A hot working method for stabilizing the microstructure and properties of TC18 alloy forgings
By using hot working methods such as die forging, primary annealing, and secondary annealing, the size and properties of the α phase in TC18 alloy forgings are controlled, solving the problem of mismatch between microstructure and mechanical properties in existing technologies and achieving high-quality forging production.
Patent Information
- Application Number
- CN202611260529.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies make it difficult to simultaneously control the size and properties of the α phase during the hot working of TC18 alloy forgings, resulting in the forgings failing to meet specifications in terms of microstructure and mechanical properties, thus affecting the first-time inspection pass rate.
By employing hot working methods of die forging, primary annealing, and secondary annealing, and by controlling the heating temperature and holding time at different stages, the size of the α phase and the precipitation mode of the metastable β phase in the forging are adjusted to ensure that the forging obtains the microstructure and properties that meet the specifications at various temperatures.
The microstructure and mechanical properties of TC18 alloy forgings were stabilized, ensuring that the α phase length was less than 0.125 mm, meeting the specifications for tensile strength, yield strength and elongation, and improving the production qualification rate of forgings.
Smart Images

Figure CN123108455A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal hot working, and specifically relates to a hot working method for stabilizing the microstructure and properties of TC18 alloy forgings. Background Technology
[0002] TC18 is a near-β type titanium alloy with a nominal composition of Ti-5Al-5Mo-5V-1Cr-1Fe. It possesses advantages such as high strength, high plasticity, good hardenability, and weldability. These advantages make TC18 widely used in the aerospace industry, commonly used to manufacture high-load-bearing structures such as landing gear and main frames of large aircraft. The harsh service environments of these forgings demand extremely high reliability, thus requiring very stringent microstructure and mechanical properties.
[0003] Currently, there are standardized specifications for TC18 forgings in a single-annealing + double-annealing state. Forging employs quasi-β forging technology, resulting in a basketweave microstructure after hot treatment. Performance requirements include tensile strength ≥1080–1230 MPa, yield strength ≥1010 MPa, elongation ≥8 / 7 / 7%, reduction of area ≥20 / 16 / 16%, and α-phase length not exceeding 0.125 mm. However, in actual production applications, achieving coordinated control of α-phase size and performance presents significant challenges. Often, TC18 alloy forgings exhibit α-phase lengths exceeding 0.125 mm after heat treatment, or α-phase sizes are appropriate but forging performance does not meet standard requirements, significantly reducing the first-pass yield. This is because the heating temperature at each stage of hot working significantly impacts the microstructure and properties of TC18 alloy forgings. This inherent contradiction between size and performance has become a prominent technical bottleneck restricting the high-quality and stable production of special components from TC18 alloy forgings. Therefore, there is an urgent need in this field to develop a new hot working method that can precisely control the α phase dimensions of TC18 alloy forgings. Summary of the Invention
[0004] Purpose of the invention: A hot working method is provided to stabilize the microstructure and properties of TC18 alloy forgings. This method not only ensures that all mechanical properties meet the specifications and have a certain margin, but also that the α phase length is less than 0.125 mm, which meets the specifications.
[0005] Technical solution: A hot working method for stabilizing the microstructure and properties of TC18 alloy forgings includes the following steps: Step 1: Die forging The prepared TC18 alloy billet is heated to 20-50°C below the phase transformation point and held for 30-60 minutes. The temperature is then increased to the first preset temperature at a rate of 2-4°C / min and held for 30-60 minutes. Finally, it is die-forged and air-cooled. Step 2, First Annealing: The forged TC18 alloy forging is reheated to the second preset temperature and held for 1 to 3 hours. Then, it is furnace cooled to 730 to 750°C at a cooling rate of 0.3 to 1.0°C / min, held for 1 to 3 hours, and then air cooled. Step 3, Secondary Annealing: The TC18 alloy forging, which was cooled to room temperature in step two, is heated to the third preset temperature, held at that temperature for 2–6 hours, and then air-cooled. First preset temperature: Tβ + (10~15)℃; Second preset temperature: 835℃~845℃; Third preset temperature: 610℃~620℃.
[0006] Furthermore, the microstructure of the TC18 alloy billet used in step one requires the following: The tissue is an α+β dual-state tissue, with the primary α term accounting for 20%–30%.
[0007] Furthermore, in step one, Forging heating: The forgings must be fully supported, with a distance of ≥100mm from the furnace bottom and a spacing of ≥200mm between forgings.
[0008] Furthermore, in steps two and three, after heat treatment heating, the forgings are placed in a single layer after entering the furnace. The spacing between forgings is equal to the distance coefficient × the effective thickness of the forging. The distance coefficient is 1.5 to 3. Anti-warping measures must be taken for structural forgings.
[0009] Furthermore, the furnace temperature for the first annealed forging is the second preset temperature, and the furnace is preheated for ≥20 minutes before loading the forging; the cooling and transfer time for the first annealed forging is ≤120 seconds. Furthermore, the furnace temperature for the second annealing is the third preset temperature, and the furnace is kept in the empty furnace for ≥30 minutes before loading the forgings.
[0010] Furthermore, the forging temperature is adjusted according to the size of the α phase in the forging; the smaller the size of the secondary α phase, the lower the forging temperature.
[0011] Furthermore, the primary annealing temperature is adjusted according to the size of the α phase in the forging; the smaller the size of the secondary α phase, the higher the primary annealing temperature. For every 1°C decrease in the forging temperature, the primary annealing temperature increases by 2°C to 5°C.
[0012] Furthermore, the secondary annealing temperature is adjusted according to the size of the α phase; the smaller the size of the secondary α phase, the lower the secondary annealing temperature. For every 1°C decrease in the forging temperature, the secondary annealing temperature decreases by 1°C to 2°C.
[0013] Beneficial effects: (1) The forging temperature in step one of this invention is selected based on the size of the α phase of the forging. After the TC18 alloy forging is quasi-β forged, the alloy structure is lamellar. As the forging temperature increases, the β grains of the TC18 alloy grow, and the length of the secondary α phase in the grain will increase with the growth of the grain size. Therefore, this method controls the forging temperature to meet the requirements of different α phases.
[0014] (2) Step two of this invention adjusts the forging temperature to improve the performance of the forging and ensure that the mechanical properties of the forging are improved while meeting the standard requirements. In the first stage of the heat treatment annealing process of TC18 alloy forgings, the temperature is close to the α+β→β transformation temperature. After holding at this temperature for a period of time to stabilize the microstructure, a strengthening process can occur due to the decomposition of the metastable β phase. Then, it is furnace cooled to 740-760℃ and held at this temperature. The β phase at this temperature has high stability and can be fixed during air cooling, which is a stabilization treatment. This method can ensure that TC18 alloy forgings at different forging temperatures can obtain a large number of metastable β phases to achieve higher tensile strength.
[0015] (3) In step three of this invention, the secondary annealing temperature is adjusted from the forging temperature to further improve the performance requirements of the forging. During the secondary annealing process, the metastable β phase completely decomposes and precipitates the secondary α phase. As the secondary annealing temperature increases, the nucleation of the α phase is difficult due to the small cooling temperature of the process. However, the higher temperature provides a higher growth driving force, which reduces the volume fraction of the α phase, while increasing its size, resulting in lower strength and improved plasticity. This method can ensure that TC18 alloy forgings at different forging temperatures can obtain a properly proportioned dispersed α phase, achieving the best match between alloy strength and plasticity, and having a large margin.
[0016] In summary, this invention, by considering the influence of different hot working methods on the microstructure and properties of forgings, describes in detail the hot working process parameters for TC18 alloy forgings, specifically the combination of die forging, primary annealing, and secondary annealing. By controlling the size and morphology of the α phase and the precipitation pattern of the metastable β phase, it is possible to obtain a microstructure in TC18 alloys with different element ratios, characterized by β grain sizes of 300–400 μm, discontinuous α grain boundaries, woven α grains within the β grains, and secondary α phase thicknesses of 1–5 μm with a length <0.125 mm, while meeting all specified performance parameters. The process is stable, easy to operate, and suitable for industrial production. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. The drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 This is a magnified 200x microstructure diagram of the TC18 alloy forging after heat treatment in Example 1. Figure 2 This is a magnified 500x microstructure diagram of the TC18 alloy forging after heat treatment in Example 1. Detailed Implementation
[0019] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0020] The features and illustrative embodiments of various aspects of the present invention will now be described in detail. Numerous specific details are set forth in the following detailed description to provide a thorough understanding of the invention. However, it will be apparent to those skilled in the art that the invention may be practiced without requiring some of these specific details. The following description of embodiments is merely intended to provide a better understanding of the invention by illustrating examples of the invention. The invention is by no means limited to any specific setups and methods set forth below, but covers any improvements, substitutions, and modifications to structures, methods, and devices without departing from the spirit of the invention. Well-known structures and techniques are not shown in the drawings and the following description to avoid unnecessarily obscuring the invention.
[0021] In the description of this invention, it should be noted that the directions or positional relationships indicated by terms such as "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer" are based on the directions or positional relationships shown in the accompanying drawings and are only for the convenience of describing and simplifying the invention, and should not be construed as limiting the invention. Furthermore, the use of ordinal numbers (e.g., "first and second," etc.) is for distinguishing objects and is not limited to this order, and should not be construed as indicating or implying relative importance.
[0022] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly, encompassing both direct connection and indirect connection via an intermediate medium. Those skilled in the art can understand the specific meaning of these terms in this invention based on the specific circumstances.
[0023] It should be noted that, unless otherwise specified, the embodiments of the present invention and the features thereof can be combined with each other, and the various embodiments can be referenced and cited in each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0024] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings, but the embodiments of the present invention are not limited thereto.
[0025] In the early stages of production, TC18 alloy forgings frequently encountered microstructural mismatch issues. Therefore, understanding the influence of primary annealing, secondary annealing, and forging temperature on the microstructure and properties of forgings is crucial. Developing precise heat treatment regimes for different forging temperatures, optimizing heat treatment processes, and comprehensively improving the first-pass yield of forgings can be achieved.
[0026] The heat treatment method for TC18 alloy forgings provided by this invention includes: Step 1: Die forging The prepared TC18 alloy billet is heated to 20–50°C below the phase transformation point and held for 30–60 minutes. The temperature is then increased to the first preset temperature at a rate of 2–4°C / min and held for another 30–60 minutes. Finally, it is forged and air-cooled. Step 2: First Annealing The forged TC18 alloy forging is reheated to the second preset temperature and held for 1 to 3 hours. Then, it is furnace cooled to 730 to 750°C at a cooling rate of 0.3 to 1.0°C / min, held for 1 to 3 hours, and then air cooled. Step 3: Secondary annealing The TC18 alloy forging, which was cooled to room temperature in step one, is heated to the third preset temperature, held for 2 to 6 hours, and then air-cooled.
[0027] Optionally, the microstructure of the TC18 alloy billet used in step one should be α+β biphase, with the primary α phase content being 20%–30%. The amount of α phase has a significant impact on the grain size of TC18 alloy and provides a basis for the growth of the α phase in subsequent forgings.
[0028] Optional heating methods include forging: forgings must be fully supported, with a distance of ≥100mm from the furnace bottom and a spacing of ≥200mm between forgings; for heat treatment heating: after entering the furnace, forgings should be placed in a single layer, with the spacing between forgings = distance coefficient × effective thickness of the forging, and the distance coefficient being 1.5~3. Structural forgings must be protected against warping. Titanium alloys have poor thermal conductivity, making the heating uniformity of forgings crucial. The spacing between forgings must be increased to ensure heating uniformity. Furthermore, TC18 has many structural components; therefore, appropriate heat treatment fixtures should be selected during furnace loading to ensure proper packing and stability, reducing warping caused by stress release.
[0029] Optionally, for the first annealing, the furnace temperature for the forging is the final heating temperature, and the furnace is held empty for ≥20 minutes before loading the forging. For the second annealing, the furnace temperature for the forging is the final heating temperature, and the furnace is held empty for ≥30 minutes before loading the forging. The cooling and transfer time for the forging after the first annealing is ≤120 seconds. This promotes uniform cooling of the forging to obtain a uniform forging.
[0030] Optionally, the first preset temperature is Tβ + (10~15)℃, preferably Tβ + 15℃; the second preset temperature is 835℃~845℃, preferably 840℃; and the third preset temperature is 610℃~620℃, preferably 615℃. As the forging temperature decreases, the grain size and α-phase size of the forging decrease, but at the same time, the alloy's properties decrease, especially its fracture toughness. The primary and secondary annealing temperatures of the heat treatment process are adjusted according to the forging temperature to improve the mechanical properties of the forging, thereby improving its performance while ensuring that the microstructure meets the standard requirements.
[0031] Optionally, the forging temperature can be adjusted according to the size of the α phase in the forging. The smaller the required size of the secondary α phase, the lower the forging temperature. As the forging temperature decreases, the β grain size decreases, and the length of the intragranular α phase decreases accordingly.
[0032] Optionally, the primary annealing temperature can be adjusted according to the size of the α phase in the forging. The smaller the required size of the secondary α phase, the higher the primary annealing temperature. Specifically, for every 1°C decrease in the die forging temperature, the primary annealing temperature should be increased by 2°C to 5°C. Increasing the primary annealing temperature results in a greater number of metastable β phases, leading to the precipitation of more secondary α phases in the subsequent secondary annealing. Simultaneously, the α phases become longer, improving both the strength and fracture toughness of the forging.
[0033] Optionally, the secondary annealing temperature can be adjusted according to the size of the α phase. The smaller the size of the secondary α phase, the lower the secondary annealing temperature should be. Specifically, for every 1°C decrease in the die forging temperature, the secondary annealing temperature should be decreased by 1°C to 2°C. When the secondary annealing temperature is lower, due to the large degree of supercooling and the large nucleation driving force, the α phase is easy to nucleate, but diffusion is difficult and it is not easy to grow. This will result in the formation of fine and dispersed α phase, which increases the strength of the forging and reduces its plasticity.
[0034] The invention will now be described in further detail with reference to actual production examples.
[0035] Example The TC18 alloy forgings with dimensions of 448×121×72 mm and an effective thickness of 72 mm are used. The first step involves heating the prepared TC18 alloy forging to 30°C below the phase transformation point, holding for 45 min, then increasing the temperature by 3°C / min to 15°C above the phase transformation point, holding for 30 min, and then performing die forging followed by air cooling. The second step involves heating the forged TC18 alloy forging to 835°C, holding for 150 min, cooling to 750°C, holding for 150 min, and then air cooling in a dispersed manner. Within 120 seconds, the forging is transferred to a cooling rack with a spacing ≥200 mm. Finally, the forging cooled to room temperature in the first step is heated to 618°C, held for 5 hours, and then air cooled.
[0036] The mechanical properties of TC18 alloy forgings are shown in Tables 2 and 4, and the microstructure is as follows: Figure 1 and 2 The 50µm indicates a magnification of 200x, while the 20µm on the right indicates a magnification of 500x.
[0037] Table 1
[0038] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.
Claims
1. A method of hot working a TC18 alloy forging to stabilize the microstructure and properties of the forging, the method comprising: Includes the following steps: Step 1: Die forging The prepared TC18 alloy billet is heated to 20-50°C below the phase transformation point and held for 30-60 minutes. The temperature is then increased to the first preset temperature at a rate of 2-4°C / min and held for 30-60 minutes. Finally, it is die-forged and air-cooled. Step 2, First Annealing: The forged TC18 alloy forging is reheated to the second preset temperature and held for 1 to 3 hours. Then, it is furnace cooled to 730 to 750°C at a cooling rate of 0.3 to 1.0°C / min, held for 1 to 3 hours, and then air cooled. Step 3, Secondary Annealing: The TC18 alloy forging, which was cooled to room temperature in step two, is heated to the third preset temperature, held at that temperature for 2–6 hours, and then air-cooled. First preset temperature: Tβ + (10~15)℃; Second preset temperature: 835℃~845℃; Third preset temperature: 610℃~620℃.
2. The hot working method according to claim 1, characterized in that The microstructure requirements for the TC18 alloy billet used in step one are as follows: The tissue is an α+β dual-state tissue, with the primary α term accounting for 20%–30%.
3. The hot working method of claim 1 wherein, In step one, forging heating: the forgings must be completely supported, with a distance of ≥100mm from the furnace bottom and a spacing of ≥200mm between forgings.
4. The hot working method of claim 1 wherein, In steps two and three, after heat treatment heating, the forgings are placed in a single layer after entering the furnace. The spacing between forgings is equal to the distance coefficient × the effective thickness of the forging. The distance coefficient is 1.5 to 3. Anti-warping measures must be taken for structural forgings.
5. The hot working method of claim 1 wherein, The furnace temperature for the first annealed forging is the second preset temperature. The furnace is kept in the empty furnace for ≥20 minutes before loading the forging. The cooling and transfer time for the first annealed forging is ≤120 seconds.
6. The hot working method of claim 1 wherein, The secondary annealing furnace temperature is the third preset temperature, and the empty furnace is kept warm for ≥30 minutes before loading the forgings into the furnace.
7. The hot working method according to claim 5, characterized in that, The forging temperature is adjusted according to the size of the α phase in the forging. The smaller the size of the secondary α phase, the lower the forging temperature.
8. The hot working method according to claim 5, characterized in that, The primary annealing temperature is adjusted according to the size of the α phase in the forging. The smaller the size of the secondary α phase, the higher the primary annealing temperature should be. For every 1°C decrease in the forging temperature, the primary annealing temperature increases by 2°C to 5°C.
9. The hot working method according to claim 5, characterized in that, The secondary annealing temperature is adjusted according to the size of the α phase. The smaller the size of the secondary α phase, the lower the secondary annealing temperature should be. For every 1°C decrease in the forging temperature, the secondary annealing temperature decreases by 1°C to 2°C.