum master alloy, and strontium modifier; impurity hard control limits: Ca < 0.003%, Na ≤ 0.002%, reducing the risk of coarse grains and inclusions of brittle phases; then the remelting materials are graded and screened, and die-casting gate and waste casting remelting materials are sorted separately, removing those with rust, oil stains, bonded refractory sand, and surface spraying. Waste from coating processes; large pieces of recycled material are crushed to a particle size of 50-120mm, and then screened using a vibrating screen to remove mud, sand, refractory material debris, and solid inclusions of metallic foreign matter; next, the raw material surface is pretreated to remove the surface oxide layer and oil stains, i.e., virgin aluminum ingots and qualified recycled material are sent to a dry sandblasting cleaning device, using white corundum fine sand for low-pressure sandblasting to thoroughly remove oxide scale, rust, mold release agent, and oil stains from the aluminum surface; after sandblasting, compressed air is used to blow away residual sand powder to prevent sand particles from being carried into the smelting furnace and forming refractory inclusions. Debris; Sorting out scrap aluminum materials that still exhibit severe oxidation and peeling after sandblasting is prohibited from entering the furnace; Cleaned aluminum ingots, broken remelted materials, and intermediate alloys are packaged into high-temperature resistant material frames and sent to a sealed preheating oven, where the oven is kept at a constant temperature of 180℃ for ≥90 minutes. After preheating, they are immediately transferred to the smelting furnace inlet to avoid prolonged storage at room temperature and reabsorption of moisture from the air. This thoroughly removes moisture adsorbed on the surface and in the crevices of the raw materials, preventing water from reacting with the molten aluminum during the melting stage. The reaction formula is: This can simultaneously reduce the formation of alumina inclusions and the amount of dissolved hydrogen in the molten aluminum. Then, a high-precision electronic batching scale is used to accurately weigh the main material, intermediate alloy, and recycled material according to the formula, with the weighing error controlled within ±0.2kg. The two types of alloy raw materials, DC05 and HJ-09B, are stored in separate areas and fed in batches independently to prevent the two alloys from being mixed and causing the composition to exceed the standard. Before feeding, a visual inspection is carried out again: no mud, no oil stains, no water-containing raw materials, and no foreign solid impurities. After confirming that they are qualified, they are sent to the smelting furnace.
[0057] In this embodiment, by classifying and controlling the composition, harmful impurities can be limited, and the basic composition requirements of brazable and high-strength alloys can be matched, thus avoiding brittle inclusions and brazing failures from the root. By screening and sandblasting to remove solid impurities, solid foreign inclusions such as sand, oxide scale, and sand powder can be removed in advance, reducing large slag clumps in the subsequent aluminum liquid. It can also eliminate the core source of hydrogen production and alumina production from water vapor, significantly reducing the degassing pressure in subsequent refining. By feeding materials separately in different furnaces, alloy cross-contamination can be prevented, ensuring the stability of the basic composition of each furnace of aluminum liquid.
[0058] S2: Gradient heating melting, the aluminum material is heated and melted in three stages in a closed melting furnace: low temperature, medium temperature and high temperature. Argon gas is introduced throughout the process to isolate the air, so as to melt the aluminum material gently, suppress secondary oxidation and gas absorption during the melting process, and avoid the generation of a large number of new fine alumina inclusions.
[0059] It should be noted that in this application, the maximum operating temperature of the sealed melting furnace is 730℃, and the temperature control accuracy of the entire process is stable at ±8℃. The online processing unit needs to integrate the dual functions of rotary degassing and electromagnetic synchronous stirring. When the room temperature rises to 420℃, the heating rate is 45℃ / h; when the temperature rises from 420℃ to 650℃, the heating rate is 60℃ / h; and when the temperature rises from 650℃ to 720-730℃, the heating rate is 30℃ / h.
[0060] In practice, the DC05 or HJ-09B alloy raw materials, preheated to S1 and free of moisture and impurities, are first loaded into the melting furnace in layers. Aluminum ingots are placed at the bottom, crushed recycled material in the middle, and intermediate alloy at the top to prevent localized overheating. The two types of alloys are melted separately in separate furnaces, without mixing. The furnace door is closed, all feed ports and observation ports are sealed, and the argon purging pipeline is opened. High-purity argon gas is continuously introduced into the furnace cavity at a low flow rate of 0.8 L / min for 10 minutes to replace the existing air and moisture, establishing an inert protective atmosphere. Argon gas is continuously supplied in a small amount throughout the entire melting process. The furnace is then kept slightly positive to prevent outside air from seeping in. The closed-loop temperature control system is then activated, setting the parameters for the first stage of the heating curve: target temperature 420℃, heating rate stable at 45℃ / h, real-time temperature fluctuation locked within ±8℃, and low-temperature holding operation: after reaching 420℃, maintain a constant temperature for 15 minutes. The purpose of this process is to thoroughly dry any residual adsorbed moisture in the raw material's gaps, preventing rapid heating from causing instantaneous vaporization and entrapment into the molten aluminum, leading to oxidation and hydrogen production. At low temperatures, the aluminum material is not softened and will not undergo molten oxidation. Afterwards, the temperature control program automatically switches to the second stage... The second heating curve involves increasing the heating rate to 60℃ / h and reaching a final temperature of 650℃, with continuous argon gas protection throughout. After reaching 650℃, the temperature is held constant for 20 minutes. The purpose of this step is to gradually soften the aluminum material from a solid state and allow the surface layer to begin melting. The slow heating prevents rapid melting of localized aluminum layers and avoids large areas of molten aluminum being exposed to the trace amounts of air in the furnace, thus reducing the formation of a large amount of surface oxide scale. Then, the third heating program is switched, reducing the heating rate to 30℃ / h and slowly heating to the final melting temperature of 720-730℃. A temperature control upper limit of 730℃ is set to prevent overheating. After reaching 720℃, visually inspect the materials inside the furnace to confirm that all solid raw materials have been completely melted into a continuous, homogeneous aluminum liquid pool. If solid aluminum blocks still exist, slightly increase the furnace temperature, not exceeding 730℃, and extend the holding time until complete melting. Temperature fluctuations throughout the process are compensated in real time by the temperature control system, and the furnace temperature deviation at any given time shall not exceed ±8℃. Once all materials have melted into a homogeneous aluminum liquid, maintain a constant and stable temperature of 720℃ for 10 minutes to ensure uniform aluminum liquid temperature across the entire process, eliminate local temperature differences within the furnace, continuously maintain argon protection, and proceed directly to the next process without opening the furnace door to avoid oxidation caused by opening the door midway.
[0061] In this embodiment, pre-purging with sealed argon gas can remove moisture from the furnace air in advance, establishing an inert environment and suppressing oxidation and gas absorption from an environmental perspective. Through three-stage gradient differential heating, low-speed heating buffering avoids boiling of water vapor and violent oxidation of aluminum material due to rapid melting, significantly reducing newly formed fine alumina inclusions during the melting stage. Segmented constant temperature holding can thoroughly remove water and achieve stable melting in stages, preventing local overheating. High-precision temperature control with a locked upper limit of 730℃ ± 8℃ can prevent overheating from aggravating aluminum oxidation, stabilize the aluminum melting conditions, and reduce the load on subsequent S3 and S4 refining and impurity removal.
[0062] S3: Composite flux layered refining. After the aluminum liquid is completely melted, the bottom layer of coarse refining flux and the top layer of covering refining flux are added in sequence. After bottom blowing argon gas stirring, the mixture is allowed to stand and remove slag to remove large-sized inclusions and free hydrogen.
[0063] It should be noted that in this application, the bottom crude refining flux is NaCl, NaF, and cryolite, mixed in a mass ratio of 5:3:2; the surface refining flux is KCl mixed with trace amounts of rare earth chlorides; the bottom refining argon bottom blowing stirring time is 8 minutes, followed by an initial settling time of 12 minutes after refining, and the specific steps are as follows:
[0064] S31: Bottom roughing and refining operation, used to remove large particles of refractory slag and large pieces of alumina inclusions;
[0065] S32: Surface rare earth coating refining, used to agglomerate fine inclusions, adsorb and dissolve hydrogen, and prevent secondary oxidation;
[0066] S33: Initial long-term static stratification to complete slag-aluminum separation;
[0067] S34: Thoroughly remove floating scum and bottom sediment to complete step S3;
[0068] In practice, after the molten aluminum stabilizes at a constant temperature of 720℃, the top charging port is slightly opened, and 0.3% of the total mass of the molten aluminum is weighed and evenly added to the depth of the molten aluminum at the bottom of the furnace. Then, the charging port is sealed, and the bottom argon blowing pipeline is opened with an argon flow rate of 1.2L / min, and bottom blowing and stirring are carried out continuously for 8 minutes. The bubbles carry the flux to roll throughout the furnace, and the flux wets and coats large particles of alumina, refractory debris, and brittle inclusions between metals in the molten aluminum. Relying on the density difference, the flux carries the slag clumps down. After the bottom blowing and stirring are completed, let it stand for 5 minutes to allow large slag clumps to settle completely. Use a long-handled slag skimmer to remove the initial floating oxide slag from the surface. Weigh out 0.2% of the total mass of the molten aluminum as a surface refining flux (KCl composite trace rare earth chloride) and spread it evenly on the entire surface of the molten aluminum to quickly form a continuous and dense protective flux layer. The function of the flux layer is: 1. To isolate trace amounts of air in the furnace and prevent secondary oxidation of the molten aluminum to form new inclusions; 2. To disperse the rare earth components and micron-sized oxides in the molten aluminum. Aluminum and aluminum nitride micro-inclusions undergo an interfacial reaction, agglomerating the fine inclusions into larger, settleable particles. Simultaneously, free hydrogen from the molten aluminum is captured and released as bubbles. After spreading, the furnace door is sealed, and a slight positive pressure of argon gas is maintained throughout the process, without any additional stirring or disturbance. After the surface flux is applied, the furnace is held at a constant temperature of 720℃ for 12 minutes, with temperature fluctuations controlled to ≤±8℃ throughout. The furnace door is not opened, and the molten aluminum is not stirred. During this settling period, the agglomerated composite inclusions continue to settle to the bottom of the furnace by gravity, while hydrogen bubbles continue to rise. The flux layer is floated out; the aluminum liquid, the slag layer, and the bottom slag layer are clearly separated into three layers; after the settling time reaches the standard, the furnace door is slightly opened, and all the aged oxidized slag and the failed flux layer on the liquid surface are first removed. Then, the furnace bottom slag removal auxiliary tool is used to extract the slag layer with a large amount of coarse inclusions at the bottom of the furnace to reduce the residual macroscopic slag clumps inside the aluminum liquid. After the slag removal is completed, the furnace door is immediately closed and the argon protection is restored. The aluminum liquid is kept at a constant temperature of 710-720℃ and directly transferred to the S4 online integrated degassing + electromagnetic stirring unit.
[0069] In this embodiment, by adding chloride composite flux to the furnace bottom and bottom blowing argon stirring, large-sized foreign inclusions and primary oxide slag can be captured and settled, removing more than 80% of macroscopic inclusions visible to the naked eye. By coating the surface with rare earth flux, air can be isolated to prevent secondary oxidation, agglomerate micron-sized fine inclusions, and adsorb free hydrogen, thereby reducing the hydrogen content of the aluminum liquid. A 12-minute constant temperature settling period allows sufficient time for gravity settling, achieving full stratification of slag and aluminum. The double-layer slag removal operation can remove both floating slag and bottom slag in one go, significantly reducing the overall inclusion base of the aluminum liquid and alleviating the pressure of subsequent S4 deep purification.
[0070] S4: Online integrated degassing and electromagnetic stirring, used for deep and fine purification. The aluminum liquid is passed into the online processing unit with integrated rotary rotor degassing and low-frequency electromagnetic stirring, and the fine dispersed impurities and dissolved hydrogen in the aluminum liquid that cannot be removed in S3 are removed simultaneously.
[0071] It should be noted that in this application, the online processing unit rotates a rotor and is introduced with a mixture of argon and trace amounts of chlorine gas, wherein the rotor speed is 280 r / min; the low-frequency electromagnetic stirring current is 250 A; the online synchronous processing time is 15 min; and the processing temperature is maintained at 710-720℃.
[0072] In practice, the aluminum liquid, after slag removal by S3 and with a stable temperature of 710-720℃, is first transported to the online integrated processing chamber through a sealed, insulated flow channel. A small amount of argon gas is continuously introduced into the flow channel, ensuring no contact with air during transport to prevent the formation of new oxide inclusions. The unit temperature control system is activated to maintain the aluminum liquid temperature in the chamber at 710-720℃, with a temperature control deviation of ≤±8℃ throughout the process. Simultaneously, equipment parameters are adjusted: rotor speed preset to 280 r / min, electromagnetic stirring current preset to 250A, and the mixed protective gas ratio of 98% argon + 2% chlorine. The chamber is confirmed to be well-sealed, and a small amount of argon gas is continuously purged to establish an inert protective atmosphere. Then, the bottom rotating rotor mechanism is activated, and an argon-chlorine mixed gas is introduced. The high-speed rotation of the rotor shears the introduced gas into micron-sized microbubbles, which are evenly distributed throughout the aluminum liquid. As these microbubbles rise, they capture ultrafine alumina and aluminum nitride inclusions dispersed within the aluminum liquid, while simultaneously adsorbing dissolved hydrogen to form bubbles that rise to the surface. The system is activated synchronously 30 seconds after the rotor starts. The low-frequency electromagnetic stirring module maintains a stable stirring current of 250A. Electromagnetic force drives the overall directional circulation of the molten aluminum, allowing dispersed suspended micro-inclusions to continuously collide and agglomerate into large-size composite particles. This improves the efficiency of microbubble capture of inclusions and prevents localized accumulation of micro-inclusions. The rotary degassing and electromagnetic stirring mechanisms operate synchronously and continuously, with the entire online processing time strictly controlled to 15 minutes. During this process, the cavity temperature is monitored in real time. If the temperature exceeds the 710-720℃ range, the system automatically replenishes heat / dissipates heat to ensure fluctuations do not exceed ±8℃. After the 15-minute synchronous processing time is reached, the electromagnetic stirring module, the rotary rotor gas supply system, and the rotor drive motor are sequentially shut down, maintaining uninterrupted argon gas protection in the cavity. The connecting channel is opened, and the deeply purified molten aluminum is returned to the main holding furnace in a sealed manner. After the return is completed, the connecting channel between the online unit and the main furnace is sealed, and the floating slag layer in the unit cavity is cleaned to prevent residual inclusions from contaminating the next batch of molten aluminum. The main furnace maintains a constant temperature of 710-720℃, directly entering the S5 precise constant temperature settling process.
[0073] In this embodiment, the air is isolated by the closed-loop transfer system, preventing the pre-purified aluminum liquid from oxidizing again and generating new inclusions during transport. Dual-device parameter pre-adjustment locks the rotor speed, stirring current, and processing temperature, ensuring stable and consistent impurity and hydrogen removal effects across batches. Microbubble degassing and impurity capture by the rotor captures micron-sized inclusions and removes dissolved hydrogen, overcoming the limitation of traditional refining methods in removing ultrafine dispersed impurities. Synchronous electromagnetic circulation stirring enhances the collision and aggregation of fine inclusions, improving bubble capture efficiency and further reducing the content of residual inclusions in the aluminum liquid. Furthermore, the 15-minute continuous synchronous processing time standardizes the processing duration, balancing purification effect and production efficiency. Finally, the purified liquid is returned in a closed loop with inert atmosphere protection throughout, preventing secondary contamination and facilitating subsequent settling processes.
[0074] S5: Precise constant temperature static setting allows the composite inclusions after S4 agglomeration to completely settle due to gravity, thoroughly separating the aluminum liquid from the impurities.
[0075] In practice, the process begins by receiving the purified aluminum liquid from the S4 reflux. Throughout the process, the furnace door and connecting passages are kept sealed, and a small amount of argon gas is continuously introduced to maintain a slightly positive pressure inert atmosphere inside the furnace, preventing the entry of external air and moisture. The furnace's closed-loop temperature control program is then activated to precisely maintain the aluminum liquid temperature at 715℃. The system automatically compensates for heat in real time, and temperature fluctuations are strictly controlled within ±8℃. The liquid surface is checked to ensure a continuous and complete protective flux layer remains. If the flux layer is damaged, a small amount of refined flux is added to the surface to seal the exposed aluminum liquid area. Then, all stirring, bottom blowing, and rotor agitation equipment inside the furnace are shut down. The furnace door is not opened and the aluminum liquid is not stirred throughout the process, maintaining a completely still state. The constant-temperature settling time is strictly controlled at 22 minutes, divided into two stages: 1. The first 10 minutes: the aggregated composite inclusions slowly sink, and fine particles continuously collide and combine, forming a denser slag agglomerate; 2. The last 12 minutes: the slag agglomerates continue to sink to the bottom of the furnace, and the upper layer of the aluminum liquid gradually forms... The aluminum melt has a low-impurity, clean layer with clear slag and aluminum separation. The temperature control system continuously monitors the furnace temperature, and if the temperature deviates from 715℃ by more than ±8℃, it automatically activates heating / heat dissipation adjustment to stabilize the settling environment temperature. After the settling time reaches the standard, the furnace top feeding observation port is slightly opened. First, the aging slag and ineffective rare earth flux layer on the surface of the melt are thoroughly scraped off with a slag scraper, and all floating impurities are collected. The furnace bottom slag removal tool is then inserted into the high-impurity enrichment area at the bottom of the furnace to extract the settled composite slag layer and remove the fine inclusions and precipitates concentrated at the bottom of the aluminum melt. The slag removal operation is completed quickly, with each door opening lasting no more than 3 minutes. During the operation, the argon gas flow rate is increased to reduce secondary oxidation caused by air intrusion. After the slag removal is completed, the furnace door is immediately closed, and the original trace argon gas protection flow rate is restored. The aluminum melt in the furnace is kept at a constant temperature of 715℃ for 5 minutes. After visually confirming that there is no exposed aluminum melt and no obvious slag on the surface, and that the cleanliness of the aluminum melt meets the standard, the furnace is kept in a sealed state and proceeds to the next process, S6 online real-time composition fine-tuning.
[0076] In this embodiment, a stable 715℃ constant temperature environment and ±8℃ high-precision temperature control can be achieved through reflux and closed-loop temperature locking, preventing temperature fluctuations from disrupting inclusion settling. Simultaneously, the flux layer isolates the aluminum liquid from air, preventing re-oxidation and hydrogen absorption during the settling stage. A 22-minute undisturbed settling period allows sufficient time for gravity settling, enabling the fine inclusions agglomerated by S4 to settle fully and separating suspended ultrafine impurities from the main body of the aluminum liquid. Thorough slag removal through layering simultaneously removes surface slag and bottom slag, concentrating and discharging most of the residual inclusions in the system, significantly reducing the overall inclusion content of the aluminum liquid. A short-term constant temperature transition stabilizes the temperature and uniformity of the aluminum liquid, preventing sudden temperature changes from affecting the accuracy of subsequent component detection and providing stable operating conditions for online spectral sampling and fine-tuning.
[0077] S6: Real-time online composition fine-tuning, direct-reading spectral online detection of aluminum liquid elements, addition of alloying elements for two types of substrates and short-term stirring and settling to control cross-batch composition deviation;
[0078] The specific steps of S6 are as follows:
[0079] S61: Stable aluminum liquid conditions, online sampling and testing preparation, used to balance the temperature and composition of aluminum liquid, ensuring the authenticity and reliability of test data;
[0080] S62: Online spectral sampling distinguishes substrates and determines compositional deviations, enabling full-coverage detection of key elements and complete understanding of the composition and state of molten aluminum.
[0081] S63: Targeted and precise replenishment of intermediate alloy raw materials, targeted replenishment of materials according to the base material, precise replenishment of the alloy elements required for performance, feeding through the closed feeding channel on the furnace side without opening the main furnace door, adding alloy in small amounts multiple times to avoid local alloy concentration surges and segregation, while argon protection throughout the process to prevent air intrusion and impurity generation.
[0082] S64: Low-speed short-time stirring ensures uniform alloy composition. The added intermediate alloy will briefly gather near the feeding port. Low-intensity electromagnetic stirring allows alloying elements to diffuse evenly in the molten aluminum, ensuring consistent composition throughout the entire furnace of molten aluminum.
[0083] S65: Secondary settling and re-inspection to ensure consistent batch composition. Short-term settling allows trace amounts of fine slag stirred up by stirring to settle again, restoring the high purity of the molten aluminum and preventing impurities from flowing into the die-casting process with the molten aluminum.
[0084] In practice, after the S5 process is completed, the aluminum liquid inside the furnace is maintained at a constant temperature of 715℃ under a closed argon gas micro-positive pressure protection system. It is left undisturbed for 5 minutes to ensure uniform temperature and composition distribution. The dedicated online sampling channel on the furnace side is then opened (without opening the main furnace door). The spectral sampling probe is inserted into the middle region of the aluminum liquid to avoid interference from surface slag and bottom slag. The direct-reading spectrometer is started, and zero-point calibration is completed to prepare for collecting full-element composition data of the aluminum liquid. The probe is then immersed in the aluminum liquid for sampling. The spectrometer detects the content of all key elements, including Si, Mg, Cu, Ti, Mn, Zr, Sr, Fe, Ca, Pb, and Sn, in real time, automatically generating a composition analysis report. Two categories of judgment criteria are applied based on the type of substrate smelted in this furnace: 1. DC05... Brazing casting aluminum alloy judgment criteria: Core control: Si≤4.5%, Fe≤0.12%, Pb+Sn≤0.01%. If the silicon content exceeds the standard, a dense and difficult-to-wet oxide film will be formed during brazing, which cannot meet the brazing baseline and the capability baseline of Huawei 2116H. Insufficient Mg, Cu, and Ti content will reduce the basic mechanical properties of the base material. Second, HJ-09B high-strength casting aluminum alloy judgment criteria, core control: Mn and Zr are the core elements for grain strengthening, Ca<0.003%. Low Mn and Zr content will cause coarse grains and reduced tensile strength in the casting, which cannot meet the high strength requirements of low-altitude economic load-bearing components. The system automatically compares the measured values with the standard ratio and calculates the difference between the missing / exceeding values of various alloy elements. Based on the detection deviation, As a result, the corresponding intermediate alloy is added in small amounts through the furnace-side feeding channel via a closed automatic feeder, without disrupting the sealed atmosphere of the furnace throughout the process. The feeding rules for DC05 substrate are as follows: Low Si, Mg, Cu, and Ti content: Add small amounts of metallic silicon, pure magnesium, copper-aluminum intermediate alloy, and titanium-aluminum refining agent according to the calculated difference; Excessive Si content: Record the data for this furnace, reduce the amount of silicon raw material added in the next batching stage, and avoid large-scale dilution in this furnace to ensure production efficiency; Excessive Fe, Pb, and Sn impurities: Treat separately and do not enter the die-casting process. The feeding rules for HJ-09B substrate are as follows: Insufficient Mn and Zr: Add manganese-aluminum and zirconium-aluminum intermediate alloys to refine the grains and improve the strength of the casting; Insufficient Sr modifier content: Add a small amount of strontium-aluminum alloy to improve the internal structure of the casting; Insufficient Ca impurities: Add a small amount of Ca modifier to improve the internal structure of the casting; Quality issues: Extend the settling time for the next S3 refining batch and intensify impurity removal; control the weighing accuracy of the added alloy raw materials to ±0.1kg, adding them in small amounts in batches to avoid sudden changes in local element concentrations; after the alloy is added, start a low-speed electromagnetic stirrer, reduce the stirring current to 80A, and stir for 3 minutes. The low-intensity circulating stirring is only used to mix the added alloy elements and will not stir up the already settled inclusions at the bottom of the furnace, thus avoiding a secondary decrease in the cleanliness of the aluminum liquid. After stirring, turn off the stirring equipment and keep the aluminum liquid still; after stirring and mixing, keep it at a constant temperature of 715℃ for 5 minutes to allow the aluminum liquid with uneven concentrations to fully homogenize, while the small inclusions stirred up by the stirring settle again; conduct a second online sampling spectral re-examination to confirm that the content of all elements meets the standards, and control the composition deviation across batches within ±0.Within 0.3%; after passing the re-inspection, maintain a constant temperature of 705-715℃ in the furnace and directly transfer to the S7 inert protection transfer die-casting process; if deviations are still found after the re-inspection, repeat the S6.3-S6.5 fine-tuning process until the composition fully meets the standard.
[0085] In this embodiment, closed-loop online sampling and testing are used to prevent air from entering the molten alumina and accurately obtain true composition data. By differentiating the composition of different base materials, the performance requirements of brazable and high-strength alloys can be matched separately, ensuring brazing capability and mechanical strength from the composition source. By adding precise amounts of alloys, compositional deviations can be corrected, solving the problems of large batch composition fluctuations and unstable product performance in traditional smelting. By mixing at low speed and for a short time, alloying elements can be added evenly without disturbing the sedimentation inclusions at the bottom of the furnace, balancing compositional uniformity and molten aluminum cleanliness. Through static re-inspection and closed-loop verification, the composition of each furnace of molten aluminum can be kept stable and uniform, meeting the baseline consistency requirements of customers such as Huawei, DJI, and Invenview.
[0086] S7: Inert protection transfer die casting, the aluminum liquid is transferred to the die casting station under the protection of argon atmosphere, and the flow channel is protected against oxidation to suppress the generation of new inclusions and pores during the transfer process.
[0087] In practice, the aluminum molten metal conveying trough is first cleaned in advance, removing residual aluminum slag and oxide scale from the trough walls. A boron nitride (BN) anti-oxidation isolation coating is then evenly sprayed onto the inner wall of the trough, dried, and cured. The top cover plate and end flanges of the trough are then sealed. Argon gas is then continuously purged inside the trough for 12 minutes to replace air and moisture, maintaining a slightly positive pressure inert environment. The integrity of the trough's insulation layer is checked to ensure that heat loss from the aluminum molten metal is controllable throughout the transfer process, and that the aluminum molten metal temperature is stably maintained within the range of 705-715℃. Then, open the sealed connecting gate between the smelting furnace and the transfer trough without opening the main furnace door to prevent a large influx of air. Simultaneously, slightly increase the argon gas supply flow rate inside the furnace to form an outward airflow barrier, preventing air backflow. The molten aluminum flows slowly into the insulated trough due to the liquid level difference. The conveying flow rate is controlled smoothly to prevent the molten aluminum from impacting and entraining air at high speed, forming bubbles and oxide scale. Throughout the transfer process, the trough cover is completely closed, and a low flow rate of high-purity argon gas is continuously introduced to isolate the molten aluminum from contact with the atmosphere and water vapor, thus preventing alumina inclusions from occurring during the conveying process. The dissolved hydrogen is newly generated; the molten aluminum is transported through a closed flow channel to the pre-heating buffer furnace of the die-casting machine. The buffer furnace is also sealed and purged with argon gas, with the temperature controlled and locked at 705-715℃. After entering the buffer furnace, the molten aluminum is briefly kept at a constant temperature for 3 minutes to eliminate trace suspended bubbles and fine oxide particles generated during the transportation process, allowing them to float and separate. The temperature of the buffer furnace is monitored in real time, and temperature fluctuations are controlled within ±8℃ to avoid excessively high temperatures that exacerbate aluminum oxidation and excessively low temperatures that result in insufficient fluidity and affect die-casting. The die-casting machine's sprue and gating system are preheated and sprayed with a coating. With the BN anti-oxidation coating, a small amount of argon gas is simultaneously introduced into the scoop channel during the casting operation. A low-speed and stable casting process is adopted to reduce the degree of turbulence in the aluminum liquid filling process and reduce the air entrapment during filling. During the single batch die casting production process, the buffer furnace is continuously supplied with argon gas and the furnace body is not exposed to the aluminum liquid for a long time. After the single batch of aluminum liquid is die-cast, the argon gas supply is turned off, and the residual cold aluminum and slag in the runner, buffer furnace and sprue are cleaned. The furnace is then purged and sprayed with the BN coating for later use to prevent residual oxide slag from mixing into the next batch of aluminum liquid and introducing foreign inclusions.
[0088] In this embodiment, pretreatment of the flow channel and BN coating can eliminate impurities inherent in the conveying channel. The coating isolates the molten aluminum from the refractory material, preventing the reaction from generating new inclusions. A closed argon gas transport system throughout the process blocks contact between air, water vapor, and the high-purity molten aluminum, preventing the previous S1-S6 purification processes from failing and avoiding the regeneration of alumina and hydrogen bubbles. Low-temperature constant-temperature buffering (705-715℃) reduces the oxidizing activity of the molten aluminum, gradually eliminating trace bubbles and fine slag introduced during the conveying process. Inert atmosphere die casting reduces gas entrapment during molding, lowering porosity and subsurface oxide inclusion defects in the casting from the forming end. Post-batch cleaning and maintenance prevents slag residue from cross-contaminating the next batch of molten aluminum, ensuring consistent cleanliness across different batches.
[0089] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for melting and processing brazable cast aluminum alloys with reduced inclusion content, characterized in that, The processing method includes the following steps: S1: Raw material ratio pre-control, the raw materials are sandblasted to remove oxide scale and preheated to remove moisture, and the materials are prepared separately according to two types of base materials: DC05 brazable cast aluminum alloy and HJ-09B high-strength cast aluminum alloy. The content of impurity elements is strictly limited to reduce the original inclusions from the source. S2: Gradient heating melting, the aluminum material is heated and melted in three stages in a closed melting furnace: low temperature, medium temperature and high temperature. Argon gas is introduced throughout the process to isolate the air, so as to melt the aluminum material gently, suppress secondary oxidation and gas absorption during the melting process, and avoid the generation of a large number of new fine alumina inclusions. S3: Composite flux layered refining. After the aluminum liquid is completely melted, the bottom layer of coarse refining flux and the top layer of covering refining flux are added in sequence. After bottom blowing argon gas stirring, the mixture is allowed to stand and remove slag to remove large-sized inclusions and free hydrogen. S4: Online integrated degassing and electromagnetic stirring, used for deep and fine purification. The aluminum liquid is passed into the online processing unit with integrated rotary rotor degassing and low-frequency electromagnetic stirring, and the fine dispersed impurities and dissolved hydrogen in the aluminum liquid that cannot be removed in S3 are removed simultaneously. S5: Precise constant temperature static setting allows the composite inclusions after S4 agglomeration to completely settle due to gravity, thoroughly separating the aluminum liquid from the impurities. S6: Real-time online composition fine-tuning, direct-reading spectral online detection of aluminum liquid elements, addition of alloying elements for two types of substrates and short-term stirring and settling to control cross-batch composition deviation; S7: Inert protection transfer die casting. The aluminum liquid is transferred to the die casting station under the protection of argon atmosphere. The flow channel is protected against oxidation to suppress the generation of new inclusions and pores during the transfer process.
2. The method for smelting and processing brazable cast aluminum alloys with reduced inclusion content according to claim 1, characterized in that: The gradient heating in S2 is as follows: when the room temperature rises to 420℃, the heating rate is 45℃ / h; when the room temperature rises to 650℃, the heating rate is 60℃ / h; and when the room temperature rises to 720-730℃, the heating rate is 30℃ / h.
3. The method for smelting and processing brazable cast aluminum alloys with reduced inclusion content according to claim 1, characterized in that: The bottom layer crude refining flux in S3 is NaCl, NaF and cryolite, mixed in a mass ratio of 5:3:2; the surface refining flux is KCl mixed with trace amounts of rare earth chlorides; the bottom layer refining argon bottom blowing stirring time is 8 min, and the initial standing time after refining is 12 min.
4. The method for melting and processing brazable cast aluminum alloys with reduced inclusion content according to claim 1, characterized in that: In the S4 online processing unit, a mixture of argon and trace amounts of chlorine gas is introduced into the rotating rotor, with a rotor speed of 280 r / min; the low-frequency electromagnetic stirring current is 250 A; the online synchronous processing time is 15 min; and the processing temperature is maintained at 710-720℃.
5. The method for smelting and processing brazable cast aluminum alloys with reduced inclusion content according to claim 1, characterized in that: The constant temperature in S5 is 715℃, the static time is 22 minutes, and the temperature fluctuation of the furnace body is ≤±8℃ throughout the process.
6. The method for smelting and processing brazable cast aluminum alloys with reduced inclusion content according to claim 1, characterized in that: The DC05 brazable cast aluminum alloy in S1 is used for structural components of Huawei communication equipment and structural components of new energy vehicles; the HJ-09B high-strength cast aluminum alloy is used for load-bearing components of low-altitude economic aircraft.
7. The method for melting and processing brazable cast aluminum alloy with reduced inclusion content according to claim 1, characterized in that: The maximum operating temperature of the sealed melting furnace is 730℃, and the temperature control accuracy of the entire process is stable at ±8℃. The online processing unit needs to integrate the dual functions of rotary degassing and electromagnetic synchronous stirring.
8. The method for smelting and processing brazable cast aluminum alloys with reduced inclusion content according to claim 1, characterized in that: The specific steps of S1 are as follows: S11: Base material classification and preparation, with two sets of formulas for precise batching to distinguish the two target alloys. The raw material components and impurity limits are defined separately and stored separately to prevent mixing. The main materials, intermediate alloys, and remelted materials of the two alloys are stored and labeled separately to prevent mixing of different alloy raw materials and avoid the aluminum liquid composition exceeding the standard, brazing, and strength performance failure in the later stage. S12: Raw material surface pretreatment to remove the original alumina skin, reduce the amount of smelting inclusions, remove oil, mold release agents and other organic contaminants, and inhibit hydrogen and gas production; S13: Low-temperature preheating of raw materials is used to remove adsorbed water vapor, completely eliminate water vapor, and block the core reactions of hydrogen production and alumina production in molten aluminum. S14: Batching and metering verification, zoned feeding to isolate two alloys, used for high-precision weighing control, and stabilizing the basic composition of molten aluminum.
9. A method for melting and processing brazable cast aluminum alloys with reduced inclusion content according to claim 1, characterized in that: The specific steps of S3 are as follows: S31: Bottom roughing and refining operation, used to remove large particles of refractory slag and large pieces of alumina inclusions; S32: Surface rare earth coating refining, used to agglomerate fine inclusions, adsorb and dissolve hydrogen, and prevent secondary oxidation; S33: Initial long-term static stratification to complete slag-aluminum separation; S34: Thoroughly remove floating scum and bottom sediment to complete the S3 process.
10. A method for melting and processing brazable cast aluminum alloys with reduced inclusion content according to claim 1, characterized in that: The specific steps of S6 are as follows: S61: Stable aluminum liquid conditions, online sampling and testing preparation, used to balance the temperature and composition of aluminum liquid, ensuring the authenticity and reliability of test data; S62: Online spectral sampling distinguishes substrates and determines compositional deviations, enabling full-coverage detection of key elements and complete understanding of the composition and state of molten aluminum. S63: Targeted and precise replenishment of intermediate alloy raw materials, targeted replenishment of materials according to the base material, precise replenishment of the alloy elements required for performance, feeding through the closed feeding channel on the furnace side without opening the main furnace door, adding alloy in small amounts multiple times to avoid local alloy concentration surges and segregation, while argon protection throughout the process to prevent air intrusion and impurity generation. S64: Low-speed short-time stirring ensures uniform alloy composition. The added intermediate alloy will briefly gather near the feeding port. Low-intensity electromagnetic stirring allows alloying elements to diffuse evenly in the molten aluminum, ensuring consistent composition throughout the entire furnace of molten aluminum. S65: Secondary settling and re-inspection to ensure consistent batch composition. Short-term settling allows trace amounts of fine slag stirred up by stirring to settle again, restoring the high purity of the molten aluminum and preventing impurities from flowing into the die-casting process with the molten aluminum.
Citation Information
Patent Citations
2-series aluminum alloy smelting casting method
CN110438378A