A method for manufacturing high-strength cold-rolled steel sheet for enamel enamel
By rationally adding multiple elements to enamel steel and adopting a hot-rolled slow-cooling and cold-rolled continuous annealing process, fine spherical precipitates are formed, which solves the problems of large strength reduction and poor anti-scaling performance of enamel steel before and after enamel firing, and achieves comprehensive mechanical properties of high strength and excellent anti-scaling performance.
Patent Information
- Application Number
- CN202611411162.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing enamel steels exhibit a significant strength reduction before and after enamel firing and have poor resistance to spalling, making it difficult to maintain both high strength and excellent resistance to spalling. Furthermore, they suffer from high fracture sensitivity during the plastic deformation of the steel plate.
By rationally adding multiple elements and combining specific hot-rolled slow cooling and cold-rolled continuous annealing and over-aging processes, a large number of stable and fine spherical precipitates, such as Ti(C,N), BN and Ce oxides, are formed in the matrix, which inhibits the coarsening of the matrix structure and improves the thermal stability and hydrogen trapping ability of the steel plate.
It achieves a yield strength reduction of less than 50 MPa after enameling, excellent anti-scaling performance, and an elongation of over 44%, meeting the high strength and anti-scaling requirements of enamel products and avoiding scaling defects.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of steel material manufacturing technology, and particularly relates to a method for manufacturing high-strength cold-rolled steel sheet for enamel. Background Technology
[0002] In recent years, with social development and technological progress, there is a growing demand for high-strength enamel steel plates. However, enamel steel presents several problems. First, there is the issue of spalling; second, the yield strength of the steel plate decreases significantly after enameling, often exceeding 50 MPa, making it difficult to guarantee the structural strength of the finished product. Furthermore, the anti-spalling performance (TH value) decreases significantly after enameling. Therefore, ensuring that the steel plate maintains high strength before and after enameling, or minimizes the strength reduction while possessing excellent anti-spalling properties, has become a pressing technical challenge. To improve the anti-spalling performance of the steel plate, enamel steel is typically low-carbon steel. This is because increasing the carbon content causes the steel plate to release CO, CO2, H2, etc., during enameling. The higher the carbon content, the more harmful gases are produced during enameling, leading not only to pinhole defects but also spalling defects, thus damaging the enamel quality. However, increasing the strength of the steel plate often means adding more carbon, which can result in severe spalling and pinhole defects, further compromising the enamel quality. Therefore, the most common method at present is to add Ti to the steel, that is, to use a ratio model of Ti + other elements and to clearly define the relationship between the content of Ti and the content of other elements, so as to form Ti-containing precipitates, such as strong hydrogen traps such as TiN, Ti4C2S2, and TiC. For example, patents with publication number CN1704494A and patent name “Cold-rolled enamel steel with excellent anti-scaling and ultra-deep drawing properties and its manufacturing method”, CN102899565A and patent name “A cold-rolled enamel steel and its manufacturing method”, CN1045813AA and patent name “Enameled steel plate and its manufacturing method”, CN100396808CA and patent name “Cold-rolled enamel steel with excellent anti-scaling and ultra-deep drawing properties and its manufacturing method”, CN101684532AA and patent name “A cold-rolled enamel steel for water heaters and its production method”, CN100396808C and patent name “Cold-rolled enamel steel with excellent anti-scaling and ultra-deep drawing properties and its manufacturing method”, and CN 117535490 and patent name… Patent AA is titled "Preparation Method of Cold-Rolled High-Strength Enameled Steel" and patent publication number CN101812630A is titled "Hot-Rolled High-Strength Enameled Steel Sheet for Deep Drawing and its Manufacturing Method". However, excessive Ti content in the steel reduces the adhesion between the enamel and the substrate, affecting the overall enamel coating performance of the steel sheet. Therefore, some researchers have reduced the Ti content in the steel and added Cu, Nb, and Mo elements to improve the strength and anti-scaling properties of the enamel steel, resulting in the formation of Mn-Nb or other elemental composite oxides in the steel sheet. For example, patent publication number CN 116200670A is titled "A Cold-Rolled Enameled Steel Sheet with Excellent Adhesion Performance and its Manufacturing Method" and patent publication number CN 101586210A is titled "High-Strength Enameled Steel and its Production and Enameling Process".In addition, some researchers have used methods such as adding Mn to steel to improve its strength, increasing the manganese and titanium content in low-carbon steel, or adding one or more alloying elements from Cu, Cr, Ni, Mo, and B to steel to generate Mn-containing composite oxides with other elements, increasing hydrogen trapping, etc., to simultaneously improve the anti-scaling performance and strength of enamel steel. For example, patent publication number CN 102251174A is entitled "A method for manufacturing enamel steel and its cold-rolled sheet", and patent publication number CN 115305411A is entitled "A method for efficient production of ultra-deep drawing cold-rolled enamel steel". In addition, high-oxygen steel is another method to improve the anti-scaling performance of steel plates, such as the patents CN111057828A entitled "A High-Oxygen Enamel Steel and Its Production Method", CN107916371A entitled "A Production Method of Enamel Steel", and CN121874669A entitled "A High-Oxygen Cold-Rolled Enamel Steel and Its Preparation Method". However, although these methods improve the strength and anti-scaling performance of enamel steel, they have other shortcomings: 1) Excessive strip-shaped MnS in the steel will exacerbate the anisotropy of the steel plate; 2) Mo will make the appearance of white porcelain and light-colored porcelain products unqualified; 3) B in the steel preferentially reacts with N to form BN, reducing the amount of TiN and Nb (C,N) formed, thereby reducing the anti-scaling performance of the steel plate. In fact, due to the presence of Ti-containing precipitates in enamel steel, the particle shape is square or rectangular, while the particles of oxides such as MnO and Al2O3 are triangular. Because these particles are hard, they cause stress concentration in the steel matrix during the plastic deformation process of the steel plate. This leads to increased fracture sensitivity of the steel and a decrease in the elongation of the steel plate. Therefore, how to ensure excellent anti-scaling performance while maintaining high strength and minimizing the strength reduction before and after enameling, and at the same time maintaining good elongation performance, has become a pressing technical challenge for enamel steel. Summary of the Invention
[0003] The purpose of this invention is to provide a method for manufacturing high-strength cold-rolled steel sheets for enamel. This invention utilizes a rational multi-element composite addition process, combined with a specific hot-rolled slow cooling and cold-rolled continuous annealing and over-aging process, to form a large number of stable, fine spherical precipitates in the matrix. These thermally stable second phases effectively pinnate grain boundaries during the subsequent 850℃ high-temperature enamel firing process, inhibiting matrix coarsening and a sharp decrease in dislocation density. This results in a yield strength decrease of less than 50 MPa after enamel firing, and an absolute change in TH2 value of <2 min / mm2 after high-temperature enamel firing, meeting the performance requirements of anti-scaling properties and high strength for enamel products.
[0004] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0005] This invention discloses a method for manufacturing high-strength cold-rolled steel sheet for enamel enamel, the method comprising the following steps:
[0006] 1) Smelt according to chemical composition requirements and continuously cast into ingots or billets;
[0007] 2) Heat the ingot or billet to 1200-1250℃, hold it at that temperature, and then roll it out of the furnace. The rough rolling temperature is above 1050℃, the total hot rolling reduction is ≥65%, and the final rolling temperature is controlled at 880-950℃.
[0008] 3) After hot rolling, the coiling temperature is 550~700℃ / s to 560~600℃;
[0009] 4) Perform cold rolling, with a cold rolling reduction rate of not less than 85% to 93%, to obtain cold-rolled sheet;
[0010] 5) Continuous annealing treatment of cold-rolled sheet: first heat to 680-700℃, hold for 3-6 minutes, cool to 480-520℃ at a rate of 30-50℃ / s, hold for 8-15 minutes, and then air cool to room temperature;
[0011] 6) The steel plate is enameled at a high temperature of 850-880℃ for 4-15 minutes. After enameling, the yield strength of the steel plate is ≥325MPa, and the difference between the yield strength and the yield strength before enameling is ≤50MPa. Furthermore, the absolute change in TH2 value before and after enameling is <2 min / mm. 2 ;
[0012] The chemical composition of the cold-rolled steel sheet, by mass percentage, is as follows: C: 0.04%–0.06%, Si: ≤0.02%, Mn: 0.20%–0.40%, P: ≤0.015%, S: ≤0.035%, Alt: 0.015%–0.04%, Cu: 0.01%–0.03%, Ti: 0.10%–0.14%, N: 0.004%–0.008%, B: 0.002%–0.004%, O: 0.03%–0.05%, Ce: 0.001%–0.010%, with the balance being Fe and unavoidable impurities.
[0013] Furthermore, the relationship between the contents of S, Ti, Mn, and Cu is: S + 0~0.02% = [(0.5~1.5)(Ti-2C)] + 0.01Mn + 0.3~0.5Cu.
[0014] Furthermore, the yield strength after cold rolling and continuous annealing can reach over 350 MPa, while the elongation is over 44%, and the hydrogen permeation time (TH2) is ≥9 min / mm. 2 .
[0015] Furthermore, the chemical composition of the cold-rolled steel sheet by mass percentage is as follows: C: 0.047%, Si: 0.01%, Mn: 0.35%, P: 0.01%, S: 0.03%, Alt: 0.025%, Cu: 0.02%, Ti: 0.12%, N: 0.006%, B: 0.003%, O: 0.038%, Ce: 0.007%, with the balance being Fe and unavoidable impurities.
[0016] Furthermore, the ingot is heated to 1250°C, held for 30 minutes, and then hot-rolled on a two-roll mill with a total reduction of 70% and a final rolling temperature of 900°C. After hot rolling, it is rapidly cooled to 580°C and held at that temperature for 1 hour, after which it is slowly cooled to room temperature in the furnace.
[0017] Furthermore, cold rolling is then carried out, with a cold rolling reduction rate of 90%.
[0018] Furthermore, the cold-rolled sheet was subjected to simulated continuous annealing: heated to 685℃, held for 4 min 35 s, then rapidly cooled to 500℃ at 50℃ / s, held for 10 min, and then air-cooled to room temperature.
[0019] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0020] 1) High strength with minimal decrease after enameling. This invention utilizes a reasonable relationship between the contents of S, Ti, Mn, and Cu, combined with a specific hot-rolled slow cooling and cold-rolled continuous annealing and over-aging process, to form a large number of stable, fine spherical precipitates in the matrix, including Ti(C,N), BN and Ce composites, and rare earth oxide sulfides. These thermally stable second phases effectively pinn grain boundaries and inhibit matrix coarsening during the subsequent 850℃ high-temperature enameling process, resulting in a yield strength decrease of less than 50 MPa after enameling, while still maintaining high strength to meet the load-bearing requirements of the product.
[0021] 2) Excellent and stable resistance to hydrogen splattering. The abundant dispersed spheroidized precipitates provide irreversible hydrogen traps, ensuring the steel plate maintains a high-density hydrogen capture capacity both before and after enameling. Actual measurements show that the hydrogen splatter (TH) value shows almost no decrease after high-temperature enameling, fundamentally eliminating splattering defects.
[0022] 3) Excellent comprehensive mechanical properties. The yield strength of the steel plate before enameling can reach more than 350MPa, the tensile strength exceeds 400MPa, and the elongation is as high as 44% or more. After enameling, the decrease is less than 50MPa. It has both high strength and excellent formability, which fully meets the stringent requirements of stamping and final enamel products for the substrate. Detailed Implementation
[0023] A high-strength cold-rolled steel sheet for enamel coating has the following chemical composition by weight percentage: C: 0.04%–0.06%, Si: ≤0.02%, Mn: 0.30%–0.40%, P: ≤0.015%, S: ≤0.035%, Alt: 0.02%–0.03%, Cu: 0.01%–0.03%, Ti: 0.10%–0.14%, N: 0.004%–0.008%, B: 0.002%–0.004%, O: 0.03%–0.05%, Ce: 0.005%–0.010%, with the balance being Fe and unavoidable impurities. The relationship between the contents of S, Ti, Mn, and Cu is: S + 0~0.02% = [(0.5~1.5)(Ti-2C)] + 0.01Mn + 0.3~0.5Cu. The manufacturing process is as follows:
[0024] 1) Smelt according to the above chemical composition and continuously cast into ingots or billets;
[0025] 2) Heat the ingot or billet to 1200-1250℃, hold it at that temperature, and then roll it out of the furnace. The rough rolling temperature is above 1050℃, the total hot rolling reduction is ≥65%, and the final rolling temperature is controlled at 880-950℃.
[0026] 3) After hot rolling, the coiling temperature is 550~700℃ / s to 560~600℃;
[0027] 4) Perform cold rolling, with a cold rolling reduction rate of not less than 85% to 93%, to obtain cold-rolled sheet;
[0028] 5) Perform continuous annealing on cold-rolled sheets: first heat to 680-700℃, hold for 3-6 minutes, cool to 480-520℃ at a rate of 30-50℃ / s, hold for 8-15 minutes, and then air cool to room temperature.
[0029] 6) The steel plate is enameled at a high temperature of 850-880℃ for 4-15 minutes. After enameling, the yield strength of the steel plate is ≥325MPa, and the difference between the yield strength and the yield strength before enameling is ≤50MPa. Furthermore, the absolute change in TH2 value before and after enameling is <2 min / mm. 2 .
[0030] Example
[0031] The steel was smelted and cast into ingots according to the composition of No. 1 steel shown in Table 1.
[0032] Table 1 Chemical composition (wt%) of the steel in the examples
[0033] serial number C Si Mn P S Alt Cu Ti N B O Ce Fe 1# 0.047 0.01 0.35 0.01 0.03 0.025 0.02 0.12 0.006 0.003 0.038 0.007 the remaining
[0034] The ingots with the composition shown in Table 1 were heated to 1250℃ and held for 30 min, then hot-rolled on a two-roll mill with a total reduction of 70% and a final rolling temperature of 900℃. After hot rolling, the ingots were rapidly cooled to 580℃ and held at this temperature for 1 hour, followed by slow furnace cooling to room temperature. Cold rolling was then performed with a reduction of 90%. Simulated continuous annealing was then applied to the cold-rolled sheets: heating to 685℃, holding for 4 min 35 s, then rapidly cooling to 500℃ at a rate of 50℃ / s, holding for 10 min, and finally air-cooling to room temperature.
[0035] Two tensile specimens were cut from the annealed plate along the rolling direction. After surface mechanical polishing, they were subjected to uniaxial tensile testing at room temperature at a rate of 0.5 mm / min on a Zwick-100 tensile testing machine, and the average value was taken. Hydrogen permeation tests were conducted using conventional methods to obtain the TH value. Another cold-rolled annealed plate was heated to 850℃ and held for 4 minutes to simulate enameling. Tensile and hydrogen permeation tests were also performed on the enameled specimens. Specific results are shown in Table 2.
[0036] Table 2. Test results of mechanical properties and TH values of cold-rolled annealed sheets and simulated enameling sheets.
[0037] Sample number Yield strength (MPa) Tensile strength (MPa) Elongation after fracture (%) <![CDATA[TH2(min / mm 2 )]]> Cold rolling annealing-1 351 401 44 19.8 Cold rolling annealing-2 363 414 45 19.5 Enameling-1 328 398 48 20.1 Enameling-2 333 398 44 19.3
[0038] As shown in Table 2, the cold-rolled annealed steel plate of the present invention has a yield strength of 351–363 MPa, with an average value of 357 MPa, a tensile strength of 401–414 MPa, an elongation of 44–45%, and a TH2 value of 19.5–19.8 min / mm. 2 After simulated enameling at 850℃, the yield strength was 328–333 MPa, with an average of 331 MPa, a decrease of only 26–30 MPa compared to before enameling; the average TH2 value after enameling was 19.3–20.1 min / mm. 2 There was no significant change compared to before the enamel firing.
[0039] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A method of manufacturing a high-strength cold-rolled steel sheet for enamel, characterized by, The manufacturing process steps are as follows: 1) Smelt according to chemical composition requirements and continuously cast into ingots or billets; 2) Heat the ingot or billet to 1200-1250℃, hold it at that temperature, and then roll it out of the furnace. The rough rolling temperature is above 1050℃, the total hot rolling reduction is ≥65%, and the final rolling temperature is controlled at 880-950℃. 3) After hot rolling, the coiling temperature is 550~700℃ / s to 560~600℃; 4) Perform cold rolling, with a cold rolling reduction rate of not less than 85% to 93%, to obtain cold-rolled sheet; 5) Continuous annealing treatment of cold-rolled sheet: first heat to 680-700℃, hold for 3-6 minutes, cool to 480-520℃ at a rate of 30-50℃ / s, hold for 8-15 minutes, and then air cool to room temperature; 6) the steel plate is fired at high temperature, 850-880℃, the firing time is 4-15min, the yield strength of the steel plate after firing is ≥325MPa, and the difference value with the yield strength before firing is ≤50MPa, and the absolute change amount of TH2 value before and after firing is <2min / mm 2 ; The chemical composition of the cold-rolled steel sheet, by mass percentage, is as follows: C: 0.04%–0.06%, Si: ≤0.02%, Mn: 0.20%–0.40%, P: ≤0.015%, S: ≤0.035%, Alt: 0.015%–0.04%, Cu: 0.01%–0.03%, Ti: 0.10%–0.14%, N: 0.004%–0.008%, B: 0.002%–0.004%, O: 0.03%–0.05%, Ce: 0.001%–0.010%, with the balance being Fe and unavoidable impurities.
2. The method for manufacturing high-strength cold-rolled steel sheet for enamel as described in claim 1, characterized in that, The relationship between the contents of S, Ti, Mn and Cu is: S + 0 ~ 0.02% = [(0.5 ~ 1.5 )(Ti - 2C)] + 0.01Mn + 0.3 ~ 0.5Cu.
3. The method for manufacturing high-strength cold-rolled steel sheet for enamel as described in claim 1, characterized in that, The yield strength of the cold-rolled continuous annealing treated steel can reach 350 MPa or more, and the elongation is as high as 44% or more, and the hydrogen permeation time TH2 value is ≥9 min / mm 2 .
4. The method for manufacturing high-strength cold-rolled steel sheet for enamel as described in claim 1, characterized in that, The chemical composition of the cold-rolled steel sheet, by mass percentage, is: C: 0.047%, Si: 0.01%, Mn: 0.35%, P: 0.01%, S: 0.03%, Alt: 0.025%, Cu: 0.02%, Ti: 0.12%, N: 0.006%, B: 0.003%, O: 0.038%, Ce: 0.007%, with the balance being Fe and unavoidable impurities.
5. The method for manufacturing high-strength cold-rolled steel sheet for enamel as described in claim 4, characterized in that, The ingot is heated to 1250℃ and held for 30 minutes. It is then hot rolled on a two-roll mill with a total reduction of 70% and a final rolling temperature of 900℃. After hot rolling, it is rapidly cooled to 580℃ and held at that temperature for 1 hour. After that, it is slowly cooled to room temperature in the furnace.
6. The method for manufacturing high-strength cold-rolled steel sheet for enamel as described in claim 5, characterized in that, It is then subjected to cold rolling with a reduction rate of 90%.
7. The method for manufacturing high-strength cold-rolled steel sheet for enamel as described in claim 6, characterized in that, Simulated continuous annealing of cold-rolled steel sheets: heating to 685℃, holding for 4 min 35 s, then rapidly cooling to 500℃ at 50℃ / s, holding for 10 min, and then air cooling to room temperature.
Citation Information
Patent Citations
Cold rolling glass-lined steel having excellent scale cracking resistance and extra-deep drawing property and manufacturing method thereof
CN100396808C
High strength enamel steel and producing technology and enamel firing technology thereof
CN101586210A
Enamel steel for cold rolling water heater and manufacturing method thereof
CN101684532A
Hot-rolling high-strength enamel sheet for deep drawing and manufacturing method thereof