An aluminum alloy casting rod and its preparation method

By using specific element ratios and composite processing, the problems of uneven composition and internal defects in traditional aluminum alloy casting rods have been solved, resulting in the production of high-strength, tough, fine-grained aluminum alloy casting rods, which significantly improves the metallurgical quality of the casting rods.

CN123108370APending Publication Date: 2026-11-17JIANGYIN DINGXIN ALUMINUM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611609725.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional aluminum alloy cast rods suffer from defects such as simple component ratio, unreasonable micro-refinement, coarse and uneven grains, and are prone to porosity, air holes and component segregation.

Method used

A high-strength, high-toughness, fine-grained aluminum alloy ingots are prepared by using a specific element ratio aluminum alloy casting formula, combined with segmented gradient temperature-controlled melting, two-stage composite refining and impurity removal, multi-stage online grain refinement, composite field treatment and oil-gas semi-continuous casting, and by leveraging the synergistic effect of Zr and Er and pulsed magnetic field-driven melt convection.

Benefits of technology

This method achieves high strength, toughness, and fine grain structure in aluminum alloy cast rods, significantly reduces internal defects such as porosity, looseness, and segregation, and improves metallurgical quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of aluminum alloy casting technology, and more particularly to an aluminum alloy casting rod and its preparation method, comprising the following components by mass percentage (wt%): Fe: 0.08-0.12%; Si: 0.04-0.08%; Cu: 0.15-0.25%; Mg: 2.2-2.5%; Zn: 6.5-6.9%; Mn≤0.01%; Ti: 0.08-0.15%; Zr: 0.05-0.12%; Er: 0.03-0.08%. In this invention, by introducing Zr and Er dual microalloying elements into a low-Cu, high-Zn-Mg aluminum alloy matrix, and with elemental ratio constraints, the Al3Zr dispersed particles formed by Zr pin grain boundaries and inhibit grain growth, while the Al3Er particles formed by Er act as heterogeneous nucleation cores to promote fine grain solidification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aluminum alloy casting technology, and in particular to an aluminum alloy casting rod and its preparation method. Background Technology

[0002] Aluminum alloy cast rods are used as blanks for subsequent processing such as extrusion and forging, and their metallurgical quality directly affects the performance of the final product. Currently, traditional aluminum alloy cast rods have many technical defects: First, the composition ratio is simple, the micro-refining and anti-corrosion elements are not properly matched, the cast rod grains are coarse and uneven in size, and defects such as porosity, pores and compositional segregation are very easy to occur inside. Summary of the Invention

[0003] To address the problems mentioned in the background section, this invention provides an aluminum alloy casting rod and its preparation method.

[0004] To achieve the above objectives, the present invention adopts the following technical solution: An aluminum alloy casting rod and its preparation method, comprising the following components by mass percentage (wt%): Fe: 0.08–0.12%; Si: 0.04–0.08%; Cu: 0.15–0.25%; Mg: 2.2–2.5%; Zn: 6.5–6.9%; Mn≤0.01%; Ti: 0.08–0.15%; Zr: 0.05–0.12%; Er: 0.03–0.08%; unavoidable single impurity element ≤0.03%, total impurity content ≤0.12%; balance being metallic aluminum; and simultaneously satisfying the following three sets of synergistic element ratio constraints: 1) Zn / Mg mass ratio = 2.70~3.05; 2) Total mass fraction of Ti + Zr = 0.13–0.27%; 3) The mass ratio of Cu / (Zn+Mg) is 0.013 to 0.021.

[0005] 2. A method for preparing an aluminum alloy casting rod, comprising the following steps: S1: Ingredients and Pretreatment Ingredients: Mix ingredients according to the specified proportions; Pretreatment: Remove oxide scale, oil stains and impurities from the surface of the ingredients, and dry all ingredients at 120-150℃ for 2-3 hours. S2: Segmented gradient temperature-controlled melting The first stage involves heating to 690–710℃ and holding at that temperature for 35–45 minutes to completely melt the aluminum ingot. In the second stage, the temperature is raised to 720-735℃, and some intermediate alloy is added in sequence. After stirring evenly, the temperature is maintained for 15-20 minutes. In the third stage, the temperature is lowered to 710-720℃, Zr and Er master alloys are added, and the mixture is stirred at low speed for 15-20 minutes to obtain a uniformly mixed aluminum alloy stock solution. Step S3: Two-stage compound refining and impurity removal The aluminum alloy molten metal obtained in step S2 is heated to 740–760°C, and high-purity argon gas (purity ≥99.99%) is introduced by rotary jetting for the first stage of refining and degassing. The refining time is 15–25 min, and the argon gas flow rate is 8–15 L / min. Then, 0.4–0.7% of sodium-free refining agent by weight of the melt is added for the second stage of refining and slag removal. The refining time is 15–25 min. After refining, the mixture is allowed to stand for 20–30 min, and the surface slag is removed. Step S4: Multi-level online grain refinement The refined aluminum alloy melt from step S3 is introduced into a flow channel. Three grain refiner addition points are sequentially set along the melt flow direction on the flow channel: the first addition point is located at the beginning of the flow channel, the second addition point is located before the inlet of the degassing box, and the third addition point is located after the outlet of the filter box. Al-Ti-B grain refiner is added to the three addition points by wire feeding, with a total addition amount of 0.06-0.16% of the melt weight. The first addition point accounts for 45-55% of the total addition amount, the second addition point accounts for 30-40%, and the third addition point accounts for 25-35%. Step S5: Composite Field Treatment The aluminum alloy melt, which has undergone multi-stage grain refinement, is sequentially processed in the flow tank as follows: (a) Ultrasonic treatment: An ultrasonic vibration device is installed in the middle section of the flow channel; (b) Pulse magnetic field treatment: A pulse magnetic field generator is installed at the end of the flow channel; Step S6: Two-stage filtration The aluminum alloy melt after composite field treatment is sequentially filtered through a 30ppi (pores per inch) foam ceramic filter plate and a 50ppi foam ceramic filter plate for two-stage filtration, with a filtration temperature of 720-745℃. Step S7: Oil-gas semi-continuous casting Aluminum alloy cast rods were obtained by casting using an oil-gas semi-continuous casting machine. Step S8: Gradient homogenization heat treatment The aluminum alloy casting obtained in step S7 is subjected to gradient homogenization heat treatment: (a) First stage homogenization: Heat to 340-410℃ at a rate of 35-65℃ / h and hold for 3-4 hours; (b) Second-stage homogenization: Heat to 540-570℃ at a rate of 25-45℃ / h and hold for 9-17 hours; (c) Cooling: After homogenization, the temperature is first slowly cooled to 200-250°C at a rate of 60-100°C / h, and then cooled to room temperature by spraying water mist to obtain the final high-strength, high-toughness, fine-grained aluminum alloy casting rod.

[0006] Step S9: After the heat treatment in step (S8), the casting rod is surface-polished and non-destructive tested to remove unqualified billets containing porosity, cracks, and segregation.

[0007] Furthermore, in step (S2), inert gas protection is used throughout the melting process, and high-purity argon gas is introduced into the furnace to isolate air and prevent the alloy liquid from oxidizing and burning.

[0008] Further, in step (S5), the ultrasonic frequency is 25-35kHz, the ultrasonic power is 1.5-3kW, and the melt is subjected to continuous ultrasonic treatment; the pulse frequency is 5-20Hz, and the magnetic induction intensity is 0.1-0.5T, and the melt is subjected to pulsed magnetic field treatment.

[0009] Furthermore, in step (S7), the casting temperature is 700-730℃, the casting speed is 50-120mm / min, the cooling water flow rate is 80-200L / min, and the oil-gas lubrication parameters are: gas pressure 0.3-0.6MPa and lubricating oil flow rate 0.5-2.0L / h.

[0010] In this invention, by introducing Zr and Er dual microalloying elements into a low-Cu, high-Zn-Mg aluminum alloy matrix, and with element ratio constraints, the Al3Zr dispersed particles formed by Zr pin the grain boundaries and inhibit grain growth, while the Al3Er particles formed by Er act as heterogeneous nucleation cores to promote fine grain solidification. The synergistic effect of the two makes the microcrystalline grain size grade G in the core of the cast rod stable and greater than 4. In addition, the pulsed magnetic field drives the melt convection to accelerate the floating of inclusions. The two work together to control the hydrogen content of the melt below 0.14 ml / 100 mg Al, and the low magnification structure of the cast rod is free of defects such as porosity and looseness. Detailed Implementation

[0011] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0012] Unless otherwise specified, the raw materials used in this invention are all from commercially available conventional products. Example

[0013] An aluminum alloy casting rod, with the following composition by mass percentage (wt%): Fe: 0.10%, Si: 0.06%, Cu: 0.20%, Mg: 2.35%, Zn: 6.70%, Mn: 0.005%, Ti: 0.11%, Zr: 0.08%, Er: 0.05%; single impurity 0.02%, total impurities 0.10%, balance Al; proportioning calculation: Zn / Mg = 2.85; Ti + Zr = 0.18%; Cu / (Zn + Mg) = 0.018; A method for preparing an aluminum alloy casting rod includes the following steps: S1: Ingredients and Pretreatment (a) Ingredients: Ingredients are prepared according to the specified proportions; (b) Pretreatment: Remove oxide scale, oil and impurities from the surface of the ingredients, dry all ingredients at 130°C for 2.5 hours to remove adsorbed moisture and avoid porosity defects during the melting process. S2: Segmented gradient temperature-controlled melting The first stage involves heating to 700℃ and holding for 40 minutes to completely melt the aluminum ingot. The second stage involves heating to 720℃, adding some intermediate alloy, stirring evenly, and then holding at that temperature for 20 minutes. In the third stage, the temperature is lowered to 710℃, Zr and Er intermediate alloys are added, and the mixture is stirred at low speed for 15 minutes to avoid high-temperature burn-off of highly active alloying elements, resulting in a uniformly mixed aluminum alloy stock solution. Step S3: Two-stage compound refining and impurity removal The aluminum alloy molten metal obtained in step S2 is heated to 750℃, and high-purity argon gas (purity ≥99.99%) is introduced by rotary jetting for the first stage of refining and degassing. The refining time is 20 min and the argon gas flow rate is 10 L / min. Then, 0.5% sodium-free refining agent by weight of the melt is added for the second stage of refining and slag removal. The refining time is 20 min. After refining, the mixture is allowed to stand for 25 min, and the surface slag is removed. Step S4: Multi-level online grain refinement The refined aluminum alloy melt from step S3 is introduced into a flow channel. Three grain refiner addition points are sequentially set along the melt flow direction on the flow channel: the first addition point is located at the beginning of the flow channel, the second addition point is located before the inlet of the degassing box, and the third addition point is located after the outlet of the filter box. Al-Ti-B grain refiner is added to the three addition points by wire feeding, with a total addition amount of 0.1% of the melt weight. The first addition point accounts for 45% of the total addition amount, the second addition point accounts for 30%, and the third addition point accounts for 25%. Step S5: Composite Field Treatment The aluminum alloy melt, which has undergone multi-stage grain refinement, is sequentially processed in the flow tank as follows: (a) Ultrasonic treatment: An ultrasonic vibration device is installed in the middle section of the flow channel. The ultrasonic frequency is 30kHz and the ultrasonic power is 2.0kW to continuously ultrasonically treat the melt. (b) Pulse magnetic field treatment: A pulse magnetic field generator with a magnetic induction intensity of 0.2T is installed at the end of the flow channel to treat the melt with a pulse magnetic field. Step S6: Two-stage filtration The aluminum alloy melt after composite field treatment is filtered in two stages: a 30ppi (pores per inch) foam ceramic filter plate and a 50ppi foam ceramic filter plate, with a filtration temperature of 730℃. Step S7: Oil-gas semi-continuous casting The casting was carried out using an oil-gas semi-continuous casting machine at a casting temperature of 710℃, a casting speed of 80mm / min, a cooling water flow rate of 100L / min, and oil-gas lubrication parameters of 0.5MPa gas pressure and 1.0L / h lubricating oil flow rate to obtain aluminum alloy cast rods. Step S8: Gradient homogenization heat treatment The aluminum alloy casting obtained in step S7 is subjected to gradient homogenization heat treatment: (a) First stage homogenization: Heat to 360℃ at a rate of 45℃ / h and hold for 34 hours; (b) Second-stage homogenization: Heat to 550℃ at a rate of 30℃ / h and hold for 12 hours; (c) Cooling: After homogenization, the temperature is first slowly cooled to 210°C at a rate of 80°C / h, and then cooled to room temperature by spraying water mist to obtain the final high-strength, high-toughness, fine-grained aluminum alloy casting rod. Step S9: After the heat treatment in step (S8), the casting rod is surface-polished and non-destructive tested to remove unqualified billets containing porosity, cracks, and segregation.

[0014] The cast rod obtained in Example 1 was tested, and the results are as follows: the hydrogen content of the melt was 0.09 ml / 100 mg Al; the thickness of the surface segregation layer did not exceed 1 mm; the microcrystalline grain size grade G of the core of the cast rod was greater than 4; there was no overheated microstructure after homogeneous heat treatment; the low magnification structure was free of cracks, pores, metallic inclusions, non-metallic inclusions, feather crystals, white spots, bright grains and coarse metallic compound segregation; the porosity grade did not exceed grade 1. Example

[0015] An aluminum alloy casting rod, with the following composition by mass percentage (wt%): Fe: 0.09%, Si: 0.05%, Cu: 0.18%, Mg: 2.30%, Zn: 6.60%, Mn: 0.008%, Ti: 0.12%, Zr: 0.09%, Er: 0.06%; single impurity: 0.02%; total impurity content: 0.11%, balance Al; Zn / Mg = 2.87%, Ti+Zr = 0.23%, Cu / (Zn+Mg) = 0.016%; A method for preparing an aluminum alloy casting rod includes the following steps: S1: Ingredients and Pretreatment (a) Ingredients: Ingredients are prepared according to the specified proportions; (b) Pretreatment: Remove oxide scale, oil and impurities from the surface of the ingredients, dry all ingredients at 130°C for 2.5 hours to remove adsorbed moisture and avoid porosity defects during the melting process. S2: Segmented gradient temperature-controlled melting The first stage involves heating to 700℃ and holding for 40 minutes to completely melt the aluminum ingot. The second stage involves heating to 720℃, adding some intermediate alloy, stirring evenly, and then holding at that temperature for 20 minutes. In the third stage, the temperature is lowered to 710℃, Zr and Er intermediate alloys are added, and the mixture is stirred at low speed for 15 minutes to avoid high-temperature burn-off of highly active alloying elements, resulting in a uniformly mixed aluminum alloy stock solution. Step S3: Two-stage compound refining and impurity removal The aluminum alloy molten metal obtained in step S2 is heated to 750℃, and high-purity argon gas (purity ≥99.99%) is introduced by rotary jetting for the first stage of refining and degassing. The refining time is 20 min and the argon gas flow rate is 10 L / min. Then, 0.5% sodium-free refining agent by weight of the melt is added for the second stage of refining and slag removal. The refining time is 20 min. After refining, the mixture is allowed to stand for 25 min, and the surface slag is removed. Step S4: Multi-level online grain refinement The refined aluminum alloy melt from step S3 is introduced into a flow channel. Three grain refiner addition points are sequentially set along the melt flow direction on the flow channel: the first addition point is located at the beginning of the flow channel, the second addition point is located before the inlet of the degassing box, and the third addition point is located after the outlet of the filter box. Al-Ti-B grain refiner is added to the three addition points by wire feeding, with a total addition amount of 0.1% of the melt weight. The first addition point accounts for 45% of the total addition amount, the second addition point accounts for 30%, and the third addition point accounts for 25%. Step S5: Composite Field Treatment The aluminum alloy melt, which has undergone multi-stage grain refinement, is sequentially processed in the flow tank as follows: (a) Ultrasonic treatment: An ultrasonic vibration device is installed in the middle section of the flow channel. The ultrasonic frequency is 30kHz and the ultrasonic power is 2.0kW to continuously ultrasonically treat the melt. (b) Pulse magnetic field treatment: A pulse magnetic field generator with a magnetic induction intensity of 0.2T is installed at the end of the flow channel to treat the melt with a pulse magnetic field. Step S6: Two-stage filtration The aluminum alloy melt after composite field treatment is filtered in two stages: a 30ppi (pores per inch) foam ceramic filter plate and a 50ppi foam ceramic filter plate, with a filtration temperature of 730℃. Step S7: Oil-gas semi-continuous casting The casting was carried out using an oil-gas semi-continuous casting machine at a casting temperature of 710℃, a casting speed of 80mm / min, a cooling water flow rate of 100L / min, and oil-gas lubrication parameters of 0.5MPa gas pressure and 1.0L / h lubricating oil flow rate to obtain aluminum alloy cast rods. Step S8: Gradient homogenization heat treatment The aluminum alloy casting obtained in step S7 is subjected to gradient homogenization heat treatment: (a) First stage homogenization: Heat to 360℃ at a rate of 45℃ / h and hold for 34 hours; (b) Second-stage homogenization: Heat to 550℃ at a rate of 30℃ / h and hold for 12 hours; (c) Cooling: After homogenization, the temperature is first slowly cooled to 210°C at a rate of 80°C / h, and then cooled to room temperature by spraying water mist to obtain the final high-strength, high-toughness, fine-grained aluminum alloy casting rod. Step S9: After the heat treatment in step (S8), the casting rod is surface-polished and non-destructive tested to remove unqualified billets containing porosity, cracks, and segregation.

[0016] The cast rod obtained in Example 2 was tested, and the results are as follows: the hydrogen content of the melt was 0.08 ml / 100 mg Al; the thickness of the surface segregation layer did not exceed 1 mm; the microcrystalline grain size grade G of the core of the cast rod was greater than 4; there was no overheated microstructure after homogeneous heat treatment; the low magnification structure was free of cracks, pores, metallic inclusions, non-metallic inclusions, feather crystals, white spots, bright grains and coarse metallic compound segregation; the porosity grade did not exceed grade 1.

[0017] An aluminum alloy casting rod, the mass percentages of each component are as follows (wt%): Fe: 0.09%, Si: 0.05%, Cu: 0.18%, Mg: 2.30%, Zn: 6.60%, Mn: 0.008%, Ti: 0.12%; single impurity 0.02%; total impurity content 0.11%, balance Al; Zn / Mg = 2.87%, Cu / (Zn+Mg) = 0.016%.

[0018] The alloy formulation and preparation process are the same as in Example 1, except that Zr and Er are not added, while the other components and preparation methods are the same as in Example 1.

[0019] The cast rod obtained in Comparative Example 1 was tested. Due to the lack of grain boundary pinning effect of Al3Zr dispersed particles and heterogeneous nucleation promotion effect of Al3Er particles, the grain refinement effect of the core of the cast rod was significantly reduced, and the core microcrystalline grain size grade G was not greater than 4; feather crystals or white spots appeared in the low magnification structure; the surface segregation layer thickness exceeded 2 mm; and the porosity grade exceeded 1.

[0020] An aluminum alloy casting rod, with the following composition by mass percentage (wt%): Fe: 0.10%, Si: 0.06%, Cu: 0.20%, Mg: 2.35%, Zn: 6.70%, Mn: 0.005%, Ti: 0.11%, Zr: 0.08%, Er: 0.05%; single impurity 0.02%, total impurity content 0.10%, balance Al; proportioning calculation: Zn / Mg = 2.85%; Ti + Zr = 0.18%; Cu / (Zn + Mg) = 0.018%; The alloy formulation and preparation process of Example 1 are the same as those of Example 1, except that the ultrasonic vibration and pulsed magnetic field composite field synergistic treatment step in step S5 is removed. The casting rod obtained in Comparative Example 2 was tested. Due to the lack of the nucleation-promoting effect of ultrasonic cavitation on dissolved hydrogen bubbles and the driving effect of pulsed magnetic field on melt convection, the hydrogen content of the melt increased to more than 0.14 ml / 100 mg Al. Porosity and looseness defects appeared inside the casting rod, and the thickness of the surface segregation layer increased.

[0021] The performance test results of the aluminum alloy cast rods are as follows:

[0022] As shown in the table above, the cast rods obtained in Examples 1 and 2 all met the microstructure and performance requirements specified in this invention in all six test indicators, and their overall metallurgical quality was significantly better than that of the comparative examples.

[0023] In the description of this specification, the terms "preparation example," "example," "various examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that example or preparation example, which are included in at least one example or preparation example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same example or preparation example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more examples or preparation examples.

[0024] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. An aluminum alloy ingot bar characterized by, Composed of the following components by mass percentage (wt%): Fe: 0.08–0.12%; Si: 0.04–0.08%; Cu: 0.15–0.25%; Mg: 2.2–2.5%; Zn: 6.5–6.9%; Mn≤0.01%; Ti: 0.08–0.15%; Zr: 0.05–0.12%; Er: 0.03–0.08%; unavoidable single impurity element ≤0.03%, total impurity content ≤0.12%; balance is metallic aluminum; and simultaneously meets the following three sets of synergistic element ratio constraints: 1) Zn / Mg mass ratio = 2.70~3.05; 2) Total mass fraction of Ti + Zr = 0.13–0.27%; 3) The mass ratio of Cu / (Zn+Mg) is 0.013 to 0.

021.

2. A method of producing an aluminum alloy ingot for use in the aluminum alloy ingot as claimed in claim 1, characterized by, Includes the following steps: S1: Ingredients and Pretreatment (a) Ingredients: Ingredients are prepared according to the specified proportions; (b) Pretreatment: Remove oxide scale, oil and impurities from the surface of the ingredients, and dry all ingredients at 120-150℃ for 2-3 hours. S2: Segmented gradient temperature-controlled melting The first stage involves heating to 690–710℃ and holding at that temperature for 35–45 minutes to completely melt the aluminum ingot. In the second stage, the temperature is raised to 720-735℃, and some intermediate alloy is added in sequence. After stirring evenly, the temperature is maintained for 15-20 minutes. In the third stage, the temperature is lowered to 710-720℃, Zr and Er master alloys are added, and the mixture is stirred at low speed for 15-20 minutes to obtain a uniformly mixed aluminum alloy stock solution. Step S3: Two-stage compound refining and impurity removal The aluminum alloy molten metal obtained in step S2 is heated to 740–760°C, and high-purity argon gas (purity ≥99.99%) is introduced by rotary jetting for the first stage of refining and degassing. The refining time is 15–25 min, and the argon gas flow rate is 8–15 L / min. Then, 0.4–0.7% of sodium-free refining agent by weight of the melt is added for the second stage of refining and slag removal. The refining time is 15–25 min. After refining, the mixture is allowed to stand for 20–30 min, and the surface slag is removed. Step S4: Multi-level online grain refinement The refined aluminum alloy melt from step S3 is introduced into a flow channel. Three grain refiner addition points are sequentially set along the melt flow direction on the flow channel: the first addition point is located at the beginning of the flow channel, the second addition point is located before the inlet of the degassing box, and the third addition point is located after the outlet of the filter box. Al-Ti-B grain refiner is added to the three addition points by wire feeding, with a total addition amount of 0.06-0.16% of the melt weight. The first addition point accounts for 45-55% of the total addition amount, the second addition point accounts for 30-40%, and the third addition point accounts for 25-35%. Step S5: Composite Field Treatment The aluminum alloy melt, which has undergone multi-stage grain refinement, is sequentially processed in the flow tank as follows: (a) Ultrasonic treatment: An ultrasonic vibration device is installed in the middle section of the flow channel; (b) Pulse magnetic field treatment: A pulse magnetic field generator is installed at the end of the flow channel; Step S6: Two-stage filtration The aluminum alloy melt after composite field treatment is sequentially filtered through a 30ppi (pores per inch) foam ceramic filter plate and a 50ppi foam ceramic filter plate for two-stage filtration, with a filtration temperature of 720-745℃. Step S7: Oil-gas semi-continuous casting Aluminum alloy cast rods were obtained by casting using an oil-gas semi-continuous casting machine. Step S8: Gradient homogenization heat treatment The aluminum alloy casting obtained in step S7 is subjected to gradient homogenization heat treatment: (a) First stage homogenization: Heat to 340-410℃ at a rate of 35-65℃ / h and hold for 3-4 hours; (b) Second-stage homogenization: Heat to 540-570℃ at a rate of 25-45℃ / h and hold for 9-17 hours; (c) Cooling: After homogenization, the temperature is first slowly cooled to 200-250℃ at a rate of 60-100℃ / h, and then cooled to room temperature by spraying water mist to obtain the final high-strength, high-toughness, fine-grained aluminum alloy casting. Step S9: After the heat treatment in step (S8), the casting rod is surface-polished and non-destructive tested to remove unqualified billets containing porosity, cracks, and segregation.

3. A method of producing an aluminum alloy ingot according to claim 2, characterized by: In step (S2), inert gas is used for the entire melting process, and high-purity argon is introduced into the furnace to isolate the air and prevent the alloy liquid from oxidizing and burning.

4. A method of producing an aluminum alloy ingot according to claim 3, characterized by: In step (S5), the ultrasonic frequency is 25-35 kHz, the ultrasonic power is 1.5-3 kW, and the melt is subjected to continuous ultrasonic treatment. The pulse frequency is 5-20 Hz, the magnetic induction intensity is 0.1-0.5 T, and the melt is subjected to pulsed magnetic field treatment.

5. A method of producing an aluminum alloy ingot according to claim 4, characterized by: In step (S7), the casting temperature is 700-730℃, the casting speed is 50-120mm / min, the cooling water flow rate is 80-200L / min, and the oil-gas lubrication parameters are: gas pressure 0.3-0.6MPa and lubricating oil flow rate 0.5-2.0L / h.