Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion gradient and its preparation method

By using Ce-Nb microalloying and graded carburizing processes, combined with vacuum quenching and deep cryogenic tempering, the problem of steep hardness gradient in the carburized layer was solved, achieving a smooth transition of the hardness gradient and improved fatigue resistance, making it suitable for high-temperature heavy-load service in aerospace bearings.

CN123108437APending Publication Date: 2026-11-17CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611455108.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing carburizing process results in a steep hardness gradient in the carburized layer of M50NiL steel, which easily leads to stress concentration in the transition zone and uneven carbide precipitation, causing premature bearing failure and making it difficult to meet the high-temperature and heavy-load service requirements of aerospace bearings.

Method used

The process employs Ce-Nb microalloying and graded variable diffusion ratio pulse carburizing, combined with vacuum quenching and double deep cryogenic vacuum tempering, to control the gradual hardness gradient of the carburized layer. Rare earth Ce purifies the molten steel, while Nb refines the grains. The combination of Ce and Nb inhibits grain growth and carbide precipitation. The graded carburizing process regulates the gradual decrease in carbon concentration, eliminating abrupt changes in hardness.

Benefits of technology

It achieves a smooth transition of the hardness gradient of the carburized layer, eliminates abrupt changes in hardness and stress concentration in the transition zone of the carburized layer, improves the bearing's resistance to spalling and contact fatigue, reduces production difficulty, and facilitates large-scale application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108437A_ABST
    Figure CN123108437A_ABST
Patent Text Reader

Abstract

This invention discloses a Ce-Nb microalloyed M50NiL bearing steel with a gentle carburized layer gradient and its preparation method, belonging to the field of metallic materials and their heat treatment technology. This bearing steel is based on M50NiL bearing steel with the addition of 0.0020–0.0035% rare earth Ce and 0.1–0.3% Nb, with the balance being Fe and unavoidable impurities. Its preparation involves vacuum induction melting + vacuum arc remelting, homogenization, forging annealing, followed by three-stage pulsed carburizing with progressively increasing diffusion ratios (diffusion ratios of 6:1–10:1, 50:1–60:1, and 250:1–300:1), and then vacuum quenching and double deep-cryogenic vacuum tempering. The carburized layer of this invention exhibits a gentle hardness gradient without steep inflection points, no network carbides on the surface, fine grains in the core, and excellent resistance to spalling and contact fatigue, making it suitable for high-temperature, heavy-load applications such as aero-engine bearings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metallic materials and their heat treatment technology, and in particular to a Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion layer gradient and its preparation method. Background Technology

[0002] M50NiL is a low-carbon, high-alloy carburized bearing steel, a core bearing material for aero-engines. It primarily relies on surface carburizing hardening and maintaining high strength and toughness in the core to achieve high-temperature, heavy-load service. Aero-engine bearings endure cyclic contact compressive stress and alternating shear stress during operation, placing extremely high demands on the fatigue life of the bearing steel. This requires not only a good balance of strength and toughness within the material but also high surface hardness to withstand high-speed, high-load operating conditions. Industrially, surface carburizing is commonly used to improve the surface hardness of the material, thereby increasing its fatigue life. The variation in carbon concentration along the depth of the carburized layer directly determines the precipitation morphology of carbides and the distribution of phase transformation stress in the matrix. These two factors jointly dominate the entire process of bearing fatigue crack initiation and propagation, and are the core factors controlling contact fatigue spalling and pitting failure.

[0003] However, existing carburizing processes generally employ a fixed diffusion ratio unidirectional pulse carburizing method, which easily leads to a steep hardness gradient and stress concentration in the transition zone of the carburized layer of M50NiL steel. When the carbon concentration on the carburized surface is too high and the carbon concentration drops rapidly from the surface to the center, the carbon element in the surface austenite becomes severely supersaturated. During quenching and tempering, continuous, coarse network-like M7C3 and M23C6 chromium-molybdenum-vanadium alloy carbides are easily precipitated. These carbides have extremely high hardness and near-zero plasticity, and the interfacial bonding force between them and the martensitic matrix is ​​weak. Under cyclic contact loads, microcracks preferentially form at the carbide-matrix interface. At the same time, the network-like carbides form continuous brittle channels in the subsurface layer. The microcracks extend rapidly along the carbide network towards the center, developing into macroscopic spalling pits in a short time, directly causing premature bearing failure. Meanwhile, the steep carbon concentration gradient causes a significant difference in lattice distortion between the high-carbon martensite on the surface and the low-carbon martensite in the core. This leads to the accumulation of high residual tensile stress in the carburized transition zone, and the alternating load further amplifies the stress concentration effect, drastically shortening the crack initiation cycle. Under high-temperature service conditions, carbide coarsening and uneven interfacial stress relaxation further accelerate crack propagation, resulting in a significant reduction in high-temperature contact fatigue life. If the carbon concentration drops sharply at the end of the carburized layer, the properties of the hardened layer and the core matrix change abruptly, which can easily trigger subsurface plastic flow and induce fatigue pitting corrosion originating from the subsurface. For example, the prior art CN116497262B discloses a method for improving the surface hardness of low-carbon high-alloy martensitic bearing steel, which uses long-cycle progressive pulse carburizing with a constant large diffusion ratio (the ratio of total diffusion time to total strong carburizing time ≥ 15:1). The hardness at the end of the carburized layer drops sharply, with the hardness at 1 mm dropping abruptly from 1000 HV to 600 HV. The gradient change is extremely large, which is difficult to meet the requirements of aerospace bearings for a smooth transition. CN118880000A discloses a method for improving the uniformity of carbides in the carburized layer of high-temperature bearing steel. It improves the uniformity of carbides by combining critical zone rolling with vacuum pulse carburizing. However, this method relies heavily on critical zone rolling to refine the grain size, resulting in a narrow process window and greater difficulty in industrial production.

[0004] Therefore, the smoothness of the hardness and carbon concentration gradient of the carburized layer from the surface to the core directly determines the carbide precipitation morphology, interfacial residual stress level, contact fatigue life, and resistance to surface spalling. These are core indicators restricting the long-term reliable service of aerospace bearings. How to control the smooth transition of hardness and carbon concentration in the carburized layer, while ensuring the depth of the carburized layer and the high-temperature surface hardness, and eliminating abrupt hardness changes in the transition zone, has become a pressing technical problem to be solved in improving the overall performance of bearing steel and extending bearing service life. Summary of the Invention

[0005] To overcome the above-mentioned shortcomings of existing carburized bearing steels and their carburizing processes, the technical problem to be solved by the present invention is to provide a Ce-Nb microalloyed M50NiL bearing steel with a gentle carburized layer hardness gradient, no steep drop inflection point, excellent resistance to spalling and contact fatigue, and low difficulty in industrial production, as well as its preparation method.

[0006] The technical solution adopted by this invention to solve its technical problem is: A Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion gradient comprises the following chemical composition by mass percentage: C: 0.11–0.15%, Cr: 4.00–4.25%, Mo: 4.00–4.50%, V: 1.13–1.33%, Ni: 3.20–3.60%, Mn: 0.15–0.35%, Si: 0.10–0.25%, Co≤0.25%, W≤0.15%, rare earth Ce: 0.0020–0.0035%, Nb: 0.1–0.3%, with the balance being Fe and unavoidable impurities.

[0007] Furthermore, this invention also provides a method for preparing Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion layer gradient, using the chemical composition of the bearing steel as the target composition, and mainly including the following steps: S1. The ingot is prepared by vacuum induction and vacuum self-consumption melting, and the ingot is homogenized. S2. The homogenized ingot is forged and deformed, then annealed and machined until the surface is bright. S3. Graded pulse carburizing: Carburizing is divided into three independent pulse segments. The diffusion ratio of the first stage strong carburizing stage is 6:1 to 10:1, the diffusion ratio of the second stage uniform carburizing stage is 50:1 to 60:1, and the diffusion ratio of the third stage slow diffusion stage is 250:1 to 300:1. S4. Vacuum quench the carburized workpiece. S5. The quenched workpiece is subjected to double deep cryogenic vacuum tempering treatment to obtain finished bearing steel.

[0008] Furthermore, the homogenization process described in step S1 involves heating the cast steel ingot to 1180°C and holding it there for 48 hours.

[0009] Furthermore, the forging deformation temperature range in step S2 is 950–1100℃, the total deformation is 85–95%, and the annealing is performed at 650℃ for 30–40 hours.

[0010] Furthermore, in step S3, the carburizing furnace temperature for the graded pulse carburizing is 940–960°C, the furnace pressure is 600–900 Pa, the carburizing medium is high-purity acetylene, the protective diffusion medium is high-purity nitrogen, and the total carburizing time is 16–20 h.

[0011] Furthermore, in step S3, the first-stage strong carburizing stage is circulated 8-10 times with a gas flow rate of 1200-1500 L / h; the second-stage uniform carburizing stage is circulated 12-15 times with a gas flow rate of 800-1000 L / h; and the third-stage slow diffusion stage is circulated 3-5 times with a gas flow rate of 50-100 L / h.

[0012] Furthermore, in step S3, the duration of the single pulse within each of the three independent pulse segments increases progressively, and the concentration of carburizing gas in the three pulse segments decreases in a stepwise manner.

[0013] Furthermore, in step S4, the vacuum quenching is performed by holding the carburized workpiece at 1050–1070°C for 1.5–3 hours and then performing vacuum oil quenching.

[0014] Furthermore, the double cryogenic vacuum tempering process described in step S5 is as follows: after quenching, the workpiece is subjected to a first cryogenic holding at -85℃ for 2 hours. After the cryogenic holding is completed, it is placed in water and slowly heated to room temperature. Then, it is vacuum tempered at 545±5℃ for 2 hours. After the tempering is completed, it is furnace cooled to room temperature. Then, it is cryogenically held at -85℃ for 2 hours again. After the temperature is raised to room temperature, it is vacuum tempered at 545±5℃ for 2 hours. Finally, it is furnace cooled to obtain the finished bearing steel.

[0015] The beneficial effects of this invention are: 1. By adding rare earth elements Ce and Nb, composite microalloying is achieved. Ce purifies molten steel, removes impurities and reduces element segregation. At the same time, an appropriate amount of Ce can increase the activation energy of grain boundary migration, thereby inhibiting grain growth. Nb forms fine and dispersed NbC particles that pin grain boundaries and refine grains. Both refine the material grains from the source, thus maintaining fine and dispersed grains during the carburizing process. This effectively inhibits the precipitation of network carbides, and the grain size of the core of the finished bearing steel can reach 4.5 to 6 grades. 2. A graded variable diffusion-ratio pulse carburizing process is adopted, which divides the carburizing process into three independent pulse segments: strong diffusion, uniform carburizing, and slow diffusion. The diffusion-ratio increases from 6:1 to 10:1 to 250:1 to 300:1. With the pulse duration gradient increasing and the carburizing gas concentration decreasing stepwise, the ratio of strong diffusion to diffusion duration is dynamically adjusted in segments. The carbon concentration is controlled from the source to smoothly decrease from the surface to the core, so as to obtain a carburizing hardness gradient with no steep drop inflection point and a smooth transition. 3. By matching vacuum quenching and combining it with double deep cryogenic vacuum tempering for synergistic optimization, the finished product surface is free of network carbides, the carbides in the carburized layer are uniformly distributed, there is no acicular martensite, and the content of retained austenite is low, which eliminates the sudden hardness change in the transition zone of the carburized layer and reduces the interfacial stress. 4. While ensuring the depth of the diffusion layer and the high-temperature hardness of the surface, it significantly improves the anti-stripping and anti-contact fatigue performance of aerospace bearings; the process does not rely on difficult-to-control pretreatment processes such as critical zone rolling, has a wide process window, low industrial production difficulty, and is easy to promote and apply on a large scale. Attached Figure Description

[0016] Figure 1 This is a metallographic image of the carburized layer in Embodiment 1 of the present invention; Figure 2 This is a diagram of the core grain structure of Embodiment 1 of the present invention; Figure 3 This is the hardness gradient curve of the carburized layer in Embodiment 1 of the present invention; Figure 4 This is a metallographic image of the carburized layer in Embodiment 2 of the present invention; Figure 5 This is a diagram of the core grain structure of Embodiment 2 of the present invention; Figure 6 This is the hardness gradient curve of the carburized layer in Embodiment 2 of the present invention; Figure 7 This is a metallographic image of the carburized layer in Comparative Example 1 of the present invention; Figure 8 This is a diagram of the core grain structure of Comparative Example 1 of the present invention; Figure 9 This is the hardness gradient curve of the carburized layer in Comparative Example 1 of the present invention; Figure 10 This is a metallographic image of the carburized layer in Comparative Example 2 of the present invention; Figure 11 This is a diagram of the core grain structure of Comparative Example 2 of the present invention; Figure 12 This is the hardness gradient curve of the carburized layer in Comparative Example 2 of the present invention; Figure 13 This is a metallographic image of the carburized layer in Comparative Example 3 of the present invention; Figure 14 This is a diagram of the core grain structure of Comparative Example 3 of the present invention; Figure 15 This is the hardness gradient curve of the carburized layer in Comparative Example 3 of the present invention. Detailed Implementation

[0017] The present invention will be further described below with reference to the accompanying drawings and embodiments.

[0018] The present invention provides a Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion layer gradient, comprising the following chemical composition by mass percentage: C: 0.11-0.15%, Cr: 4.00-4.25%, Mo: 4.00-4.50%, V: 1.13-1.33%, Ni: 3.20-3.60%, Mn: 0.15-0.35%, Si: 0.10-0.25%, Co≤0.25%, W≤0.15%, rare earth Ce: 0.0020-0.0035%, Nb: 0.1-0.3%, with the balance being Fe and unavoidable impurities. The bearing steel is made with the above-mentioned chemical composition as the target composition. After vacuum induction and vacuum self-consumption melting, homogenization treatment, forging deformation, post-forging annealing, and turning, it undergoes graded pulse carburizing with three independent pulse segments, and then vacuum quenching and double deep cryogenic vacuum tempering treatment to obtain the finished bearing steel.

[0019] The following explains the role of each chemical component in the bearing steel of this invention and the basis for determining its content: Carbon (C): Carbon is the most basic and effective strengthening element in steel, and it is crucial for ensuring the core strength and hardenability of carburized bearing steel. When the C content is too low, the core martensite strength is insufficient, making it difficult to support the carburized hardened layer and withstand high contact loads; when the C content is too high, the core toughness decreases, and the tendency for carbide precipitation during melting and solidification increases, which is detrimental to the balance of strength and toughness. This invention controls the C content to 0.11–0.15%, enabling the core to obtain high-strength, low-carbon martensite after quenching and tempering, thus achieving a balance between core strength and toughness.

[0020] Cr: Cr is a key alloying element for improving hardenability and enhancing resistance to tempering softening. It is also a strong carbide-forming element, participating in the formation of alloy carbides such as M7C3 and M23C6 in the carburized layer, ensuring the high-temperature hardness and wear resistance of the layer. If the Cr content is too low, hardenability and high-temperature hardness are insufficient; if it is too high, the carbides are coarse and easily precipitate along grain boundaries in a network pattern, impairing fatigue performance. This invention controls the Cr content to 4.00–4.25%.

[0021] Mo: Mo is a strong carbide-forming element with significant secondary hardening effect and resistance to temper softening. It can improve the high-temperature hardness and red hardness of bearing steel and suppress temper brittleness. When the Mo content is too low, the secondary hardening effect is insufficient; when it is too high, coarse primary carbides are easily formed, reducing toughness. In this invention, the Mo content is controlled at 4.00-4.50%.

[0022] V: V combines with C to form fine and dispersed VC carbides, producing a strong precipitation strengthening and secondary hardening effect. It also refines the grain size and improves tempering stability, making it a core element for ensuring the high-temperature hardness of the carburized layer. Too low a V content results in insufficient strengthening; too high a content leads to coarsening and aggregation of VC, which can become a source of fatigue crack initiation. This invention controls the V content to 1.13–1.33%.

[0023] Ni: Ni can significantly improve the hardenability and core toughness of steel, and lower the ductile-brittle transition temperature. It is a key element to ensure the high strength and toughness of the core in low-carbon high-alloy carburized bearing steel. Too low a Ni content results in insufficient core toughness; too high a Ni content leads to increased retained austenite and higher costs. This invention controls the Ni content to 3.20–3.60%.

[0024] Mn and Si: Mn and Si mainly play a role in deoxidation and solid solution strengthening, and can improve hardenability; however, excessive content of either will impair the toughness of steel and increase the content of inclusions. In this invention, the Mn content is controlled at 0.15-0.35%, and the Si content is controlled at 0.10-0.25%.

[0025] Co and W: Co and W are controlled as limiting elements in the steel of this invention, with Co ≤ 0.25% and W ≤ 0.15%, to avoid uncontrollable influence on carburizing behavior and carbide precipitation, while controlling raw material costs.

[0026] Rare earth element Ce: Ce has a strong affinity for O and S in molten steel, forming fine, dispersed, near-spherical rare earth oxides and sulfides. These compounds modify MnS and oxide inclusions, purify grain boundaries, and significantly reduce elemental segregation during solidification, thereby weakening the nucleation and growth tendency of network carbides. Existing research shows that adding approximately 0.0027% La / Ce mixed rare earth to gear steel can significantly reduce the number of inclusions, essentially eliminating inclusions larger than 30 μm, and significantly improving the fatigue limit. Adding an appropriate amount of rare earth to bearing steel can also greatly improve fatigue life. When the Ce content is too low (below 0.0020%), the modification and purification effect on inclusions is insufficient, and the improvement effect is not obvious. When the Ce content is too high (above 0.0035%), large rare earth inclusions easily form and aggregate in the molten steel. These inclusions have weak interfacial bonding with the matrix and become a preferential source for contact fatigue crack initiation, deteriorating fatigue performance. In this invention, the rare earth Ce content is controlled to be 0.0020-0.0035%.

[0027] Nb: Nb is a strong carbide-nitride forming element. The fine NbC particles it forms can pin austenite grain boundaries, hindering grain growth. It should be noted that the carburizing temperature of this invention is 940–960℃, and the total carburizing time is as long as 16–20 hours. Under these high-temperature, long-duration carburizing conditions, the solid solubility of NbC in austenite increases significantly. The NbC particles formed by conventional microalloying content (0.02–0.05%) will largely dissolve back, resulting in insufficient grain boundary pinning particles and difficulty in continuously suppressing grain coarsening throughout the carburizing process. Therefore, this invention increases the Nb content to 0.1–0.3%, combined with a homogenization treatment at 1180℃ for 48 hours and a large forging deformation of 85–95%, allowing NbC to fully dissolve before precipitating in a fine, dispersed form. This ensures that a sufficient number of fine NbC particles pin the grain boundaries throughout the carburizing and quenching heating process, maintaining the core grain size stably at level 4.5–6. When the Nb content is below 0.1%, the grain refinement effect under high-temperature long-term carburizing is not obvious; when the Nb content is above 0.3%, coarse primary NbC is easily formed and agglomerates during solidification. These coarse carbides are hard and brittle, disrupting the continuity of the matrix and becoming fatigue crack initiation sites. Therefore, this invention controls the Nb content to 0.1-0.3%.

[0028] The following details each step in preparing this bearing steel: Step S1: Ingots are produced using vacuum induction melting and vacuum arc remelting, and then homogenized. Vacuum induction melting avoids oxidation and inclusion contamination caused by atmospheric metallurgy, and precisely controls the chemical composition; vacuum arc remelting further removes gases and inclusions, improving the density and compositional uniformity of the ingots. The two processes constitute a dual melting process, providing high-purity billets for aerospace-grade bearing steel.

[0029] The homogenization process described in step S1 involves heating the cast steel ingot to 1180℃ and holding it for 48 hours. The preferred method is as follows: if the homogenization temperature is too low or the holding time is too short, the dendritic segregation formed by strong carbide-forming elements such as Cr, Mo, and V during solidification is difficult to eliminate, and NbC cannot be fully dissolved. This leads to the precipitation of coarse network carbides in the segregation zone during subsequent forging and carburizing processes. If the homogenization temperature is too high, the risk of ingot overheating increases, abnormal grain growth occurs, and energy consumption also rises significantly. This invention preferably uses a homogenization process of 1180℃ for 48 hours, which can effectively eliminate solidification component segregation and allow most of the cast NbC to dissolve, creating conditions for the re-precipitation of fine, dispersed NbC during subsequent forging.

[0030] Step S2: Forge the homogenized ingot, anneal it after forging, and turn it until the surface is bright.

[0031] The forging deformation temperature range in step S2 is 950–1100℃, and the total deformation is 85–95%. The annealing is performed at 650℃ for 30–40 hours. The preferred method is based on the following: when the forging temperature is below 950℃, the material has high deformation resistance and is prone to cracking; above 1100℃, the grains coarsen and oxidation loss intensifies; when the total deformation is less than 85%, the as-cast dendritic structure and coarse carbides are not sufficiently broken up; when the total deformation is greater than 95%, the forging passes are difficult to arrange and anisotropy is easily generated. Post-forging annealing at 650℃ for 30–40 hours can effectively eliminate forging stress, soften the structure, and promote the spheroidization and uniform distribution of carbides, providing a billet with uniform composition and fine grains for subsequent carburizing; too short an annealing time results in insufficient softening, while too long an annealing time reduces production efficiency. After annealing, the surface is machined to a bright finish to avoid surface oxide scale and machining defects affecting the uniformity of the carburized layer.

[0032] Step S3: Graded Pulse Carburizing. This step is the core step in obtaining a smooth carburized layer gradient in this invention. Carburizing is divided into three independent pulse segments: the first stage, a strong carburizing stage, has a diffusion ratio of 6:1 to 10:1. A high carbon concentration is rapidly established on the workpiece surface using a relatively small diffusion ratio and a high-flow-rate carburizing atmosphere, forming the driving force for carburizing; the second stage, a uniform carburizing stage, has a diffusion ratio of 50:1 to 60:1. A large diffusion ratio allows surface carbon atoms to diffuse fully inwards, smoothing out the peak carbon concentration on the surface while maintaining the advancement of the carburized layer; the third stage, a slow diffusion stage, has a diffusion ratio of 250:1 to 300:1. An ultra-large diffusion ratio and an extremely low-flow-rate carburizing atmosphere allow carbon atoms at the end of the carburized layer to slowly diffuse towards the center, eliminating the sharp drop in concentration at the end of the carburized layer. The diffusion ratios of the three stages increase by orders of magnitude, achieving a smooth decrease in carbon concentration from the surface to the center.

[0033] In step S3, the graded pulse carburizing process involves a carburizing furnace temperature of 940–960°C, a furnace pressure of 600–900 Pa, a high-purity acetylene carburizing medium, and a high-purity nitrogen protective diffusion medium. The total carburizing time is 16–20 hours. The optimal conditions are as follows: below 940°C, the carbon atom diffusion rate is slow, requiring too much time to reach the target carburized layer depth; above 960°C, the austenite grain coarsening tendency intensifies, and the risk of carbide precipitation increases. The furnace pressure of 600–900 Pa falls within the conventional pressure window for low-pressure vacuum carburizing, preventing carbon black formation and ensuring the carburizing rate. High-purity acetylene decomposes on the workpiece surface to produce active carbon atoms, resulting in rapid carburization and strong penetration. High-purity nitrogen serves as the protective dilution medium during the diffusion stage, ensuring stable furnace pressure and preventing intergranular oxidation. The total carburizing time of 16–20 hours matches the three-stage pulse system, balancing the target carburized layer depth with a gentle gradient.

[0034] Furthermore, in step S3, the first-stage strong carburizing stage involves 8-10 cycles with a gas flow rate of 1200-1500 L / h; the second-stage uniform carburizing stage involves 12-15 cycles with a gas flow rate of 800-1000 L / h; and the third-stage slow diffusion stage involves 3-5 cycles with a gas flow rate of 50-100 L / h. The optimal approach is as follows: the first-stage strong carburizing stage requires rapid establishment of surface carbon concentration, necessitating high flow rates and multiple cycles to ensure sufficient surface carburization; the second-stage uniform carburizing stage focuses on diffusion homogenization, with a corresponding decrease in flow rate and an increase in the number of cycles to broaden the carbon concentration plateau; the third-stage slow diffusion stage only requires a small amount of carburizing atmosphere to prevent surface decarburization, thus a flow rate reduced to 50-100 L / h and 3-5 cycles are sufficient for a smooth finish. The decreasing cycle count and gas flow rate at each stage ensure a smooth transition of carbon concentration between the three stages without abrupt changes.

[0035] In addition, in step S3, within the three independent pulse segments, the duration of a single pulse within each segment increases progressively, and the concentration of carburizing gas in the three pulse segments decreases in a stepwise manner. Specifically, the duration of a single pulse (the sum of the strong permeation time and the diffusion time within a single pulse) can be set as follows: the duration of a single pulse in the first-stage strong permeation stage is 8–22 min, of which the strong permeation time of a single pulse is 1–2 min and the diffusion time is 6–20 min (the ratio of diffusion time to strong permeation time, i.e., the diffusion-permeation ratio, is 6:1–10:1), and the duration of a single pulse within this stage increases progressively from approximately 8 min to approximately 22 min; the duration of a single pulse in the second-stage uniform carburization stage is 25–60 min, of which the strong permeation time ... is 6:1–10:1), and the duration of a single pulse within this stage increases progressively from approximately 8 min to approximately 22 min; The initial diffusion time is 0.5–1 min, and the diffusion time is 25–59 min (diffusion-to-permeability ratio 50:1–60:1). Within this stage, the single pulse duration gradually increases from approximately 25 min to approximately 60 min. The single pulse duration of the third-stage slow diffusion section is 60–180 min, with the strong permeation time being 0.2–0.6 min and the diffusion time being 50–180 min (diffusion-to-permeability ratio 250:1–300:1). Within this stage, the single pulse duration gradually increases from approximately 60 min to approximately 180 min. As carburizing progresses, the thickness of the carburized layer increases, and the path for carbon atoms to diffuse inward becomes longer. The gradual increase in the single pulse duration within each stage provides carbon atoms with diffusion time that matches the increase in carburized layer depth, ensuring a consistently smooth carbon concentration profile. After multiplying the pulse duration of each stage by the corresponding number of cycles, the total duration of the three stages is consistent with the total carburizing time of 16–20 h. The concentration of the carburizing gas decreases in a stepwise manner. Specifically, the acetylene flow rate in the three-stage pulse section decreases stepwise from 1200-1500 L / h in the first-stage strong carburizing stage to 800-1000 L / h in the second-stage uniform carburizing stage, and then further decreases stepwise to 50-100 L / h in the third-stage slow diffusion stage. By decreasing the flow rate stepwise, the carbon supply intensity of the carburizing atmosphere in each stage is reduced, avoiding the re-formation of carbon concentration peaks on the surface in the later stages of carburizing, and ensuring a smooth transition at the end of the carburized layer.

[0036] Step S4: Vacuum quench the carburized workpiece.

[0037] The vacuum quenching process involves holding the carburized workpiece at 1050–1070℃ for 1.5–3 hours followed by vacuum oil quenching. The preferred method is based on the following: when the quenching temperature is below 1050℃, the alloy carbides in the carburized layer are not fully dissolved, resulting in insufficient high-temperature hardness; when the temperature is above 1070℃, the austenite grains coarsen, and the amount of residual austenite increases after quenching. Holding for 1.5–3 hours ensures sufficient austenitization of both the carburized layer and the core; vacuum oil quenching provides uniform cooling with minimal distortion and avoids surface oxidation and decarburization.

[0038] Step S5: Perform double deep cryogenic vacuum tempering on the quenched workpiece to obtain the finished bearing steel.

[0039] The double cryogenic vacuum tempering process is as follows: After quenching, the workpiece undergoes a first cryogenic holding at -85℃ for 2 hours. After cryogenic treatment, it is placed in water and slowly heated to room temperature, followed by vacuum tempering at 545±5℃ for 2 hours. After tempering, it is furnace cooled to room temperature. Then, it undergoes another cryogenic holding at -85℃ for 2 hours, followed by a second vacuum tempering at 545±5℃ for 2 hours, and finally furnace cooling to obtain the finished bearing steel. The first cryogenic treatment causes most of the retained austenite in the quenched microstructure to transform into martensite. The subsequent vacuum tempering at 545±5℃ fully tempers the newly formed martensite and precipitates fine, dispersed alloy carbides, resulting in secondary hardening. The second cryogenic-tempering cycle further transforms the retained austenite, eliminates acicular martensite, and relaxes interfacial stress. Slowly heating the workpiece to room temperature after cryogenic treatment reduces thermal stress caused by the temperature difference between the inside and outside of the workpiece, preventing cryogenic cracking. After two deep cryogenic vacuum tempering processes, the microstructure of the infiltrated layer consists of tempered martensite and fine dispersed carbides, with a low content of residual austenite and a stable and gentle hardness gradient.

[0040] The finished bearing steel prepared by the above process has no network carbides on the surface and the carbides in the carburized layer are evenly distributed. It has no acicular martensite, low residual austenite content, and the hardness gradient curve of the carburized layer transitions smoothly from the surface to the core without steep inflection points. The core has fine grains with a grain size of 4.5 to 6.

[0041] The present invention will be further illustrated below through specific embodiments and comparative examples. All chemical components in the embodiments and comparative examples are expressed as mass percentages.

[0042] Example 1 The chemical composition, by mass percentage, is as follows: C: 0.14%, Cr: 4.23%, Mo: 4.33%, V: 1.18%, Ni: 3.52%, Mn: 0.27%, Si: 0.24%, Co: 0.09%, W: 0.0018%, rare earth Ce: 0.0020%, Nb: 0.23%, with the balance being Fe and unavoidable impurities.

[0043] The bearing steel is produced by vacuum induction and vacuum arc remelting. The cast steel ingot is heated to 1180℃ and held for 48 hours to homogenize it and eliminate solidification component segregation. After homogenization, the ingot is forged and deformed in the range of 950–1100℃, with a total deformation of 90%. After the forged bar is deformed, it is annealed at 650℃ for 36 hours. After annealing, it is machined to a bright surface and then subjected to graded carburizing. The carburizing furnace temperature was 960℃, the furnace pressure was 700Pa, the carburizing medium was high-purity acetylene, and the protective diffusion medium was high-purity nitrogen. The total carburizing time was approximately 16 hours. The carburizing process was divided into three independent pulse stages: Stage 1: Strong Carburizing (8 cycles, gas flow rate 1200 L / h, diffusion ratio 10:1, single pulse duration gradually increasing from approximately 8 minutes to approximately 15 minutes); Stage 2: Uniform Carburizing (12 cycles, gas flow rate 800 L / h, diffusion ratio 50:1, single pulse duration gradually increasing from approximately 26 minutes to approximately 51 minutes); Stage 3: Slow Diffusion (3 cycles, gas flow rate 50 L / h, diffusion ratio 250:1, single pulse duration gradually increasing from approximately 63 minutes to approximately 125 minutes). Within each stage, the single pulse duration gradually increased, and the carburizing gas concentration decreased stepwise across the three pulse stages. After carburizing, the sample was subjected to vacuum quenching and double deep cryogenic vacuum tempering: the carburized workpiece was held at 1060℃ for 1.5h and then vacuum oil quenched; then it was subjected to a first deep cryogenic holding at -85℃ for 2h, after which it was placed in water and slowly heated to room temperature, then vacuum tempered at 540℃ for 2h, after which it was furnace cooled to room temperature; then it was again deep cryogenically held at -85℃ for 2h, heated to room temperature, and then vacuum tempered at 540℃ for 2h, and furnace cooled to obtain the finished bearing steel.

[0044] The resulting finished bearing steel has no network of carbides on its surface and the carbides in the carburized layer are evenly distributed (see...). Figure 1 It has no acicular martensite, low retained austenite content, and a smooth transition in the hardness gradient curve (see...). Figure 3 Furthermore, the core grains are fine, with a grain size of 5–5.5 (see...). Figure 2 ).

[0045] Example 2 The chemical composition, by mass percentage, is as follows: C: 0.13%, Cr: 4.10%, Mo: 4.18%, V: 1.30%, Ni: 3.52%, Mn: 0.25%, Si: 0.15%, Co: 0.10%, W: 0.0018%, rare earth Ce: 0.0032%, Nb: 0.30%, with the balance being Fe and unavoidable impurities.

[0046] The bearing steel is produced by vacuum induction and vacuum arc remelting. The cast steel ingot is heated to 1180℃ and held for 48 hours to homogenize it and eliminate solidification component segregation. After homogenization, the ingot is forged and deformed in the range of 950–1100℃, with a total deformation of 95%. After the forged bar is deformed, it is annealed at 650℃ for 40 hours. After annealing, it is machined to a bright surface and then subjected to graded carburizing. The carburizing furnace temperature was 940℃, the furnace pressure was 900Pa, the carburizing medium was high-purity acetylene, and the protective diffusion medium was high-purity nitrogen. The total carburizing time was 20 hours. Carburizing was divided into three independent pulse stages: Stage 1: Strong carburizing stage; 10 cycles, gas flow rate 1500L / h, diffusion ratio 6:1, single pulse duration gradually increasing from approximately 10 minutes to approximately 14 minutes; Stage 2: Uniform carburizing stage; 15 cycles, gas flow rate 1000L / h, diffusion ratio 60:1, single pulse duration gradually increasing from approximately 31 minutes to approximately 61 minutes; Stage 3: Slow diffusion stage; 5 cycles, gas flow rate 100L / h, diffusion ratio 300:1, single pulse duration gradually increasing from approximately 60 minutes to approximately 120 minutes. The single pulse duration within each stage gradually increased, and the carburizing gas concentration in the three pulse stages decreased in a stepwise manner. After carburizing, the sample was subjected to vacuum quenching and double deep cryogenic vacuum tempering: the carburized workpiece was held at 1070℃ for 1.5h and then vacuum oil quenched; then it was subjected to a first deep cryogenic holding at -85℃ for 2h, after which it was placed in water and slowly heated to room temperature, then vacuum tempered at 545℃ for 2h, after which it was furnace cooled to room temperature; then it was again deep cryogenically held at -85℃ for 2h, heated to room temperature, and then vacuum tempered at 545℃ for 2h, and furnace cooled to obtain the finished bearing steel.

[0047] The resulting finished bearing steel has no network of carbides on its surface (see...). Figure 4 It has no acicular martensite, low retained austenite content, and a smooth transition in the hardness gradient curve (see...). Figure 6 Furthermore, the core grains are fine, with a grain size of 5–5.5 (see...). Figure 5 ).

[0048] Comparative Example 1 The chemical composition, by mass percentage, is as follows: C: 0.13%, Cr: 4.15%, Mo: 4.25%, V: 1.20%, Ni: 3.40%, Mn: 0.25%, Si: 0.20%, Co: 0.09%, W: 0.0018%, with the balance being Fe and unavoidable impurities. The difference from Example 1 is that rare earth elements Ce and Nb are not added.

[0049] The bearing steel was obtained by vacuum induction melting and vacuum arc remelting. The cast steel ingot was heated to 1180℃ and held for 48 hours for homogenization. After homogenization, the ingot was forged and deformed in the range of 950-1100℃, with a total deformation of 90%. The forged bar was annealed at 650℃ for 36 hours, turned to a bright surface, and then subjected to graded carburizing. The carburizing process was the same as in Example 1: carburizing furnace temperature 960℃, furnace pressure 700Pa, high-purity acetylene carburizing, and high-purity nitrogen. Gas diffusion was performed, with a total carburizing time of approximately 16 hours. The first stage of strong carburizing involved 8 cycles at a flow rate of 1200 L / h and a diffusion ratio of 10:1. The second stage of uniform carburizing involved 12 cycles at a flow rate of 800 L / h and a diffusion ratio of 50:1. The third stage of slow diffusion involved 3 cycles at a flow rate of 50 L / h and a diffusion ratio of 250:1. After carburizing, the carburized ...

[0050] The surface of the finished bearing steel has a network of carbides (see...) Figure 7 It contains a large amount of acicular martensite, and the hardness gradient curve transitions smoothly (see...). Figure 9 However, the core grains are coarse, with a grain size of only grade 4 (see...). Figure 8 Comparative Example 1 shows that, without the addition of Ce and Nb, even with the graded variable diffusion ratio pulse carburizing process of the present invention, it is still impossible to suppress the precipitation of network carbides and the formation of acicular martensite, and the grain refinement effect in the core is also insufficient.

[0051] Comparative Example 2 The chemical composition, by mass percentage, is as follows: C: 0.13%, Cr: 4.10%, Mo: 4.18%, V: 1.30%, Ni: 3.52%, Mn: 0.25%, Si: 0.15%, Co: 0.10%, W: 0.0018%, rare earth Ce: 0.0032%, Nb: 0.30%, with the balance being Fe and unavoidable impurities. The difference from Example 2 is that the carburizing process employs a fixed diffusion ratio progressive pulse carburizing process, a technique already known.

[0052] The smelting, homogenization, forging, and annealing processes were the same as in Example 2. After annealing and machining, the samples were carburized: the absolute pressure for carburizing was 2 Pa, and the sample was heated to the carburizing temperature of 960°C with the furnace. The carburizing process adopted a progressive pulse carburizing method, with the time of the next pulse process being greater than or equal to the time of the previous pulse process. The diffusion ratio was 8:1, and the number of cycles was 20. In the strong carburizing stage, the carburizing medium was high-purity acetylene, the carburizing pressure was 500 Pa, the medium flow rate was 1500 L / h, and the strong carburizing time for each stage was 1–10 min. In the diffusion stage, the medium was nitrogen, and the diffusion time for each stage was 3–60 min. The total carburizing time was approximately 16 h. Next, the carburized sample was subjected to vacuum high-temperature quenching at 1080℃ for 1 hour, followed by oil quenching. After oil quenching, the sample underwent its first cold treatment at -85℃ for 2 hours. Subsequently, the sample underwent its first vacuum tempering at 540℃ for 2 hours. After tempering, the sample was furnace cooled to room temperature. Then, it was cryogenically held at -85℃ for 2 hours, heated to room temperature, and then subjected to a second vacuum tempering at 545±5℃ for 2 hours. Finally, it was furnace cooled to obtain the finished bearing steel.

[0053] The resulting finished bearing steel has no network of carbides on its surface (see...). Figure 10 However, it contains a large amount of acicular martensite, and a certain amount of retained austenite is present in the outermost layer. The hardness gradient curve is not smooth enough (see...). Figure 12 The core grains are coarse, with a grain size of 3-4 (see...). Figure 11 Comparative Example 2 shows that even with the addition of Ce and Nb, the existing gradual pulse carburizing process with a fixed diffusion ratio still cannot achieve a smooth carburizing hardness gradient.

[0054] Comparative Example 3 The chemical composition, by mass percentage, is as follows: C: 0.14%, Cr: 4.23%, Mo: 4.33%, V: 1.18%, Ni: 3.52%, Mn: 0.27%, Si: 0.24%, Co: 0.09%, W: 0.0018%, rare earth Ce: 0.0020%, Nb: 0.23%, with the balance being Fe and unavoidable impurities. The difference from Example 1 is that some carburizing and heat treatment process parameters deviate from the scope defined in this invention.

[0055] The smelting, homogenization, forging, and annealing processes are the same as in Example 1; staged carburizing: carburizing furnace temperature 960℃, furnace pressure 750Pa, total carburizing time approximately 15h; first-stage strong carburizing: 8 cycles, gas flow rate 1500L / h, diffusion ratio 10:1; second-stage uniform carburizing: 12 cycles, gas flow rate 800L / h, diffusion ratio 60:1; third-stage slow diffusion stage: 2 cycles, gas flow rate 50L / h, diffusion ratio 180:1 (both the number of cycles and diffusion ratio are lower than the range of the third-stage slow diffusion stage defined in this invention); after carburizing, the workpiece is held at 1050℃ for 1h and then vacuum oil quenched (the holding time is lower than the range of 1.5-3h defined in this invention); subsequently, the same double cryogenic vacuum tempering treatment as in Example 1 is performed.

[0056] The surface of the finished bearing steel has a very small amount of network carbides (see...) Figure 13 It contains no acicular martensite, but retains residual austenite on the surface, and the hardness gradient curve transitions smoothly (see...). Figure 15 The core grains are fine, with a grain size of 5-6 (see...). Figure 14Comparative Example 3 shows that when the number of cycles, diffusion ratio, and quenching holding time of the three-stage slow diffusion section deviate from the limits of this invention, the carburizing and quenching-tempering effects cannot be fully realized, and the finished product still has the problem of excessive network carbides and retained austenite.

[0057] Comparing the test results of Examples 1-2 with those of Comparative Examples 1-3, it can be seen that: Comparative Example 1 did not add Ce and Nb, and although it adopted the graded carburizing process of the present invention, there were network carbides on the surface and a large number of acicular martensite, and the core grain size was only level 4; Comparative Example 2 added Ce and Nb, but used progressive pulse carburizing with a fixed diffusion ratio, and the hardness gradient curve transition was not smooth enough, and the core grain size was only level 3-4; The parameters of the three-stage slow diffusion section and the quenching and holding time of Comparative Example 3 deviated from the range of the present invention, and there were still a very small amount of network carbides on the surface and the residual austenite on the surface exceeded the standard. Only by simultaneously employing the Ce-Nb microalloying composition design and graded variable diffusion ratio pulse carburizing process of the present invention, along with the double deep cryogenic vacuum tempering of Examples 1 and 2, can finished bearing steel with no network carbides on the surface, no acicular martensite, low content of retained austenite, gentle hardness gradient, and core grain size of 4.5 to 6 be obtained. This indicates that there is a synergistic effect between composition design and graded carburizing process, and neither can be dispensed with.

[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion layer gradient, characterized in that, The chemical composition includes the following percentages by mass: C: 0.11–0.15%, Cr: 4.00–4.25%, Mo: 4.00–4.50%, V: 1.13–1.33%, Ni: 3.20–3.60%, Mn: 0.15–0.35%, Si: 0.10–0.25%, Co≤0.25%, W≤0.15%, rare earth Ce: 0.0020–0.0035%, Nb: 0.1–0.3%, with the balance being Fe and unavoidable impurities.

2. A method for preparing Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion layer gradient, characterized in that, Using the chemical composition of the bearing steel according to claim 1 as the target composition, the method includes the following steps: S1. The ingot is prepared by vacuum induction and vacuum self-consumption melting, and the ingot is homogenized. S2. The homogenized ingot is forged and deformed, then annealed and machined until the surface is bright. S3. Graded pulse carburizing: Carburizing is divided into three independent pulse segments. The diffusion ratio of the first stage strong carburizing stage is 6:1 to 10:1, the diffusion ratio of the second stage uniform carburizing stage is 50:1 to 60:1, and the diffusion ratio of the third stage slow diffusion stage is 250:1 to 300:

1. S4. Vacuum quench the carburized workpiece. S5. The quenched workpiece is subjected to double deep cryogenic vacuum tempering treatment to obtain finished bearing steel.

3. The method for preparing Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion layer gradient as described in claim 2, characterized in that, The homogenization process described in step S1 involves heating the cast steel ingot to 1180°C and holding it there for 48 hours.

4. The method for preparing Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion layer gradient as described in claim 2, characterized in that, The forging deformation temperature range in step S2 is 950-1100℃, and the total deformation is 85-95%. The annealing is carried out at 650℃ for 30-40 hours.

5. The method for preparing Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion layer gradient as described in claim 2, characterized in that, In step S3, the carburizing furnace temperature for the graded pulse carburizing is 940–960°C, the furnace pressure is 600–900 Pa, the carburizing medium is high-purity acetylene, the protective diffusion medium is high-purity nitrogen, and the total carburizing time is 16–20 h.

6. The method for preparing Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion layer gradient as described in claim 5, characterized in that, In step S3, the first-stage strong carburizing stage is circulated 8-10 times with a gas flow rate of 1200-1500 L / h; the second-stage uniform carburizing stage is circulated 12-15 times with a gas flow rate of 800-1000 L / h; and the third-stage slow diffusion stage is circulated 3-5 times with a gas flow rate of 50-100 L / h.

7. The method for preparing Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion layer gradient as described in claim 6, characterized in that, In step S3, the duration of the single pulse in each of the three independent pulse segments increases progressively, and the concentration of carburizing gas in the three pulse segments decreases in a stepwise manner.

8. The method for preparing Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion layer gradient as described in claim 2, characterized in that, In step S4, the vacuum quenching is performed by holding the carburized workpiece at 1050-1070℃ for 1.5-3 hours and then performing vacuum oil quenching.

9. The method for preparing Ce-Nb microalloyed M50NiL bearing steel with a gentle diffusion layer gradient as described in claim 2, characterized in that, The double cryogenic vacuum tempering process described in step S5 is as follows: After quenching, the workpiece is subjected to a first cryogenic holding at -85℃ for 2 hours. After the cryogenic holding is completed, it is placed in water and slowly heated to room temperature. Then, it is vacuum tempered at 545±5℃ for 2 hours. After the tempering is completed, it is furnace cooled to room temperature. Then, it is cryogenically held at -85℃ for 2 hours again. After the temperature is raised to room temperature, it is vacuum tempered at 545±5℃ for 2 hours. Finally, it is furnace cooled to obtain the finished bearing steel.

Citation Information

Patent Citations

  • Method for improving carbide uniformity of carburized layer of high-temperature bearing steel

    CN118880000A