A method for increasing the equiaxed grain ratio in high-carbon steel billets

By optimizing the rare earth addition timing and continuous casting parameters in the production of high carbon steel billets, the problems of high columnar crystal ratio and low rare earth residue were solved, achieving a stable increase in the equiaxed crystal ratio and improved billet quality, thereby enhancing the performance of rolled products and batch consistency.

CN123108398APending Publication Date: 2026-11-17INNER MONGOLIA BAOTOU STEEL UNION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611411971.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The proportion of columnar crystals in existing high-carbon steel billets is too high. The unreasonable timing of rare earth addition results in a low effective rare earth residue, making it impossible to steadily increase the proportion of equiaxed crystals. Furthermore, the existing process cannot be adapted to a 150mm cross-section and a continuous casting speed of 2m/min, making it difficult to eliminate carbon segregation and porosity defects in the billet. The shrinkage rate and drawing stability of the rolled wire rod do not meet the standards.

Method used

After converter smelting, LF refining is carried out to control the oxygen content of the molten steel. At the end of the refining process, a lanthanum-cerium mixed rare earth ferroalloy is added in one go. Combined with appropriate argon blowing and constant casting speed, the residual amount of rare earth is controlled at 80ppm. The cooling parameters of the crystallizer and the secondary cooling zone are optimized to ensure uniform distribution of rare earth and equiaxed crystal nuclei.

Benefits of technology

It significantly increased the proportion of equiaxed crystals to over 52%, improved the porosity and carbon segregation in the center of the billet, reduced the shrinkage rate and wire breakage rate of the rolled product, and improved the consistency of product quality and mechanical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for increasing the equiaxed crystal ratio in high-carbon steel billets, belonging to the field of high-quality high-carbon steel continuous casting production technology. It is used for the production of 150mm×150mm SWRH82B steel billets, with a constant continuous casting speed of 2m / min. After pre-deoxidation in a converter, the billets are refined by LF (sulfurized iron-phosphate) refining. A lanthanum-cerium mixed rare earth ferroalloy is added once at the end of refining and before soft blowing to control the total residual rare earth content in the molten steel. The chemical composition of the SWRH82B steel is as follows: C 0.80-0.83, Si 0.18-0.26, Mn 0.60-0.75, P≤0.012, S≤0.008, Cr0.02-0.06, Re0.0080, with the balance being iron and unavoidable impurities. The purpose of this invention is to solve the problems of "difficulty in eliminating carbon segregation and porosity defects in billets, and insufficient reduction of area and drawing stability of rolled wire rods."
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of high-quality high-carbon steel continuous casting production technology, and particularly relates to a method for increasing the equiaxed crystal ratio of high-carbon steel billets. Background Technology

[0002] SWRH82B high-carbon steel has a high carbon content and a wide solidification range. Under conventional smelting and continuous casting processes, the molten steel exhibits strong directional heat transfer characteristics during solidification, with columnar crystal zones accounting for over 70% of the billet's interior and equiaxed crystals accounting for less than 30%. The well-developed columnar crystals easily induce central carbon segregation and core porosity defects, leading to a high wire breakage rate during subsequent wire drawing. Existing methods for improving equiaxed crystal formation fall into two categories: one is electromagnetic stirring in the crystallizer with light pressure at the end, which has high equipment modification costs and significantly diminishes grain refinement effects under high drawing speeds; the other is adding rare earth elements to the steel. Current processes often involve adding rare earth elements at converter tapping or ladle entry, resulting in premature reaction and loss of rare earth elements with oxygen and sulfur in the steel, leading to low effective residual amounts and an inability to stably induce equiaxed crystal nucleation. The existing rare earth addition process is not matched with the high-speed solidification characteristics of SWRH82B, and the rare earth inclusions are too large to serve as heterogeneous nucleation cores. In addition, there is a lack of a complete set of processes that can fix the target amount of rare earth residue and are suitable for the 2m / min casting speed of 150mm square billet. The consistency of microstructure control is poor, the equiaxed crystal ratio of the same batch of billets fluctuates by more than 15%, and the mechanical properties are too discrete. Summary of the Invention

[0003] The purpose of this invention is to provide a method for increasing the proportion of equiaxed crystals in high-carbon steel billets, thereby solving the problems of "existing high-carbon steel billet columnar crystal ratio, high investment cost of electromagnetic stirring equipment; unreasonable rare earth addition sequence leading to low effective rare earth residue, making it impossible to stably increase the proportion of equiaxed crystals; lack of a rare earth precision quantity control smelting process suitable for 150mm cross-section, 2m / min continuous casting speed, and SWRH82B steel grade, making it difficult to eliminate carbon segregation and porosity defects in billets, and failing to meet the requirements for cross-sectional shrinkage rate and drawing stability of rolled wire rods".

[0004] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0005] This invention discloses a method for increasing the equiaxed grain ratio in high-carbon steel billets, used in the production of 150mm×150mm SWRH82B steel billets with a constant continuous casting speed of 2m / min; characterized by comprising the following steps:

[0006] After pre-deoxidation in the converter, the steel is refined by LF (sulfurized iron-oxide) refining. In the early stage of LF refining, white slag is generated to reduce the total oxygen content of the molten steel to below 18 ppm. At the end of refining and before soft blowing, a lanthanum-cerium mixed rare earth ferroalloy is added once to control the total residual rare earth content of the molten steel to 80 ppm. After the rare earth is added, bottom blowing with argon is performed for 12-15 minutes, with an argon flow rate of 0.18-0.22 Nm³ / t steel. After quenching, 150 mm square billets are continuously cast at a constant casting speed of 2 m / min. The cooling water flow rate of the crystallizer is 2200-2400 L / min, and the water content in the secondary cooling zone is 0.95 L / kg steel (preferably 0.95 L / kg steel).

[0007] The chemical composition of the SWRH82B steel by mass fraction is: C 0.80-0.83, Si 0.18-0.26, Mn 0.60-0.75, P≤0.012, S≤0.008, Cr0.02-0.06, Re0.0080, with the balance being iron and unavoidable impurities.

[0008] Furthermore, during the converter tapping stage, the slag basicity is controlled at 2.8-3.2, and the slag TFe ≤ 1.2%.

[0009] Furthermore, the resulting slab has an equiaxed crystal ratio of ≥52%, a tensile strength of 1180-1230 MPa in the rolled wire rod, a reduction of area of ​​≥34%, and a carbon segregation index of ≤1.03.

[0010] Furthermore, the converter smelting of SWRH82B resulted in a final carbon content of 0.80 wt%, pre-deoxidation at tapping, and a ladle slag basicity of 3.0 with TFe = 1.05%.

[0011] Furthermore, during the early stage of LF refining, white slag treatment resulted in 16 ppm of total oxygen in the molten steel; and before soft blowing at the end of refining, lanthanum-cerium rare earth iron alloy was added, resulting in 80 ppm of residual Re in the molten steel.

[0012] Furthermore, soft argon blowing was performed for 13 minutes at an argon flow rate of 0.20 Nm³ / t steel.

[0013] Furthermore, the continuous casting process involves 150mm square billets, a casting speed of 2m / min, a crystallizer water flow rate of 2300L / min, and a secondary cooling water flow rate of 0.95L / kg steel.

[0014] Furthermore, the continuous casting process involves 150mm square billets, a casting speed of 2m / min, a crystallizer water flow rate of 2300L / min, and a secondary cooling water flow rate of 0.95L / kg steel.

[0015] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0016] 1) Rare earth is added at the end of refining to avoid rare earth loss caused by deoxidation and desulfurization in the early stage, and to achieve an effective rare earth residue of 80ppm with precision and stability. The rare earth oxysulfide size is 2-4μm, which is uniformly distributed and acts as a solidification heterogeneous nucleation core, greatly inhibiting columnar crystal elongation; 2) The process is adapted to 150mm cross section and 2m / min high-speed continuous casting, without the need to add electromagnetic stirring and light reduction equipment. The investment in production line transformation is low, and the original smelting and continuous casting equipment can be put into production directly; 3) The proportion of equiaxed crystals is increased to more than 52%, the porosity of the billet center and carbon segregation are significantly improved, the section shrinkage rate of rolled material is increased by 6-8 percentage points, and the downstream wire breakage rate is reduced by more than 40%; 4) The soft blowing parameters are matched with the rare earth addition sequence. The fluctuation of the equiaxed crystal ratio of the same batch of billets is ≤5%, the dispersion of product mechanical properties is reduced, and the batch quality consistency is improved. Detailed Implementation

[0017] Example 1 (Process of the Invention)

[0018] 1) Converter smelting of SWRH82B, final carbon content 0.80wt%, pre-deoxidation at tapping, ladle slag basicity 3.0, TFe=1.05%; 2) White slag treatment in the early stage of LF refining, total oxygen in molten steel 16ppm; Lanthanum-cerium rare earth ferroalloy added before soft blowing at the end of refining, residual Re in molten steel 80ppm; 3) Soft blowing with argon for 13min, argon flow rate 0.20Nm³ / t steel; 4) Continuous casting of 150mm square billet, casting speed 2m / min, crystallizer water flow rate 2300L / min, secondary cooling water flow rate 0.95L / kg steel. Measured equiaxed crystal ratio of the billet was 54%; wire rod tensile strength was 1205MPa, reduction of area was 35.2%, and carbon segregation index was 1.02.

[0019] Comparative Example 1 (Rare earth elements were added during steelmaking; other parameters were the same as in Example 1)

[0020] An equal amount of rare earth alloy was added simultaneously with the converter tapping process, followed by LF refining and soft blowing for 13 minutes, using the same continuous casting parameters. The residual rare earth in the molten steel was only 32 ppm, the equiaxed crystal ratio of the billet was 27%, the section reduction rate of the wire rod was 27.1%, and the central carbon segregation index was 1.09.

[0021] Comparative Example 2 (no rare earth added, conventional process)

[0022] No rare earth elements were added throughout the process, and all other smelting and continuous casting parameters were consistent with those in Example 1. The equiaxed crystal content of the billet was 26%, the section shrinkage rate of the wire rod was 26.5%, and the frequency of wire breakage during drawing was significantly higher.

[0023] Comparative Example 3 (rare earth residue 50 ppm, other parameters the same as Example 1)

[0024] Reducing rare earth addition at the end of refining resulted in a residual Re content of 50 ppm in the molten steel. The equiaxed crystal content of the billet was 38%, failing to achieve the desired stable microstructure optimization.

[0025] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A method for increasing the equiaxed grain ratio in high-carbon steel billets, used in the production of 150mm×150mm billets of SWRH82B steel, with a constant continuous casting speed of 2m / min; characterized in that, Includes the following steps: After pre-deoxidation in the converter, the steel is refined by LF (sulfurized iron-phosphate) refining. In the early stage of LF refining, white slag is generated to reduce the total oxygen in the molten steel to below 18 ppm. At the end of refining and before soft blowing, a lanthanum-cerium mixed rare earth ferroalloy is added once to control the total residual amount of rare earth in the molten steel. After the rare earth is added, bottom blowing and argon soft blowing are performed for 12-15 minutes with an argon flow rate of 0.18-0.22 Nm³ / t steel. After killing, 150 mm square billets are continuously cast at a constant casting speed of 2 m / min. The cooling water flow rate in the crystallizer is 2200-2400 L / min, and the water flow rate in the secondary cooling zone is 0.9-1.0 L / kg steel. The chemical composition of the SWRH82B steel by mass fraction is: C 0.80-0.83, Si 0.18-0.26, Mn 0.60-0.75, P≤0.012, S≤0.008, Cr0.02-0.06, Re0.0080, with the balance being iron and unavoidable impurities.

2. The method for increasing the equiaxed grain ratio of high-carbon steel billets according to claim 1, characterized in that, During the converter tapping stage, the slag basicity should be controlled at 2.8-3.2, and the slag TFe ≤ 1.2%.

3. The method for increasing the equiaxed grain ratio of high-carbon steel billets according to claim 1, characterized in that, The resulting slab has an equiaxed crystal ratio of ≥52%, a tensile strength of 1180-1230 MPa for the rolled wire rod, a reduction of area of ​​≥34%, and a carbon segregation index of ≤1.

03.

4. The method for increasing the equiaxed grain ratio of high-carbon steel billets according to claim 1, characterized in that, SWRH82B was smelted in a converter, with a final carbon content of 0.80 wt%, pre-deoxidized before tapping, and the ladle slag basicity of 3.0 and TFe=1.05%.

5. The method for increasing the equiaxed grain ratio of high-carbon steel billets according to claim 4, characterized in that, During the early stage of LF refining, white slag treatment resulted in 16 ppm of total oxygen in the molten steel. Before soft blowing at the end of refining, lanthanum-cerium rare earth iron alloy was added, resulting in 80 ppm of residual Re in the molten steel.

6. The method for increasing the equiaxed grain ratio of high-carbon steel billets according to claim 5, characterized in that, Soft blowing of argon for 13 minutes, argon flow rate 0.20 Nm³ / t steel.

7. The method for increasing the equiaxed grain ratio of high-carbon steel billets according to claim 6, characterized in that, Continuous casting of 150mm square billets, casting speed of 2m / min, crystallizer water flow of 2300L / min, secondary cooling water flow of 0.95L / kg steel.

8. The method for increasing the equiaxed grain ratio of high-carbon steel billets according to claim 7, characterized in that, Continuous casting of 150mm square billets, casting speed of 2m / min, crystallizer water flow of 2300L / min, secondary cooling water flow of 0.95L / kg steel.