X100QS Thick-walled Seamless Pipeline Steel Pipe and Its Preparation Method
By using low-alloy design and enhanced heat treatment processes, the problems of uneven microstructure and insufficient corrosion resistance of X100QS grade thick-walled seamless pipeline steel pipes have been solved, achieving a balance between high strength and excellent acid corrosion resistance, reducing production costs, and making it suitable for oil and gas pipelines.
Patent Information
- Application Number
- CN202611297241.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies make it difficult to manufacture thick-walled seamless pipeline steel pipes resistant to acid corrosion under high strength conditions, especially at the X100QS level. These pipes suffer from uneven microstructure, large performance fluctuations, and insufficient corrosion resistance. Furthermore, traditional high-alloy steel designs are costly and have poor weldability.
The steel pipe is designed with a low alloy composition and undergoes KR desulfurization, electric furnace smelting, LF refining, RH vacuum treatment, continuous casting, billet heat treatment, rolling and tempering steps. Combined with Ca-Si line treatment and high-temperature diffusion, the Ti/N ratio and Nb+V content are controlled to ensure the purity and uniformity of the steel pipe. Specific quenching and tempering treatments are used to achieve a uniform tempered martensite structure across the entire cross section.
Under the condition of low crack sensitivity index (CEV≤0.52%), the high strength, low yield strength ratio and excellent resistance to HIC/SSCC of X100QS grade seamless pipeline steel pipe with wall thickness of 40~80mm were synergistically matched, which reduced production costs and improved the purity and corrosion resistance of the steel pipe.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of seamless pipeline steel pipe manufacturing technology, and in particular to an X100QS thick-walled seamless pipeline steel pipe and its preparation method. Background Technology
[0002] Currently, fossil fuels such as oil and natural gas dominate global energy demand. With the development of the world economy and drastic changes in the international situation, the demand for fossil fuels is also growing rapidly. After more than a century of extraction, onshore and offshore oil and gas resources are facing depletion. Therefore, the development of acidic oil and gas fields has gradually increased. Acidic oil and gas fields are characterized by the presence of acidic gases such as H2S and HCl in the oil or natural gas. These acidic gases can severely corrode pipelines, leading to leaks, ruptures, and other serious consequences.
[0003] For seamless pipelines transporting acidic gases, the highest commercially available steel grade is X70QS. Higher grades of thick-walled seamless pipeline steel have not yet achieved industrial application. Acid-resistant pipelines require materials that possess both high strength and excellent resistance to acidic corrosion. Acid-resistant pipelines primarily withstand two corrosion mechanisms: HIC (hydrogen-induced cracking) and SSCC (hydrogen sulfide stress corrosion). As the strength of the steel increases, the material's sensitivity to acid corrosion rises sharply, multiplying the risk of cracking and even breakage.
[0004] Pipeline pipes manufactured using traditional processes suffer from the following technical bottlenecks: On the one hand, to meet the performance requirements of thick, high-strength pipeline pipes, conventional composition design tends to add higher contents of alloying elements such as Cr, Mo, Ni, and V to improve the hardenability of the steel and strengthen the matrix structure. However, the high alloying scheme has obvious shortcomings: it significantly increases the production cost of pipes, and the excessive alloy content exacerbates segregation and increases structural stress. At the same time, it increases the carbon equivalent and welding crack sensitivity, and deteriorates the resistance to HIC / SSCC, which conflicts with the working conditions required for field welding of pipeline pipes.
[0005] On the other hand, on-site welding of pipelines imposes strict limitations on the crack sensitivity index of materials (usually requiring CEV ≤ 0.55%), and the low carbon equivalent constraint directly limits the amount of alloying elements added, further weakening the hardenability of the steel. For thick-walled seamless pipelines with a wall thickness ≥ 25.4 mm, due to insufficient hardenability, traditional quenching processes cannot ensure that the core structure of the pipe material is fully transformed into tempered martensite, easily generating a mixed structure of ferrite, pearlite, or bainite, resulting in uneven mechanical properties in the wall thickness direction, deterioration of low-temperature toughness, and a significant reduction in the pipe material's resistance to hydrogen-induced cracking (HIC) and sulfide stress corrosion cracking (SSCC).
[0006] Due to the aforementioned limitations, there is currently no production of X100QS grade high-strength, corrosion-resistant pipeline pipes domestically or internationally. In view of this, the present invention is proposed. Summary of the Invention
[0007] To address the aforementioned shortcomings in existing technologies, the present invention aims to provide an economical X100QS thick-walled seamless pipeline steel pipe and its preparation method. Through the synergistic process design of low alloy composition, high-purity smelting, and enhanced heat treatment, the invention solves the technical problems of uneven microstructure, poor strength-toughness matching, and insufficient acid corrosion resistance in thick-walled pipes under conditions of low crack sensitivity index (CEV≤0.52%). This achieves a synergistic match of high strength, low yield strength ratio, and excellent resistance to HIC / SSCC in X100QS grade seamless pipeline pipes with wall thicknesses of 40~80mm.
[0008] To achieve the above objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides an X100QS thick-walled seamless pipeline steel pipe, wherein the chemical composition and mass percentage of the thick-walled seamless pipeline steel pipe are as follows: C 0.13-0.17%, Si 0.50-0.70%, Mn 1.45-1.65%, P≤0.015%, S≤0.005%, Cr 0.10-0.18%, Mo 0.10-0.18%, Ni 0.10-0.18%, Cu≤0.05%, V 0.01-0.05%, Ti 0.010-0.030%, N 0.006-0.012%, O≤0.002%, Al≤0.040%, Nb 0.010-0.020%, with the remainder being iron and unavoidable impurity elements; wherein, Ti / N≥3, Nb+V≤0.06%; The crack sensitivity index (CEV) of the steel pipe is ≤0.52%; The wall thickness of the steel pipe is 40mm or more.
[0009] This invention primarily targets thick-walled pipes with a wall thickness exceeding 40mm. By adding alloys such as Ni, the hardenability of the material is increased, ensuring uniform performance across the entire cross-section. Controlling the sulfur (S) content below 0.005% promotes spheroidization of sulfide inclusions, improving steel purity and reducing stress concentration during corrosion. Controlling the manganese (Mn) content below 1.7% effectively mitigates Mn segregation, resulting in a uniform and fine initial microstructure. By controlling the Ti / N ratio to ≥3, an appropriate amount of TiN precipitates is formed in the steel, fully utilizing its grain-refining, strength-enhancing, and corrosion-resistant properties. Simultaneously, excessive TiN aggregation to form large inclusions is avoided, preventing the resulting decrease in impact toughness and corrosion resistance. The combined addition of Nb and V, with controlled dosage, further enhances grain refinement and precipitation strengthening effects, achieving X100QS strength requirements in a low-alloy system. Excessive total Nb and V addition prevents complete solid solution, leading to increased segregation, more coarse carbonitrides, and a significant increase in the material's stress corrosion sensitivity.
[0010] Furthermore, the chemical composition and mass percentage of the thick-walled seamless pipeline steel pipe are as follows: C 0.13-0.16%, Si 0.50-0.60%, Mn 1.50-1.60%, P≤0.015%, S≤0.005%, Cr 0.12-0.18%, Mo 0.12-0.18%, Ni 0.12-0.18%, Cu≤0.05%, V 0.01-0.04%, Ti 0.015-0.025%, N 0.006-0.010%, O≤0.002%, Al≤0.040%, Nb 0.010-0.020%, with the remainder being iron and unavoidable impurity elements.
[0011] Furthermore, the outer diameter of the steel pipe is 219-533mm, and the wall thickness is 40-80mm.
[0012] Furthermore, the steel pipe has a yield strength of 690-810 MPa, a tensile strength of 760-960 MPa, a yield-to-tensile ratio of ≤0.95, an elongation of ≥20%, a CSR of ≤2%, a CLR of ≤15%, and a CTR of ≤5%.
[0013] In a second aspect, the present invention provides a method for preparing X100QS thick-walled seamless pipeline steel pipe as described in the first aspect, the method comprising the following steps in sequence: KR desulfurization, electric furnace smelting, LF refining, RH vacuum treatment, continuous casting, billet heat treatment, rolling and quenching and tempering; wherein, the LF refining includes Ca-Si wire treatment.
[0014] Furthermore, in the LF refining step, the amount of Ca-Si wire added is 8-10 mm / ton of molten steel; and the inclusions of A-sulfides, B-alumina, C-silicates, and D-spherical oxides in the molten steel are controlled to be no higher than grade 0.5.
[0015] Furthermore, in the RH vacuum treatment step, the holding time for an absolute pressure less than 66 Pa is greater than 10 minutes and less than 30 minutes, and the total vacuum time is greater than 15 minutes and less than 35 minutes.
[0016] Furthermore, the diameter of the continuously cast round billet obtained by the continuous casting step is 155-500mm.
[0017] Furthermore, in the billet heat treatment step, the continuously cast round billet is heated and held at a temperature of less than or equal to 1280°C for a duration of more than or equal to 4 hours.
[0018] Furthermore, in the heat treatment step of the cast billet, the holding temperature is 1260~1280℃ and the holding time is 6~8h.
[0019] Furthermore, the rolling process is carried out using an ASSEL tube rolling mill; the initial rolling temperature is greater than or equal to 1250℃, and the final rolling temperature is greater than or equal to 900℃.
[0020] Furthermore, the rolling process is carried out using an ASSEL tube rolling mill; the initial rolling temperature is less than 1300℃, and the final rolling temperature is less than 1200℃.
[0021] Furthermore, the quenching and tempering step includes quenching heat treatment and tempering heat treatment.
[0022] Furthermore, the quenching heat treatment is performed at a quenching temperature of 880-930℃, and the holding time is calculated based on the wall thickness of the steel pipe and is greater than 1 minute / mm.
[0023] Furthermore, the quenching and holding time of the quenching heat treatment is calculated according to the wall thickness of the steel pipe, which is 1.5-2.5 minutes / mm.
[0024] Furthermore, the quenching cooling of the quenching heat treatment is water cooling until the surface temperature of the steel pipe is room temperature.
[0025] Furthermore, the cooling rate of the quenching heat treatment is greater than or equal to 120°C / min.
[0026] Furthermore, for steel pipes with a wall thickness of 40-60mm, the water cooling rate is greater than or equal to 130℃ / min; for steel pipes with a wall thickness greater than 60mm and not greater than 80mm, the water cooling rate is greater than or equal to 120℃ / min.
[0027] Furthermore, the tempering heat treatment temperature is 620-680℃; the holding time is calculated according to the wall thickness of the steel pipe and is greater than 2.5 minutes / mm; after tempering, the steel pipe is removed from the furnace and air-cooled to room temperature.
[0028] Furthermore, the tempering heat treatment temperature is 640-680℃; the holding time is calculated according to the wall thickness of the steel pipe, 3-5 minutes / mm.
[0029] The X100QS thick-walled seamless pipeline steel pipe and its manufacturing method provided by this invention have at least one of the following beneficial effects: (1) High-purity smelting and inclusion control significantly improve acid corrosion resistance. By controlling the S content below 0.005% and combining it with LF refining Ca-Si line treatment, sulfide inclusions are fully spheroidized, effectively reducing stress concentration during corrosion. At the same time, high-vacuum RH vacuum treatment is used to significantly reduce the total amount of inclusions and gas content in the steel, thereby improving the purity of the steel from the source. The resulting steel pipe meets the requirements of CSR≤2%, CLR≤15%, and CTR≤5% for HIC resistance, and meets the requirements of NACE MR 0177 for SSCC resistance, achieving a synergistic match between high strength and excellent acid resistance. (2) Microalloy precipitation control, taking into account both grain refinement and microstructure purity. By increasing the proportion of certain metal components in the alloy, such as Ni, the quenching cooling rate is increased to ensure the hardenability of the material and to ensure the uniformity of the performance of the entire cross section. By controlling Ti / N≥3, an appropriate amount of TiN precipitates are formed in the steel, giving full play to its role in refining grains, improving strength, toughness and corrosion resistance; at the same time, excessive TiN agglomeration is avoided to form large inclusions, thus preventing the problems of decreased impact toughness and deterioration of corrosion resistance caused by this. The composite addition of Nb+V and the control of its addition amount further enhance the grain refinement and precipitation strengthening effects, achieving the X100QS strength requirement in the low alloy system. If the total addition of Nb and V is too much, they cannot be completely dissolved, resulting in increased segregation, increased coarse carbonitrides, and a significant increase in the stress corrosion sensitivity of the material; (3) Full-process segregation control and microstructure homogenization process to systematically solve the problem of uneven microstructure in the core of thick-walled tubes. The Mn content is controlled below 1.7%, and Mn segregation is effectively reduced through integrated control of continuous casting, high-temperature diffusion (cast billet heat treatment) and specific rolling processes to obtain a uniform and fine original microstructure. On this basis, the tempering step adopts quenching and strengthening water-cooling heat treatment to ensure that the entire cross section of the thick-walled tube obtains a uniform tempered martensite microstructure, thus completely solving the technical problems of uneven microstructure and large performance fluctuations in the core under traditional processes. (4) Economical composition design and efficient process route, combining technological advancement and industrial feasibility. Under the condition of low crack sensitivity index (CEV≤0.52%), this invention does not rely on high content of precious alloys. Through the synergistic effect of microalloying and process strengthening, it achieves stable preparation of X100QS grade pipeline steel pipes with wall thickness of 40~80mm and outer diameter of 219~533mm. The yield strength is 690~810MPa, tensile strength is 760~960MPa, yield ratio is ≤0.95, and elongation is ≥20%. The overall performance is excellent, and the process is highly compatible with existing seamless pipe production lines, which has good prospects for large-scale application. Detailed Implementation
[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Those skilled in the art should understand that the embodiments described are merely illustrative of the invention and should not be considered as specific limitations thereof. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention. Process parameters not specifically specified in the following embodiments are generally performed under conventional conditions.
[0031] The endpoints and any values of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention.
[0032] According to a first aspect of the present invention, the present invention provides an X100QS thick-walled seamless pipeline steel pipe, wherein the chemical composition and mass percentage of the thick-walled seamless pipeline steel pipe are as follows: C 0.13-0.17%, Si 0.50-0.70%, Mn 1.45-1.65%, P≤0.015%, S≤0.005%, Cr 0.10-0.18%, Mo 0.10-0.18%, Ni 0.10-0.18%, Cu≤0.05%, V 0.01-0.05%, Ti 0.010-0.030%, N 0.006-0.012%, O≤0.002%, Al≤0.040%, Nb0.010-0.020%, with the remainder being iron and unavoidable impurity elements; wherein, Ti / N≥3, Nb+V≤0.06%; The crack sensitivity index (CEV) of the steel pipe is ≤0.52%; The wall thickness of the steel pipe is 40mm or more.
[0033] The formula for calculating CEV (%) in this invention is as follows: CEV = C + Mn / 6 + (Cr + Mo + V) / 5 + (Ni + Cu) / 15, where C, Mn, V, Ni, Cr, Cu, and Mo represent the mass percentage of each chemical component.
[0034] This invention primarily targets thick-walled pipes with a wall thickness exceeding 40mm. By adding alloys such as Ni, the hardenability of the material is increased, ensuring uniform performance across the entire cross-section. Controlling the sulfur (S) content below 0.005% promotes spheroidization of sulfide inclusions, improving steel purity and reducing stress concentration during corrosion. Controlling the manganese (Mn) content below 1.7% effectively mitigates Mn segregation, resulting in a uniform and fine initial microstructure. By controlling the Ti / N ratio to ≥3, an appropriate amount of TiN precipitates is formed in the steel, fully utilizing its grain-refining, strength-enhancing, and corrosion-resistant properties. Simultaneously, excessive TiN aggregation to form large inclusions is avoided, preventing the resulting decrease in impact toughness and corrosion resistance. The combined addition of Nb and V, with controlled dosage, further enhances grain refinement and precipitation strengthening effects, achieving X100QS strength requirements in a low-alloy system. Excessive total Nb and V addition prevents complete solid solution, leading to increased segregation, more coarse carbonitrides, and a significant increase in the material's stress corrosion sensitivity.
[0035] As an optional embodiment, the chemical composition and mass percentage of the thick-walled seamless pipeline steel pipe are as follows: C: 0.13%, 0.14%, 0.15%, 0.16% or 0.17%; Si: 0.50%, 0.51%, 0.53%, 0.55%, 0.58%, 0.60%, 0.65% or 0.70%; Mn: 1.45%, 1.50%, 1.55%, 1.60% or 1.65%; P: 0.008%, 0. 0.10%, 0.011%, 0.012%, 0.013%, 0.014% or 0.015%; S: 0.001%, 0.002%, 0.003%, 0.004% or 0.005%; Cr: 0.10%, 0.12%, 0.14%, 0.15%, 0.16%, 0.17% or 0.18%; Mo: 0.10%, 0.12%, 0.14%, 0.15%, 0.16%, 0.17% or 0.015%. 0.18%; Ni: 0.10%, 0.12%, 0.14%, 0.15%, 0.16%, 0.17% or 0.18%; Cu: 0.03%, 0.04% or 0.05%; V: 0.01%, 0.02%, 0.03%, 0.04% or 0.05%; Ti: 0.010%, 0.015%, 0.019%, 0.020%, 0.022%, 0.025% or 0.030%; N: 0.006 %, 0.007%, 0.008%, 0.009%, 0.010%, 0.011% or 0.012%; O: 0.0010%, 0.0011%, 0.0013%, 0.0015% or 0.0020%; Al: 0.020%, 0.025%, 0.030%, 0.035% or 0.040%; Nb: 0.010%, 0.015% or 0.020%, with the remainder being iron and unavoidable impurity elements.
[0036] As an optional implementation, the chemical composition and mass percentage of the thick-walled seamless pipeline steel pipe are as follows: C 0.13-0.16%, Si 0.50-0.60%, Mn 1.50-1.60%, P≤0.015%, S≤0.005%, Cr 0.12-0.18%, Mo 0.12-0.18%, Ni 0.12-0.18%, Cu≤0.05%, V 0.01-0.04%, Ti 0.015-0.025%, N 0.006-0.010%, O≤0.002%, Al≤0.040%, Nb 0.010-0.020%, with the remainder being iron and unavoidable impurity elements.
[0037] In the chemical composition of the preferred steel pipe of the present invention, the ranges of C, Si, Mn, Cr, Mo, Ni, V, Ti, and N are further limited, especially the lower limit of Ni (0.12%), which enhances hardenability; the upper limit of V (0.04%) is reduced to avoid excessive precipitation of carbonitrides; the content of Ti and N is further controlled to ensure the grain refinement effect; and a better balance between economy and performance is achieved, making it suitable for stable industrial production.
[0038] As an optional implementation, the outer diameter of the steel pipe is 219-533mm (e.g., 219mm, 250mm, 300mm, 350mm, 377mm, 400mm, 457mm, 500mm or 533mm), and the wall thickness is 40-80mm (e.g., 40mm, 50mm, 60mm, 70mm or 80mm).
[0039] As an optional embodiment, the steel pipe has a yield strength of 690-810 MPa (e.g., 690 MPa, 700 MPa, 716 MPa, 720 MPa, 737 MPa, 758 MPa, 780 MPa, 800 MPa or 810 MPa), a tensile strength of 760-960 MPa (e.g., 760 MPa, 782 MPa, 803 MPa, 817 MPa, 850 MPa, 880 MPa, 900 MPa or 960 MPa), a yield strength ratio ≤0.95, an elongation ≥20%, a CSR ≤2%, a CLR ≤15%, and a CTR ≤5%.
[0040] In this invention, the X100QS thick-walled seamless pipeline steel pipe is sampled and tested according to the NACE™ 0284 standard. The sample is immersed in an aqueous solution containing 5wt% NaCl and 0.5wt% CH3COOH, and H2S gas at a pressure of 15PSI is introduced. After maintaining this for 72 hours, the steel pipe has a CLR ≤ 15%, and / or CTR ≤ 5%, and / or CSR ≤ 2%.
[0041] In this invention, the X100QS thick-walled seamless pipeline steel pipe is sampled and tested according to the NACE MR 0177 standard. The sample is a type C sample. The sample is immersed in an aqueous solution containing 5wt% NaCl and 0.5wt% CH3COOH, and H2S gas at a pressure of 15PSI is introduced. At the same time, a pressure of 500MPa is applied to the sample and maintained for 720 hours. The sample should not break.
[0042] According to a second aspect of the present invention, the present invention provides a method for preparing X100QS thick-walled seamless pipeline steel pipe as described in the first aspect, the method comprising the following steps in sequence: KR desulfurization, electric furnace smelting, LF refining, RH vacuum treatment, continuous casting, billet heat treatment, rolling and quenching and tempering; wherein the LF refining includes Ca-Si wire treatment.
[0043] This invention forms a closed-loop technology through an eight-step process: KR desulfurization, electric furnace smelting, LF refining, RH vacuum treatment, continuous casting, billet heat treatment, rolling, and tempering. LF refining, combined with Ca-Si line treatment, improves purity and lays the foundation for subsequent microstructure homogenization. Furthermore, continuous casting, high-temperature diffusion (homogenization treatment during billet heating), and specific rolling processes are used to control microstructure segregation in the steel.
[0044] In this invention, the method steps not described in detail are conventional steps in the art. For example, KR desulfurization refers to a process in which the desulfurizing agent is thoroughly mixed and reacted with molten iron through strong mechanical stirring, thereby deeply removing sulfur from the molten iron. Electric furnace smelting involves mixing molten iron and scrap steel for smelting, with the core tasks being decarburization, heating, and dephosphorization.
[0045] As an optional implementation, in the LF refining step, molten steel with a Ca-Si line of 8-10 mm / ton (e.g., 8 mm / ton, 9 mm / ton, or 10 mm / ton) is added; and the inclusions of A sulfides, B alumina, C silicates, and D spherical oxides in the molten steel are controlled to be no higher than grade 0.5.
[0046] In the LF refining step of this invention, the added Ca-Si wire is mainly used to improve the size of Class A inclusions, controlling them to below grade 0.5, which is more than two grades higher than that of conventional pipeline steel (grade 1.5-2.0), thereby reducing their impact on corrosion susceptibility. Controlling S to below 0.005% and using Ca treatment to spheroidize sulfide inclusions optimizes the morphology of inclusions in the steel and reduces stress concentration during corrosion. Sulfide inclusions are the most preferential sites for hydrogen-induced crack initiation; inclusion spheroidization combined with low S (≤0.005%) synergistically reduces the number of HIC cracks to zero. Spheroidized inclusions can eliminate sharp stress notches, reduce stress concentration, and improve matrix connectivity. Simultaneously, it reduces the area of interfacial defects, thereby reducing hydrogen adsorption and aggregation capacity, avoiding the formation of high-pressure hydrogen molecules, and correspondingly increasing the SSCC critical stress.
[0047] As an optional implementation, in the RH vacuum treatment step, the holding time of the absolute pressure less than 66 Pa is greater than 10 minutes and less than 30 minutes, and the total vacuum time is greater than 15 minutes and less than 35 minutes.
[0048] In the RH vacuum treatment step of this invention, insufficient absolute vacuum pressure and inadequate vacuum treatment time result in insufficient removal of inclusions and gases; conversely, excessive vacuum time leads to severe refractory corrosion and the introduction of large particle inclusions. This invention further limits the vacuum level and vacuum holding time to ensure sufficient removal of inclusions and gases. By limiting the total vacuum time, deep degassing is completed before the critical point of refractory corrosion, achieving the preparation of high-purity molten steel.
[0049] As an optional implementation, the diameter of the continuously cast round billet obtained by the continuous casting step is 155-500mm (e.g., 155mm, 160mm, 180mm, 200mm, 230mm, 250mm, 280mm, 300mm, 350mm, 390mm, 400mm, 460mm, 480mm or 500mm).
[0050] As an optional implementation, in the billet heat treatment step, the continuously cast round billet is heated and held at a temperature of less than or equal to 1280℃, preferably 1260~1280℃ (e.g., 1260℃, 1262℃, 1264℃, 1268℃, 1270℃, 1272℃, 1274℃, 1276℃, 1278℃ or 1280℃), and the holding time is greater than or equal to 4 hours, preferably 6~8 hours (e.g., 6.0h, 6.2h, 6.4h, 6.6h, 6.8h, 7.0h, 7.2h, 7.4h, 7.6h, 7.8h or 8.0h).
[0051] In the heat treatment step of the billet in this invention, the holding temperature and holding time of the billet are reasonably controlled to promote the diffusion of elements such as Mn, significantly reduce segregation, improve the uniformity of the microstructure, especially improve the uniformity of the microstructure in the core, eliminate the pearlite / bainite mixed crystal zone, and obtain tempered martensite with full cross-section.
[0052] As an optional implementation, the rolling is performed using an ASSEL tube rolling mill; the initial rolling temperature is greater than or equal to 1250°C, for example, 1250°C, 1260°C, 1270°C or 1280°C, and the final rolling temperature is greater than or equal to 900°C, for example, 900°C, 905°C, 910°C, 915°C, 920°C, 950°C, 980°C, 1000°C, 1020°C, 1050°C, 1100°C or 1150°C.
[0053] As an optional implementation, the rolling is performed using an ASSEL tube rolling mill; the initial rolling temperature is less than 1300°C, and the final rolling temperature is less than 1200°C.
[0054] The ASSEL tube rolling mill used in this invention is suitable for rolling thick-walled tubes. By controlling the initial rolling temperature and the final rolling temperature, rolling is carried out in the austenite partially recrystallized or non-recrystallized region. Through deformation-induced precipitation and dislocation strengthening, the rolled microstructure is refined compared to conventional rolling. Rolling is avoided in the two-phase region (<800℃) to prevent mixed-grain structures and ensure uniform microstructure after rolling, which is beneficial for subsequent quenching to obtain full-section martensite.
[0055] As an optional implementation, the quenching and tempering step includes quenching heat treatment and tempering heat treatment.
[0056] In this invention, tempering includes quenching and tempering. Forced cooling during the quenching process solves the problem of uneven microstructure in the core of thick-walled tubes.
[0057] As an optional implementation, the quenching heat treatment is performed at a quenching temperature of 880-930℃ (e.g., 880℃, 890℃, 900℃, 910℃, 920℃ or 930℃), and the holding time is calculated based on the wall thickness of the steel pipe and is greater than 1 minute / mm.
[0058] As an optional implementation, the quenching holding time of the quenching heat treatment is calculated according to the wall thickness of the steel pipe and is 1.5-2.5 minutes / mm (e.g., 1.5 minutes / mm, 1.8 minutes / mm, 2.0 minutes / mm, 2.3 minutes / mm or 2.5 minutes / mm).
[0059] As an optional implementation, the quenching cooling of the quenching heat treatment is water cooling until the surface temperature of the steel pipe is at room temperature (e.g., 25°C); the water cooling is an overall immersion water cooling method for the steel pipe.
[0060] As an optional implementation, the cooling rate of the quenching heat treatment is greater than or equal to 120°C / min.
[0061] As an optional implementation, for steel pipes with a wall thickness of 40-60mm, the water cooling rate is greater than or equal to 130℃ / min, for example, it can be 130℃ / min, 131℃ / min, 132℃ / min, 133℃ / min, 134℃ / min, 135℃ / min, 136℃ / min, 137℃ / min, 138℃ / min, 139℃ / min, 140℃ / min, 141℃ / min, 142℃ / min, 143℃ / min or 144℃ / min; for steel pipes with a wall thickness greater than 60mm and not greater than 80mm, the water cooling rate is greater than or equal to 120℃ / min, for example, it can be 120℃ / min, 121℃ / min, 122℃ / min, 123℃ / min, 124℃ / min, 125℃ / min, 126℃ / min, 127℃ / min, 128℃ / min or 129℃ / min.
[0062] The cooling method of the present invention can help solve the problem of uneven microstructure in the core of thick-walled tubes, and can also improve cooling efficiency.
[0063] As an optional implementation, the tempering heat treatment temperature is 620-680℃ (e.g., 620℃, 630℃, 640℃, 650℃, 660℃, 670℃ or 680℃); the holding time is calculated according to the wall thickness of the steel pipe and is greater than 2.5 minutes / mm; after tempering, the steel pipe is removed from the furnace and air-cooled to room temperature.
[0064] As an optional implementation, the tempering heat treatment temperature is 640-680℃; the holding time is calculated according to the wall thickness of the steel pipe, 3-5 minutes / mm (e.g., 3.0 minutes / mm, 3.2 minutes / mm, 3.4 minutes / mm, 3.6 minutes / mm, 3.8 minutes / mm, 4.0 minutes / mm, 4.2 minutes / mm, 4.4 minutes / mm, 4.6 minutes / mm, 4.8 minutes / mm or 5.0 minutes / mm).
[0065] In this invention, the quenching and tempering steps include quenching heat treatment and tempering heat treatment. By controlling the quenching holding temperature and holding time, austenite homogenization is ensured. By setting the cooling rate according to the wall thickness of the steel pipe, core hardening is ensured. By controlling the tempering temperature and holding time, a good balance of strength and toughness is achieved. Through the above operations, the problem of uneven microstructure in the core of thick-walled pipes is completely solved, achieving a uniform tempered martensite microstructure across the entire cross-section and improving the resistance of thick-walled pipes to HIC / SSCC.
[0066] The present invention will now be described in further detail with reference to specific embodiments and comparative examples.
[0067] Example 1 This embodiment provides an X100QS thick-walled seamless pipeline steel pipe and its preparation method, as detailed below: 1) Chemical composition The chemical composition and mass percentage of the steel pipe are shown in Table 1 below: Table 1 Where, Ti / N = 0.022 / 0.007 ≈ 3.143 ≥ 3, Nb + V = 0.02 + 0.04 = 0.06%, The crack sensitivity index (CEV) is calculated as follows: CEV = C + Mn / 6 + (Cr+Mo+V) / 5 + (Ni+Cu) / 15 = 0.13 + 1.50 / 6 + (0.17 + 0.16 + 0.04) / 5 + (0.17 + 0.03) / 15 ≈ 0.467% ≤ 0.52% 2) Steel pipe specifications Outer diameter: 457 mm; Wall thickness: 80 mm; 3) Preparation method The steel pipe is prepared sequentially through the following steps: 1. KR desulfurization: Add a mixture of lime and fluorite (mass ratio of 9:1) to molten iron at a rate of 15 kg / ton of molten iron; stir with a stirrer for 15 minutes and then remove the slag to control the sulfur content in the molten iron to ≤0.005%, thus providing a foundation for subsequent low-sulfur smelting; 2. Electric furnace smelting: 40wt% molten iron and 60wt% scrap steel are charged into the electric furnace; when the molten steel temperature reaches 1630℃, the oxide slag is removed; after the molten steel temperature stabilizes at 1610℃ and the composition is uniform, the steel is tapped; tapping control: C 0.05-0.11%, P≤0.008%; during the tapping process, aluminum ingots are added at 1.2 kg / ton of steel for precipitation and deoxidation; 3. LF refining: Add 8 mm / ton of Ca-Si wire to the molten steel, and control the inclusions of A (sulfides), B (alumina), C (silicates), and D (spherical oxides) in the steel to be ≤0.5 grade; 4. RH vacuum treatment: Absolute pressure less than 66Pa, holding time 15min, total vacuum time 25min, effectively removing gas and inclusions from steel; 5. Continuous casting: Casting into continuously cast round billets with a diameter of 460 mm; 6. Heat treatment of the billet: Heat the continuously cast round billet to 1280℃ and hold for 8 hours to promote element diffusion and reduce segregation; 7. Rolling: The ASSEL tube rolling mill is used for rolling. The initial rolling temperature is 1270℃ and the final rolling temperature is 920℃. The tubes are rolled into seamless steel pipes with an outer diameter of 457 mm and a wall thickness of 80 mm. 8. Conditioning and tempering: Quenching heat treatment: holding temperature 930℃, holding time 200 minutes (based on a wall thickness of 80 mm, holding time 2.5 minutes / mm); cooling method is overall immersion water cooling to room temperature, cooling rate is 127℃ / min; Tempering heat treatment: tempering temperature 640℃, holding time 400 minutes (based on a wall thickness of 80 mm, holding time 5 minutes / mm); after tempering, remove from the furnace and air cool to room temperature.
[0068] 4) Performance test results Sampling and testing were conducted according to relevant standards, and the results are as follows: Tensile properties (ASTM E8): Meets X100QS steel grade requirements: yield strength 716 MPa, tensile strength 782 MPa, yield ratio 0.92, elongation 22%; Grain size (ASTM E112): Grade 7, uniform structure; Anti-HIC performance (NACE™ 0284): CLR=1%, CTR=0%, CSR=0%; Resistance to SSCC (NACE MR 0177): The C-type specimen did not fracture after being kept in a solution containing H2S for 720 hours under a stress of 500 MPa.
[0069] In summary, the X100QS thick-walled seamless pipeline steel pipe described in this embodiment achieves a synergistic match of high strength, high toughness, and excellent acid corrosion resistance under the conditions of low alloy and low crack sensitivity index (CEV≤0.52%), meeting the requirements for industrial application of X100QS grade thick-walled pipes.
[0070] Examples 2-3 and Comparative Examples 1-6 Materials were prepared according to the chemical composition and mass percentage (%) of the thick-walled seamless pipeline steel pipes in Table 2-1. The production method of the thick-walled seamless pipeline steel pipes followed the steps of KR desulfurization, electric furnace smelting, LF refining, RH vacuum treatment, continuous casting, billet heat treatment, rolling, and quenching and tempering as described in Example 1. Specific process parameters are detailed in Table 2-2. The mechanical properties of the examples and comparative examples are shown in Table 2-3, and the corrosion resistance properties of the examples and comparative examples are shown in Table 2-4.
[0071] Table 2-1 Table 2-2 Table 2-3 Sampling location: Center of wall thickness.
[0072] The tensile testing method is ASTM E8; the grain size testing method is ASTM E112.
[0073] Table 2-4 Sampling location: Center of wall thickness.
[0074] The test data in Tables 2-1, 2-3, 2-4 clearly show that Examples 1-3, by satisfying the chemical composition range (especially Ti / N≥3, Nb+V≤0.06%, CEV≤0.52%) and process parameter range (cast billet heat treatment temperature 1260-1280℃, time 6-8h, tempering parameters within the preferred range) of the present invention, achieved a synergistic match of high strength (yield strength 690-810MPa, tensile strength 760-960MPa), high plasticity (elongation ≥20%), fine grain structure (grain size ≥7 grade), and excellent resistance to HIC / SSCC. Moreover, the data distribution is reasonable with no obvious outliers, verifying the stability of the composition and process of the present invention.
[0075] In Comparative Example 1, Ti / N = 2.5 < 3, making TiN prone to agglomeration and forming large inclusions, which become hydrogen-induced crack initiation points, resulting in failures in HIC and SSCC. In Comparative Example 2, Nb + V = 0.10% > 0.06%, indicating incomplete solid solution of V and Nb, leading to increased segregation, a rise in coarse carbonitrides, and a significant increase in the material's stress corrosion sensitivity, resulting in failures in HIC and SSCC. In Comparative Example 3, the yield strength (631 MPa) and tensile strength (705 MPa) are both below the standard lower limit because the content of elements such as C, Mn, Cr, Mo, and Ni is too low, resulting in insufficient thick-wall performance and hardenability, although the corrosion resistance is acceptable. In Comparative Example 4, the content of elements such as C, Mn, Cr, Mo, and Ni is too high, with CEV = 0.623% > 0.52%, resulting in poor weldability, decreased plasticity, high structural stress, and an elongation of only 19%, below the standard requirement of 20%, leading to failures in HIC and SSCC. Comparative Example 5's billet was held at 1300℃ (above 1280℃) for 10 hours (longer than 8 hours), resulting in grain coarsening (grain size grade 4), but its corrosion resistance was acceptable because the microstructure, although coarse, was uniform and no obvious crack initiation was formed. Comparative Example 6's billet was held at 1200℃ (below 1260℃) for 4 hours (shorter than 6 hours), resulting in insufficient elimination of Mn segregation, poor microstructure uniformity, and problems with corrosion resistance.
[0076] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the technical solutions of the embodiments of the present invention.
Claims
1. An X100QS thick-walled seamless pipeline steel pipe, characterized in that, The chemical composition and mass percentage of the thick-walled seamless pipeline steel pipe are as follows: C 0.13-0.17%, Si 0.50-0.70%, Mn 1.45-1.65%, P≤0.015%, S≤0.005%, Cr 0.10-0.18%, Mo 0.10-0.18%, Ni 0.10-0.18%, Cu≤0.05%, V 0.01-0.05%, Ti 0.010-0.030%, N 0.006-0.012%, O≤0.002%, Al≤0.040%, Nb 0.010-0.020%, with the remainder being iron and unavoidable impurities; wherein, Ti / N≥3, Nb+V≤0.06%; The crack sensitivity index (CEV) of the steel pipe is ≤0.52%; The wall thickness of the steel pipe is 40mm or more.
2. The X100QS thick-walled seamless pipeline steel pipe according to claim 1, characterized in that, The chemical composition and mass percentage of the thick-walled seamless pipeline steel pipe are as follows: C 0.13-0.16%, Si 0.50-0.60%, Mn 1.50-1.60%, P≤0.015%, S≤0.005%, Cr 0.12-0.18%, Mo 0.12-0.18%, Ni 0.12-0.18%, Cu≤0.05%, V 0.01-0.04%, Ti 0.015-0.025%, N 0.006-0.010%, O≤0.002%, Al≤0.040%, Nb 0.010-0.020%, with the remainder being iron and unavoidable impurity elements.
3. The X100QS thick-walled seamless pipeline steel pipe according to claim 1, characterized in that, The outer diameter of the steel pipe is 219-533mm, and the wall thickness is 40-80mm; And / or, the steel pipe has a yield strength of 690-810 MPa, a tensile strength of 760-960 MPa, a yield-to-tensile ratio of ≤0.95, an elongation of ≥20%, a CSR of ≤2%, a CLR of ≤15%, and a CTR of ≤5%.
4. A method for preparing X100QS thick-walled seamless pipeline steel pipe as described in any one of claims 1-3, characterized in that, The method includes, in sequence, the following steps: KR desulfurization, electric furnace smelting, LF refining, RH vacuum treatment, continuous casting, billet heat treatment, rolling, and quenching and tempering; wherein, the LF refining includes Ca-Si wire treatment.
5. The method for preparing X100QS thick-walled seamless pipeline steel pipe according to claim 4, characterized in that, In the LF refining step, the amount of Ca-Si wire added is 8-10 mm / ton of molten steel; and the inclusions of A sulfides, B alumina, C silicates, and D spherical oxides in the molten steel are controlled to be no higher than grade 0.
5.
6. The method for preparing X100QS thick-walled seamless pipeline steel pipe according to claim 4, characterized in that, In the RH vacuum treatment step, the holding time for an absolute pressure less than 66 Pa is greater than 10 minutes and less than 30 minutes, and the total vacuum time is greater than 15 minutes and less than 35 minutes.
7. The method for preparing X100QS thick-walled seamless pipeline steel pipe according to claim 4, characterized in that, The diameter of the continuously cast round billet obtained by the continuous casting step is 155-500 mm; And / or, in the billet heat treatment step, the continuously cast round billet is heated and held at a temperature of less than or equal to 1280°C, preferably 1260~1280°C, and the holding time is greater than or equal to 4 hours, preferably 6~8 hours.
8. The method for preparing X100QS thick-walled seamless pipeline steel pipe according to claim 4, characterized in that, The rolling process is performed using an ASSEL tube rolling mill; the initial rolling temperature is greater than or equal to 1250℃, and the final rolling temperature is greater than or equal to 900℃; preferably, the initial rolling temperature is less than 1300℃, and the final rolling temperature is less than 1200℃.
9. The method for preparing X100QS thick-walled seamless pipeline steel pipe according to claim 4, characterized in that, The quenching and tempering steps include quenching heat treatment and tempering heat treatment.
10. The method for preparing X100QS thick-walled seamless pipeline steel pipe according to claim 9, characterized in that, The quenching holding temperature for the quenching heat treatment is 880-930℃, and the holding time is calculated according to the wall thickness of the steel pipe, which is greater than 1 minute / mm, preferably 1.5-2.5 minutes / mm; And / or, the quenching cooling of the quenching heat treatment is water cooling until the surface temperature of the steel pipe is room temperature; preferably, the cooling rate is greater than or equal to 120°C / min; more preferably, for steel pipes with a wall thickness of 40-60mm, the water cooling rate is greater than or equal to 130°C / min; for steel pipes with a wall thickness greater than 60mm and not greater than 80mm, the water cooling rate is greater than or equal to 120°C / min. And / or, the tempering heat treatment temperature is 620-680℃, preferably 640-680℃; the holding time is calculated according to the wall thickness of the steel pipe, and is greater than 2.5 minutes / mm, preferably 3-5 minutes / mm; after tempering, the steel pipe is removed from the furnace and air-cooled to room temperature.