Aluminum and aluminum alloy strip and its preparation method

By utilizing reaction capture purification units and differential cold rolling technology in the aluminum alloy strip manufacturing process, the process conflict between V and Ti depth control and solidification refinement was resolved, achieving efficient boride filtration and microstructure uniformity, and adapting to thin strip bending conditions.

CN123108337APending Publication Date: 2026-11-17GUIZHOU ENXINDA NEW MATERIALS CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611354427.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing aluminum alloy strip manufacturing process, there is a process conflict between the control of V and Ti depth and the solidification and refinement of Ti-containing materials, and the borides need to migrate a long distance before being filtered, resulting in low production efficiency.

Method used

Electrolytic aluminum liquid is mixed and smelted with clean aluminum cold material to form aluminum melt. V and Ti are purified by reaction capture and purification unit. Boration reaction is fixed in the flow direction of aluminum melt by using porous alumina framework and AlB12 boron-containing reactive material to form V and Ti borides, which are retained in the terminal interception layer to avoid the addition of Ti-containing grain refinement material. A double surface fine grain region and a central grain region are constructed by differential speed cold rolling.

Benefits of technology

The process achieves synergy between V and Ti depth control and solidification refinement, reduces boride migration paths, improves production efficiency and finished product microstructure uniformity, and adapts to the actual working conditions required for thin strip bending.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108337A_ABST
    Figure CN123108337A_ABST
Patent Text Reader

Abstract

This invention provides aluminum and aluminum alloy strips and their preparation method, relating to the field of aluminum alloy strip processing technology. The method involves mixing and melting electrolytic aluminum liquid with clean aluminum cold material (50%–60% of the total metal mass). After testing for V, Ti, and B, the aluminum melt is introduced into a boron-containing porous reaction trapping layer, causing V and Ti to form borides at the pore reaction interface and remain in the reaction trapping layer and terminal retention layer. After purification, without adding Ti-containing grain-refining materials, the product undergoes twin-roll casting, a first-stage same-speed cold rolling, and intermediate complete recrystallization. It then sequentially undergoes two differential-speed cold rollings with opposite shear directions and a same-speed precision rolling. After cleaning and slitting, the finished product is recrystallized. The finished product forms a first surface fine-grained region, a central grain region, and a second surface fine-grained region along its thickness. The conductivity is ≥70% IACS. This invention continuously connects the V and Ti purification process with the control of Ti-free solid-state structure, and is suitable for manufacturing conductive connecting strips in electrolytic aluminum baths and high-current flexible aluminum conductive strips.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aluminum alloy strip processing technology, specifically to aluminum and aluminum alloy strip and their preparation method. Background Technology

[0002] Aluminum and aluminum alloy strips possess high conductivity, corrosion resistance, and ductility, making them suitable for stable applications in electrolytic aluminum equipment, power equipment, and high-current flexible connection structures. For electrolytic aluminum cell connecting strips, the material continuously carries current during service and undergoes bending deformation during assembly, thermal cycling, and mechanical displacement. Therefore, the material's chemical purity, conductivity, elongation, surface microstructure, and batch stability must simultaneously meet industrial application requirements.

[0003] V, Ti, and Cr in high-purity aluminum are transition elements that require strict control. V and Ti, upon entering the aluminum matrix solid solution, alter the electron scattering state; in particular, increased V content leads to a decrease in conductivity. Current production methods use an Al-B master alloy to treat the aluminum melt, causing V and Ti to form borides, which are then separated from the melt through sedimentation, refining, and filtration. In this route, the boration reaction occurs throughout the entire molten pool. The resulting fine borides first enter the bulk melt and then migrate into the filter medium, separating the reaction site from the separation site. Smaller boride particle sizes also increase the subsequent filtration load.

[0004] On the other hand, the purification process requires reducing the Ti content, while traditional casting and rolling production uses Ti-containing grain-refining materials to adjust the solidification structure. Reintroducing Ti after purification alters the low-Ti melt state formed during the previous purification process; therefore, there is a mutually restrictive relationship between controlling high conductivity and solidification refinement. Traditional processes often use obtaining uniform fine grains across the entire thickness as the microstructure control target. However, when the strip bends, the tensile and compressive strains on the two surfaces are higher than in the center region, and the uniform grain design does not account for the actual service strain differences along the thickness direction.

[0005] Based on the above-mentioned technical problems, this invention changes the location of the V and Ti boronizing reaction, fixes the boron-containing reactive material at the porous interface through which the continuously flowing aluminum melt passes, and allows the boronizing reaction and particle retention to be completed continuously in the same purification unit. After purification, Ti-containing grain refinement material is not added again, but the final grain control task is transferred to the solid-state processing stage. A unified microstructure starting point is established through complete recrystallization in the middle, and a double-surface additional energy storage is constructed through two differential cold rolling stages with opposite shear directions. The double-surface fine grain region and the central grain region are formed through the recrystallization of the finished product. Summary of the Invention

[0006] Technical problems to be solved

[0007] To address the shortcomings of existing technologies, this invention provides an aluminum and aluminum alloy strip and its preparation method, resolving the process conflict between V and Ti depth control and Ti-containing solidification and refinement during the manufacturing of high-conductivity aluminum strip, and solving the problem that borides need to migrate long distances and be filtered after the whole-furnace phase boration.

[0008] Technical solution

[0009] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing aluminum and aluminum alloy strip, comprising the following steps: mixing and melting electrolytic aluminum liquid with clean aluminum cold material to form an aluminum melt; detecting the mass fractions of V, Ti, and B in the aluminum melt; continuously introducing the detected aluminum melt into a reaction capture and purification unit, wherein the reaction capture and purification unit, along the flow direction of the aluminum melt, sequentially includes an inlet flow stabilization cavity, a flow distribution zone, a boron-containing reaction capture layer, a transition buffer cavity, a terminal interception layer, and an outlet flow collection cavity; the boron-containing reaction capture layer includes a porous alumina skeleton and AlB disposed within the channels of the porous alumina skeleton. 12 In a boron-containing reactive material, V and Ti in the aluminum melt react with B in the boron-containing reaction trapping layer to form V-containing boride and Ti-containing boride, respectively. These V-containing boride and Ti-containing boride remain within the boron-containing reaction trapping layer and the terminal retention layer. The aluminum melt exiting the reaction trapping and purification unit is subjected to compositional analysis. Under the condition that the mass fraction of V is not higher than 0.002%, the mass fraction of Ti is not higher than 0.002%, and the mass fraction of B is not higher than 0.006%, the aluminum melt is fed into a twin-roll mill. No Ti-containing grain-refining material is added between the reaction trapping and purification unit and the twin-roll mill to form a cast-rolled strip. The cast-rolled strip... After the billet undergoes the first stage of cold rolling at the same speed, intermediate recrystallization annealing is performed. The strip after intermediate recrystallization annealing is then subjected to first differential speed cold rolling and second differential speed cold rolling in sequence. In the first differential speed cold rolling, the surface linear velocity of the upper work roll is greater than that of the lower work roll, and in the second differential speed cold rolling, the surface linear velocity of the lower work roll is greater than that of the upper work roll. After the second differential speed cold rolling is completed, the upper and lower work rolls are restored to the same surface linear velocity and cold rolling continues until the finished cold-rolled thickness is reached. After cleaning and hard slitting, the cold-rolled strip is subjected to finished product recrystallization annealing to obtain a first surface fine grain region, a central grain region, and a second surface fine grain region that are distributed sequentially along the thickness direction of the strip.

[0010] Preferably, the components of the finished strip, by mass percentage, include Al ≥ 99.70%, Si ≤ 0.05%, Fe 0.11%–0.18%, Cu ≤ 0.01%, Mn ≤ 0.003%, Mg ≤ 0.01%, Zn ≤ 0.03%, Cr ≤ 0.003%, B ≤ 0.006%, V ≤ 0.002%, Ti ≤ 0.002%, and the total amount of other unavoidable impurities ≤ 0.015%, with any single unavoidable impurity < 0.003%, and the balance being Al; the clean aluminum cold material accounts for 50%–60% of the total mass of the electrolytic aluminum liquid and the clean aluminum cold material, and the temperature of the aluminum melt after melting the clean aluminum cold material is 730–750℃.

[0011] Preferably, the boron-containing reaction trapping layer comprises a first limiting layer, a boron-containing porous reaction layer, and a second limiting layer arranged along the flow direction of the aluminum melt. The boron-containing porous reaction layer comprises an open-pore alumina ceramic framework and AlB distributed on the surface of the pores of the open-pore alumina ceramic framework. 12 The particles, the first limiting layer and the second limiting layer are both aluminum-resistant melt ceramic porous structures, and the terminal retention layer is set downstream of the second limiting layer and spaced apart from the boron-containing porous reaction layer.

[0012] Preferably, the temperature of the aluminum melt entering the boron-containing reaction capture layer is 720-745°C. The theoretical boron reaction load for the current furnace is determined based on the mass of the aluminum melt at the inlet of the reaction capture and purification unit, the mass fraction of V, and the mass fraction of Ti. The design effective boron capacity for the current furnace is determined based on the theoretical boron reaction load, the reaction margin coefficient, and the effective boron utilization rate of the boron-containing reaction capture layer. The reaction margin coefficient is 1.10-1.30.

[0013] Preferably, the reaction capture and purification unit includes a first reaction capture module and a second reaction capture module that are switched and connected to each other. The theoretical boron reaction load of each furnace of aluminum melt processed by the same reaction capture module is accumulated. When the accumulated theoretical boron reaction load reaches 80% of the maximum stable theoretical boron reaction load of the reaction capture module, a pre-replacement state is recorded. When the accumulated theoretical boron reaction load reaches 90% of the maximum stable theoretical boron reaction load of the reaction capture module, the aluminum melt flow path is switched to another reaction capture module.

[0014] Preferably, the purified aluminum melt enters a twin-roll mill at 690–720°C to form a cast-rolled strip with a thickness of 6–8 mm. The cast-rolled strip is then thinned to 1.00–1.20 mm by a first-stage cold rolling process with the same surface linear velocity of the upper and lower work rolls. The intermediate recrystallization annealing temperature is 550–590°C, and the holding time is 1.5–2.5 h.

[0015] Preferably, in the first differential speed cold rolling, the ratio of the surface linear velocity of the upper work roll to the surface linear velocity of the lower work roll is 1.05 to 1.20, and in the second differential speed cold rolling, the ratio of the surface linear velocity of the lower work roll to the surface linear velocity of the upper work roll is 1.05 to 1.20. After completing the first and second differential speed cold rolling, the strip is thinned to 0.50 mm by cold rolling with the same surface linear velocity of the upper and lower work rolls. The cleaned 0.50 mm hard strip is cut into widths of 100 to 300 mm, and the recrystallization annealing temperature of the finished product is 450 to 490°C, with a holding time of 3 to 4 hours.

[0016] Preferably, an aluminum and aluminum alloy strip comprises, by mass percentage: Al ≥ 99.70%, Si ≤ 0.05%, Fe 0.11%–0.18%, Cu ≤ 0.01%, Mn ≤ 0.003%, Mg ≤ 0.01%, Zn ≤ 0.03%, Cr ≤ 0.003%, B ≤ 0.006%, V ≤ 0.002%, Ti ≤ 0.002%, and the remaining unavoidable impurities ≤ 0.015%. The single unavoidable impurity is <0.003%, with the balance being Al; the aluminum and aluminum alloy strip has a first surface fine grain region, a central grain region, and a second surface fine grain region along the thickness direction. The thickness of one side of the first surface fine grain region and the second surface fine grain region accounts for 15% to 30% of the total thickness of the aluminum and aluminum alloy strip, respectively. The average grain size of the first surface fine grain region and the second surface fine grain region is 50 to 80 μm, respectively, and the average grain size of the central grain region is 100 to 200 μm.

[0017] Preferably, an aluminum melt reaction capture and purification device includes an inlet flow stabilizing cavity, a flow distribution plate, a boron-containing reaction capture layer, a transition buffer cavity, a terminal interception layer, and an outlet flow collecting cavity, which are sequentially connected along the flow direction of the aluminum melt. The boron-containing reaction capture layer includes a first limiting layer, a boron-containing porous reaction layer, and a second limiting layer. The boron-containing porous reaction layer includes an open-pore alumina ceramic skeleton and AlB distributed on the surface of the pores of the open-pore alumina ceramic skeleton. 12 The particles, the first limiting layer, the second limiting layer and the terminal retention layer are all porous aluminum-resistant melt ceramic structures, and the transition buffer cavity is formed between the boron-containing reaction capture layer and the terminal retention layer.

[0018] Preferably, an aluminum and aluminum alloy strip production system includes a melting furnace, a holding furnace, a reaction capture and purification unit, a twin-roll mill, a first cold rolling mill, an intermediate annealing furnace, a differential mill, a finishing mill, a cleaning and slitting unit, and a finished product annealing furnace connected in sequence. It also includes a composition detection device, a melt temperature detection device, a melt flow detection device, an upper and lower work roll speed detection device, a strip thickness detection device, a rolling force detection device, a tension detection device, and a control unit. The reaction capture and purification unit includes a first reaction capture module and a second reaction capture module capable of switching the aluminum melt flow path. The upper and lower work rolls of the differential mill are respectively connected to independent drive mechanisms.

[0019] Beneficial effects

[0020] This invention provides aluminum and aluminum alloy strips and a method for preparing the same. It has the following beneficial effects:

[0021] This invention will use AlB 12 Boron-containing reactive materials are fixed on the pore surface of the open-pore alumina ceramic skeleton, allowing V and Ti to complete boration at the confined pore reaction interface. This also allows the generated particles to remain in the reaction trapping layer and the terminal retention layer, shortening the migration path of borides from the generation site to the retention site and reducing the large-scale suspended boride load formed by phase boration throughout the furnace.

[0022] This invention does not add Ti-containing grain-refining materials after V and Ti purification. Instead, it shifts the final grain control from the melt chemical nucleation stage to the solid deformation and recrystallization stage, allowing the low Ti composition state to run through the casting, rolling and subsequent processing. It also eliminates the previous microstructure history through intermediate complete recrystallization, and then constructs a symmetrical surface energy storage distribution through two differential speed cold rolling stages in opposite directions.

[0023] The strip obtained by this invention forms recrystallized grains on both surfaces with smaller sizes than those in the central region, corresponding to the actual working condition where the two surfaces bear higher tensile and compressive strains when the thin strip is bent; the central region maintains a continuous aluminum matrix of the same material, without setting a dissimilar metal composite interface. The reaction capture module adopts cumulative V and Ti theoretical reaction load management and maintains continuous production through dual-module switching, forming an engineered production path from melt purification to finished product structure. Attached Figure Description

[0024] Figure 1 This is a flowchart illustrating the overall process flow of the method for preparing aluminum and aluminum alloy strips according to the present invention.

[0025] Figure 2 This is a schematic diagram of the reaction capture and purification unit of the present invention;

[0026] Figure 3 This is a schematic diagram of the flow path switching between the first reaction capture module and the second reaction capture module of the present invention;

[0027] Figure 4 This is a schematic diagram of the first differential speed cold rolling state of the present invention;

[0028] Figure 5 This is a schematic diagram of the second differential speed cold rolling state of the present invention;

[0029] Figure 6 This is a microstructure distribution diagram of the finished strip of the present invention along the thickness direction;

[0030] Figure 7 This is a schematic diagram illustrating the data acquisition and closed-loop process relationship in the production process of this invention. Detailed Implementation

[0031] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Specific Implementation Example 1:

[0033] like Figures 1 to 7 As shown, a method for preparing aluminum and aluminum alloy strip includes raw material preparation, low-superheat melt establishment, three-position composition detection, theoretical boron reaction load calculation, reaction capture and purification, outlet composition determination, Ti-free twin-roll casting and rolling, first-stage same-speed cold rolling, intermediate complete recrystallization, first-differential-speed cold rolling, second-reverse-differential-speed cold rolling, same-speed finishing rolling, cleaning, hard-state slitting, and finished product recrystallization. Data is linked according to heat number and coil number, and melt composition, reaction capture module status, casting and rolling data, rolling data, annealing data, and finished product inspection data are correspondingly saved.

[0034] The finished strip, by mass percentage, comprises Al ≥ 99.70%, Si ≤ 0.05%, Fe 0.11%–0.18%, Cu ≤ 0.01%, Mn ≤ 0.003%, Mg ≤ 0.01%, Zn ≤ 0.03%, Cr ≤ 0.003%, B ≤ 0.006%, V ≤ 0.002%, Ti ≤ 0.002%, with the remaining unavoidable impurities ≤ 0.015%, and any single unavoidable impurity < 0.003%, with the balance being Al. This composition system primarily targets V and Ti for reaction capture and purification, while Fe is maintained within a stable range of 0.11%–0.18%. Cu, Mn, Mg, Zn, and Cr are controlled within their respective upper limits through raw material selection and smelting management.

[0035] The molten aluminum and clean aluminum cold feed together constitute the smelting raw materials, with the clean aluminum cold feed accounting for 50% to 60% of the total metal mass. The clean aluminum cold feed uses pure aluminum scrap, trimmed scrap, or recycled material of the same grade that has undergone composition testing and meets the target composition requirements. After the molten aluminum enters the smelting furnace, the clean aluminum cold feed is added in batches. After all the raw materials have melted and homogenized, the temperature of the molten aluminum is controlled at 730 to 750°C.

[0036] The reaction capture and purification unit is located between the outlet side of the holding furnace and the casting and rolling pre-box, and includes an inlet flow stabilizing chamber, a flow distribution plate, a first limiting layer, a boron-containing porous reaction layer, a second limiting layer, a transition buffer chamber, a terminal interception layer, and an outlet flow collecting chamber. The boron-containing porous reaction layer adopts an open-pore alumina ceramic framework, AlB... 12 The particles are fixedly distributed on the surface of the through-holes. As the molten aluminum passes through the holes, V and Ti are carried by melt convection into the holes and transferred to the reaction interface on the hole walls, in the AlB reaction. 12 The adjacent regions of the reaction materials form V-containing borides and Ti-containing borides, respectively, and the generated particles are retained by the boron-containing porous reaction layer and the terminal retention layer.

[0037] After reaction capture and purification, the molten aluminum exiting the process is tested for V, Ti, and B. When the mass fractions of V, Ti, and B are not higher than 0.002%, Ti, and B respectively, the molten aluminum enters the casting and rolling process. No Ti-containing grain-refining material is added between the outlet of the reaction capture and purification unit and the roll gap of the twin-roll casting mill. The purified molten aluminum enters the twin-roll casting mill at 690–720°C and forms a cast strip with a thickness of 6–8 mm.

[0038] The cast-rolled strip is first thinned to 1.00–1.20 mm using a constant-speed cold rolling process, followed by intermediate recrystallization annealing at 550–590℃ for 2.5–3.5 hours. After intermediate annealing, the strip enters a differential-speed mill with independently driven upper and lower work rolls. First, a first-speed differential cold rolling process is performed where the upper roll's linear speed is higher than the lower roll's linear speed. Then, a second-speed differential cold rolling process is performed where the lower roll's linear speed is higher than the upper roll's linear speed. These two differential-speed stages introduce additional shear deformation into the first and second surface layers of the strip, respectively. Subsequently, the same surface linear speed is restored between the upper and lower rolls, and cold rolling continues until the strip is 0.50 mm thick.

[0039] After degreasing, washing, and drying, 0.50mm rigid strip is slit to a width of 100–300mm, and then recrystallized at 450–490℃ for 2.5–3.5 hours. The finished product forms a first surface fine-grained region, a central grain region, and a second surface fine-grained region along its thickness direction. The thickness of each of the two surface fine-grained regions accounts for 15%–30% of the total thickness, with average grain sizes of 20–80μm, respectively. The average grain size of the central grain region is 80–200μm.

[0040] The production system is sequentially configured with a melting furnace, holding furnace, reaction capture and purification unit, casting and rolling pre-box, twin-roll casting and rolling mill, first cold rolling mill, intermediate annealing furnace, differential speed rolling mill, finishing mill, cleaning and slitting unit, and finished product annealing furnace. The melting furnace and holding furnace are equipped with melt temperature detection devices. The inlet of the reaction capture and purification unit is equipped with flow rate and temperature detection devices. The upper and lower work rolls of the differential speed rolling mill are each equipped with independent drive mechanisms and speed detection devices. The cold rolling equipment is equipped with inlet thickness, outlet thickness, rolling force, inlet tension, and outlet tension detection devices. The intermediate annealing furnace and finished product annealing furnace record the furnace temperature and the representative coil metal temperature.

[0041] Each batch of raw materials entering the melting furnace is assigned a unique heat number, and after casting and rolling into coils, a coil number is created under the heat number. Raw material batch, raw material quality, raw material composition, melt three-position detection data, reaction capture module number, reaction capture module cumulative load, casting and rolling parameters, cold rolling parameters, annealing parameters, and finished product inspection results are all recorded in the corresponding heat number or coil number record. When compositional anomalies occur, tracing is performed along the melt data chain; when grain structure anomalies occur, tracing is performed along the rolling and annealing data chains.

[0042] Before the electrolytic aluminum liquid enters the furnace, its source, furnace batch, quality, temperature, and chemical composition are recorded. After clean aluminum cold stock is stored, it undergoes batch-by-batch spectral analysis, recording the contents of Al, Si, Fe, Cu, Mn, Mg, Zn, Cr, B, V, and Ti, and is stored separately according to batch. Clean aluminum cold stock entering this process is not mixed with recycled materials of unknown origin. Cold stock with severe oil content undergoes degreasing treatment before entering the furnace, and cold stock with surface water is dried before entering the furnace.

[0043] The batching list is formulated based on a clean aluminum cold charge ratio of 50%–60% of the total metal mass. The molten aluminum first enters the melting furnace, followed by batches of clean aluminum cold charge. The first batch of cold charge is controlled at 35%–45% of the total cold charge in the furnace. After the surface of the first batch of cold charge is completely wetted by the molten aluminum and begins to melt, the second batch of cold charge is added, also controlled at 35%–45% of the total cold charge in the furnace. The remaining cold charge is added as the third batch. After all the metal has melted, low-disturbance homogenization is performed. The temperatures of the main melting zone and the outlet zone are monitored separately. When the temperature difference between the two locations does not exceed 10℃ and the temperature of the main melt is between 730 and 750℃, the composition sampling stage begins.

[0044] Samples were taken from the furnace near the feed side, the middle of the furnace body, and the outlet side, and V, Ti, and B were detected using the same direct-reading spectrometer. The same sample preparation method was used for each location, and the test results were stored for each furnace. The average mass fraction of V was determined according to formula (1).

[0045]

[0046] In equation (1), The V-mean mass fraction represents the average mass fraction at three sampling locations and is a dimensionless number; character Indicates the mass fraction of an element; the superscript indicates the arithmetic mean; subscript... This represents the element vanadium; This indicates the mass fraction V at the first sampling location; This indicates the mass fraction V at the second sampling location; Indicates the mass fraction V at the third sampling location; subscript , , These represent the three sampling locations; symbols This indicates the sum of corresponding mass fractions; the horizontal fraction bar indicates the numerator divided by the denominator; the numbers... This indicates the number of sampling locations involved in the average calculation.

[0047] The average mass fraction of Ti is determined according to formula (2).

[0048]

[0049] In equation (2), This represents the average mass fraction of Ti at three sampling locations, and is a dimensionless number; character Indicates the mass fraction of an element; the superscript indicates the arithmetic mean; subscript... This represents the element titanium; , and These represent the Ti mass fractions at the first, second, and third sampling locations, respectively; subscripts. , , Indicates the sampling location number; symbol This indicates the sum of corresponding mass fractions; the horizontal fraction bar indicates the numerator divided by the denominator; the numbers... This indicates the number of sampling locations involved in the average calculation.

[0050] Determine the maximum and minimum values ​​among the three detection values ​​V and Ti, and calculate the difference between the maximum and minimum values. When the range of the three detection values ​​of V exceeds... Or the range of the three Ti detection values ​​exceeds At this point, melt homogenization continues and samples are taken again. In the formula, the coefficient... It represents 15% of the average quality score; the multiplication sign indicates the product of the coefficient and the average quality score.

[0051] Once the uniformity of the three-position composition meets the requirements, the theoretical boron reaction load is calculated based on the current furnace aluminum melt mass, average V mass fraction, and average Ti mass fraction, and the calculation formula is (3).

[0052]

[0053] In equation (3), This indicates the theoretical mass of boron (B) corresponding to the reaction of V and Ti in the diboride form during the current furnace run, in kg; Indicates quality; subscript In Represents the element boron, number Indicates the theoretical state; This indicates the total mass of molten aluminum entering the reaction capture and purification unit in the current furnace batch, in kg. This represents the molar mass of B, taken as 10.81 g / mol; This represents the molar mass of V, taken as 50.94 g / mol; This represents the molar mass of Ti, taken as 47.87 g / mol; and These represent the average mass fractions of V and Ti in the current furnace batch, respectively; (Numbers) This represents the stoichiometric coefficient of 2 mol B atoms for every 1 mol of metal atoms when forming VB2 or TiB2; parentheses indicate that two terms are summed first; symbol This indicates that V corresponds to the theoretical B demand and Ti corresponds to the theoretical B demand; the horizontal fraction bar indicates the corresponding molar mass ratio; the multiplication of adjacent characters indicates the product of the corresponding quantities.

[0054] The effective boron capacity required for the reaction capture module is determined according to equation (4).

[0055]

[0056] In equation (4), This indicates the design effective boron capacity corresponding to the current furnace batch, in kg; subscript In Represents the element boron. Indicates the design status; The reaction balance coefficient is a dimensionless number, ranging from 1.10 to 1.30; subscript... Indicates the reaction balance; The theoretical boron reaction load obtained from equation (3) is expressed in kg. The effective boron utilization rate of the boron-containing reaction trapping medium is a dimensionless number greater than 0 and not greater than 1; Greek letters Indicates utilization rate; subscript The horizontal fraction line represents the element boron; the horizontal fraction line represents the molecule. Divide by the denominator The product of adjacent characters represents the product of the reaction balance coefficient and the theoretical boron reaction load.

[0057] Effective boron utilization was obtained through calibration runs before the reaction capture module was first put into production. Aluminum melt with stable V and Ti inlet contents was selected and passed through the new reaction capture module. The mass fractions of V and Ti at the inlet and outlet, as well as the mass of aluminum melt passing through the module, were recorded. The actual reduction in V and Ti mass was converted into the actual B mass participating in the reaction according to the stoichiometric relationship between VB2 and TiB2, and then compared with the AlB content within the module. 12 The ratio of the nominal B-load mass of the reactants is used as the specification for the module at the specified temperature and flow rate. Calibration value.

[0058] The reaction capture and purification unit adopts a detachable refractory box structure. The outer shell is composed of refractory castable and an insulation layer. The interior, arranged sequentially along the aluminum melt flow direction, includes an inlet flow stabilizing cavity, a flow distribution plate, a first limiting layer, a boron-containing porous reaction layer, a second limiting layer, a transition buffer cavity, a terminal interception layer, and an outlet flow collecting cavity. The cross-sectional area of ​​the inlet flow stabilizing cavity is larger than that of the inlet flow channel. The flow distribution plate is made of alumina-based refractory ceramic plate with uniformly distributed through holes on its surface.

[0059] The first and second limiting layers utilize open-cell ceramic plates for aluminum-resistant melt, with pore sizes smaller than the overall dimensions of the boron-containing porous reaction layer while maintaining the continuity of the aluminum melt. The boron-containing porous reaction layer employs an open-cell alumina foam ceramic framework, with interconnected tortuous channels within the framework. The terminal retention layer uses alumina-based filter media, with an average effective pore size smaller than the average through-pore size of the boron-containing porous reaction layer. The transition buffer chamber maintains a flow space free of solid fillers, allowing the aluminum melt leaving the boron-containing porous reaction layer to undergo lateral redistribution before entering the terminal retention layer.

[0060] In the fabrication of the boron-containing porous reactive layer, the open-cell alumina foam ceramic skeleton is first subjected to dust removal and drying. AlB2 with a particle size D50 of 10–45 μm is then used. 12 Powder is added to high-purity alumina sol to form a loaded slurry, AlB 12 The powder accounts for 60% to 80% of the dry solid mass. After the alumina ceramic skeleton is completely immersed in the loading slurry, it is removed and the channel is purged from one main flow direction by compressed inert gas to remove the excess slurry blocking the channel. Then it is dried at 100 to 150°C for 2 to 4 hours, and then held at 450 to 550°C for 1 to 2 hours under argon protection to complete the stabilization treatment of the loading layer.

[0061] After the treatment is completed, the mass of the reaction layer is weighed, and AlB is obtained by measuring the mass difference before and after loading. 12 Load. According to AlB 12The nominal loading mass of B is converted from the mass ratio of B, and the reaction layer number is recorded. Before assembly, all main through holes are inspected, and reaction layers with completely closed channels are not allowed to enter the production module. The first limiting layer, the boron-containing porous reaction layer, and the second limiting layer are pressed and positioned inside the refractory box. The circumferential direction of the reaction layer is sealed with aluminum-resistant ceramic fiber to prevent aluminum melt from bypassing the edge of the reaction layer.

[0062] After the new module is installed, it undergoes a stepped preheating process. The module is heated from room temperature to 300°C and held for 30 minutes, then heated to 500°C and held for 30 minutes, and finally heated to 650–700°C and maintained until it is put into use. During startup, a small amount of molten aluminum is used to wet the inlet flow stabilizing chamber, flow distribution plate, and reaction layer, and then the flow rate is gradually increased to the calibrated production flow rate, while the inlet molten aluminum temperature is maintained at 720–745°C. During the preheating process, direct contact between the low-temperature ceramic structure and the high-temperature molten aluminum is avoided to prevent excessive transient thermal stress.

[0063] After entering the boron-containing porous reaction layer through the flow distribution plate, the molten aluminum flows along the tortuous through-holes. V and Ti are carried into the pores by the aluminum melt through convection and mass transfer occurs in the adjacent regions of the pore walls. AlB 12 The load layer provides a local B reaction source under the contact conditions of the aluminum melt, and V and Ti form V-containing borides and Ti-containing borides, respectively. After the generated particles come into contact with the pore wall, they remain on the pore surface or in the pore junction area. Particles that do not remain in the reaction layer enter the transition buffer cavity with the aluminum melt and are further intercepted by the terminal interception layer.

[0064] During this process, the temperature of the molten aluminum at the inlet of the reaction layer is controlled at 720–745℃. When the temperature is below 720℃, the flow rate to the reaction capture module is stopped and the inlet melt temperature is restored. When the temperature is above 745℃, the outlet temperature of the holding furnace is reduced, and production resumes once the inlet temperature returns to the specified range. The reaction capture module is equipped with a bypass shutdown structure; in production mode, the bypass is in the closed position, and all the molten aluminum passes through the flow distribution plate and the reaction layer.

[0065] When a reaction capture module of the same specification is put into production for the first time, the rated aluminum liquid flow rate of the equipment is used as the benchmark, and four flow rates of 70%, 85%, 100%, and 115% are executed sequentially. After each flow rate has been running stably for three times the liquid replacement time inside the module, an outlet sample is taken to test V, Ti, and B. The flow rates with an outlet V mass fraction not exceeding 0.002%, Ti mass fraction not exceeding 0.002%, and B mass fraction not exceeding 0.006% are recorded as the qualified flow rate range. The mass production flow rate is the maximum flow rate within the qualified range that does not exceed the rated flow rate.

[0066] During mass production, the frequency of outlet detection is increased at the beginning of each furnace and after the current reaction capture module's cumulative load enters the pre-replacement state. If outlet V or Ti exceeds the specified upper limit and outlet B is still below the specified upper limit, the aluminum melt flow rate is reduced by one calibrated level and resampling is performed; if the re-detection still does not meet the requirements, the standby module is switched. If outlet V and Ti meet the requirements but B exceeds 0.006%, the standby module is switched directly.

[0067] When the same reaction capture module processes multiple furnaces consecutively, the cumulative theoretical boron reaction load is determined according to formula (5).

[0068]

[0069] In equation (5), Indicates the process before the same reaction capture module. The cumulative theoretical boron reaction load after each furnace cycle, in kg; Indicates cumulative reaction load; subscript Indicates the cumulative number of furnace runs; symbol This represents the summation of each term from the initial furnace batch to the current furnace batch; Indicates the furnace number in the summation; lower limit This indicates that the accumulation starts from the first furnace run; the upper limit is... This indicates the last batch that has been processed. Indicates the first The mass of molten aluminum entering the reaction capture module of the furnace, in kg; , and These represent the molar masses of B, V, and Ti, respectively. Indicates the first Average mass fraction of V in the molten aluminum at the furnace inlet; Indicates the first Average Ti mass fraction in the aluminum melt at the furnace inlet; numerical The stoichiometric coefficients of boron atoms in the diboride reaction are represented; parentheses indicate that the theoretical boron loads of V and Ti in the current furnace are added together; symbols The horizontal fraction line represents the sum of the two loads; the horizontal fraction line represents the corresponding molar mass ratio.

[0070] The maximum stable theoretical boron reaction load was determined through life calibration of modules of the same specifications. .in, This indicates the maximum cumulative theoretical boron reaction load that the module can withstand when the composition conditions of V, Ti, and B at the outlet are continuously met, in kg; subscript This represents the maximum stable value. When... achieve Establish a pre-replacement record in a timely manner; when achieve Module switching is performed on time. Coefficient and These represent 80% and 90% of the maximum stable theoretical boron reaction load, respectively; the multiplication of adjacent characters represents the product of the proportionality coefficient and the maximum stable theoretical boron reaction load.

[0071] The liquid outlet channel of the holding furnace is divided into a first branch and a second branch. The first branch connects to the first reaction capture module, and the second branch connects to the second reaction capture module. The outlets of the two branches converge into the same casting and rolling front box. Each branch inlet is equipped with a high-temperature resistant gate. The working module maintains the production opening according to the gate, while the standby module remains closed after preheating is completed.

[0072] When the module switching conditions are met, first open the inlet gate of the standby module to the starting position, allowing a small amount of molten aluminum to enter the standby module for wetting. After the outlet aluminum liquid stabilizes, gradually increase the opening of the standby module while simultaneously decreasing the opening of the original working module until all molten aluminum is switched to the standby module. The module that has stopped working is drained of residual aluminum liquid, cooled, and then the boron-containing porous reaction layer and terminal retention layer are replaced. After preheating, it is switched to standby mode.

[0073] After the molten aluminum meets the conditions of V≤0.002%, Ti≤0.002%, and B≤0.006%, it enters the pre-casting box. No Al-Ti-B wire feeding device is installed between the outlet of the reaction capture and purification unit and the roll gap of the twin-roll casting mill, and no Al-Ti-C materials or other Ti-containing grain-refining materials are added. The temperature of the molten aluminum entering the twin-roll casting mill is controlled at 690–720℃, and the inside of the casting rolls is cooled by circulating water, forming a continuous cast strip with a thickness of 6–8 mm.

[0074] During the casting and rolling process, the inlet aluminum melt temperature, casting and rolling speed, roll gap setting, actual exit thickness, and exit temperature are recorded. If the cast and rolled strip exhibits through-thickness cracks, continuous center cracks, or shape defects preventing subsequent cold rolling, the coil is not allowed to proceed to the next normal process, and the inlet temperature, speed, and roll gap records are verified. The casting and rolling process does not involve adding Ti-containing materials to correct the microstructure.

[0075] After the cast-rolled strip is cooled to room temperature, it enters the first cold rolling mill. The upper and lower work rolls maintain the same surface linear velocity, and multiple passes of cold rolling are used to reduce the 6-8 mm strip to 1.00-1.20 mm. The reduction rate per pass is determined based on the mill's rated rolling force, strip shape, and edge condition, and is fixed in the production process card. For each pass, the entry thickness, exit thickness, rolling force, rolling speed, front tension, rear tension, and rolling oil temperature are recorded.

[0076] After the first stage of cold rolling is completed, the sheet shape and edge condition are inspected. Coils with continuous edge cracks and crack depths extending into the effective width of the finished product are discontinued for further production. Qualified coils proceed to intermediate recrystallization annealing.

[0077] The intermediate annealing temperature is set at 550–590℃, and the effective holding time is set at 1.5–2.5 hours. After the coil is placed in the furnace, it is heated according to the predetermined heating regime of the furnace type. The moment when the temperature of the coil metal reaches the set temperature range is taken as the starting point of the effective holding time. For the first batch of process calibration, thermocouples are placed in the outer, middle, and inner layers of the coil to establish the delay relationship between the furnace temperature and the actual metal temperature. During the mass production stage, the corresponding heating regime is selected according to the coil weight, coil diameter, and furnace loading method.

[0078] After annealing, cross-sectional samples are taken from the beginning, middle, and end of the coil for metallographic observation. Intermediate recrystallization is considered complete when no continuous fibrous, unrecrystallized structure is found across the field of view at any of the three locations. Coils that do not meet this condition are not allowed to proceed to differential speed cold rolling; instead, the actual metal temperature and effective holding time are rechecked.

[0079] After complete recrystallization, the strip enters a differential rolling mill with independently driven upper and lower work rolls. In the first differential cold rolling, the surface linear velocity of the upper work roll is higher than that of the lower work roll, and the first differential ratio is determined according to formula (6).

[0080]

[0081] In equation (6), The roll speed ratio represents the first differential cold rolling stage and is a dimensionless number; Greek letters. Indicates the roller speed ratio; subscript This indicates the first differential speed cold rolling stage; This indicates the surface linear velocity of the work rolls in the first differential speed cold rolling stage, in m / min; character Indicates surface linear velocity; subscript Indicates the upper working roller; This indicates the surface linear velocity of the work rolls during the first differential speed cold rolling stage, in m / min; subscript The lower work roll is indicated; the transverse fraction line represents the surface linear velocity of the upper work roll divided by the surface linear velocity of the lower work roll. First differential ratio. Set it to 1.05~1.20.

[0082] Before the first differential speed cold rolling begins, both strip surfaces are kept clean, and the rolling oil spray position and flow rate are fixed according to the process card. During production, the linear speeds of the upper and lower rollers are read in real time and the actual speed is calculated. The start and end positions of the roll length sections whose actual values ​​exceed the set range are recorded. After the first differential speed cold rolling, no annealing is performed; the strip directly enters the second differential speed cold rolling.

[0083] The second differential cold rolling reverses the fast and slow roll relationship, and the surface linear velocity of the lower work roll is higher than that of the upper work roll. The second differential ratio is determined according to formula (7).

[0084]

[0085] In equation (7), The roll speed ratio represents the second differential cold rolling stage and is a dimensionless number; Greek letters. Indicates the roller speed ratio; subscript This indicates the second differential speed cold rolling stage; This indicates the surface linear velocity of the work roll during the second differential cold rolling stage, in m / min. This indicates the surface linear velocity of the work rolls in the second differential cold rolling stage, in m / min; character Indicates surface linear velocity; subscript and These represent the lower and upper work rolls, respectively; the transverse fraction line represents the surface linear velocity of the lower work roll divided by the surface linear velocity of the upper work roll. Second differential speed ratio. Set it to 1.05~1.20.

[0086] The first and second differential speed cold rolling processes use the same or adjacent roll speed ratios, and the single-pass reduction rate for both stages is determined by the initial product calibration. The first differential speed stage introduces additional shear deformation into the first surface layer, while the second differential speed stage introduces additional shear deformation in the opposite direction into the second surface layer. After both stages, the process transitions to thickness-setting cold rolling with the upper and lower rolls operating at the same speed.

[0087] When developing a product of the same specification for the first time, four sets of coils were obtained from the same heat and the same intermediate annealing batch, using four roll speed ratios of 1.05, 1.10, 1.15, and 1.20 respectively. The first and second differential speed ratios of each set were the same, the fast roll in the first stage was the upper work roll, and the fast roll in the second stage was the lower work roll; the total reduction in the differential speed stages of each set remained the same, and the final thickness after finishing rolling at the same speed was 0.50 mm, and the final annealing process remained consistent.

[0088] After final annealing, grain size was measured layer by layer from both surfaces towards the center. Regions with a continuous average grain size in the range of 20–80 μm were designated as the surface fine-grained zone. When the thickness of the fine-grained zone on one side was less than 15% of the total thickness, the differential speed ratio or the reduction amount during the differential speed stage was increased in the next calibration group; when the thickness of the fine-grained zone on one side was more than 30% of the total thickness, the differential speed ratio or the reduction amount during the differential speed stage was decreased in the next calibration group. Finally, the parameter group where both surface layers fell within the 15%–30% thickness range and the central grain size was between 80 and 200 μm was selected as the parameters for the mass production process card.

[0089] After completing the bidirectional differential cold rolling, the upper and lower work rolls are adjusted to the same surface linear speed and cold rolling continues to 0.50 mm. The total cold rolling rate from the intermediate annealing to the finished cold-rolled thickness of 0.50 mm is determined according to formula (8).

[0090]

[0091] In equation (8), This indicates the total cold rolling percentage from intermediate annealing to the finished cold-rolled thickness, expressed as %; character Indicates processing rate; subscript Indicates the final cold rolling stage; This indicates the strip thickness after intermediate annealing and before the final cold rolling, in mm; character Indicates strip thickness; subscript Indicates the start of the final cold rolling process; This indicates the strip thickness after the final cold rolling process, in mm; subscript Indicates the final state of cold rolling; symbol The horizontal fraction bar represents the difference between the initial and final thicknesses; the horizontal fraction bar represents the thickness difference divided by the initial thickness; the symbol... Represents multiplication; numbers With symbols This indicates that the dimensionless thickness variation ratio is converted to a percentage. When and hour, It is 50%.

[0092] 0.50mm cold-rolled coils are kept in a hardened state before entering the continuous degreasing and cleaning line. First, an alkaline degreasing solution is used to remove rolling oil, followed by a two-stage rinsing with industrial water. Finally, surface free water is removed by squeezing rollers and a hot air drying device. After cleaning, the coils are inspected by wiping with a white cloth; if no visible oil film residue appears in the continuously wiped areas, they proceed to the slitting process.

[0093] The slitting width is set to 100–300 mm, and the slitting equipment operates in a rigid coil state. After slitting, the edge burrs, coil shape, and surface indentations are inspected. Qualified coils proceed to the finished product annealing process. Slitting is completed before finished product annealing to prevent 0.50 mm completely soft coils from passing through the multi-roll slitting equipment again.

[0094] The finished product annealing temperature is set at 450–490℃, and the effective holding time is set at 1.5–2.5 hours. The initial process calibration uses 480℃ and 2 hours as the core conditions. Similar to intermediate annealing, the effective holding time is taken as the point at which the temperature of the coil metal enters the set temperature range. After annealing, the temperature is lowered to below 100℃ according to the predetermined cooling regime of the furnace type before being removed from the furnace.

[0095] The first and second surface layers form higher additional deformation energy storage in the two preceding differential speed stages, while the central region does not experience the same degree of additional shear. After uniform annealing, the two surface layers form a higher recrystallization nucleation density, while the central region forms a lower recrystallization nucleation density, ultimately establishing a fine-grained region in the first surface layer, a central grain region, and a fine-grained region in the second surface layer.

[0096] For a 0.50mm finished strip, the first surface fine-grained region extends 0.075–0.150mm inward from the first surface, and the second surface fine-grained region extends 0.075–0.150mm inward from the second surface. The average grain size of the two surface fine-grained regions is 20–80μm, and the average grain size of the central grain region is 80–200μm. All three regions belong to the same continuous aluminum substrate, and no dissimilar metal composite layer is provided.

[0097] Grain size analysis was performed using metallographic samples of the strip cross-section. Measurement areas were established at the first surface, a position 0.10 mm from the first surface, the thickness center, a position 0.10 mm from the second surface, and the second surface. At least three non-overlapping fields of view were selected for each area, and grain size was statistically analyzed using the cross-section method or the area method. Samples were taken from the beginning, middle, and end of the roll. Conductivity, tensile properties, thickness, width, and chemical composition were tested using corresponding production inspection equipment. Finished product criteria included conductivity not less than 61% IACS, elongation not less than 30%, V ≤ 0.002%, Ti ≤ 0.002%, B ≤ 0.006%, and an average grain size of not more than 200 μm across the entire cross-section.

[0098] When the strip is used in a flexible conductive connection structure, the engineering strain of the outer surface is estimated based on the finished product thickness and the designed inner bending radius, and the calculation formula is (9).

[0099]

[0100] In equation (9), Represents the bending engineering strain of the outermost surface of the strip, a dimensionless number; Greek letter Indicates engineering strain; subscript Indicates the position of the strip surface; This indicates the thickness of the strip, in mm. This indicates the inner surface bending radius of the strip after bending, in mm; (numerical value) This represents the geometric coefficient formed when half the thickness is distributed from the neutral position to both sides of the surface; symbol express and Add them together; the horizontal fraction bar represents the strip thickness divided by the corresponding outer surface diameter increment. This formula serves as the design input for different product bending conditions, while actual assembly verification still uses physical bending tests with a specified radius.

[0101] The raw material data comes from the weighing records and spectral detection records before entering the furnace. The data includes the mass of the electrolytic aluminum liquid, the mass of the cold material, the raw material temperature, and the content of each major element. The data is used in the batching of the furnace and the initial V and Ti load judgment. The melt data comes from the three-position spectral detection and temperature detection device. The data is used in the calculation of equations (1) to (4). The purification data comes from the module number record, melt flow detection, inlet temperature detection, and outlet composition detection. The data is used in the module flow adjustment and the cumulative load calculation of equation (5).

[0102] The casting and rolling data comes from the casting and rolling mill control system, including the aluminum melt inlet temperature, casting and rolling speed, roll gap, exit thickness, and exit temperature. The cold rolling data comes from the mill speed encoder, thickness detection device, rolling force sensor, and tension detection device. The actual linear speeds of the upper and lower rolls are substituted into equations (6) and (7) respectively to verify the true differential speed ratio. The annealing data comes from the furnace temperature record and the thermocouple record representing the coil. The finished product data comes from spectral analysis, conductivity, tensile testing, metallographic analysis, and dimensional inspection.

[0103] All data are linked by furnace number and roll number. When the finished product conductivity is lower than the specified value and the grain structure meets the requirements, the raw material composition, V, Ti, B and Fe, Si records before and after purification are checked; when the finished product composition meets the requirements but the thickness of the two surface fine grain zones deviates from the set range, the first differential speed ratio, the second differential speed ratio, the differential speed stage reduction and finished product annealing data are checked; when the two surface structures are asymmetrical, the actual linear speed of the upper and lower rollers, the lubrication status of the two surfaces and the front and rear tension data are checked. Specific Implementation Example 2:

[0105] This embodiment focuses on the production of flexible conductive connecting strips for electrolytic aluminum baths. The total metal mass of a single furnace is 10,000 kg, with a target thickness of 0.50 mm and a target width of 200 mm. The batching consists of 4,500 kg of molten electrolytic aluminum and 5,500 kg of clean aluminum cold charge, with the clean aluminum cold charge comprising 55% of the total. After the molten electrolytic aluminum enters the melting furnace, the clean aluminum cold charge is added in three batches according to the feeding sequence described in this instruction manual. After complete melting and homogenization, the temperature of the main melt is controlled at 740°C.

[0106] Three-position spectral detection yielded V mass fractions of 0.0041%, 0.0039%, and 0.0040%, and Ti mass fractions of 0.0031%, 0.0029%, and 0.0030%, respectively. These were obtained according to equations (1) and (2). , The ranges of V and Ti at all three locations did not exceed 15% of their corresponding average values, and were therefore included in the reaction loading calculation.

[0107] The total mass of V in this furnace is 0.40 kg, and the total mass of Ti is 0.30 kg. According to formula (3), the theoretical mass of B corresponding to V is 0.170 kg, and the theoretical mass of B corresponding to Ti is 0.135 kg. The theoretical boron reaction load... It is 0.305 kg. Reaction balance coefficient. The effective boron utilization rate is set to 1.20, based on the initial calibration of the production line. Substituting into equation (4), the remaining effective boron capacity is selected to be no less than The working module.

[0108] The working module has been preheated to 650–700℃ according to a stepped heating system. Molten aluminum at 740℃ enters the working module via a holding furnace, with the inlet temperature maintained at 720–745℃. The initial flow rate is 85% of the module's rated flow rate. The molten aluminum passes through the inlet flow stabilizing chamber, flow distribution plate, boron-containing porous reaction layer, transition buffer chamber, and terminal interception layer before entering the outlet collecting chamber. After outlet sampling and testing to ensure V ≤ 0.002%, Ti ≤ 0.002%, and B ≤ 0.006%, the furnace is then... Included in work module .

[0109] After the purified aluminum molten metal enters the pre-casting box, no Ti-containing grain-refining material is added. It enters a twin-roll casting mill at 705℃ and is cast to form a 7.0mm strip. After cooling, the cast-rolled coil is thinned to 1.00mm using multi-pass cold rolling at the same speed on both the upper and lower rolls. It then undergoes effective intermediate recrystallization annealing at 580℃ for 2 hours. After intermediate annealing, samples are taken from the coil head, middle, and tail to confirm that there is no continuous fibrous non-recrystallized structure in the cross-section before it enters differential rolling.

[0110] The first differential speed cold rolling adopts The upper work roll is a fast roll; the second differential speed cold rolling mill adopts... The lower work roll is a fast roll. The single-pass reduction rate for the two differential speed stages uses the differential speed parameter calibration value pre-completed by the mill. After the two stages are completed, the same surface linear velocity is restored for both the upper and lower work rolls, and the strip is further cold-rolled to 0.50 mm. The 0.50 mm hard coil is degreased, washed, dried, and then slit to a width of 200 mm, followed by effective finished product annealing at 480℃ for 2 hours.

[0111] Samples are taken from the head, middle and tail of the finished coil, and chemical composition, electrical conductivity, tensile property and cross-sectional grain detection are performed. The product release conditions are set as V≤0.002%, Ti≤0.002%, B≤0.006%, electrical conductivity ≥61%IACS, elongation ≥30%, the single-side thickness of the two surface fine grain zones accounts for 15% to 30% of the total thickness, the average grain size of the two surface fine grain zones is 20 to 80μm, and the average grain size of the central grain zone is 80 to 200μm. The actual detected values are recorded in the quality record corresponding to the coil number. If any release condition is not met, the product shall not be dispatched as a qualified product of this specification.

[0112] When the finished product is used for flexible conductive connections of electrolytic aluminum cells, the 200mm wide strip is cut according to the designed length of the connection structure and stacked. According to the minimum inner bending radius given by the actual connection structure and the finished product thickness , the outer surface bending engineering strain is calculated using formula (9), and assembly bending verification is carried out with the same inner bending radius. The surface inspection results after bending verification are archived together with the coil number, cross-sectional grain data and differential speed rolling parameters, so as to form a traceability relationship between material manufacturing parameters and actual service conditions.

[0113] To verify the process difference between the reaction capture purification process and the traditional whole-furnace boriding route, two groups of test batches are separated from the aluminum melt of the same source. The first group adopts the treatment route of adding Al-B to the whole furnace before entering the filter medium, and the second group adopts the treatment route of the reaction capture module of the present invention. The inlet V, Ti, B, outlet V, Ti, B, the pressure difference change before and after filtration, and the consumption of boron-containing material corresponding to per unit mass of aluminum melt are recorded for the two groups respectively. The comparison data is used to establish the and , and no improvement percentage is preset based on unobtained experimental results.

[0114] To verify the formation mechanism of the double surface layer structure, three groups of coil segments are obtained from the strip of the same furnace batch and the same intermediate annealing state. The first group adopts cold rolling with upper and lower rolls at the same speed throughout the whole process, the second group only adopts the first differential speed cold rolling, and the third group sequentially adopts the first differential speed cold rolling and the second reverse differential speed cold rolling. All three groups are processed with the same final thickness and the same finished product annealing system. After annealing, the grain size is measured along the thickness direction, the grain distribution of the two surface layers and the central region of the three coil segments is compared, and the mass production differential speed parameters are determined in combination with the bending test of the specified radius.

[0115] When V or Ti at the outlet of the reaction capture purification exceeds the specified upper limit, first check whether the inlet temperature is within 720 to 745℃ and whether the current module has reached the pre-replacement interval. If the inlet temperature meets the requirements and is lower than If the flow rate is reduced by one calibrated level and retested, and still exceeds the specified upper limit after retesting, switch to the backup module. If the flow rate at outlet B exceeds 0.006%, stop the liquid supply of the current module and switch to the backup module.

[0116] When continuous central cracks or sheet shape defects preventing subsequent cold rolling occur during casting and rolling, verify the casting and rolling inlet temperature, linear speed, roll gap, and outlet thickness, without correcting them by adding Ti-containing grain-refining materials. If continuous non-recrystallized fibrous structures exist after intermediate annealing, re-verify the actual metal temperature and effective holding time. If the thickness difference between the two surface fine-grained zones of the finished product exceeds the range specified in the production process card, verify the actual differential speed ratio, lubrication flow rate, inlet tension, and outlet tension twice; if the central grain size exceeds 200 μm, verify the final total machining rate and the actual annealing temperature of the finished metal.

[0117] This invention controls the sources of V and Ti from the melt end on the electrolytic aluminum bath conductive connecting strip production line. A boron-containing porous reaction layer fixes the boration sites of transition elements at the pore interface, and particle retention is completed within the same purification unit. No Ti is added after purification, maintaining the low-Ti chemical state until the cast and rolled strip. Subsequently, a first-stage same-speed cold rolling and intermediate complete recrystallization remove the cast and rolled microstructure and large deformation history. Then, bidirectional differential-speed cold rolling incorporates the additional deformation energy stored in the two surface layers into the material. Finally, recrystallization of the finished product converts the energy storage difference into a difference in grain size along the thickness direction.

[0118] This application process establishes a clear causal chain of material states before and after the process: reaction capture and purification establish a low-V, low-Ti melt state; prohibiting Ti addition maintains a low-Ti state; complete recrystallization in the middle establishes a unified solid-state microstructure starting point; double-sided reverse differential rolling establishes a symmetrical energy storage state; and finished product recrystallization transforms the energy storage state into a double-surface fine-grained structure. The entire method does not rely on a black-box prediction model; the core calculations are derived from mass conservation, stoichiometry, cumulative load, and rolling geometry. On-site detection data is directly used for corresponding process judgment and parameter correction.

[0119] It should be noted that, in this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising a reference structure" does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes the element.

[0120] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing aluminum and aluminum alloy strips, characterized in that, Includes the following steps: Electrolytic aluminum liquid is mixed and smelted with clean aluminum cold material to form an aluminum melt. The mass fractions of V, Ti, and B in the aluminum melt are detected. The detected aluminum melt is continuously introduced into a reaction capture and purification unit. The reaction capture and purification unit includes, in sequence along the flow direction of the aluminum melt, an inlet flow stabilization chamber, a flow distribution zone, a boron-containing reaction capture layer, a transition buffer chamber, a terminal interception layer, and an outlet flow collection chamber. The boron-containing reaction capture layer includes a porous alumina framework and AlB disposed within the channels of the porous alumina framework. 12 In a boron-containing reactive material, V and Ti in the aluminum melt react with B in the boron-containing reaction trapping layer to form V-containing boride and Ti-containing boride, respectively. These V-containing boride and Ti-containing boride remain within the boron-containing reaction trapping layer and the terminal retention layer. The aluminum melt exiting the reaction trapping and purification unit is subjected to compositional analysis. Under the condition that the mass fraction of V is not higher than 0.002%, the mass fraction of Ti is not higher than 0.002%, and the mass fraction of B is not higher than 0.006%, the aluminum melt is fed into a twin-roll mill. No Ti-containing grain-refining material is added between the reaction trapping and purification unit and the twin-roll mill to form a cast-rolled strip. The cast-rolled strip... After the billet undergoes the first stage of cold rolling at the same speed, intermediate recrystallization annealing is performed. The strip after intermediate recrystallization annealing is then subjected to first differential speed cold rolling and second differential speed cold rolling in sequence. In the first differential speed cold rolling, the surface linear velocity of the upper work roll is greater than that of the lower work roll, and in the second differential speed cold rolling, the surface linear velocity of the lower work roll is greater than that of the upper work roll. After the second differential speed cold rolling is completed, the upper and lower work rolls are restored to the same surface linear velocity and cold rolling continues until the finished cold-rolled thickness is reached. After cleaning and hard slitting, the cold-rolled strip is subjected to finished product recrystallization annealing to obtain a first surface fine grain region, a central grain region, and a second surface fine grain region that are distributed sequentially along the thickness direction of the strip.

2. The method for preparing aluminum and aluminum alloy strips according to claim 1, characterized in that, The components of the finished strip, by mass percentage, include Al ≥ 99.70%, Si ≤ 0.05%, Fe 0.11%–0.18%, Cu ≤ 0.01%, Mn ≤ 0.003%, Mg ≤ 0.01%, Zn ≤ 0.03%, Cr ≤ 0.003%, B ≤ 0.006%, V ≤ 0.002%, Ti ≤ 0.002%, and the total amount of other unavoidable impurities ≤ 0.015%, with any single unavoidable impurity < 0.003%, and the balance being Al; the clean aluminum cold material accounts for 50%–60% of the total mass of the electrolytic aluminum liquid and the clean aluminum cold material, and the temperature of the aluminum melt after melting the clean aluminum cold material is 730–750℃.

3. The method for preparing aluminum and aluminum alloy strips according to claim 1, characterized in that, The boron-containing reaction trapping layer comprises a first limiting layer, a boron-containing porous reaction layer, and a second limiting layer arranged along the flow direction of the aluminum melt. The boron-containing porous reaction layer comprises an open-pore alumina ceramic framework and AlB distributed on the surface of the pores of the open-pore alumina ceramic framework. 12 The particles, the first limiting layer and the second limiting layer are both porous aluminum-resistant melt ceramic structures, and the terminal retention layer is set downstream of the second limiting layer and spaced apart from the boron-containing porous reaction layer.

4. The method for preparing aluminum and aluminum alloy strips according to claim 3, characterized in that, The temperature of the aluminum melt entering the boron-containing reaction trapping layer is 720-745℃. The theoretical boron reaction load for the current furnace is determined based on the mass of the aluminum melt at the inlet of the reaction trapping and purification unit, the mass fraction of V, and the mass fraction of Ti. The design effective boron capacity for the current furnace is determined based on the theoretical boron reaction load, the reaction margin coefficient, and the effective boron utilization rate of the boron-containing reaction trapping layer. The reaction margin coefficient is 1.10-1.

30.

5. The method for preparing aluminum and aluminum alloy strips according to claim 4, characterized in that, The reaction capture and purification unit includes a first reaction capture module and a second reaction capture module that are switched and connected to each other. The theoretical boron reaction load of each furnace of aluminum melt processed by the same reaction capture module is accumulated. When the accumulated theoretical boron reaction load reaches 80% of the maximum stable theoretical boron reaction load of the reaction capture module, a pre-replacement state is recorded. When the accumulated theoretical boron reaction load reaches 90% of the maximum stable theoretical boron reaction load of the reaction capture module, the aluminum melt flow path is switched to another reaction capture module.

6. The method for preparing aluminum and aluminum alloy strips according to claim 1, characterized in that, The purified aluminum melt enters a twin-roll mill at 690–720°C and forms a cast-rolled strip with a thickness of 6–8 mm. The cast-rolled strip is then thinned to 1.00–1.20 mm by a first-stage cold rolling process with the same surface linear speed of the upper and lower work rolls. The intermediate recrystallization annealing temperature is 550–590°C and the holding time is 1.5–2.5 h.

7. The method for preparing aluminum and aluminum alloy strips according to claim 6, characterized in that, In the first differential speed cold rolling, the ratio of the surface linear velocity of the upper work roll to that of the lower work roll is 1.05 to 1.

20. In the second differential speed cold rolling, the ratio of the surface linear velocity of the lower work roll to that of the upper work roll is 1.05 to 1.

20. After completing the first and second differential speed cold rolling, the strip is thinned to 0.50 mm by cold rolling with the same surface linear velocity of the upper and lower work rolls. The cleaned 0.50 mm hard strip is cut into widths of 100 to 300 mm. The recrystallization annealing temperature of the finished product is 450 to 490 °C, and the holding time is 3 to 4 hours.

8. An aluminum and aluminum alloy strip, characterized in that, The aluminum and aluminum alloy strip comprises, by mass percentage, Al ≥ 99.70%, Si ≤ 0.05%, Fe 0.11%–0.18%, Cu ≤ 0.01%, Mn ≤ 0.003%, Mg ≤ 0.01%, Zn ≤ 0.03%, Cr ≤ 0.003%, B ≤ 0.006%, V ≤ 0.002%, Ti ≤ 0.002%, and the total amount of unavoidable impurities ≤ 0.015%, with any single unavoidable impurity < 0.003%, and the balance being Al. The aluminum and aluminum alloy strip has, along its thickness direction, a first surface fine-grained region, a central grain region, and a second surface fine-grained region. The thickness of one side of the first and second surface fine-grained regions accounts for 15%–30% of the total thickness of the aluminum and aluminum alloy strip, respectively. The average grain size of the first and second surface fine-grained regions is 50–80 μm, respectively, and the average grain size of the central grain region is 100–200 μm.