A cold-pressed sintered BiSbTe-based thermoelectric material and its preparation method
High-performance BiSbTe-based thermoelectric materials were prepared by cold pressing sintering and CsCl doping, which solved the problems of high cost and supply chain instability of existing BiSbTe materials. The materials achieved high conductivity and Seebeck coefficient optimization, improved room temperature ZT value, and are suitable for consumer electronics and low-grade waste heat recovery scenarios.
Patent Information
- Application Number
- CN202611208852.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing processes for preparing BiSbTe-based thermoelectric materials suffer from high costs, complexity, and supply chain instability, making it difficult to achieve low-cost, large-scale production and performance improvement.
CsCl-doped BiSbTe-based thermoelectric materials were prepared by using a cold pressing sintering process, introducing a specific stoichiometric ratio of CsCl as a dopant phase into Bi, Sb, and Te elemental raw materials, and combining a complete process of melt water quenching, wet ball milling, and segmented sintering.
This study achieves an optimized balance between high electrical conductivity and Seebeck coefficient in BiSbTe-based thermoelectric materials, improves room temperature ZT value, reduces production costs, and solves the problems of insufficient precise temperature control and conversion efficiency of traditional BiSbTe materials at room temperature. It has the potential to replace commercial Bi2Te3-based materials.
Smart Images

Figure CN123108347A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of thermoelectric materials technology, specifically to a cold-pressed sintered BiSbTe-based thermoelectric material and its preparation method. Background Technology
[0002] Thermoelectric materials enable the conversion between thermal and electrical energy, showing significant application potential in fields such as industrial waste heat recovery power generation and solid-state refrigeration. Their conversion efficiency is determined by the dimensionless thermoelectric figure of merit (ZT), calculated using the following formula: Where S is the Seebeck coefficient, σ is the electrical conductivity, κ is the thermal conductivity, and T is the Kelvin temperature. σ and S together determine the electrical transport properties of the material, and are usually combined and referred to as the power factor PF. The total thermal conductivity κ can be decomposed into lattice thermal conductivity. Carrier thermal conductivity Bipolar thermal conductivity The sum of the three parts.
[0003] at present, With its excellent thermoelectric figure of merit, the base material is the mainstream system that has taken the lead in completing the full-chain technology implementation and has the highest commercial maturity in the room temperature thermoelectric field. It has achieved large-scale mass production applications in scenarios such as consumer electronics refrigeration and industrial low-temperature waste heat recovery. The two core branches under this system show stable differentiation in conductivity characteristics: BiSbTe (BST) material often exhibits p-type characteristics, while BiTeSe (BTS) material often exhibits n-type characteristics.
[0004] Currently, the main technical approaches to improving the performance of thermoelectric materials fall into two categories: enhancing electrical transport properties and reducing thermal conductivity. However, there is a strong coupling relationship between thermal and electrical properties; for example, increasing electrical conductivity σ will affect carrier thermal conductivity. The simultaneous improvement of thermal and electrical properties, leading to an increase in conductivity κ, limits the improvement of ZT values. The search for a method to effectively decouple the thermal and electrical properties of materials, enabling independent control or synergistic optimization of these properties, is crucial for current research. Further improvements in the performance of the base material are of great significance.
[0005] Alkali metal doping is currently a proven and effective technical route for decoupling thermoelectric properties, and various schemes such as elemental doping, telluride doping, halide doping, and Trojan doping have been developed in the industry. Among them, elemental and telluride doping schemes have problems such as high operation threshold, high safety risks, and easy introduction of oxygen pollution, making them difficult to adapt to the requirements of large-scale and standardized industrial production; while Trojan doping has a complex process and cannot meet the needs of simple, low-cost, and scalable mass production.
[0006] Alkali metal halide doping has become the most promising doping route for industrialization due to its significant advantages such as low oxygen introduction risk, high doping amount, controllable precision, and simple and safe process. However, existing alkali metal halide doping schemes still face obstacles to industrialization: for example, although CsBr-doped BiSbTe can achieve a ZT value of up to 1.2 at 323K, its preparation relies on discharge plasma sintering, which has extremely high equipment costs and technical barriers, making it impossible to support large-scale production and promotion; at the same time, the acquisition of Br-based raw materials is highly dependent on geographical location, and the supply chain is not stable enough. The industry still needs to develop alkali metal chloride doping alternatives that are more suitable for mass production needs. Summary of the Invention
[0007] This invention aims to overcome the shortcomings of the prior art and provide a cold-pressed sintered BiSbTe-based thermoelectric material and its preparation method.
[0008] To achieve the above objectives, the present invention provides the following technical solution:
[0009] In a first aspect, the present invention provides a method for preparing a cold-pressed sintered BiSbTe-based thermoelectric material, comprising the following steps:
[0010] S1. Weigh Bi, Sb, and Te elemental powders with a purity of 4N and 60 mesh, along with CsCl powder, precisely according to the molar ratio of Bi:Sb:Te:CsCl 1:3:6:2x, where the value of x ranges from 0.005 to x ≤ 0.015.
[0011] S2. Place all the raw materials weighed in step S1 into a mortar and grind them until they are evenly mixed. Then, vacuum seal the mixed powder in a quartz test tube.
[0012] S3. Place the sealed quartz test tube obtained in step S2 into a tube furnace and heat it until it melts, so that the raw material forms a uniform melt. After holding it at the temperature, immerse the entire quartz test tube in deionized water at room temperature for water quenching. After breaking the tube, an alloy ingot is obtained.
[0013] S4. After the alloy ingot obtained in step S3 is initially crushed, it is subjected to wet ball milling to refine the alloy powder with the target particle size. Then, the powder is dried under an inert gas protective atmosphere and cooled to obtain the refined alloy powder.
[0014] S5. The refined alloy powder obtained in step S4 is loaded into a mold and cold-pressed and densified by a tablet press to obtain a cold-pressed preform.
[0015] S6. Place the cold-pressed preform obtained in step S5 into a tube furnace, and complete the sintering and heat preservation by segmented heating. Finally, let it cool naturally to room temperature with the furnace to obtain the CsCl-doped BiSbTe-based thermoelectric material.
[0016] Furthermore, in step S2, the mixed powder is vacuum-sealed in a quartz test tube, with a vacuum degree of [missing information]. Pa.
[0017] Furthermore, in step S3, after placing the sealed quartz test tube into the tube furnace, the temperature is increased to 700-800℃ at a heating rate of 5-10℃ / min, and held at that temperature for 10 hours.
[0018] Furthermore, in step S4, the wet ball milling uses anhydrous ethanol as the grinding medium, the ball milling speed is 300 r / min, the ball milling time is 60 min, the ball-to-material ratio is 10:1, and the medium-to-material ratio is 1:1. After ball milling, alloy powder with a particle size of 10~30 μm is obtained.
[0019] Furthermore, in step S4, the drying process is carried out under an Ar atmosphere, with the temperature increased to 60°C at a heating rate of 5°C / min and held for 180 min, and the Ar gas flow rate is set to 50 sccm.
[0020] Furthermore, in step S5, the pressure of the cold pressing densification process is set to 100 MPa, and the holding time is 60 min.
[0021] Furthermore, in step S6, the segmented heating curve of the tubular furnace is as follows: the temperature is increased to 300°C at a rate of 2°C / min, then increased to 400°C at a rate of 5°C / min and held for 300 min, and finally cooled naturally to room temperature with the furnace.
[0022] Secondly, the present invention provides a thermoelectric material prepared according to the above-described preparation method.
[0023] Based on the above technical solution, the embodiments of the present invention can produce at least the following technical effects:
[0024] 1. This invention introduces a specific stoichiometric ratio of CsCl as a dopant phase into a Bi, Sb, and Te elemental raw material system. Combined with a complete process design of "melt water quenching - wet ball milling - cold pressing - segmented sintering," it achieves precise control of the microstructure of thermoelectric materials without relying on high-cost discharge plasma sintering equipment. The CsCl doping control coefficient is controlled within the range of 0.005 ≤ x ≤ 0.015, achieving a temperature close to 340 Scm at room temperature in a sample with x = 0.08. -1 The high electrical conductivity was increased by 24% compared to the undoped sample, while only a slight decrease in the Seebeck coefficient was observed, achieving an optimal balance between the two core parameters of electrical transport properties. The peak power factor exceeded 22 μW·cm at room temperature of 300K. -1 ·K -2It can maintain high conductivity throughout the commonly used thermoelectric operating temperature range of 300K~425K, significantly reducing Joule heat loss of the device; ultimately, the room temperature ZT value of BiSbTe-based polycrystalline materials is stably maintained in the range of 1.17~1.21, which is not only nearly double that of the room temperature ZT of samples prepared by the traditional RbOH-doped HTS process (about 0.6), but also close to or better than the samples prepared by the currently disclosed CsBr-doped SPS and KCl-doped melt methods. It solves the industry pain points of traditional BiSbTe materials in terms of precise temperature control at room temperature and insufficient conversion efficiency. When combined with commercial Bi2Te3 materials, this material can be directly applied to the field of low-grade heat energy recovery in the room temperature range.
[0025] 2. This invention applies a cold-pressing sintering scheme to the preparation process of alkali metal-doped BiSbTe polycrystalline materials, which is completely different from the high-cost SPS sintering and supergravity remelting special processes that are commonly used in existing high-performance BiSbTe materials. Compared with traditional secondary sintering methods such as hot pressing and discharge plasma sintering, it has significant advantages such as low cost, independent and flexible control of pressure and heat effects, good process compatibility, and low threshold for industrialization. It significantly reduces the industrialization threshold while achieving high ZT at room temperature, avoids the high equipment and high environmental requirements caused by complex micro-defect control, and solves the industry problem of low-cost mass production of high-performance BiSbTe materials. It has stronger commercial competitiveness in consumer electronics micro-refrigeration and civilian low-grade waste heat recovery scenarios.
[0026] 3. This invention provides an efficient and feasible alternative to alkali metal bromide dopants: Cl is widely available as a raw material, unlike Br which has significant regional dependence, resulting in stronger supply chain stability. Furthermore, CsCl doping achieves an optimal room-temperature ZT value of 1.20, comparable to the performance of the CsBr doping system, significantly reducing the raw material procurement and supply chain risks for high-performance BiSbTe materials. The introduction of CsCl not only acts as a carrier concentration regulator, but its dissociation also generates Cl... - Ions and Cs + Ions also exert unique regulatory effects on lattice defects and phonon scattering mechanisms within the material; the electrical and thermal transport properties of the system exhibit non-monotonic and opposite variation patterns, proving that the dominant mechanisms of dopant on carrier and phonon transport differ significantly under different doping concentrations.
[0027] 4. The samples prepared in the embodiments of the present invention can maintain a high ZT value of over 1.0 in the range of 300~350K, which can fully meet the usage requirements of specific scenarios such as constant temperature precision temperature control and near room temperature operation without the need for a wide temperature range. In such targeted application scenarios, a lower overall cost can be achieved. The CsCl-doped BiSbTe-based thermoelectric material has the potential to replace the existing commercial Bi2Te3-based thermoelectric material, which is of great practical significance for promoting the industrialization and technological iteration of room temperature thermoelectric materials. Attached Figure Description
[0028] Figure 1 This is a flowchart illustrating the preparation process of the BiSbTe-based thermoelectric material according to an embodiment of the present invention.
[0029] Figure 2 Here is a photograph of the BiSbTe-based thermoelectric material prepared in Example 2 of this invention;
[0030] Figure 3 The electrical transport properties of BiSbTe-based thermoelectric materials under different CsCl doping control coefficients are shown in the figure. (a) is a comparison curve of conductivity versus temperature; (b) is a comparison curve of Seebeck coefficient versus temperature; (c) is a trend curve of carrier concentration and carrier mobility versus doping ratio at room temperature of 300K; and (d) is a comparison curve of power factor versus temperature.
[0031] Figure 4 The results show the thermal transport properties of BiSbTe-based thermoelectric materials under different CsCl doping control coefficients; (a) is a comparison curve of total thermal conductivity versus temperature; (b) is a comparison curve of carrier thermal conductivity versus temperature; and (c) is a comparison curve of the sum of lattice thermal conductivity and bipolar thermal conductivity versus temperature.
[0032] Figure 5 The thermoelectric figure of merit (ZT) results of BiSbTe-based thermoelectric materials under different CsCl doping control coefficients are shown; where (a) is a comparison curve of ZT values of all examples and comparative samples as a function of temperature; and (b) is a comparison curve of ZT values of the samples of the present invention and the published alkali metal doping research results. Detailed Implementation
[0033] To make the objectives, technical solutions, and advantages of this invention clearer, specific embodiments of this invention will be described in detail below. However, the following embodiments are only for illustrating this invention and should not be considered as limiting the scope of this invention. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention. Furthermore, the technical solutions of various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed by this invention.
[0034] Example 1:
[0035] See Figure 1 As shown, a method for preparing a cold-pressed sintered BiSbTe-based thermoelectric material includes the following steps:
[0036] S1. Weigh Bi, Sb, and Te elemental powders with a purity of 4N and 60 mesh with CsCl powder precisely according to the molar ratio of Bi:Sb:Te:CsCl 1:3:6:2x, where x is 0.005.
[0037] S2. Place all the raw materials weighed in step S1 into a mortar and grind them evenly. Then seal the mixed powder in a quartz test tube, controlling the vacuum degree inside the tube to be [value missing]. Pa;
[0038] S3. Place the sealed quartz test tube obtained in step S2 into a tube furnace and heat it to 800°C at a heating rate of 5°C / min to completely melt the raw material and form a uniform melt. After holding the temperature for 10 hours, immerse the entire quartz test tube in deionized water at room temperature for water quenching. After breaking the tube, an alloy ingot is obtained.
[0039] S4. The alloy ingot obtained in step S3 is initially crushed by hammer and then wet ball milled using anhydrous ethanol as the grinding medium. The ball milling speed is 300 r / min, the ball milling time is 60 min, the ball-to-material ratio is 10:1, and the medium-to-material ratio is 1:1, to obtain powder with a particle size distribution of 10~30 μm. After the powder settles, it is dried under an Ar protective atmosphere with a flow rate of 50 sccm, heated to 60℃ at a heating rate of 5℃ / min, and held at that temperature for 180 min. After cooling to room temperature, it is taken out to obtain refined alloy powder.
[0040] S5. The alloy powder obtained in step S4 is loaded into an alloy cylindrical mold and cold-pressed and densified by a tablet press. The cold pressing pressure is set to 100MPa and the holding time is 60min to obtain a cold-pressed preform.
[0041] S6. Place the cold-pressed preform obtained in step S5 into a tube furnace for secondary sintering. First, heat the preform to 300°C at a rate of 2°C / min, then heat it to 400°C at a rate of 5°C / min and hold it for 300 min. Finally, allow it to cool naturally to room temperature in the furnace to obtain the CsCl-doped thermoelectric material.
[0042] Example 2:
[0043] A method for preparing a cold-pressed sintered BiSbTe-based thermoelectric material includes the following steps:
[0044] S1. Weigh Bi, Sb, and Te elemental powders with a purity of 4N and 60 mesh with CsCl powder precisely according to the molar ratio of Bi:Sb:Te:CsCl 1:3:6:2x, where x is 0.008.
[0045] S2. Place all the raw materials weighed in step S1 into a mortar and grind them evenly. Then seal the mixed powder in a quartz test tube, controlling the vacuum degree inside the tube to be [value missing]. Pa;
[0046] S3. Place the sealed quartz test tube obtained in step S2 into a tube furnace and heat it to 800°C at a heating rate of 5°C / min to completely melt the raw material and form a uniform melt. After holding the temperature for 10 hours, immerse the entire quartz test tube in deionized water at room temperature for water quenching. After breaking the tube, an alloy ingot is obtained.
[0047] S4. The alloy ingot obtained in step S3 is initially crushed by hammer and then wet ball milled using anhydrous ethanol as the grinding medium. The ball milling speed is 300 r / min, the ball milling time is 60 min, the ball-to-material ratio is 10:1, and the medium-to-material ratio is 1:1, to obtain powder with a particle size distribution of 10~30 μm. After the powder settles, it is dried under an Ar protective atmosphere with a flow rate of 50 sccm, heated to 60℃ at a heating rate of 5℃ / min, and held at that temperature for 180 min. After cooling to room temperature, it is taken out to obtain refined alloy powder.
[0048] S5. The alloy powder obtained in step S4 is loaded into an alloy cylindrical mold and cold-pressed and densified by a tablet press. The cold pressing pressure is set to 100MPa and the holding time is 60min to obtain a cold-pressed preform.
[0049] S6. Place the cold-pressed preform obtained in step S5 into a tube furnace for secondary sintering. First, heat to 300℃ at a rate of 2℃ / min, then heat to 400℃ at a rate of 5℃ / min and hold for 300min. Finally, allow it to cool naturally to room temperature in the furnace to obtain the CsCl-doped thermoelectric material. Figure 2 As shown.
[0050] Example 3:
[0051] A method for preparing a cold-pressed sintered BiSbTe-based thermoelectric material includes the following steps:
[0052] S1. Weigh Bi, Sb, and Te elemental powders with a purity of 4N and 60 mesh with CsCl powder precisely according to the molar ratio of Bi:Sb:Te:CsCl 1:3:6:2x, where x is 0.01.
[0053] S2. Place all the raw materials weighed in step S1 into a mortar and grind them evenly. Then seal the mixed powder in a quartz test tube, controlling the vacuum degree inside the tube to be [value missing]. Pa;
[0054] S3. Place the sealed quartz test tube obtained in step S2 into a tube furnace and heat it to 800°C at a heating rate of 5°C / min to completely melt the raw material and form a uniform melt. After holding the temperature for 10 hours, immerse the entire quartz test tube in deionized water at room temperature for water quenching. After breaking the tube, an alloy ingot is obtained.
[0055] S4. The alloy ingot obtained in step S3 is initially crushed by hammer and then wet ball milled using anhydrous ethanol as the grinding medium. The ball milling speed is 300 r / min, the ball milling time is 60 min, the ball-to-material ratio is 10:1, and the medium-to-material ratio is 1:1, to obtain powder with a particle size distribution of 10~30 μm. After the powder settles, it is dried under an Ar protective atmosphere with a flow rate of 50 sccm, heated to 60℃ at a heating rate of 5℃ / min, and held at that temperature for 180 min. After cooling to room temperature, it is taken out to obtain refined alloy powder.
[0056] S5. The alloy powder obtained in step S4 is loaded into an alloy cylindrical mold and cold-pressed and densified by a tablet press. The cold pressing pressure is set to 100MPa and the holding time is 60min to obtain a cold-pressed preform.
[0057] S6. Place the cold-pressed preform obtained in step S5 into a tube furnace for secondary sintering. First, heat the preform to 300°C at a rate of 2°C / min, then heat it to 400°C at a rate of 5°C / min and hold it for 300 min. Finally, allow it to cool naturally to room temperature in the furnace to obtain the CsCl-doped thermoelectric material.
[0058] Example 4:
[0059] A method for preparing a cold-pressed sintered BiSbTe-based thermoelectric material includes the following steps:
[0060] S1. Weigh Bi, Sb, and Te elemental powders with a purity of 4N and 60 mesh, along with CsCl powder, precisely according to the molar ratio of Bi:Sb:Te:CsCl 1:3:6:2x, where x is 0.015.
[0061] S2. Place all the raw materials weighed in step S1 into a mortar and grind them evenly. Then seal the mixed powder in a quartz test tube, controlling the vacuum degree inside the tube to be [value missing]. Pa;
[0062] S3. Place the sealed quartz test tube obtained in step S2 into a tube furnace and heat it to 800°C at a heating rate of 5°C / min to completely melt the raw material and form a uniform melt. After holding the temperature for 10 hours, immerse the entire quartz test tube in deionized water at room temperature for water quenching. After breaking the tube, an alloy ingot is obtained.
[0063] S4. The alloy ingot obtained in step S3 is initially crushed by hammer and then wet ball milled using anhydrous ethanol as the grinding medium. The ball milling speed is 300 r / min, the ball milling time is 60 min, the ball-to-material ratio is 10:1, and the medium-to-material ratio is 1:1, to obtain powder with a particle size distribution of 10~30 μm. After the powder settles, it is dried under an Ar protective atmosphere with a flow rate of 50 sccm, heated to 60℃ at a heating rate of 5℃ / min, and held at that temperature for 180 min. After cooling to room temperature, it is taken out to obtain refined alloy powder.
[0064] S5. The alloy powder obtained in step S4 is loaded into an alloy cylindrical mold and cold-pressed and densified by a tablet press. The cold pressing pressure is set to 100MPa and the holding time is 60min to obtain a cold-pressed preform.
[0065] S6. Place the cold-pressed preform obtained in step S5 into a tube furnace for secondary sintering. First, heat the preform to 300°C at a rate of 2°C / min, then heat it to 400°C at a rate of 5°C / min and hold it for 300 min. Finally, allow it to cool naturally to room temperature in the furnace to obtain the CsCl-doped thermoelectric material.
[0066] Comparative Example 1: Includes the following steps:
[0067] S1. Weigh Bi, Sb, and Te elemental powders with a purity of 4N and 60 mesh with CsCl powder precisely according to the molar ratio of Bi:Sb:Te:CsCl 1:3:6:2x, where x is 0.02.
[0068] S2. Place all the raw materials weighed in step S1 into a mortar and grind them evenly. Then seal the mixed powder in a quartz test tube, controlling the vacuum degree inside the tube to be [value missing]. Pa;
[0069] S3. Place the sealed quartz test tube obtained in step S2 into a tube furnace and heat it to 800°C at a heating rate of 5°C / min to completely melt the raw material and form a uniform melt. After holding the temperature for 10 hours, immerse the entire quartz test tube in deionized water at room temperature for water quenching. After breaking the tube, an alloy ingot is obtained.
[0070] S4. The alloy ingot obtained in step S3 is initially crushed by hammer and then wet ball milled using anhydrous ethanol as the grinding medium. The ball milling speed is 300 r / min, the ball milling time is 60 min, the ball-to-material ratio is 10:1, and the medium-to-material ratio is 1:1, to obtain powder with a particle size distribution of 10~30 μm. After the powder settles, it is dried under an Ar protective atmosphere with a flow rate of 50 sccm, heated to 60℃ at a heating rate of 5℃ / min, and held at that temperature for 180 min. After cooling to room temperature, it is taken out to obtain refined alloy powder.
[0071] S5. The alloy powder obtained in step S4 is loaded into an alloy cylindrical mold and cold-pressed and densified by a tablet press. The cold pressing pressure is set to 100MPa and the holding time is 60min to obtain a cold-pressed preform.
[0072] S6. Place the cold-pressed preform obtained in step S5 into a tube furnace for secondary sintering. First, heat the preform to 300°C at a rate of 2°C / min, then heat it to 400°C at a rate of 5°C / min and hold it for 300 min. Finally, allow it to cool naturally to room temperature in the furnace to obtain the CsCl-doped thermoelectric material.
[0073] Comparative Example 2: A blank control group without CsCl powder. The remaining process steps were exactly the same as in Example 2, except that the CsCl component in the raw materials was removed. The process included the following steps:
[0074] S1. Weigh Bi, Sb, and Te elemental powders with a purity of 4N and a mesh size of 60 as follows: accurately according to the molar ratio of Bi:Sb:Te 1:3:6.
[0075] S2. Place all the raw materials weighed in step S1 into a mortar and grind them evenly. Then seal the mixed powder in a quartz test tube, controlling the vacuum degree inside the tube to be [value missing]. Pa;
[0076] S3. Place the sealed quartz test tube obtained in step S2 into a tube furnace and heat it to 800°C at a heating rate of 5°C / min to completely melt the raw material and form a uniform melt. After holding the temperature for 10 hours, immerse the entire quartz test tube in deionized water at room temperature for water quenching. After breaking the tube, an alloy ingot is obtained.
[0077] S4. The alloy ingot obtained in step S3 is initially crushed by hammer and then wet ball milled using anhydrous ethanol as the grinding medium. The ball milling speed is 300 r / min, the ball milling time is 60 min, the ball-to-material ratio is 10:1, and the medium-to-material ratio is 1:1, to obtain powder with a particle size distribution of 10~30 μm. After the powder settles, it is dried under an Ar protective atmosphere with a flow rate of 50 sccm, heated to 60℃ at a heating rate of 5℃ / min, and held at that temperature for 180 min. After cooling to room temperature, it is taken out to obtain refined alloy powder.
[0078] S5. The alloy powder obtained in step S4 is loaded into an alloy cylindrical mold and cold-pressed and densified by a tablet press. The cold pressing pressure is set to 100MPa and the holding time is 60min to obtain a cold-pressed preform.
[0079] S6. Place the cold-pressed preform obtained in step S5 into a tube furnace for secondary sintering. First, heat the preform to 300°C at a rate of 2°C / min, then heat it to 400°C at a rate of 5°C / min and hold it for 300 min. Finally, allow it to cool naturally to room temperature in the furnace to obtain a pure phase BiSbTe-based thermoelectric material without CsCl doping.
[0080] Thermoelectric performance testing and analysis:
[0081] All thermoelectric material bulk samples prepared in the examples and comparative examples were polished sequentially with 800-mesh and 3000-mesh metallographic sandpaper, and then polished with corundum polishing liquid with a particle size of 14μm and a mass fraction of 20%, and then thermoelectric performance was tested.
[0082] 1. Electrical transport performance test: The conductivity σ of the sample was measured using the ZEM-3 Seebeck coefficient / resistance measurement system (corresponding to...). Figure 3 (a)), Seebeck coefficient S (corresponding to) Figure 3 (b) The power factor PF is calculated based on the formula PF=σS² (corresponding to Figure 3 (d) to evaluate the electrical transport properties of the material; the carrier concentration and carrier mobility of the sample (corresponding to) were obtained by Hall measurement. Figure 3 (c));
[0083] Figure 3 (a) The curves show the conductivity of BiSbTe-based thermoelectric materials as a function of temperature under different doping parameters, revealing the conductivity characteristics of this system: the conductivity σ of all samples continuously decreases with temperature from 300K to 425K, reflecting the characteristics of a degenerate semiconductor. Essentially, the increased temperature intensifies the scattering effect of lattice vibrations on free carriers, reducing carrier mobility and leading to a gradual decrease in macroscopic conductivity. The doping control coefficient x has a significant effect on conductivity regulation. When x gradually increases from 0 to 0.015, the conductivity of the three samples with x=0.008, 0.010, and 0.015 remains at 350 Scm at room temperature (300K). -1Near the same temperature range, it can maintain high conductivity throughout the commonly used thermoelectric operating temperature range of 300K~425K, significantly reducing the Joule heat loss of the device and providing a key foundation for achieving a high thermoelectric figure of merit (ZT). When the doping control coefficient x is further increased to 0.020, the conductivity actually begins to decline, and the carrier mobility collapses, indicating that excessive doping will introduce additional carrier scattering defects, which will offset the gain brought by the increase in carrier concentration. x=0.020 is the group with the lowest conductivity among all samples, and its conductivity is always weaker than the other samples throughout the entire temperature range.
[0084] Figure 3 (b) This paper demonstrates the complete evolution of the Seebeck coefficient of BiSbTe-based thermoelectric materials with temperature under different CsCl doping control coefficients: the Seebeck coefficients of all tested samples show a highly uniform trend, but due to different doping concentrations, their peak temperatures increase sequentially with increasing doping concentration in the range of 300 K to 350 K. Although some individual samples deviate slightly, the overall trend is consistent. As the temperature further increases to 425 K, the Seebeck coefficients of all samples continuously decrease from their respective peak values. From the perspective of the effect of doping control, the introduction of CsCl has a significant and regular influence on the Seebeck coefficient: in most test ranges from 300 K to close to 400 K, the undoped Seebeck coefficient is at the highest level among all samples. As the CsCl doping control coefficient gradually increases, the Seebeck coefficient of the materials at the same temperature generally shows a stepwise decrease, with the sample with x=0.020 having the lowest Seebeck coefficient among all samples at most test temperature points. This phenomenon is essentially due to the fact that CsCl doping alters the carrier concentration inside the material. While improving conductivity, it inevitably leads to a decrease in the Seebeck coefficient. The sample with x=0.008 achieves an optimal balance between the two core parameters: it shows only a very small decrease in the Seebeck coefficient compared to the undoped sample, and it does not exhibit the significant deterioration of the Seebeck coefficient seen in the highly doped sample with x=0.020. It achieves high conductivity while preserving a high Seebeck coefficient to the maximum extent, avoiding excessive imbalance of thermoelectric parameters. It is the sample with the best overall transport performance under this doping system.
[0085] Figure 3 (d) Performance curves showing the power factor of BiSbTe-based thermoelectric materials with different CsCl doping control coefficients as a function of temperature are displayed. The figures show that the power factor of all samples exhibits a monotonically decreasing trend with increasing temperature, reaching its peak performance at room temperature (300 K). The sample with a doping concentration of x=0.008 exhibits the highest power factor at most test temperatures, with a peak value exceeding 22 μW·cm at 300 K. -1 ·K -2The power factor of the overdoped sample (x=0.020) is significantly higher than that of the undoped sample. The power factor of the overdoped sample (x=0.020) is the lowest among all groups across the entire temperature range. This indicates that appropriate CsCl doping can achieve synergistic regulation of conductivity and Seebeck coefficient by optimizing carrier concentration, thereby significantly improving the overall electrical transport performance of the material.
[0086] 2. Thermal performance testing: The thermal diffusivity α and specific heat capacity of the material were directly measured using an LFA 457 laser scintillation thermal conductivity analyzer. The sample density ρ is obtained using the formula K = α is calculated to the total thermal conductivity κ of the material (corresponding to) Figure 4 (a)); Take the Lorentz coefficient L = 2.44 × W·Ω / ; through formula K e =L T is calculated to obtain the carrier thermal conductivity K. e (correspond Figure 4 (b) using the total thermal conductivity decomposition formula κ=K e +K1+K b The sum of lattice thermal conductivity and bipolar thermal conductivity was calculated. (correspond Figure 4 (c)).
[0087] Figure 4 (a) The performance curves show the variation of the total thermal conductivity of BiSbTe-based thermoelectric materials with different CsCl doping control coefficients as a function of temperature. The graphs show that the total thermal conductivity of all samples generally increases with increasing temperature. The sample with a doping concentration of x=0.020 exhibits the highest total thermal conductivity across the entire test temperature range, and its increase with temperature is the most significant, reaching 0.67 W·m at 300 K. -1 ·K -1 Around 425K, it approaches 0.89 W·m. -1 ·K -1 As the doping concentration increases, the total thermal conductivity monotonically increases from a level lower than that of the undoped sample. When the CsCl doping concentration is x=0.005, x=0.008, and x=0.010, the total thermal conductivity of the corresponding samples increases slowly. As the doping concentration continues to increase, the total thermal conductivity of the two samples with x=0.015 and x=0.020 increases significantly and exceeds that of the undoped sample. This indicates that the CsCl doping concentration has a significant impact on the thermal conductivity of the material in this system, and this characteristic will also directly affect the overall thermoelectric conversion performance of the thermoelectric material.
[0088] Figure 4(b) The performance curves of the carrier thermal conductivity of BiSbTe-based thermoelectric materials with different CsCl doping control coefficients as a function of temperature are shown. It can be seen from the figure that the carrier thermal conductivity of most samples shows a trend of first decreasing and then increasing with increasing temperature. Among them, the sample with a doping amount of x=0.020 has the lowest carrier thermal conductivity at most test temperature points, which corresponds to the trend of the sample's electrical conductivity, proving the strong correlation between carrier thermal conductivity and electrical conductivity.
[0089] Figure 4 (c) Shows the performance curves of the lattice thermal conductivity of BiSbTe-based thermoelectric materials with different CsCl doping control coefficients as a function of temperature. The figure shows that... + The doping concentration showed a monotonically increasing trend with increasing doping concentration. Furthermore, all samples... + Within the temperature range of 300K to 425K, the thermal conductivity increases with increasing temperature. Given that the thermal conductivity of a pure lattice typically decreases monotonically with increasing temperature in this region, this upward trend can be attributed to the rapid increase in bipolar thermal conductivity. This phenomenon indicates that the material has undergone significant intrinsic excitation, and its thermoelectric properties will be strongly constrained by the bipolar effect.
[0090] 3. Comprehensive thermoelectric performance evaluation: using the formula The thermoelectric figure of merit ZT of the sample was calculated (corresponding to Figure 5 This was used to evaluate the temperature dependence of the overall thermoelectric properties of the material under different CsCl doping levels.
[0091] Figure 5 (a) The performance curves of the thermoelectric figure of merit (ZT) of BiSbTe-based thermoelectric materials with different CsCl doping control coefficients as a function of temperature are shown. It can be seen from the figure that the ZT value of each sample shows a trend of continuous decrease or slight increase followed by decrease as the temperature increases. They reach their respective performance peaks in the temperature range of 300K~325K. Among them, the ZT value of the sample with x=0.008 shows the best overall result in the test temperature range, with a ZT value close to 1.2 at 325K. Meanwhile, the ZT value of the sample with x=0.010 reaches 1.2 at 300K. However, as the doping amount is further increased to x=0.020, the ZT value of the sample is at the lowest level in the entire temperature range, and the overall thermoelectric performance shows a significant decline.
[0092] Figure 5(b) The thermoelectric figure of merit (ZT) of BiSbTe-based thermoelectric materials prepared by different processes is shown as a function of temperature; wherein, curve "this work" represents the ZT performance of the BiSbTe thermoelectric material sample prepared in Example 2 of this application, and the other curves represent the ZT performance of comparative samples prepared by CsBr-doped SPS process, RbOH-doped HTS process, and KCl-doped melting method in the prior art.
[0093] As shown in 5(b), the sample prepared in Example 2 has a ZT value close to 1.2 at 325K, which is not only significantly higher than the room temperature ZT level of only about 0.6 for samples prepared by the traditional RbOH-doped HTS process, but also reaches or exceeds the thermoelectric properties of samples prepared by the publicly disclosed CsBr-doped SPS and KCl-doped melting methods. This solves the industry pain points of traditional BiSbTe materials, such as precise temperature control at room temperature and low conversion efficiency. Unlike existing high-performance BiSbTe materials, which generally rely on high-cost special processes such as SPS sintering and supergravity remelting, this solution avoids the above-mentioned high-cost processes while achieving a high ZT at room temperature. It solves the industry problem of the difficulty in low-cost mass production of high-performance BiSbTe materials, and has stronger commercial competitiveness in consumer electronics micro-refrigeration and civilian low-grade waste heat recovery scenarios.
[0094] Meanwhile, the optimal sample in this invention has an average ZT of 1.08 in the temperature range of 300K~400K, which is suitable for specific scenarios such as constant temperature precision temperature control where a wide temperature range is not required. It can fully meet the usage requirements and achieve a lower overall cost. This solution adopts a cold pressing sintering preparation process, which can reduce production costs while maintaining excellent thermoelectric performance. CsCl-doped BiSbTe polycrystalline materials have the potential to replace existing commercial Bi2Te3-based thermoelectric materials, which is of great practical significance for promoting the industrialization and technological iteration of room temperature thermoelectric materials.
[0095] The foregoing has shown and described the basic principles and main features of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The facts and descriptions above are merely illustrative of the principles of the invention. Various changes and modifications can be made to the present invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of this invention is defined by the appended claims and their legal equivalents.
Claims
1. A method for preparing a cold-pressed sintered BiSbTe-based thermoelectric material, characterized in that, Includes the following steps: S1. Weigh Bi, Sb, and Te elemental powders with a purity of 4N and 60 mesh, along with CsCl powder, precisely according to the molar ratio of Bi:Sb:Te:CsCl 1:3:6:2x, where the value of x ranges from 0.005 to x ≤ 0.
015. S2. Place all the raw materials weighed in step S1 into a mortar and grind them until they are evenly mixed. Then, vacuum seal the mixed powder in a quartz test tube. S3. Place the sealed quartz test tube obtained in step S2 into a tube furnace and heat it until it melts, so that the raw material forms a uniform melt. After holding it at the temperature, immerse the entire quartz test tube in deionized water at room temperature for water quenching. After breaking the tube, an alloy ingot is obtained. S4. After the alloy ingot obtained in step S3 is initially crushed, it is subjected to wet ball milling to refine the alloy powder with the target particle size. Then, the powder is dried under an inert gas protective atmosphere and cooled to obtain the refined alloy powder. S5. The refined alloy powder obtained in step S4 is loaded into a mold and cold-pressed and densified by a tablet press to obtain a cold-pressed preform. S6. Place the cold-pressed preform obtained in step S5 into a tube furnace, and complete the sintering and heat preservation by segmented heating. Finally, let it cool naturally to room temperature with the furnace to obtain the CsCl-doped BiSbTe-based thermoelectric material.
2. The preparation method according to claim 1, characterized in that, In step S2, the mixed powder is vacuum-sealed in a quartz test tube, and the vacuum degree is Pa.
3. The preparation method according to claim 1, characterized in that, In step S3, after placing the sealed quartz test tube into the tube furnace, the temperature is increased to 700-800℃ at a heating rate of 5-10℃ / min and held for 10 hours.
4. The production method according to claim 1, characterized by, In step S4, the wet ball milling uses anhydrous ethanol as the grinding medium, the ball milling speed is 300 r / min, the ball milling time is 60 min, the ball-to-material ratio is 10:1, and the medium-to-material ratio is 1:
1. After ball milling, alloy powder with a particle size of 10~30 μm is obtained.
5. The preparation method according to claim 1, characterized in that, In step S4, the drying process is carried out in an Ar atmosphere, with the temperature increased to 60°C at a rate of 5°C / min and held for 180 min. The Ar gas flow rate is set to 50 sccm.
6. The preparation method according to claim 1, characterized in that, In step S5, the pressure of the cold pressing densification process is set to 100 MPa, and the holding time is 60 min.
7. The preparation method according to claim 1, characterized in that, In step S6, the segmented heating curve of the tubular furnace is as follows: the temperature is increased to 300°C at a rate of 2°C / min, then increased to 400°C at a rate of 5°C / min and held for 300 min, and finally cooled naturally to room temperature with the furnace.
8. A thermoelectric material prepared by the preparation method according to any one of claims 1 to 7.