600MPa grade high-pore-expanding pickling and baking hardening steel and its manufacturing method
By employing reasonable chemical composition and process design, the mismatch between the baking hardening performance and the high hole expansion performance of high-hole expanded steel has been solved, resulting in high-strength, low-cost high-hole expanded steel sheets suitable for the manufacture of automotive parts.
Patent Information
- Application Number
- CN202610752099.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-28
- Publication Date
- 2026-11-17
AI Technical Summary
In the current development of high-hole-expansion steel, the baking hardening performance is not well matched with the high hole-expansion performance, resulting in high production costs and unreasonable composition design, making it difficult to meet the requirements of automotive parts for high strength, formability and low cost.
The chemical composition of the 600MPa grade high-pore-expansion pickling and baking hardening steel is designed, including the reasonable ratio of elements such as C, Si, Mn, P, Al, Nb, B, and Ti. Through a three-stage laminar flow cooling process and pickling process, polygonal ferrite and bainite structures are formed to ensure high baking hardening and high pore-expansion performance.
It achieves a yield strength ≥440MPa, tensile strength ≥600MPa, elongation ≥17.0%, hole expansion rate ≥75%, and bake hardening amount ≥30MPa, meeting the high hole expansion steel standard, reducing alloy cost, improving formability and dent resistance, and meeting the requirements of automotive lightweighting.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgical technology, specifically relating to 600MPa grade high-hole-expansion pickling and baking hardening steel and its manufacturing method. Background Technology
[0002] High-expansion steel, as a type of advanced high-strength steel (AHSS), has been researched and developed for more than 20 years by international advanced steel companies such as Nippon Steel, JFE, and ThyssenKrupp. It has high strength, high elongation and high expansion performance, which can meet the requirements of complex-shaped automotive parts with high formability requirements, and is widely used in automotive chassis and body structural parts.
[0003] In recent years, due to legal and regulatory requirements on vehicle fuel consumption, the automotive industry has seen an intensified push for lightweighting. Lightweighting of passenger vehicles implies high-strength, thinner materials and more complex chassis structures, inevitably placing higher demands on material properties, surface finish, and forming technologies such as hydroforming, hot stamping, and laser welding. This translates to higher requirements for material strength, stamping performance, flanging, springback, and fatigue resistance. Since increasing material strength can degrade material properties such as formability (processability), achieving high strength without compromising formability has become crucial for developing high-perforation steel sheets.
[0004] In the actual automobile production process, steel sheets are stamped into various parts, and after assembly, they undergo a baking paint process. To adapt to this production process, low-carbon steel and ultra-low-carbon steel are often used. By strictly controlling the proportions of elements such as C, Nb, and Ti, they are made into bake-hardening steel, generally cold-rolled ultra-low-carbon BH steel. In its delivered state, it has a relatively low yield strength, ensuring good stamping performance. After baking paint treatment, a bake-hardening effect occurs, significantly increasing the yield strength. Therefore, bake-hardening steel can effectively resolve the contradiction between the stamping performance, strength, and local dent resistance of automotive sheet metal and body panels, making it one of the most effective methods for achieving automotive lightweighting. As a method that conforms to the automobile body's own production process, bake-hardening does not increase costs. Its strengthening effect can also help further reduce the thickness of the body. Therefore, the bake-hardening value is a very important indicator for steel mills and companies to measure material quality. At the same time, it is also an effective means of improving the strength of high-hole steel without affecting its formability.
[0005] Currently, there are very few requirements for bake hardening amount (BH2) in the development of high-expansion steel and related standards in China. However, there are relevant standards abroad, such as Geely Volvo's standard VDA 239-100-2016. VDA is a quality standard for the automotive industry formulated by the German Association of the Automotive Industry, which specifies some high-expansion steel plates with high bake hardening amount.
[0006] Patent CN119932426A discloses a 440MPa grade bake-hardening steel and its preparation method. This patent, by controlling the proportions of elements such as C, Mn, Cr, and B, and employing a process of continuous annealing, galvanizing, and alloying of cold-rolled steel, achieves a ferrite + martensite dual-phase structure with a porosity λ ≥ 70% and a strength (BH) ≥ 30MPa. However, it is a cold-rolled galvanized steel with a strength grade of only 440MPa, lower than the 600MPa grade of this patent, and the longer process and composition design result in higher production costs. Patent CN112522582B discloses a boron-containing high-strength, high-expansion steel and its manufacturing method. This patent improves strength and hardenability by adding microalloying elements such as Nb and B, and uses a thin-strip continuous casting + online hot rolling process for production. After rolling, gas atomization cooling is used to obtain a high-expansion steel plate with a strength of 590MPa. However, this technical solution does not mention its bake-hardening properties, and with the increase of Si content, there is a risk of red iron scale defects on the surface of the strip. Patent CN104928577B discloses a steel plate with high expansion rate and excellent enameling performance and its manufacturing method. The steel plate obtained has a high expansion rate and elongation, but it is enamel steel and its strength is lower than the 600MPa grade of this patent. Patent CN113025897A discloses a 600MPa grade hot-rolled expanded steel with excellent fatigue performance and its production method. By adding higher levels of alloying elements such as Mo and Nb, the strength and formability of the steel plate are guaranteed. However, its production cost increases sharply, and it does not have bake-hardening properties.
[0007] The steel grades developed in the aforementioned patents differ significantly from those of this invention. None of them balance bake-hardening performance with high hole-expanding performance, and their production costs or composition design also require improvement. To ensure sufficient strength for automotive parts and meet high forming and component requirements in terms of toughness, edge cracking sensitivity, and bake-hardening effect, this patent provides a 600MPa grade pickled steel sheet with excellent flanging and hole-expanding performance, high bake-hardening value, and high local dent resistance, along with its production method. Summary of the Invention
[0008] The purpose of this invention is to provide a 600MPa grade high-pore-expansion pickling and baking hardening steel and its manufacturing method, and to obtain a steel plate / coil yield strength R p0.2 ≥440MPa, tensile strength R m ≥600MPa, elongation A 50 The hole expansion rate λ≥75% meets the standard requirements for high hole expansion steel; the baking hardening amount BH2≥30MPa realizes that after the high hole expansion steel plate with a yield strength range of 440~600MPa is deformed by stamping and coated by baking treatment, it can obtain the strength of stamped parts equivalent to those made of steel plates with a yield strength of 530~690MPa.
[0009] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a 600MPa grade high-pore-expanding pickling and baking hardening steel, wherein the chemical composition and weight percentage of the hardening steel are: C: 0.06-0.10%, Si: 0.07-0.19%, Mn: 1.0-1.5%, P: 0.020-0.040%, S≤0.006%, Al: 0.025-0.055%, N≤0.007%, Nb: 0.013-0.027%, B: 0.0015-0.0035%, Ti≤0.01%, with the balance being Fe and unavoidable impurities.
[0010] The hardened steel yield strength R of the present invention p0.2 ≥440MPa, tensile strength R m ≥600MPa, elongation A 50 ≥17.0%, baking hardening amount BH2≥30MPa, average limiting porosity λ≥75%.
[0011] The hardened steel of this invention has a thickness of 2.2-5 mm and a microstructure consisting of polygonal ferrite, bainite, and nano-carbides within the ferrite grains.
[0012] Another object of the present invention is to provide a method for manufacturing a 600MPa grade high-hole-expansion pickling and baking hardening steel, the manufacturing method comprising smelting, slab heating, hot rolling, laminar flow cooling coiling, leveling and pickling processes; The laminar flow cooling process employs a three-stage laminar flow cooling method. The first stage uses water cooling to reach an intermediate temperature of 650–700°C; the second stage uses air cooling for 6–8 seconds; and the third stage uses water cooling to reach a winding temperature of 450–550°C. After cooling, winding is performed. If the winding temperature exceeds 500°C, C and N tend to diffuse easily in this temperature range, which cannot adequately ensure the presence of solid C and solid N to improve bake hardening properties. There is also a concern that the formation of coarse carbide phases such as pearlite may lead to a decrease in porosity. Therefore, a winding temperature CT of 450–500°C is adopted, and the coiled coil is allowed to cool naturally to room temperature.
[0013] The smelting process described in this invention involves steelmaking in a converter according to the required chemical composition, followed by continuous casting of molten steel into slabs after RH vacuum degassing and LF converter desulfurization treatment.
[0014] In the slab heating process of the present invention, the slab is hot-sent to a hot rolling furnace, heated at a temperature of 1230-1270°C, for a heating time of 150-220 min, and for a soaking time of 55-70 min.
[0015] The hot rolling process described in this invention has a roughing exit temperature of 1020–1080°C, a final rolling temperature of 850–900°C, and an intermediate billet thickness of 36–45 mm.
[0016] The leveling process described in this invention has a leveling elongation rate of 0.15–0.25%. In the pickling process described in this invention, the strip steel is pickled at a speed of 50-80 m / min and the temperature of the pickling tank is 70-85℃.
[0017] In the pickling process described in this invention, the strip steel is pickled through five continuous pickling tanks. The requirements for pickling tank No. 1 are: free acid concentration of 25-55 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 100-120 g / L; the requirements for pickling tank No. 2 are: free acid concentration of 35-70 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 80-100 g / L; the requirements for pickling tank No. 3 are: free acid concentration of 60-100 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 80-100 g / L.
[0018] The pickling process described in this invention requires the following conditions for pickling tank No. 4: free acid concentration of 100-150 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 10-60 g / L; and for pickling tank No. 5: free acid concentration of 150-180 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 5-50 g / L.
[0019] In the composition design of the high bake hardening high hole expansion steel described in this invention: Carbon (C) is the most economical and fundamental strengthening element in steel. It enhances steel strength through solid solution strengthening and precipitation strengthening. Therefore, the C content largely determines the strength grade of the steel; higher C content corresponds to a higher strength grade. Furthermore, a C content below 0.01% cannot obtain sufficient dissolved C for bake hardening, risking a reduction in bake hardening. Therefore, its range is set at 0.06–0.10%.
[0020] Silicon (Si) plays a solid solution strengthening role in steel. In this invention, the addition of Si also acts as a deoxidizer, improving the purity of the steel. Simultaneously, Si can expand the ferrite formation range and prevent the formation of pearlite phase. However, a Si content exceeding 0.2% can easily lead to the formation of a "red iron scale" defect on the surface of the rolled steel plate. Therefore, the Si content range used in this invention is 0.07% to 0.19%.
[0021] Mn: Manganese is one of the cheapest alloying elements. It can improve the hardenability of steel and has a considerable solid solubility in steel. It can improve the strength of steel through solid solution strengthening, while having little to no damage to the plasticity and toughness of steel. It is the most important strengthening element to improve the strength of steel. It can also play a role in deoxidation in steel. However, too high Mn content can also affect welding performance. Therefore, the Mn content in this invention is controlled at 1.0~1.5%.
[0022] Phosphorus (P) is a solid solution strengthening element, and its strengthening effect is stronger than that of other alloying elements. Therefore, this invention fully utilizes the low price and good strengthening effect of P by appropriately adding P. However, high P content easily leads to grain boundary segregation, increasing the cold brittleness of steel, worsening weldability, reducing plasticity, and deteriorating cold bending performance. In this invention, by adding trace amounts of boron (B), P segregation can be effectively suppressed, thereby effectively avoiding the disadvantages of P and fully utilizing its advantages. Therefore, this invention uses a higher P content than traditional processes, and in actual operation, a dephosphorization process is not required. The P content is controlled within the range of 0.020~0.040%.
[0023] Sulfur (S) is a harmful element in steel, causing hot brittleness, reducing ductility and toughness, and leading to cracks during rolling. S readily forms MnS in steel. The quantity and morphology of sulfides directly affect the porosity of the steel plate; in particular, linear sulfides embedded in the steel during deformation easily cause stress concentration, forming crack initiation sites. Therefore, in this invention, S is controlled as an impurity element, with a content range of ≤0.006%.
[0024] Al: Aluminum is a deoxidizer in steelmaking, effectively removing oxygen from molten steel. Appropriate amounts of Al can also improve the strength of the material. However, excessively high Al content leads to high deoxidation, making steelmaking difficult and resulting in excessively high strength, while also increasing non-metallic inclusions and deteriorating ductility. Conversely, insufficient Al content results in inadequate deoxidation. Furthermore, when the coiling temperature is set above 350°C, there is concern about the precipitation of AlN, which would fix and ineffectively utilize the solid-solution nitrogen crucial for bake hardening. Therefore, the preferred Al content is 0.025~0.055%.
[0025] N: Similar to C, N is a preferred element for increasing bake hardening. It can improve the strength of steel through interstitial solid solution. However, interstitial solid solution of N has a significant negative impact on the plasticity and toughness of steel. Moreover, if the addition is too high, the effect will saturate and the aging process will be severely deteriorated. The presence of free N will also increase the yield strength ratio of steel. Therefore, the N content cannot be too high. Thus, the N content range used in this invention is ≤0.007%.
[0026] Niobium (Nb) is an effective grain-refining strengthening element that significantly inhibits austenite grain growth and delays the γ→α transformation, thereby obtaining a finer microstructure, which is beneficial for improving strength and increasing porosity. Furthermore, the delayed γ→α transformation lowers the phase transformation temperature, which increases the supersaturation of effective solid solution C and N and improves the bake-hardening amount. However, excessive addition can lead to saturation of the effect and carries the risk of generating niobium carbonitride, which reduces the effective solid solution C and N and decreases the bake-hardening amount. Therefore, this invention uses Nb in the range of 0.013~0.027%.
[0027] B: Boron has an extremely strong ability to improve hardenability, and its effect is much greater than that of Cr, Mn and other alloying elements. Applying a trace amount of B can save a lot of alloying elements. A trace amount of B can also reduce the segregation of P at the grain boundaries and enhance the grain boundary bonding force. Therefore, the B content of this invention is 0.0015~0.0035%.
[0028] Ti: The formation of carbonitrides by element Ti leads to a decrease in the solid solution C and solid solution N. Solid solution C and N directly affect the bake hardening amount of steel plate. Therefore, in this invention, Ti is controlled as an impurity element, and its content range is ≤0.01%.
[0029] To achieve a balance between high bake hardening and high pore-expanding performance, this invention employs a micro-alloy composite reinforcement with added phosphorus and boron. This ensures bake hardening performance and steel plate strength, reduces alloy costs, and avoids the risk of reducing the content of dissolved carbon and nitrogen in the bake hardening process associated with adding titanium. Furthermore, trace amounts of boron can reduce phosphorus segregation at grain boundaries, enhance grain boundary bonding, and prevent cold brittleness caused by adding phosphorus.
[0030] The rolling process employs a three-stage laminar flow cooling process, namely water cooling-air cooling-water cooling. The purpose of this special cooling process design is twofold: first, to rapidly cool the steel plate from the austenite region to the ferrite temperature region and hold it for 6-8 seconds to ensure the formation of a certain volume percentage of ferrite; second, after a certain amount of ferrite has formed, to rapidly cool the steel plate to the bainite formation temperature region, so that the austenite that has not been transformed into ferrite will eventually transform into bainite, avoiding the appearance of pearlite, thereby ensuring that the microstructure of the steel plate is ferrite + bainite, and ensuring the high porosity of the steel plate.
[0031] The beneficial effects of adopting the above technical solution are as follows: 1. Based on ordinary high-hole-expansion steel, this invention adds bake-hardening performance requirements, which not only meets the high formability requirements of customers before stamping, but also improves the yield strength of parts through electrophoresis, baking paint and other processes after stamping, thereby enhancing the anti-dentation properties of parts, which is in line with the lightweight development trend of the automotive industry and has strong product competitiveness; 2. The relatively economical composition design of this invention uses the strengthening effect of inexpensive alloys such as P, B, and Si to replace expensive alloying elements such as Ti and Mo, reducing alloy costs. 3. This invention uses the addition of trace amounts of boron, which preferentially precipitates BN particles in high-temperature austenite, thereby inhibiting the precipitation of AlN, weakening the pinning effect of fine AlN on grain boundaries, improving grain growth ability, and thus homogenizing austenite grains, which is conducive to the high hole-expansion performance of strip steel. Detailed Implementation
[0032] The present invention will be further described in detail below with reference to specific embodiments.
[0034] Examples 1-6 A method for manufacturing 600MPa grade high-permeability pickling and baking hardening steel includes smelting, slab heating, hot rolling, laminar flow cooling coiling, leveling, and pickling processes; specific control methods are as follows: 1) Smelting process: Steel is produced in a converter according to the required chemical composition. The molten steel undergoes RH vacuum degassing and LF converter desulfurization before being continuously cast into slabs. Specific process details are as follows: The molten iron is desulfurized by KR, with the following desulfurization target values and slag removal rate: desulfurized S≤0.003%, target≤0.002%, and slag removal bright surface rate≥95%. Smelting is carried out according to the target chemical composition, using converter steelmaking, with argon blowing throughout the smelting process, and ≤1 additional blowing at the end point. A front slag plug and a rear sliding plate are used to ensure the online bottom blowing effect of the ladle. The tapping time is 4-7 minutes. High-calcium quicklime is added in the early stage of the tapping process, lime, fluorite, and refining slag are added 30 seconds after tapping, and deoxidizer and alloy are added 1 minute after tapping. The alloying order is aluminum blocks → silicon manganese → ferromanganese → ferrophosphorus → ferroniobium.
[0035] The process employs LF furnace desulfurization followed by RH vacuum degassing. During LF argon blowing, a slightly positive pressure is maintained, and argon gas is controlled to prevent molten steel exposure during the waiting period. During RH treatment, samples are taken after 5 minutes of temperature measurement and circulation. The composition is adjusted based on analysis results, with the addition of ferroboron and alloying. Samples are then taken again after 5 minutes of circulation. RH treatment is controlled according to this process, ensuring a pure degassing time of ≥8 minutes after composition and temperature adjustments.
[0036] The continuous casting process adopts full protective casting. The liquid level on the waiting platform is calmed for ≥5 minutes. The liquid level in the tundish is controlled to maintain a high liquid level during casting. The liquid level in the crystallizer is automatically controlled, with the liquid level fluctuation within ≤±3mm. Medium carbon steel protective slag is used, and a medium carbon steel control model is used for light pressing. The billet thickness is 230mm. The casting process adopts constant casting speed, which is designed to be in the range of 1.2~1.4m / min according to the billet width.
[0037] 2) Slab heating process: The slab is hot-sent to the hot rolling furnace, the heating temperature is 1230~1270℃, the heating time is 150~220min, the soaking time is 55~70min, the target value of the temperature difference between the same slab is ≤50℃, and the control parameters of each embodiment are shown in Table 2.
[0038] 3) Hot rolling process: During the hot rolling process, a hot rolling box is used for heat preservation. The roughing exit temperature is 1020-1080℃, the final rolling temperature is 850-900℃, and the intermediate billet thickness is 36-45mm. The control parameters for each embodiment are shown in Table 2.
[0039] 4) Laminar flow cooling winding process: Three-stage laminar flow cooling is adopted. The first stage uses water cooling to cool to the midpoint temperature of 650-700℃; the second stage uses air cooling for 6-8 seconds; the third stage uses water cooling to cool to the winding temperature of 450-550℃. The control parameters for each embodiment are shown in Table 3.
[0040] 5) Leveling process: The steel coil cooled to room temperature is leveled. The leveling elongation is 0.15-0.25%, and the number of leveling times is ≤2. The control parameters for each embodiment are shown in Table 3.
[0041] 6) Pickling process: Steel coils that have cooled naturally to below 50°C are pickled in hot hydrochloric acid solution to remove iron oxide scale. During the pickling process, the temperature of the pickling tank is 70-85°C and the pickling speed is 50-80 m / min. After rinsing with water and drying in the temperature range of 120-140°C, the coils are coated with anti-rust oil and then rolled up.
[0042] The steel strip is pickled in five consecutive pickling tanks, with the following acid concentrations in each tank: The requirements for pickling tank No. 1 are: free acid concentration of 25-55 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 100-120 g / L; The requirements for pickling tank No. 2 are: free acid concentration of 35-70 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 80-100 g / L; The requirements for pickling tank No. 3 are: free acid concentration of 60-100 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 80-100 g / L; The requirements for pickling tank No. 4 are: free acid concentration of 100-150 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 10-60 g / L; The requirements for pickling tank No. 5 are: free acid concentration of 150-180 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 5-50 g / L. The control parameters for each embodiment are shown in Table 4.
[0043] The hardened steel obtained in Examples 1-6 has a microstructure consisting of polygonal ferrite, bainite, and nano-carbides within the ferrite grains. The chemical composition and weight percentage are shown in Table 1, and the properties are shown in Table 5.
[0044] Table 1 Chemical composition (mass fraction, %) of steels in Examples 1-6
[0045] Table 2. Process parameters for slab heating and hot rolling processes in Examples 1-6
[0046] Table 3. Process parameters for laminar flow cooling winding and leveling processes in Examples 1-6
[0047] Table 4 Process parameters for pickling processes in Examples 1-6
[0048]
[0049]
[0050] Table 5. Properties of steels in Examples 1-6
[0051] Table 6 Changes in yield strength before and after baking in Example 1
[0052] The above embodiments are only used to illustrate and not limit the technical solutions of the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the present invention without departing from the spirit and scope of the present invention. Any modifications or partial substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A 600 MPa grade high stretch-flangeable pickleled bake hardening steel, characterized in that: The chemical composition and weight percentage of the hardened steel are as follows: C: 0.06-0.10%, Si: 0.07-0.19%, Mn: 1.0-1.5%, P: 0.020-0.040%, S≤0.006%, Al: 0.025-0.055%, N≤0.007%, Nb: 0.013-0.027%, B: 0.0015-0.0035%, Ti≤0.01%, with the balance being Fe and unavoidable impurities.
2. The 600 MPa grade high-hole expansion pickle line mill hardened steel according to claim 1, characterized in that: said hardened steel has a yield strength R p0.2 ≥ 440 MPa, a tensile strength R m ≥ 600 MPa, an elongation A 50 ≥ 17.0%, a bake hardening BH2 ≥ 30 MPa, an average limit of hole expansion λ ≥ 75%.
3. The 600 MPa grade high-hole expansion pickle line mill hardened steel according to claim 1 or 2, characterized in that: The hardened steel has a thickness of 2.2-5 mm and a microstructure consisting of polygonal ferrite, bainite, and nano-carbides within the ferrite grains.
4. Method of manufacturing a 600 MPa grade high-hole expansion pickle line mill hardened steel according to any one of claims 1 to 3, characterized in that: The manufacturing method includes smelting, slab heating, hot rolling, laminar flow cooling coiling, leveling and pickling processes; The laminar flow cooling process adopts a three-stage laminar flow cooling method. The first stage uses water cooling to cool to the midpoint temperature of 650-700℃; the second stage uses air cooling for 6-8 seconds; and the third stage uses water cooling to cool to the winding temperature of 450-550℃.
5. The method of manufacturing a 600 MPa grade high hole expandable pickleled bake hardening steel according to claim 3, characterized in that: The smelting process involves steelmaking in a converter according to the required chemical composition, followed by continuous casting of molten steel into slabs after RH vacuum degassing and LF converter desulfurization treatment.
6. The method of manufacturing a 600 MPa grade high hole expandable pickle line annealed bake hardening steel of claim 3, wherein: In the slab heating process, the slab is hot-sent to a hot rolling furnace, heated at a temperature of 1230–1270°C for 150–220 min, and soaked for 55–70 min.
7. The method for manufacturing 600MPa grade high-pore-expansion pickling and baking hardening steel according to claim 3, characterized in that: The hot rolling process has a roughing exit temperature of 1020–1080℃, a final rolling temperature of 850–900℃, and an intermediate billet thickness of 36–45 mm.
8. The method for manufacturing 600MPa grade high-pore-expansion pickling and baking hardening steel according to any one of claims 3-5, characterized in that: The leveling process has a leveling elongation rate of 0.15–0.25%. In the pickling process, the strip steel is pickled at a speed of 50-80 m / min and the temperature of the pickling tank is 70-85℃.
9. The method for manufacturing 600MPa grade high-pore-expansion pickling and baking hardening steel according to any one of claims 3-5, characterized in that: In the pickling process, the strip steel is pickled through five continuous pickling tanks. The requirements for pickling tank No. 1 are: free acid concentration of 25-55 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 100-120 g / L; the requirements for pickling tank No. 2 are: free acid concentration of 35-70 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 80-100 g / L; and the requirements for pickling tank No. 3 are: free acid concentration of 60-100 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 80-100 g / L.
10. The method for manufacturing 600MPa grade high-pore-expansion pickling and baking hardening steel according to any one of claims 3-5, characterized in that: The pickling process requires the following conditions for pickling tank No. 4: free acid concentration of 100-150 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 10-60 g / L; and pickling tank No. 5 requires the following conditions: free acid concentration of 150-180 g / L, total acid concentration of 180-200 g / L, and iron ion concentration of 5-50 g / L.
Citation Information
Patent Citations
A steel plate with high hole expansion rate and excellent enamelling performance and its manufacturing method
CN104928577B
A boron-containing high-strength, high-hole-expansion steel and its manufacturing method
CN112522582B
600MPa-grade hot-rolled reamed steel with excellent fatigue performance and production method thereof
CN113025897A
440MPa-grade bake hardening steel and preparation method thereof
CN119932426A