A gear steel suitable for extremely cold environments and its preparation method

By employing smelting, upsetting, drawing, and heat treatment processes with specific chemical compositions and process designs, the problem of insufficient gear material performance in extremely cold environments has been solved, resulting in the production of gear steel that meets the requirements for use in extremely cold environments, thereby improving its reliability and service life in such environments.

CN123108418APending Publication Date: 2026-11-17TAIYUAN HEAVY IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611131028.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing gear materials cannot meet the requirements for toughness and fatigue performance in extremely cold environments, especially at -60℃, and there is a lack of suitable materials and performance standards.

Method used

Gear steel is prepared by employing specific chemical compositions and process designs, including smelting, upsetting and drawing, and heat treatment processes. The specific steps include smelting, forging and heat treatment, and the chemical composition and process parameters are controlled to improve the material properties.

Benefits of technology

Gear steel with hardness ≥280HRW, tensile strength ≥910MPa, yield strength ≥790MPa, elongation after fracture ≥20%, reduction of area ≥65%, and Charpy V-notch impact strength ≥85J at -60℃ was prepared, meeting the requirements for use in extremely cold environments and improving the reliability and service life of gears.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108418A_ABST
    Figure CN123108418A_ABST
Patent Text Reader

Abstract

This invention discloses a gear steel suitable for extremely cold environments and its preparation method. The method includes: smelting to prepare a gear steel ingot, the chemical composition of which is: C: 0.35~0.40%, Si: 0.3~0.37%, Mn: 0.55~0.7%, Cr: 1.3~1.5%, Ni: 2.8~3.0%, Mo: 0.2~0.3%, V: 0.1~0.2%, Nb: 0.01~0.025%, S≤0.01%, P≤0.01%; forging the gear steel ingot to obtain a gear steel billet; and heat-treating the gear steel billet, including pre-heat treatment and secondary quenching. Through reasonable chemical composition and process design, this invention obtains a gear steel suitable for extremely cold environments that fully meets the requirements for toughness, fatigue resistance, and other mechanical properties in such environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal material preparation technology, and more specifically relates to a gear steel suitable for extremely cold environments and its preparation method. Background Technology

[0002] Gearboxes (such as those used in mining excavators) have a wide range of applications, often in extreme environments and harsh working conditions, especially in extremely cold environments. Typical ambient temperatures in extremely cold environments can reach -40°C, with some extreme cases reaching -60°C. These extremely low temperatures affect the material properties and meshing characteristics of gears, resulting in significant differences in reliability, load-bearing capacity, and service life compared to gears at normal temperatures. Currently, research on gear materials suitable for extremely cold environments is limited, and there are no relevant material and performance standards. Gear materials used in extremely cold environments must possess certain toughness and fatigue resistance at low temperatures. Studies have shown that the ductile-brittle transition temperature of general gear materials is between -40°C and -50°C, which is insufficient to meet performance requirements in extremely cold environments (-60°C). Summary of the Invention

[0003] To address some or all of the technical problems existing in the prior art, this invention provides a gear steel suitable for extremely cold environments and its preparation method. Through reasonable chemical composition and process design, and by adopting smelting, upsetting and drawing, and heat treatment processes, gear steel with mechanical properties that meet the requirements for use in extremely cold environments is obtained.

[0004] In a first aspect of the present invention, a gear steel suitable for extremely cold environments and a method for preparing the same are provided, comprising the following steps: S1. Smelting and preparing gear steel ingots, wherein the chemical composition of the gear steel ingots is controlled by mass percentage as follows: C: 0.35~0.40%, Si: 0.3~0.37%, Mn: 0.55~0.7%, Cr: 1.3~1.5%, Ni: 2.8~3.0%, Mo: 0.2~0.3%, V: 0.1~0.2%, Nb: 0.01~0.025%, S≤0.01%, P≤0.01%, with the balance being Fe and unavoidable impurities; S2. Forging the gear steel ingot to obtain a gear steel billet; S3. The gear steel billet is subjected to heat treatment, wherein the heat treatment includes pre-heat treatment and secondary quenching treatment.

[0005] Furthermore, in step S2, forging includes an upsetting process and a drawing process, wherein the upsetting forging ratio is controlled to be 4.4~4.6 and the drawing forging ratio is controlled to be 8.0~8.2.

[0006] Furthermore, in step S2, the heating forging temperature is controlled at 1200~1250℃, and the final forging temperature is controlled at not less than 850℃.

[0007] Further, in step S3: The preheating process includes: (1) heating the gear steel billet to 940~960℃, holding time based on the effective thickness of the gear steel billet according to 2.4~2.6h / 100mm, and air cooling; (2) heating the gear steel billet to 650~670℃, holding time based on the effective thickness of the gear steel billet according to 2.4~2.6h / 100mm, furnace cooling to ≤500℃ and then air cooling. The secondary quenching process includes: (1) heating the gear steel billet to 850~870℃, holding time based on the effective thickness of the gear steel billet at 1.9~2.1h / 100mm, and cooling method is oil cooling; (2) heating the gear steel billet to 740~760℃, holding time based on the effective thickness of the gear steel billet at 1.9~2.1h / 100mm, and cooling method is oil cooling; (3) holding at 550~570℃ and then air cooling, holding time based on the effective thickness of the gear steel billet at 4.9~5.1h / 100mm; (4) holding at 530~550℃ and then air cooling, holding time based on the effective thickness of the gear steel billet at 4.9~5.1h / 100mm.

[0008] Further, step S2 includes the following steps: S21. The heating forging temperature is controlled at 1200~1250℃, and the final forging temperature is controlled at no less than 850℃. S22. Cut the spindle, upset it to Ø320mm, and then stretch it to 200mm in octagon using an anvil. S23, upset to Ø275mm, then lengthened to 170mm using upper and lower flat anvils; S24, upset to Ø235mm, then lengthened to 130mm using upper and lower flat anvils; S25. Using a flat anvil, lengthen to 105mm×105mm×L and correct the shape.

[0009] Furthermore, in step S3: The pre-heat treatment includes: (1) heating the gear steel billet to 950°C, holding time based on the effective thickness of the gear steel billet at 2.5h / 100mm, and air cooling; (2) heating the gear steel billet to 660°C, holding time based on the effective thickness of the gear steel billet at 2.5h / 100mm, furnace cooling to 500°C and then air cooling. The secondary quenching process includes: (1) heating the gear steel billet to 860°C, holding time based on the effective thickness of the gear steel billet at 2h / 100mm, and cooling by oil cooling; (2) heating the gear steel billet to 750°C, holding time based on the effective thickness of the gear steel billet at 2h / 100mm, and cooling by oil cooling; (3) holding at 560°C and then air cooling, holding time based on the effective thickness of the gear steel billet at 5h / 100mm; (4) holding at 540°C and then air cooling, holding time based on the effective thickness of the gear steel billet at 5h / 100mm.

[0010] In a second aspect of the invention, a gear steel suitable for extremely cold environments is provided, wherein the chemical composition of the gear steel suitable for extremely cold environments is as follows by mass percentage: C: 0.35~0.40%, Si: 0.3~0.37%, Mn: 0.55~0.7%, Cr: 1.3~1.5%, Ni: 2.8~3.0%, Mo: 0.2~0.3%, V: 0.1~0.2%, Nb: 0.01~0.025%, S≤0.01%, P≤0.01%, with the balance being Fe and unavoidable impurities.

[0011] Furthermore, the gear steel suitable for extremely cold environments has a hardness ≥265HRW, tensile strength ≥860MPa, yield strength ≥680MPa, elongation after fracture ≥18%, reduction of area ≥40%, and Charpy V-notch impact strength ≥70J at -60℃.

[0012] Furthermore, the gear steel suitable for extremely cold environments has a hardness ≥280HRW, tensile strength ≥910MPa, yield strength ≥790MPa, elongation after fracture ≥20%, reduction of area ≥65%, and Charpy V-notch impact strength ≥85J at -60℃.

[0013] The gear steel suitable for extremely cold environments and its preparation method of the present invention have the following advantages and beneficial effects: This invention, through rational chemical composition and process design, employs smelting, upsetting and drawing, and heat treatment processes to obtain gear steel for extremely cold environments with a hardness ≥280HRW, tensile strength ≥910MPa, yield strength ≥790MPa, elongation after fracture ≥20%, reduction of area ≥65%, and Charpy V-notch impact strength ≥85J at -60℃. This fully meets the requirements for toughness, fatigue resistance, and other mechanical properties in extremely cold environments (-60℃), ensuring good reliability, load-bearing capacity, and service life. It fills the technological gap for gear steel suitable for extremely cold environments and is of great significance for promoting the technological development of gear materials for use in extremely cold environments. Attached Figure Description

[0014] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. In the drawings: Figure 1 This is a sequence diagram of the preheating process in the gear steel preparation method suitable for extremely cold environments according to the present invention; Figure 2 This is a sequence diagram of the secondary quenching process in the gear steel preparation method suitable for extremely cold environments of the present invention. Detailed Implementation

[0015] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with specific embodiments and corresponding drawings. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0016] The method for preparing gear steel suitable for extremely cold environments according to the present invention includes the following steps: S1. Smelting and preparing gear steel ingots, wherein the chemical composition of the gear steel ingots is controlled by mass percentage as follows: C: 0.35~0.40%, Si: 0.3~0.37%, Mn: 0.55~0.7%, Cr: 1.3~1.5%, Ni: 2.8~3.0%, Mo: 0.2~0.3%, V: 0.1~0.2%, Nb: 0.01~0.025%, S≤0.01%, P≤0.01%, with the balance being Fe and unavoidable impurities.

[0017] S2. Forging the gear steel ingot to obtain a gear steel billet; S3. The gear steel billet is subjected to heat treatment, wherein the heat treatment includes pre-heat treatment and secondary quenching treatment.

[0018] In one specific implementation, in step S2 above, forging includes an upsetting process and a drawing process. The upsetting forging ratio is controlled at 4.4~4.6, and the drawing forging ratio is controlled at 8.0~8.2. Preferably, the upsetting forging ratio is controlled at 4.5, and the drawing forging ratio is controlled at 8.1.

[0019] As a specific implementation method, in step S3 above, the preheating treatment includes: (1) heating the gear steel billet to 940~960℃, holding time based on the effective thickness of the gear steel billet according to 2.4~2.6h / 100mm, and air cooling; (2) heating the gear steel billet to 650~670℃, holding time based on the effective thickness of the gear steel billet according to 2.4~2.6h / 100mm, furnace cooling to ≤500℃ and then air cooling.

[0020] As a specific implementation method, in step S3 above, the secondary quenching process includes: (1) heating the gear steel billet to 850~870℃, holding time based on the effective thickness of the gear steel billet according to 1.9~2.1h / 100mm, and cooling method is oil cooling; (2) heating the gear steel billet to 740~760℃, holding time based on the effective thickness of the gear steel billet according to 1.9~2.1h / 100mm, and cooling method is oil cooling; (3) holding at a temperature of 550~570℃ and then air cooling, holding time based on the effective thickness of the gear steel billet according to 4.9~5.1h / 100mm; (4) holding at a temperature of 530~550℃ and then air cooling, holding time based on the effective thickness of the gear steel billet according to 4.9~5.1h / 100mm.

[0021] The chemical composition of the gear steel suitable for extremely cold environments prepared by the above-mentioned method is as follows (by mass percentage): C: 0.35~0.40%, Si: 0.3~0.37%, Mn: 0.55~0.7%, Cr: 1.3~1.5%, Ni: 2.8~3.0%, Mo: 0.2~0.3%, V: 0.1~0.2%, Nb: 0.01~0.025%, S≤0.01%, P≤0.01%, with the balance being Fe and unavoidable impurities.

[0022] The gear steel of the present invention, suitable for extremely cold environments, has a hardness ≥265HRW, tensile strength ≥860MPa, yield strength ≥680MPa, elongation after fracture ≥18%, reduction of area ≥40%, and Charpy V-notch impact strength ≥70J at -60℃.

[0023] Preferably, the gear steel of the present invention suitable for extremely cold environments has a hardness ≥280HRW, tensile strength ≥910MPa, yield strength ≥790MPa, elongation after fracture ≥20%, reduction of area ≥65%, and Charpy V-notch impact strength ≥85J at -60℃.

[0024] The following detailed description of the gear steel suitable for extremely cold environments and its preparation method according to the present invention is provided in conjunction with embodiments. The implementation methods in the following embodiments, unless otherwise specified, are carried out according to conventional methods and conditions, and the present invention does not impose specific limitations on them.

[0025] Example 1 The specific implementation process of the gear steel preparation method suitable for extremely cold environments in Embodiment 1 of the present invention is as follows: Gear steel ingots are prepared by smelting, wherein the chemical composition of the gear steel ingots is controlled by mass percentage as follows: C: 0.387%, Si: 0.367%, Mn: 0.662%, Cr: 1.453%, Ni: 2.865%, Mo: 0.25%, V: 0.156%, Nb: 0.0239%, S: 0.0034%, P: 0.0045%, with the balance being Fe and unavoidable impurities.

[0026] The gear steel ingot is upset and drawn to obtain a gear steel billet, wherein the upset forging ratio is 4.5 and the drawing forging ratio is 8.1. Specifically, the process includes: heating and forging temperature controlled at 1200~1250℃, and final forging temperature controlled at not less than 850℃; cutting the ingot, upset to Ø320mm, and drawn to octagonal 200mm using an upper and lower flat anvil with effective compaction; upset to Ø275mm, and drawn to octagonal 170mm using an upper and lower flat anvil with effective compaction; upset to Ø235mm, and drawn to octagonal 130mm using an upper and lower flat anvil with effective compaction; and drawn to 105mm×105mm×L using an upper and lower flat anvil, and then corrected and shaped.

[0027] The gear steel billet is subjected to heat treatment, which includes pre-heat treatment and secondary quenching. For example... Figure 1 As shown, the pre-heat treatment includes: (1) heating the gear steel billet to 950℃, holding time controlled at 2.5h / 100mm based on the effective thickness of the gear steel billet, and air cooling; (2) heating the gear steel billet to 660℃, holding time controlled at 2.5h / 100mm based on the effective thickness of the gear steel billet, furnace cooling to 500℃ followed by air cooling. Figure 2 As shown, the secondary quenching process includes: (1) heating the gear steel billet to 860℃, holding time based on the effective thickness of the gear steel billet according to 2h / 100mm, and cooling method is oil cooling; (2) heating the gear steel billet to 750℃, holding time based on the effective thickness of the gear steel billet according to 2h / 100mm, and cooling method is oil cooling; (3) holding at 560℃ and then air cooling, holding time based on the effective thickness of the gear steel billet according to 5h / 100mm; (4) holding at 540℃ and then air cooling, holding time based on the effective thickness of the gear steel billet according to 5h / 100mm.

[0028] The gear steel prepared using Example 1 of the present invention, suitable for extremely cold environments, has a hardness of 280 HRW, a tensile strength of 914 MPa, a yield strength of 792 MPa, an elongation after fracture of 21%, a reduction of area of ​​67%, and a Charpy V-notch impact strength of 89 J at -60℃.

[0029] In summary, the gear steel suitable for extremely cold environments and its preparation method of the present invention have the following advantages and beneficial effects: This invention, through rational chemical composition and process design, employs smelting, upsetting and drawing, and heat treatment processes to obtain gear steel for extremely cold environments with a hardness ≥280HRW, tensile strength ≥910MPa, yield strength ≥790MPa, elongation after fracture ≥20%, reduction of area ≥65%, and Charpy V-notch impact strength ≥85J at -60℃. This fully meets the requirements for toughness, fatigue resistance, and other mechanical properties in extremely cold environments (-60℃), ensuring good reliability, load-bearing capacity, and service life. It fills the technological gap for gear steel suitable for extremely cold environments and is of great significance for promoting the technological development of gear materials for use in extremely cold environments.

[0030] In the description of this specification, references to terms such as "embodiment," "example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, those skilled in the art can combine or combine the different embodiments or examples described in this specification and the features therein without causing contradiction.

[0031] It should be noted that, unless otherwise specified, the terms used herein have the meanings commonly understood by those skilled in the art. Furthermore, when a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum. Additionally, when multiple ranges are provided to describe features, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0032] It should also be noted that, in this document, the term "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, such that an article or device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such an article or device.

[0033] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit them. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the present invention.

Claims

1. A method for preparing gear steel suitable for extremely cold environments, characterized in that, Includes the following steps: S1. Smelting and preparing gear steel ingots, wherein the chemical composition of the gear steel ingots is controlled by mass percentage as follows: C: 0.35~0.40%, Si: 0.3~0.37%, Mn: 0.55~0.7%, Cr: 1.3~1.5%, Ni: 2.8~3.0%, Mo: 0.2~0.3%, V: 0.1~0.2%, Nb: 0.01~0.025%, S≤0.01%, P≤0.01%, with the balance being Fe and unavoidable impurities; S2. Forging the gear steel ingot to obtain a gear steel billet; S3. The gear steel billet is subjected to heat treatment, wherein the heat treatment includes pre-heat treatment and secondary quenching treatment.

2. The method for preparing gear steel suitable for extremely cold environments according to claim 1, characterized in that, In step S2, forging includes upsetting and drawing processes. The upsetting forging ratio is controlled at 4.4 to 4.6, and the drawing forging ratio is controlled at 8.0 to 8.

2.

3. The method for preparing gear steel suitable for extremely cold environments according to claim 1, characterized in that, In step S2, the heating forging temperature is controlled at 1200~1250℃, and the final forging temperature is controlled at no less than 850℃.

4. The method for preparing gear steel suitable for extremely cold environments according to claim 1, characterized in that, In step S3: The preheating process includes: (1) heating the gear steel billet to 940~960℃, holding time based on the effective thickness of the gear steel billet according to 2.4~2.6h / 100mm, and air cooling; (2) heating the gear steel billet to 650~670℃, holding time based on the effective thickness of the gear steel billet according to 2.4~2.6h / 100mm, furnace cooling to ≤500℃ and then air cooling. The secondary quenching process includes: (1) heating the gear steel billet to 850~870℃, holding time based on the effective thickness of the gear steel billet at 1.9~2.1h / 100mm, and cooling method is oil cooling; (2) heating the gear steel billet to 740~760℃, holding time based on the effective thickness of the gear steel billet at 1.9~2.1h / 100mm, and cooling method is oil cooling; (3) holding at 550~570℃ and then air cooling, holding time based on the effective thickness of the gear steel billet at 4.9~5.1h / 100mm; (4) holding at 530~550℃ and then air cooling, holding time based on the effective thickness of the gear steel billet at 4.9~5.1h / 100mm.

5. The method for preparing gear steel suitable for extremely cold environments according to claim 1, characterized in that: Step S2 includes the following steps: S21. The heating forging temperature is controlled at 1200~1250℃, and the final forging temperature is controlled at no less than 850℃. S22. Cut the spindle, upset it to Ø320mm, and then stretch it to 200mm in octagon using an anvil. S23, upset to Ø275mm, then lengthened to 170mm using upper and lower flat anvils; S24, upset to Ø235mm, then lengthened to 130mm using upper and lower flat anvils; S25. Using a flat anvil, lengthen the material to 105mm×105mm×L and correct its shape. In step S3: The pre-heat treatment includes: (1) heating the gear steel billet to 950°C, holding time based on the effective thickness of the gear steel billet at 2.5h / 100mm, and air cooling; (2) heating the gear steel billet to 660°C, holding time based on the effective thickness of the gear steel billet at 2.5h / 100mm, furnace cooling to 500°C and then air cooling. The secondary quenching process includes: (1) heating the gear steel billet to 860°C, holding time based on the effective thickness of the gear steel billet at 2h / 100mm, and cooling by oil cooling; (2) heating the gear steel billet to 750°C, holding time based on the effective thickness of the gear steel billet at 2h / 100mm, and cooling by oil cooling; (3) holding at 560°C and then air cooling, holding time based on the effective thickness of the gear steel billet at 5h / 100mm; (4) holding at 540°C and then air cooling, holding time based on the effective thickness of the gear steel billet at 5h / 100mm.

6. A gear steel suitable for extremely cold environments, characterized in that, The chemical composition of the gear steel suitable for extremely cold environments, by mass percentage, is as follows: C: 0.35~0.40%, Si: 0.3~0.37%, Mn: 0.55~0.7%, Cr: 1.3~1.5%, Ni: 2.8~3.0%, Mo: 0.2~0.3%, V: 0.1~0.2%, Nb: 0.01~0.025%, S≤0.01%, P≤0.01%, with the balance being Fe and unavoidable impurities.

7. The gear steel suitable for extremely cold environments according to claim 6, characterized in that, The gear steel suitable for extremely cold environments has a hardness ≥265HRW, tensile strength ≥860MPa, yield strength ≥680MPa, elongation after fracture ≥18%, reduction of area ≥40%, and Charpy V-notch impact strength ≥70J at -60℃.

8. The gear steel suitable for extremely cold environments according to claim 6, characterized in that, The gear steel suitable for extremely cold environments has a hardness ≥280HRW, tensile strength ≥910MPa, yield strength ≥790MPa, elongation after fracture ≥20%, reduction of area ≥65%, and Charpy V-notch impact strength ≥85J at -60℃.