A method for preparing transition metal-doped β-Ga2O3 thin films and an ultraviolet photodetector

By optimizing the temperature and oxygen partial pressure process windows of Ni and Fe doped β-Ga2O3 thin films, the problems of dark current suppression and multi-valence imbalance in the prior art were solved, and a high-performance ultraviolet photodetector with photosensitivity in a specific wavelength band was fabricated.

CN123108482APending Publication Date: 2026-11-17CHANGZHOU UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611332558.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for preparing transition metal-doped β-Ga2O3 thin films for photodetectors suffer from problems such as difficulty in suppressing dark current and imbalance in the proportion of Ni or Fe multivalent states within the film. This results in the photodetector lacking photosensitive response in specific wavelength bands, making it difficult to meet the requirements for high-performance detection.

Method used

By studying different temperature and oxygen partial pressure process windows for Ni and Fe, two transition metal doping elements, we achieved a balance of coexistence of multiple valence states of Ni2+/Ni3+ or Fe2+/Fe3+, optimized the crystal quality and surface roughness of the thin film, and fabricated an MSM structure ultraviolet photodetector with a dark current stable in the order of 10-10 A.

Benefits of technology

We achieved high response of Ni-doped detectors to 254 nm solar-blind deep ultraviolet and detection capability of Fe-doped detectors to 365 nm near ultraviolet. We optimized film quality and changed device function, realizing complementary detection of the same parent material in the same band.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108482A_ABST
    Figure CN123108482A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of semiconductor thin-film devices and discloses a method for preparing transition metal-doped β-Ga2O3 thin films and an ultraviolet photodetector. This invention studies the process windows for different doping elements. Specifically, when preparing Ni-doped thin films using pulsed laser deposition (PLD), a high oxygen partial pressure window of 580–620 °C and 0.01–0.05 mbar is selected; when preparing Fe-doped thin films, a high oxygen partial pressure window of 680–720 °C and 1 × 10⁻⁶ mbar is selected. ‑5 ~3×10 ‑5 The high-temperature, low-oxygen partial pressure window of mbar. The parameter selection of this invention not only achieves Ni 2+ / Ni 3+ or F 2+ / Fe 3+ Multivalent state micro-equilibrium improves the crystal quality of thin films and enables functional differentiation of the same matrix material for Ni doping in the 254nm deep ultraviolet and Fe doping in the 365nm near ultraviolet, making it suitable for high-performance band custom detectors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of ultrawide bandgap semiconductor thin film preparation and optoelectronic device technology, specifically to a transition metal-doped β-Ga2O3 thin film, its growth window control method, and an ultraviolet photodetector. Background Technology

[0002] β-Ga₂O₃ is a typical ultrawide bandgap semiconductor material with broad application prospects in ultraviolet photodetectors and high-power electronic devices. Pulsed laser deposition (PLD) is widely used to prepare β-Ga₂O₃ thin films. In recent years, to control the electronic structure, oxygen vacancies, and photoelectric response characteristics of the thin films, the introduction of transition metals with multivalent state characteristics (such as Fe and Ni) as doping has become an important research direction. The bandgap of β-Ga₂O₃ is approximately 4.8–5.3 eV. Thin films prepared by pulsed laser deposition (PLD) are sensitive to process parameters such as growth temperature and oxygen partial pressure. Different process conditions result in different oxygen vacancy concentrations and crystal defects, leading to differences in device performance.

[0003] CN201811096587.5 discloses a method for preparing gallium oxide thin films by lowering the crystallization temperature through iron doping. This method uses an Fe-doped ceramic target to prepare gallium oxide thin films at a low temperature of 425–575 °C, preferably 550 °C. The purpose of this prior art is to lower the crystallization threshold; however, in practical applications with photodetectors, the low-temperature process presents several problems: lower thermal activation energy and poor long-range order of atoms in the internal lattice of the thin film. Actual tests show that the doped thin film grown at 550 °C has a wide full width at half maximum (FWHM) of the (-201) plane diffraction peak, uncontrollable deep-level defects in the bulk, and difficulty in suppressing the dark current of the prepared detector, making it difficult to meet the requirements of high signal-to-noise ratio detection.

[0004] Current techniques often limit the study of parameters for different transition metal doping to conventional temperature and pressure ranges. However, Ni and Fe differ significantly in their redox potentials, ionic radii, and coupling energies with oxygen vacancies. Blindly applying a universal process can lead to multiple valence states of Ni or Fe within the thin film, such as Ni... 2+ / Ni 3+ or Fe 2+ / Fe 3+ Imbalance in proportions. Currently fabricated detectors have difficulty suppressing dark current, ultimately preventing the photodetectors from having photosensitivity responses in specific wavelength bands, making it difficult to meet the requirements of high-performance detection. Summary of the Invention

[0005] To address the aforementioned problems, this invention provides a method for preparing transition metal-doped β-Ga₂O₃ thin films. Different temperature and oxygen partial pressure process windows were investigated for Ni and Fe, two different transition metal doping elements, to overcome the challenge of discontinuous film formation. Ultimately, Ni was successfully doped within the thin film. 2+ / Ni 3+ or Fe 2+ / Fe 3+ The balance of multiple valence states improves the crystallinity of the thin film, significantly reduces surface roughness, and suppresses the dark current of the MSM structure detector to within 10. -10 A-level.

[0006] A method for preparing a transition metal-doped β-Ga2O3 thin film includes the following steps:

[0007] (1) Select a c-plane sapphire substrate, clean and dry it, place it in the growth chamber of the pulsed laser deposition equipment, and evacuate to achieve a back-side vacuum of 1×10⁻⁶. -5 Below mbar;

[0008] (2) Select different specific process windows for thin film deposition based on the type of transition metal doped target:

[0009] When using Ni-doped β-Ga2O3 target material, the selected process window is: growth temperature of 580℃~620℃ and oxygen partial pressure of 0.01 mbar~0.05 mbar.

[0010] When using Fe-doped β-Ga2O3 target material, the selected process window is: growth temperature of 680℃~720℃ and oxygen partial pressure of 1×10⁻⁶. -5 mbar~3×10 -5 mbar;

[0011] (3) After the thin film deposition and growth is completed, the oxygen partial pressure in the growth chamber is adjusted to 200 mbar and kept in situ at the corresponding deposition and growth temperature for 8 to 15 min; then the temperature is reduced to room temperature at a rate of 10 to 15 °C / min.

[0012] The present invention also provides an MSM structure ultraviolet photodetector, which uses a transition metal-doped β-Ga2O3 thin film prepared by the above method as a photosensitive layer, and Au / Cr interdigitated electrodes are prepared on its surface.

[0013] Using the Ni-doped and Fe-doped β-Ga2O3 thin films obtained under the above growth window as the photosensitive layer, Au / Cr interdigitated electrodes were prepared to form an MSM structure ultraviolet photodetector.

[0014] Compared with the prior art, the present invention has at least the following beneficial effects:

[0015] (1) The growth windows corresponding to the intrinsic, Ni-doped and Fe-doped β-Ga2O3 systems cannot be substituted for each other: using the growth window of one system for another system will cause the (-201) characteristic diffraction peak to disappear or the full width at half maximum (FWHM) to increase significantly.

[0016] (2) This invention discovered that the oxygen partial pressure parameters for Ni-doped and Fe-doped films do not have similar conditions, but rather differ significantly. Applying these parameters interchangeably will lead to serious consequences such as failure to form a film or crystallization degradation. This invention matches the difference in redox potentials between Ni and Fe at high temperatures, enabling the internal Ni-doped film... 2+ / Ni 3+ and Fe 2+ / Fe 3+ The equilibrium of multiple valence states keeps the dark current stably suppressed at 10. -10 A-level.

[0017] (3) Conventional parameter optimization can only change the surface roughness or the current magnitude. The Ni-doped detector prepared by this invention exhibits a high response to 254 nm solar-blind deep ultraviolet; while the Fe-doped detector successfully activated deep-level defects and exhibited the ability to detect 365 nm near ultraviolet, realizing band complementarity of the same parent material, which not only optimized the film quality, but also changed the device function.

[0018] (4) The Ni-doped and Fe-doped β-Ga2O3 thin films prepared by the method of the present invention have a full width at half maximum (FWHM) of the (-201) crystal plane diffraction peak of no more than 0.26° and a root mean square surface roughness of no more than 3 nm, and respectively form Ni 2+ / Ni 3+ Fe 2+ / Fe 3+ Coexisting valence distribution.

[0019] (5) The photocurrent of the detector constructed by the Ni-doped system is about two orders of magnitude higher than that of the dark current under 254 nm illumination; the dark current of the detector constructed by the Fe-doped system is on the same order of magnitude as that of the Ni-doped system. Attached Figure Description

[0020] Figure 1 The XRD patterns of intrinsic Ga2O3, Ni-doped Ga2O3, and Fe-doped Ga2O3 films obtained under the optimal growth conditions of this invention are shown.

[0021] Figure 2This is a curve showing the full width at half maximum (FWHM) of the (-201) crystal plane diffraction peaks of intrinsic Ga2O3, Ni-doped Ga2O3, and Fe-doped Ga2O3 films as a function of growth temperature (dual ordinates, with the intrinsic and Ni-doped films on the left ordinate and the Fe-doped film on the right ordinate).

[0022] Figure 3 This is a graph showing the full width at half maximum (FWHM) of the (-201) crystal plane diffraction peaks of intrinsic Ga2O3, Ni-doped Ga2O3, and Fe-doped Ga2O3 films as a function of oxygen pressure (dual ordinates, with the intrinsic and Ni-doped films on the left ordinate and the Fe-doped film on the right ordinate).

[0023] Figure 4 This is an AFM morphology image of the intrinsic Ga2O3 thin film obtained under the optimal growth conditions of this invention;

[0024] Figure 5 This is an AFM morphology image of the Ni-doped Ga2O3 thin film obtained under the optimal growth conditions of this invention;

[0025] Figure 6 This is an AFM morphology image of the Fe-doped Ga2O3 thin film obtained under the optimal growth conditions of this invention;

[0026] Figure 7 This is an XPS image of the Ni2p orbitals of the Ni-doped Ga2O3 thin film obtained under the optimal growth conditions of this invention;

[0027] Figure 8 This is an XPS image of the Fe2p orbitals of the Fe-doped Ga2O3 thin film obtained under the optimal growth conditions of this invention;

[0028] Figure 9 Ni in Ni-doped Ga2O3 3+ / Ni 2+ Proportion and Fe in Fe-doped Ga2O3 3+ / Fe 2+ A graph showing how the proportion changes with growth temperature;

[0029] Figure 10 Ni in Ni-doped Ga2O3 3+ / Ni 2+ Proportion and Fe in Fe-doped Ga2O3 3+ / Fe 2+ A graph showing how the proportion changes with oxygen pressure;

[0030] Figure 11 These are the IV curves of the Ni-doped Ga2O3 device under different illumination conditions under the optimal conditions of this invention;

[0031] Figure 12These are the IV curves of the Fe-doped Ga2O3 device under different illumination conditions under the optimal conditions of this invention;

[0032] Figure 13 The intrinsic Ga2O3 thin film at 600℃ and 2×10 -5 XRD patterns under mbar growth conditions;

[0033] Figure 14 The intrinsic Ga2O3 thin film at 600℃ and 2×10 -5 AFM morphology under mbar growth conditions;

[0034] Figure 15 It is a Ni-doped Ga2O3 thin film at 600℃ and 2×10 -5 XRD patterns under mbar growth conditions;

[0035] Figure 16 It is a Ni-doped Ga2O3 thin film at 600℃ and 2×10 -5 AFM morphology under mbar growth conditions;

[0036] Figure 17 It is an Fe-doped Ga2O3 thin film at 700℃ and 2×10 -2 XRD patterns under mbar growth conditions;

[0037] Figure 18 It is an Fe-doped Ga2O3 thin film at 700℃ and 2×10 -2 AFM morphology under mbar growth conditions. Detailed Implementation

[0038] Experimental materials and instructions:

[0039] Depending on the desired doping system, this invention employs one of the following three ceramic targets: intrinsic Ga₂O₃ ceramic target; Ni-doped Ga₂O₃ ceramic target; Ni to Ga atomic ratio 2:98; Fe-doped Ga₂O₃ ceramic target; Fe to Ga atomic ratio 25:75. Testing revealed that the resulting film contained approximately 1 at% Ni and approximately 2 at% Fe. Compared to the Ni system, a higher proportion of Fe is required in the target to achieve comparable film doping concentrations, indicating that the transfer efficiency of Fe during pulsed laser ablation and plasma plume transport is lower than that of Ni.

[0040] All substrates were selected from c-plane sapphire substrates. Before deposition, the substrates were ultrasonically cleaned for 15 min each with acetone, anhydrous ethanol and deionized water, and then dried with nitrogen gas.

[0041] The substrate was placed in the pulsed laser deposition chamber, and the vacuum level was evacuated to 1×10⁻⁶.-5 Below mbar. Deposition was performed using a KrF excimer laser with a wavelength of 248 nm and a laser energy density of 2.0 J / cm². 2 The laser frequency was 4 Hz, the target-substrate distance was 50 mm, and the deposition pulse count was 10,000. After the film growth was completed, the oxygen partial pressure was uniformly adjusted to 200 mbar, and the film was kept in situ at the corresponding growth temperature for 10 min, and then cooled to room temperature at a cooling rate of 12 ℃ / min.

[0042] Example 1

[0043] Preparation of intrinsic Ga2O3 thin films.

[0044] A c-plane sapphire substrate was selected and ultrasonically cleaned sequentially with acetone, anhydrous ethanol, and deionized water, with each cleaning step lasting 15 minutes. After cleaning, the substrate was dried with nitrogen. The cleaned substrate was then placed in a pulsed laser deposition chamber, and a vacuum was evacuated to a back-side vacuum of 1×10⁻⁶. -5 Below mbar, heat to 600℃ at a heating rate of 20 ℃ / min and hold for 10 min.

[0045] Intrinsic Ga2O3 ceramic target material was used, and pulsed laser deposition was performed using a KrF excimer laser with a wavelength of 248 nm and a laser energy density of 2.0 J / cm². 2 The laser frequency was 4 Hz, the target-substrate distance was 50 mm, the deposition pulse count was 10,000, and the oxygen partial pressure was fixed at 0.02 mbar during the deposition process. After the film growth was completed, the oxygen partial pressure was adjusted to 200 mbar, and the film was kept at the growth temperature for 10 min. Then, the substrate temperature was reduced to room temperature at a cooling rate of 12 ℃ / min to obtain the intrinsic Ga2O3 film.

[0046] The obtained thin film was characterized by XRD, and the results are as follows: Figure 1 As shown. The thin film was characterized by AFM, and the results are as follows. Figure 4 As shown, the root mean square roughness (RMS) of the thin film surface is 5.09 nm.

[0047] Comparative Example 1:

[0048] Compared with Example 1, the oxygen partial pressure was fixed at 0.02 mbar. The difference was that the growth temperature was adjusted to 500℃, 550℃ and 650℃ respectively, and comparative samples were prepared. These samples, along with the samples from Example 1 at 600℃, were subjected to XRD characterization.

[0049] like Figure 2As shown, the full width at half maximum (FWHM) of the (-201) crystal plane diffraction peaks corresponding to the four temperature points are 0.2306°, 0.20064°, 0.18788°, and 0.2213°, respectively, showing a trend of first decreasing and then increasing, reaching the minimum value at 600°C.

[0050] Compared to Example 1, the growth temperature was fixed at 600°C, the difference being that the oxygen partial pressure was adjusted to 2 × 10⁻⁶. -5 mbar, 2×10 -4 mbar, 2×10 -3 mbar and 0.2 mbar were used to prepare control samples. Among them, 2×10 -5 mbar and 2×10 -4 No obvious (-201) diffraction peak was detected under the mbar condition. Detailed XRD and AFM characterization results under this condition are shown in Comparative Example 2. Figure 13 , Figure 14 ); 2×10 -3 Although a (-201) diffraction peak can be fitted under the mbar condition, the peak area and peak height are about two orders of magnitude lower than under other conditions. The corresponding AFM morphology shows obvious granular / island protrusions, indicating a very weak film crystallization signal under this condition. Therefore, it is evident that the intrinsic Ga2O3 system at 600℃ is unlikely to form a detectable continuous crystalline film when the oxygen partial pressure is below 0.02 mbar. Under the conditions of 0.02 mbar and 0.2 mbar, the full width at half maximum (FWHM) of the (-201) crystal plane diffraction peak are 0.18788° and 0.20621°, respectively, with the FWHM increasing with increasing oxygen partial pressure. Figure 3 Therefore, 0.02 mbar is the minimum oxygen partial pressure required for the intrinsic Ga2O3 system to form a continuous crystalline film, and it is also the condition with the best crystal quality.

[0051] Example 2

[0052] The Ni-doped β-Ga2O3 thin film was prepared by using a Ni-doped Ga2O3 ceramic target, with a growth temperature of 600℃ and an oxygen partial pressure of 0.02 mbar during deposition. Other preparation methods were the same as in Example 1, resulting in the Ni-doped β-Ga2O3 thin film.

[0053] The obtained thin film was characterized by XRD, and the results are as follows: Figure 1 As shown, the full width at half maximum (FWHM) of the diffraction peak on the (-201) crystal plane is 0.20272°. AFM characterization of the thin film yielded the following results: Figure 5 As shown, the root mean square roughness (RMS) of the film surface is 2.31 nm. XPS characterization of the film yielded the following results: Figure 7 As shown, the Ni2p orbital spectrum, after peak fitting, reveals Ni... 2+ with Ni 3+ Characteristic peaks coexist.

[0054] Furthermore, the cross-section of the thin film was characterized by SEM, and the thickness of the Ni-doped β-Ga2O3 thin film obtained under these conditions was found to be approximately 270–490 nm on the substrate.

[0055] Example 3

[0056] Fe-doped Ga2O3 ceramic target was used, the growth temperature was set at 700℃, and the oxygen partial pressure during deposition was set at 2×10⁻⁶. -5 mbar. Other preparation methods are the same as in Example 1, yielding Fe-doped β-Ga2O3 thin films.

[0057] The obtained thin film was characterized by XRD, and the results are as follows: Figure 1 As shown, the full width at half maximum (FWHM) of the (-201) crystal plane diffraction peak is 0.23952°; apart from the characteristic diffraction peak of β-Ga2O3, no other second-phase diffraction peaks were observed within the detection sensitivity range in the XRD pattern. AFM characterization of the thin film yielded the following results: Figure 6 As shown, the root mean square roughness (RMS) of the film surface is 1.39 nm. XPS characterization of the film yielded the following results: Figure 8 As shown, the Fe2p orbital spectrum, after peak fitting, reveals Fe... 2+ with Fe 3+ Characteristic peaks coexist.

[0058] XPS characterization of the intrinsic, Ni-doped, and Fe-doped Ga2O3 films was performed at their respective growth temperatures and oxygen partial pressures. The results are as follows: Figure 9 , Figure 10 As shown. Ni-doped system Ni 3+ / Ni 2+ The proportion first increases and then decreases with growth temperature, peaking at 600℃ (0.914), consistent with the optimal growth temperature for crystallization quality of this system; it first increases and then decreases with oxygen partial pressure, reaching a peak at 2×10⁻⁶. -3 The Fe content remained high in the 0.2 mbar to 0.923 mbar range (0.923, 0.857). Fe-doped systems... 3+ / Fe 2+ The proportions showed a monotonically increasing trend with both growth temperature and oxygen partial pressure, and no inflection point was observed within the test range where the proportions decreased with further increases in temperature or oxygen partial pressure (0.458, 0.656, 0.726, and 1.753 corresponding to growth temperatures of 550–750℃; oxygen partial pressure 2×10⁻⁶). -6 ~0.2 mbar corresponds to 0.160, 1.779, 1.987, and 4.506.

[0059] Comparative Example 2:

[0060] Compared with Example 2, the oxygen partial pressure was kept constant at 0.02 mbar. The only difference was that the growth temperature was adjusted to 500℃, 550℃, and 650℃ to obtain different Ni-doped Ga2O3 thin film samples.

[0061] like Figure 2 As shown: The comparative sample was prepared and characterized by XRD: The full width at half maximum (FWHM) of the (-201) crystal plane diffraction peaks at the four temperature points of 500℃, 550℃, 600℃ and 650℃ were 0.27727°, 0.21661°, 0.20272° and 0.25854° respectively. The peak width first decreased and then increased with increasing temperature, and was narrowest at 600℃.

[0062] Compared to Example 2, the growth temperature was fixed at 600℃, the only difference being that the oxygen partial pressure was set to 2×10⁻⁶. -5 mbar, 2×10 -4 mbar, 2×10 -3 Comparative samples were prepared at mbar and 0.2 mbar and tested using XRD.

[0063] like Figure 2 As shown: where 2×10 -4 mbar, 2×10 -3 The full width at half maximum (FWHM) of the (-201) crystal plane diffraction peaks corresponding to the four conditions of mbar, 0.02 mbar, and 0.2 mbar are 1.18384°, 0.40834°, 0.20272°, and 0.45319°, respectively, showing a decrease followed by an increase, with the narrowest point at 0.02 mbar. (2×10⁻⁶) -5 The diffraction peak intensity under the mbar condition is close to the background noise, and the fitted full width at half maximum (FWHM) is abnormally low (approximately 10). -7 This phenomenon (on the order of magnitude) is related to the low effective coverage of the film or the lack of long-range ordered structure, and therefore is not included in the above comparison.

[0064] The oxygen partial pressure is 2 × 10⁻⁶ -5 The condition of mbar is the same as the optimal oxygen partial pressure determined for the Fe-doped system. Therefore, the intrinsic Ga₂O₃ film and the Ni-doped Ga₂O₃ film grown at the same temperature of 600℃ under this condition were also characterized. The XRD patterns of the intrinsic Ga₂O₃ film are shown below. Figure 13 As shown, only a very weak (-402) diffraction peak is visible in the spectrum, and the characteristic (-201) diffraction peak is not observed; its AFM morphology is as follows. Figure 14 As shown, the root mean square roughness (RMS) of the surface is only 0.14 nm. The XRD pattern of the Ni-doped Ga2O3 thin film is shown below. Figure 15 As shown, only a very weak (-402) diffraction peak is visible; its AFM morphology is as follows. Figure 16As shown, the root mean square roughness (RMS) of the surface is 0.64 nm. Combined with the corresponding XRD pattern, this indicates that the low effective coverage of the film under this low oxygen partial pressure prevents the formation of a continuous and dense crystalline film. This demonstrates that the specific low oxygen partial pressure condition for Fe doping is ineffective for both the Ni system and the intrinsic system.

[0065] Comparative Example 3:

[0066] The difference between Comparative Example 3 and Example 3 is that the oxygen partial pressure was kept constant at 0.02 mbar, and the growth temperature was adjusted to 550℃, 650℃, and 750℃ respectively to prepare comparative samples.

[0067] like Figure 2 As shown, the full width at half maximum (FWHM) of the (-201) crystal plane diffraction peaks at four temperature points of 550℃, 650℃, 700℃, and 750℃ are 0.75543°, 0.35997°, 0.34635°, and 0.37323°, respectively, showing a decrease followed by an increase, with the narrowest point at 700℃.

[0068] The difference between Comparative Example 3 and Example 3 is that the growth temperature is fixed at 700°C, and the oxygen partial pressure is adjusted to 2 × 10⁻⁶. -6 mbar, 2×10 -5 mbar, 2×10 -3 mbar and 0.2 mbar were used to prepare control samples.

[0069] like Figure 2 As shown: 2×10 -6 mbar, 2×10 -5 mbar, 2×10 -3 The full width at half maximum (FWHM) of the (-201) crystal plane diffraction peak under the four conditions of mbar, 0.2 mbar, and 0.44076°, 0.23952°, 0.31844°, and 0.66518°, respectively, showing a decrease followed by an increase, 2×10 -5 The narrowest point is at mbar.

[0070] Comparative data shows that at 700℃ and an oxygen partial pressure of 0.02 mbar (i.e., the oxygen partial pressure corresponding to the intrinsic and Ni-doped systems), the full width at half maximum (FWHM) of the (-201) plane diffraction peak in the Fe-doped thin film is 0.34635°. Figure 17 (), worse than the optimal growth window of 700℃ and 2×10 -5 0.23952° at mbar; the AFM morphology under this condition is as follows Figure 18 As shown, the root mean square roughness (RMS) of the surface is 0.54 nm.

[0071] Example 4

[0072] Fabrication and testing of Ni-doped MSM ultraviolet photodetectors.

[0073] Using the Ni-doped β-Ga2O3 thin film prepared in Example 2 as the photosensitive layer, Au / Cr interdigitated electrodes were formed on its surface by photolithography and electron beam evaporation to form an MSM structure ultraviolet photodetector; the finger length L of the interdigitated electrodes was 3452.2 μm, the electrode spacing d was 72.9 μm, the electrode width was 142.9 μm, and the effective gap number N was [missing information]. gap There are 23 in total, and the total number is 24, corresponding to an effective light-receiving area S=N. gap ×L×d≈5.7883×10 -2 cm 2 .

[0074] The IV characteristics of the device were tested in the dark state and under illumination at wavelengths of 254 nm and 365 nm within a voltage range of -15 V to 15 V. The results are as follows: Figure 11 As shown. The dark-state current is at 10. -10 The A-level, rising to 10 under 254 nm illumination. -8 The improvement is on the order of A, approximately two orders of magnitude greater than the dark state; under 365 nm illumination, it is 10. -9 The current difference is on the order of A. This relates to the Ni content in the thin film. 2+ / Ni 3+ It is related to the distribution of coexisting valence states.

[0075] Example 5

[0076] Fabrication and testing of Fe-doped MSM ultraviolet photodetectors.

[0077] The preparation process is the same as in Example 4, except that the photosensitive layer is replaced with the Fe-doped β-Ga2O3 thin film obtained in Example 3. IV test results under the same voltage range and illumination conditions are as follows: Figure 12 As shown: the dark-state current is on the same order of magnitude as that of the Ni-doped system device, and the separation between the dark-state, 254 nm, and 365 nm curves is less than that of the Ni-doped system device. Figure 11 The degree of separation between the 254 nm curve of the Ni-doped device and the other two curves. This difference is related to Fe. 2+ / Fe 3+ It is related to the distribution of valence states.

[0078] In Fe-doped devices, the photocurrent under 365 nm illumination is significantly higher than that under 254 nm illumination, which is the opposite of the characteristic exhibited by Ni-doped devices, which show the strongest response at 254 nm. This demonstrates that Fe doping effectively activates deep-level defects, achieving selective detection enhancement in the 365 nm near-ultraviolet band and realizing complementary detection capabilities within the same parent material.

[0079] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a transition metal-doped β-Ga₂O₃ thin film, characterized in that, Deposition was performed on the substrate using pulsed laser deposition. When using Ni-doped β-Ga2O3 target material, the deposition growth process conditions are: growth temperature of 580℃~620℃, and oxygen partial pressure of 0.01 mbar~0.05 mbar. When using Fe-doped β-Ga₂O₃ target material, the deposition conditions are: growth temperature of 680℃~720℃, and oxygen partial pressure of 1×10⁻⁶. -5 mbar~3×10 -5 mbar.

2. The method for preparing transition metal-doped β-Ga₂O₃ thin films according to claim 1, characterized in that, The substrate is a c-plane sapphire substrate; before pulsed laser deposition, the substrate is placed in the growth chamber, and the growth chamber is evacuated to a back-side vacuum level of 1×10⁻⁶. -5 Below mbar.

3. The method for preparing transition metal-doped β-Ga₂O₃ thin films according to claim 1, characterized in that, Pulsed laser deposition was performed using a KrF excimer laser with a wavelength of 248 nm and a laser energy density of 2.0 J / cm². 2 The laser frequency was 4 Hz, the target distance was 50 mm, and the deposition pulse count was 10,000.

4. The method for preparing transition metal-doped β-Ga₂O₃ thin films according to claim 1, characterized in that, After deposition and growth are completed, the oxygen partial pressure in the growth chamber is adjusted to 200 mbar and kept in situ at the corresponding deposition and growth temperature for 8 to 15 minutes; then the temperature is reduced to room temperature at a rate of 10 to 15 °C / min.

5. The method for preparing transition metal-doped β-Ga₂O₃ thin films according to claim 1, characterized in that, When using a Ni-doped β-Ga₂O₃ target, the growth temperature is 600℃ and the oxygen partial pressure is 0.02 mbar; when using an Fe-doped β-Ga₂O₃ target, the growth temperature is 700℃ and the oxygen partial pressure is 2 × 10⁻⁶ mbar. -5 mbar.

6. The method for preparing transition metal-doped β-Ga₂O₃ thin films according to claim 1, characterized in that, The atomic ratio of Ni to Ga in the Ni-doped β-Ga₂O₃ target is 1~3:97~99; the atomic ratio of Fe to Ga in the Fe-doped β-Ga₂O₃ target is 20~30:70~80; the Ni content in the Ni-doped β-Ga₂O₃ film is 0.8~1.2 at%; and the Fe content in the Fe-doped β-Ga₂O₃ film is 1.5~2.5 at%.

7. A transition metal-doped β-Ga₂O₃ thin film, characterized in that: The film is prepared by the method according to any one of claims 1-6; when the film is Ni-doped, Ni is formed inside the film. 2+ with Ni 3+ The coexistence of multiple valence states; the full width at half maximum (FWHM) of the (-201) crystal plane diffraction peak is less than 0.22°; when the film is Fe-doped, Fe forms inside the film. 2+ with Fe 3+ The coexistence of multiple valence states, the full width at half maximum (FWHM) of the (-201) crystal plane diffraction peak is less than 0.26°.

8. An ultraviolet photodetector, characterized in that, It includes a photosensitive layer and interdigitated electrodes deposited on the surface of the photosensitive layer, wherein the photosensitive layer is a transition metal-doped β-Ga2O3 thin film prepared by the method according to any one of claims 1-6.

Citation Information

Patent Citations

  • A method for preparing gallium oxide thin films by lowering the crystallization temperature through iron doping

    CN109411328B