ZrNiSn / carbon nanotube composite thermoelectric material and preparation method thereof
The ZrNiSn/carbon nanotube composite thermoelectric material was prepared through magnetic levitation smelting and discharge plasma sintering processes, which solved the problems of high lattice thermal conductivity and uneven distribution of carbon nanotubes of ZrNiSn-based materials, and significantly improved the thermoelectric and mechanical properties. The efficient preparation of ZrNiSn/carbon nanotube composite material is achieved.
Patent Information
- Application Number
- CN202411142463.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
AI Technical Summary
The lattice thermal conductivity of existing ZrNiSn-based thermoelectric materials is still relatively high, and carbon nanotubes are unevenly distributed in the Half-Heusler thermoelectric material matrix, making it difficult to effectively improve thermoelectric performance.
Magnetic levitation smelting and discharge plasma sintering process are used to prepare ZrNiSn/carbon nanotube composite thermoelectric material, ZrNiSn powder is prepared by wet ball milling and doped with carbon nanotubes to form a single-phase Half-Heusler thermoelectric material, improving the thermoelectric performance and interface of the material touch.
It effectively reduces the lattice thermal conductivity of ZrNiSn samples, improves the thermoelectric superior value ZT and mechanical properties, saves production costs and cycles, and solves the problem of uneven distribution of carbon nanotubes.
Smart Images

Figure CN119053226A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermoelectric materials, and in particular to a ZrNiSn / carbon nanotube composite thermoelectric material and a preparation method thereof. Background Art
[0002] Thermoelectric devices have the advantages of no noise, no moving parts, small size and long life. Thermoelectric devices can be used in conjunction with other energy conversion technologies to improve energy utilization. Currently, most of the thermoelectric materials with excellent performance used for thermoelectric power generation and refrigeration are tellurides, such as PbTe, Bi2Te3 and GeTe-AgSbTe2. However, tellurium and lead are highly toxic, and the content of tellurium in the earth's crust is relatively low. Therefore, it is of great significance to develop high-performance thermoelectric materials that do not contain Pb and Te. Based on the above principles, half-Heusler thermoelectric compounds have become very promising practical thermoelectric materials. ZrNiSn-based thermoelectric materials are n-type half-Heusler thermoelectric materials with better performance. However, since the beginning of this century, there has been no breakthrough in the research based on this system. At present, compared with other system thermoelectric materials, the thermal conductivity of ZrNiSn alloy is still relatively high. Previous researchers effectively reduced the lattice thermal conductivity by solid solution and grain refinement, reducing the lattice thermal conductivity to ~2Wm -1 K -1 However, the lattice thermal conductivity limit of ZrNiSn alloy is 0.8Wm -1 K -1 There is still a certain gap. Therefore, how to further reduce the lattice thermal conductivity has become the research focus of improving the thermoelectric properties of ZrNiSn alloys.
[0003] The performance of thermoelectric materials mainly depends on their thermoelectric figure of merit ZT. The larger the ZT value, the higher the thermoelectric conversion efficiency. Thermoelectric figure of merit is defined as ZT = α 2 σT / κ, where α is the Seebeck coefficient, σ is the conductivity, and α is the 2 σ can also be defined as the power factor PF, T is the absolute temperature, and κ is the total thermal conductivity, including the lattice (phonon) thermal conductivity κ l and the electronic thermal conductivity κ e (κ=κ l +κ e However, due to these thermoelectric parameters (Seebeck coefficient α, electrical conductivity σ and electronic thermal conductivity κ e ) has a strong dependence on the carrier concentration n and is coupled to each other, that is, obtaining a high conductivity σ by adjusting the carrier concentration n often leads to a low Seebeck coefficient α and a high electronic thermal conductivity κ e Therefore, how to effectively improve the ZT value has always been a difficult problem that has troubled the academic community.
[0004] Carbon nanotubes are unique one-dimensional materials. They have become a hot topic for scientific researchers because of their many excellent properties, such as outstanding electrical properties, good chemical stability, and excellent mechanical properties. In recent years, the study of introducing carbon nanotubes into typical thermoelectric material matrices to improve thermoelectric performance through nano-second phase composites has attracted widespread attention. However, due to their interface effects, it is difficult to evenly disperse carbon nanotubes in the composite matrix. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the present invention provides a ZrNiSn / carbon nanotube composite thermoelectric material and a preparation method thereof. The ZrNiSn / carbon nanotube composite thermoelectric material prepared by the preparation method of the ZrNiSn / carbon nanotube composite thermoelectric material provided by the present invention can effectively solve the problem of uneven distribution of carbon nanotubes in the Half-Heusler thermoelectric material matrix, and can effectively strengthen the interface contact of ZrNiSn / carbon nanotubes, so that the thermoelectric performance and mechanical properties are effectively improved.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a ZrNiSn / carbon nanotube composite thermoelectric material, comprising the following steps:
[0008] After mixing Zr particles, Ni particles and Sn particles, smelting is performed under a protective atmosphere to obtain a ZrNiSn ingot;
[0009] Grinding and drying the ZrNiSn ingot in sequence to obtain ZrNiSn powder;
[0010] After ZrNiSn powder and carbon nanotubes are mixed, spark plasma sintering is performed to obtain the ZrNiSn / carbon nanotube composite thermoelectric material.
[0011] Preferably, the protective atmosphere is argon; the smelting is magnetic suspension smelting; the smelting temperature is 1600-1800°C, the holding time is 1-5 minutes, and the argon pressure is 10 4 ~10 5 Pa; the number of smelting times is 3 to 6 times.
[0012] Preferably, the particle size of the ZrNiSn powder is 0.5-2 μm.
[0013] Preferably, the grinding is firstly performed by coarsely grinding the ingot into powder with a particle size of 0.1 to 1 mm using a mortar, and then wet ball milling is performed under an argon atmosphere.
[0014] Preferably, the medium for wet ball milling is anhydrous ethanol, the ball-to-material ratio is 10 to 20:1, the rotation speed is 200 to 600 r / min, and the wet ball milling time is 5 to 20 h.
[0015] Preferably, the mixing is: mixing the ZrNiSn powder and the carbon nanotubes in a mortar for 0.1 to 1 hour.
[0016] Preferably, the Zr particles, Ni particles and Sn particles are independently small particles of 1×2 mm to 2×5 mm.
[0017] Preferably, the mass of the carbon nanotubes is 0-10% of the total mass of the ZrNiSn powder and the carbon nanotubes.
[0018] The present invention also provides a ZrNiSn / carbon nanotube composite thermoelectric material prepared by the above-mentioned preparation method, comprising a ZrNiSn matrix and carbon nanotubes doped in the ZrNiSn matrix.
[0019] The present invention provides a method for preparing a ZrNiSn / carbon nanotube composite thermoelectric material, comprising the following steps: mixing Zr particles, Ni particles and Sn particles, and then smelting them under a protective atmosphere to obtain a ZrNiSn ingot; grinding and drying the ZrNiSn ingot in sequence to obtain a ZrNiSn powder; mixing the ZrNiSn powder and carbon nanotubes, and then performing discharge plasma sintering to obtain the ZrNiSn / carbon nanotube composite thermoelectric material. The present invention first prepares a single-phase ZrNiSn Half-Heusler thermoelectric material by a discharge plasma sintering process, then prepares a ZrNiSn powder by wet ball milling, and doping carbon nanotubes into a ZrNiSn matrix to form a ZrNiSn / carbon nanotube compound to improve the thermoelectric performance of the material. The method has the advantages of a short process, fewer steps, and easy control of the second phase distribution, and can effectively solve the problem that the distribution of carbon nanotubes cannot be effectively controlled in the traditional preparation process. Moreover, the interface composite condition of ZrNiSn and carbon nanotubes is good in this method, and long-term annealing treatment is not required, which can effectively save production cost and cycle.
[0020] The data of the embodiment show that single-phase ZrNiSn powder can be successfully prepared by magnetic levitation melting combined with spark plasma sintering process, and then different contents of carbon nanotube second phase can be successfully doped into the ZrNiSn matrix by grinding to form ZrNiSn / carbon nanotube compound, thereby improving the thermoelectric properties of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 XRD diagram of the ZrNiSn / carbon nanotube composite thermoelectric material samples prepared in Examples 1 to 4;
[0022] Figure 2 The SEM and TEM images of the ZrNiSn / carbon nanotube sample prepared in Example 3;
[0023] Figure 3 The total thermal conductivity and lattice thermal conductivity of the ZrNiSn / carbon nanotube composite thermoelectric material prepared in Examples 1 to 4;
[0024] Figure 4 Seebeck coefficient, electrical conductivity, power factor and thermoelectric figure of merit of the ZrNiSn / carbon nanotube composite thermoelectric materials prepared in Examples 1 to 4;
[0025] Figure 5 This is a comparison chart of the Vickers hardness and Young's modulus of the ZrNiSn / carbon nanotube composite thermoelectric materials prepared in Examples 1 to 4 and those of existing alloy materials. DETAILED DESCRIPTION
[0026] The present invention provides a method for preparing a ZrNiSn / carbon nanotube composite thermoelectric material, comprising the following steps:
[0027] After mixing Zr particles, Ni particles and Sn particles, smelting is performed under a protective atmosphere to obtain a ZrNiSn ingot;
[0028] Grinding and drying the ZrNiSn ingot in sequence to obtain ZrNiSn powder;
[0029] After ZrNiSn powder and carbon nanotubes are mixed, spark plasma sintering is performed to obtain the ZrNiSn / carbon nanotube composite thermoelectric material.
[0030] The invention mixes Zr particles, Ni particles and Sn particles, and then smelts them in a protective atmosphere to obtain a ZrNiSn ingot.
[0031] In the present invention, the Zr particles, Ni particles and Sn particles are independently preferably small particles of 1×2 mm to 2×5 mm. In the present invention, the purity of the Zr particles, Ni particles and Sn particles is independently preferably ≥99.9%.
[0032] In the present invention, the protective atmosphere is preferably argon; the smelting is preferably magnetic suspension smelting; the smelting temperature is preferably 1600-1800°C, more preferably 1650-1750°C; the heating rate to the smelting temperature is preferably 1000-3000°C / min, more preferably 1500-2500°C / min; the holding time is preferably 1-5min, more preferably 3-5min; during the smelting, the argon pressure is preferably 10 4 ~10 5Pa, more preferably 5×10 4 Pa; the number of smelting is preferably 3 to 6 times, more preferably 4 to 5 times.
[0033] After obtaining the ZrNiSn ingot, the present invention grinds and dries the ZrNiSn ingot in sequence to obtain ZrNiSn powder.
[0034] In the present invention, the grinding preferably comprises firstly coarsely grinding the ingot into powder with a particle size of 0.1 to 1 mm using a mortar; and then wet ball milling is performed under an argon atmosphere.
[0035] In the present invention, the particle size of the ZrNiSn powder is preferably 0.5 to 2 μm.
[0036] In the present invention, the grinding is preferably performed by first grinding the ingot into a powder of 0.1 to 1 mm using a mortar and then further wet ball milling using a high-energy ball milling device;
[0037] In the present invention, the medium of wet ball milling is independently preferably anhydrous ethanol, the ball-to-material ratio is independently preferably 10-20:1, more preferably 15:1, the rotation speed is preferably 200-600r / min, more preferably 300-500r / min; the ball milling time is preferably 6-18h.
[0038] In the present invention, after the grinding, preferably, suction filtration is also included.
[0039] In the present invention, the drying is preferably natural drying, and the natural drying step is preferably to dry the filtered powder naturally in a glove box for 12 to 48 hours, more preferably 12 to 24 hours.
[0040] After obtaining the ZrNiSn powder, the present invention mixes the ZrNiSn powder and carbon nanotubes and performs spark plasma sintering to obtain the ZrNiSn / carbon nanotube composite thermoelectric material.
[0041] In the present invention, the mass of the carbon nanotubes is preferably 0-10% of the total mass of the ZrNiSn powder and the carbon nanotubes, and more preferably 2-4%.
[0042] In the present invention, the temperature of the spark plasma sintering is preferably 800-1200°C, more preferably 900-1100°C; the heating rate to the temperature of the spark plasma sintering is preferably 100-300°C / min, more preferably 150-250°C / min; the pressure of the spark plasma sintering is preferably 80-120MPa, more preferably 100MPa, and the holding time is preferably 5-20min, more preferably 10-20min.
[0043] The present invention also provides a ZrNiSn / carbon nanotube composite thermoelectric material prepared by the above-mentioned preparation method, comprising a ZrNiSn matrix and carbon nanotubes doped in the ZrNiSn matrix.
[0044] In the present invention, carbon nanotubes are introduced into the ZrNiSn matrix to effectively improve the thermoelectric figure of merit ZT of the material.
[0045] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0046] Example 1
[0047] Preparation of ZrNiSn / carbon nanotube composite thermoelectric materials:
[0048] Material selection: Zr, Ni, and Sn are selected as small particles with a diameter × length of 2 × 5 mm, a purity of 99.9%, and are mixed according to the atomic ratio.
[0049] Melting: Place Zr, Ni, and Sn particles in a magnetic suspension melting furnace, heat to 1700°C in an argon protective atmosphere (pressure of 0.07 MPa), keep warm for 3 minutes, and repeatedly melt for 4 times to obtain an alloy ingot.
[0050] Ball milling and filtration: First, the alloy ingot was coarsely ground into powder with a particle size of 0.5 mm using a mortar, and then wet ball milled in an argon atmosphere. The wet ball milling medium was anhydrous ethanol, the ball-to-material ratio was 15:1, the rotation speed was 500 r / min, and the ball milling time was 10 h.
[0051] After wet ball milling, the alloy powder with a particle size of ~1μm was obtained by filtration.
[0052] Drying treatment: The filtered powder was naturally dried in a glove box for 24 hours.
[0053] Mixing: In a glove box, the dried ZrNiSn powder and carbon nanotubes (the carbon nanotubes account for 2% of the total mass of the ZrNiSn powder and the carbon nanotubes) were mixed in a mortar for 0.5 h.
[0054] Sintering: The mixed powder is sintered by spark plasma sintering, the sintering temperature is 1000°C, the sintering pressure is 100MP, and the holding time is 15min.
[0055] Example 2
[0056] The only difference from Example 1 is that the carbon nanotubes account for 3% of the total mass of the ZrNiSn powder and the carbon nanotubes.
[0057] Example 3
[0058] The only difference from Example 1 is that the carbon nanotubes account for 4% of the total mass of the ZrNiSn powder and the carbon nanotubes.
[0059] Example 4
[0060] The only difference from Example 1 is that the carbon nanotubes are 0% of the total mass of the ZrNiSn powder and the carbon nanotubes, that is, no carbon nanotubes are added.
[0061] The XRD patterns of the ZrNiSn / carbon nanotube composite thermoelectric material samples prepared in Examples 1 to 4 are as follows: Figure 1 As shown, Figure 1 Where x=0, x=2, x=3, and x=4 represent the case where the carbon nanotubes are 0%, 2%, 3%, and 4% of the total mass of the ZrNiSn powder and the carbon nanotubes, respectively. Figure 1 It can be seen that the ZrNiSn / carbon nanotube sample has less impurities, and high-quality samples can be prepared by using magnetic levitation melting combined with spark plasma sintering technology.
[0062] The SEM and TEM images of the ZrNiSn / carbon nanotube sample prepared in Example 3 are as follows: Figure 2 As shown, from Figure 2 It can be seen that the carbon nanotubes and the ZrNiSn matrix particles have good interface bonding and no agglomeration occurs. In addition, there is a non-coherent interface between the carbon nanotubes and the matrix particles, which will enhance the scattering of phonons and reduce the lattice thermal conductivity.
[0063] The total thermal conductivity and lattice thermal conductivity of the ZrNiSn / carbon nanotube composite thermoelectric materials prepared in Examples 1 to 4 are as follows: Figure 3 As shown, Figure 3 Where x=0, x=2, x=3, and x=4 respectively represent the case where the carbon nanotubes are 0%, 2%, 3%, and 4% of the total mass of the ZrNiSn powder and the carbon nanotubes. Figure 3 It can be seen that the incorporation of carbon nanotubes can significantly inhibit the lattice thermal conductivity of the ZrNiSn sample. When the doping amount of carbon nanotubes is 4% (x=4), the lattice thermal conductivity of the ZrNiSn / carbon nanotube sample is reduced to 3.4 W·m at 923 K. -1 ·K -1 , which is reduced by about 22% compared with the ZrNiSn matrix.
[0064] The Seebeck coefficient, electrical conductivity, power factor and thermoelectric figure of merit of the ZrNiSn / carbon nanotube composite thermoelectric materials prepared in Examples 1 to 4 are as follows: Figure 4 As shown, Figure 4 Where x=0, x=2, x=3, and x=4 represent the case where the carbon nanotubes are 0%, 2%, 3%, and 4% of the total mass of the ZrNiSn powder and the carbon nanotubes, respectively. Figure 4It can be seen that as the content of carbon nanotubes increases, the conductivity and thermoelectric figure of merit ZT of the sample gradually increase. When the temperature is 923K, the ZT value of the CNTs-ZrNiSn sample with a carbon nanotube doping amount of 4% (x=4) is increased by 21% compared with the ZrNiSn matrix sample, reaching 0.67. Therefore, the introduction of carbon nanotubes can effectively improve the conductivity and reduce the lattice thermal conductivity, so that the thermoelectric performance of the material is greatly improved.
[0065] The Vickers hardness and Young's modulus of the ZrNiSn / carbon nanotube composite thermoelectric materials prepared in Examples 1 to 4 are compared with those of existing alloy materials. Figure 5 As shown, Figure 5 Where x wt% represents the percentage of carbon nanotubes in the total mass of ZrNiSn powder and carbon nanotubes. Figure 5 It can be seen that with the increase of carbon nanotube content, the Vickers hardness and Young's modulus of the sample gradually increase. Therefore, the addition of carbon nanotubes can effectively improve the mechanical properties of ZrNiSn samples.
[0066] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a ZrNiSn / carbon nanotube composite thermoelectric material, It is characterized in that The following steps are involved: After mixing Zr particles, Ni particles and Sn particles, smelting is performed under a protective atmosphere to obtain a ZrNiSn ingot; Grinding and drying the ZrNiSn ingot in sequence to obtain ZrNiSn powder; After ZrNiSn powder and carbon nanotubes are mixed, spark plasma sintering is performed to obtain the ZrNiSn / carbon nanotube composite thermoelectric material.
2. The preparation method according to claim 1, It is characterized in that The protective atmosphere is argon; the smelting is magnetic suspension smelting; the smelting temperature is 1600-1800°C, the holding time is 1-5 minutes, and the argon pressure is 10 4 ~10 5 Pa; the number of smelting is 3 to 6 times.
3. The preparation method according to claim 1, It is characterized in that The particle size of the ZrNiSn powder is 0.5-2 μm.
4. The preparation method according to claim 1, It is characterized in that The grinding process firstly grinds the ingot into powder with a particle size of 0.1 to 1 mm using a mortar, and then performs wet ball milling in an argon atmosphere.
5. The preparation method according to claim 4, It is characterized in that The medium of the wet ball milling is anhydrous ethanol, the ball-to-material ratio is 10-20:1, the rotation speed is 200-600 r / min, and the wet ball milling time is 5-20 hours.
6. The preparation method according to claim 1, It is characterized in that The mixing is as follows: ZrNiSn powder and carbon nanotubes are mixed in a mortar for a mixing time of 0.1 to 1 hour.
7. The preparation method according to claim 1, It is characterized in that The Zr particles, Ni particles and Sn particles are independently small particles of 1×2 mm to 2×5 mm.
8. The preparation method according to claim 1, It is characterized in that The mass of the carbon nanotubes is 0-10% of the total mass of the ZrNiSn powder and the carbon nanotubes.
9. The ZrNiSn / carbon nanotube composite thermoelectric material prepared by the preparation method according to any one of claims 1 to 8, It is characterized in that The invention comprises a ZrNiSn matrix and carbon nanotubes doped in the ZrNiSn matrix.
Citation Information
Cited By
Preparation method of iodine element and carbon nanotube co-doped n-type PbTe thermoelectric material
CN120817805A