A continuous induced molding process for silver selenide thermoelectric materials

By pre-supplementing Se and using femtosecond laser parameter control, continuous induced molding of silver selenide thermoelectric materials was achieved, solving the problems of complex traditional preparation processes and Se loss, and improving the stability and preparation efficiency of the materials.

CN123108501APending Publication Date: 2026-11-17NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611377871.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional silver selenide thermoelectric materials have complex preparation processes, poor material stability, and laser processing leads to the loss of Se elements, making it difficult to achieve efficient fabrication of microscale devices.

Method used

By pre-supplementing Se elements and combining the average power, scanning speed, and defocusing distance of the femtosecond laser, the silver selenide film is continuously acted on along a preset path to achieve local release, continuous transfer, and shaping of the material, integrating material transfer and structural shaping into the same processing procedure.

Benefits of technology

The preparation process of silver selenide thermoelectric materials has been simplified, the stability and molding continuity of the materials have been improved, component segregation has been reduced, and digital and continuous preparation of silver selenide thermoelectric materials has been realized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108501A_ABST
    Figure CN123108501A_ABST
Patent Text Reader

Abstract

This invention provides a continuous induced forming process for silver selenide thermoelectric materials, relating to the field of material forming. The process includes: pre-supplementing Se elements in a magnetron sputtering target based on an Ag₂Se target composition; pre-fabricating a silver selenide thin film on the surface of a transparent substrate using the target; maintaining a certain distance between the silver selenide thin film and the acceptor substrate; setting the amplifier frequency parameters of a femtosecond pulsed laser; and then irradiating the silver selenide thin film through the transparent substrate while continuously scanning according to a preset forming path. By adjusting the average laser power, scanning speed, and defocusing distance, the silver selenide thin film undergoes localized melting and release, ultimately transferring to the surface of the acceptor substrate to form a continuous silver selenide structure. This process, through the combined effect of Se element pre-compensation and laser process parameter control, achieves non-contact, digital continuous forming of silver selenide materials, improving the preparation efficiency of silver selenide thermoelectric materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a continuous induced forming process for silver selenide thermoelectric materials, belonging to the field of material forming. Background Technology

[0002] Silver selenide thermoelectric materials possess excellent thermoelectric conversion properties and show promising application prospects in flexible electronics, micro-energy devices, and low-grade heat recovery. As silver selenide thermoelectric devices evolve towards microscale, thin-film, and integrated designs, their practical performance and reliability are increasingly influenced by factors such as material composition, microstructure, molding quality, and interface state. Traditional silver selenide thermoelectric materials typically involve multiple independent processing steps during fabrication and subsequent device integration, which not only increases process complexity but also potentially introduces problems such as material contamination, interface oxidation, and localized structural damage. This places higher demands on the high-efficiency and high-consistency fabrication of silver selenide thermoelectric materials.

[0003] The fabrication of traditional silver selenide thermoelectric materials typically involves multiple processes, including raw material powder preparation, melting or solid-state reaction, heat treatment, and subsequent shaping, for bulk materials. For microscale device applications, further processes such as thin film deposition, patterning, and integration with metal electrodes are required, making the overall process quite complex. Especially in the fabrication of microscale patterns for silver selenide thin films, traditional masking, etching, or multi-step transfer methods often require separation of material preparation and structure forming, which is detrimental to improving manufacturing efficiency. In recent years, traditional laser processing technology has been attempted to simplify the fabrication of silver selenide thermoelectric materials. However, the high instantaneous power and long pulse width of traditional lasers easily cause preferential evaporation of low-melting-boiling-point selenium, leading to severe component segregation and limiting the application of laser-based silver selenide thermoelectric materials. Summary of the Invention

[0004] The purpose of this invention is to provide a continuous induced molding process for silver selenide thermoelectric materials, so as to solve the problems of complex steps, poor material stability, and loss of Se element caused by laser processing in the existing silver selenide thermoelectric material preparation process.

[0005] This invention proposes a continuous induced forming process for silver selenide thermoelectric materials. By pre-supplementing selenium and combining the combined effects of laser average power, scanning speed, and defocus distance, a femtosecond laser continuously acts on a silver selenide thin film along a preset path, achieving localized release, continuous transfer, and direct forming of the silver selenide material on the acceptor substrate surface. This process integrates material transfer and continuous structure forming into a single process, reducing the complexity of traditional multi-step patterning processes. Furthermore, the laser processing parameters synergistically improve the stability of continuous forming of silver selenide materials, providing a new process path for the digital and continuous preparation of silver selenide thermoelectric materials.

[0006] To achieve the above objectives, the present invention provides the following technical solution:

[0007] Step 1: Based on the target composition of silver selenide and the selenium loss, the Se element is pre-supplemented in the magnetron sputtering target used to prepare the silver selenide thin film, and the target is used to prepare the silver selenide thin film on the surface of the transparent substrate to form a silver selenide thin film / transparent substrate structure.

[0008] Step 2: Perform surface cleaning pretreatment on the receptor substrate, and set the silver selenide film and its transparent substrate opposite to the receptor substrate, so that the silver selenide film faces the receptor substrate, and control the silver selenide film and the receptor substrate to maintain a preset distance.

[0009] Step 3: Set the amplifier frequency parameters of the femtosecond pulse laser so that the femtosecond pulse laser passes through the transparent substrate and acts on the silver selenide film, and performs continuous scanning according to the preset forming path;

[0010] Step 4: By adjusting the average laser power, scanning speed and defocusing distance, the energy input per unit area and per unit region of the silver selenide film is controlled, so that the silver selenide film in the laser irradiation area undergoes local melting and release, and is continuously transferred towards the acceptor substrate;

[0011] Step 5: As the femtosecond laser continuously scans along the preset path, silver selenide material is continuously deposited on the surface of the acceptor substrate and cooled and solidified to form a continuous silver selenide molding structure corresponding to the preset scanning path.

[0012] Furthermore, the silver selenide thin film is prepared using magnetron sputtering. The target material used for magnetron sputtering is based on the target stoichiometric composition of Ag₂Se, with the addition of selenium to pre-compensate for selenium loss during subsequent laser forming. Preferably, the atomic percentage of the target material is approximately Ag:Se = 63.5:36.5 at.%, and the pre-compensation amount of Se is 3.2%.

[0013] Furthermore, the total thickness of the silver selenide film is 1.5 μm.

[0014] Furthermore, the transparent substrate is one of a transparent glass substrate, a quartz glass substrate, or a fused silica substrate, preferably a JGS1 type glass substrate, and the thickness of the transparent substrate is 5 mm.

[0015] Furthermore, the pulsed laser is a femtosecond laser with a wavelength of 1056 nm and a pulse width of 300 fs.

[0016] Furthermore, the acceptor substrate is a copper substrate. Before femtosecond laser-induced continuous forming, the copper substrate undergoes grinding, polishing, and plasma cleaning. The grinding and polishing process brings the copper substrate surface to a 3000-mesh finish. The plasma cleaning uses a mixture of argon and hydrogen as the working gas. Preferably, the mixture consists of 95% argon and 5% hydrogen by volume, with a gas flow rate of 1.5 L / min and a plasma power of 3.4 W.

[0017] Furthermore, the amplifier frequency parameters of the femtosecond laser were set to 500:2 kHz.

[0018] Furthermore, in the femtosecond laser-induced continuous forming process, the average laser power is 6.0 W to 7.2 W, preferably 6.8 W; the defocus distance is -0.5 mm to -0.1 mm, preferably -0.25 mm; and the processing speed is 2000 mm / s to 3000 mm / s, preferably 2400 mm / s.

[0019] With other laser parameters kept constant, by coordinating the control of average laser power, scanning speed and defocusing distance, silver selenide films can be kept in a suitable continuous transfer state, reducing incomplete transfer and forming interruption caused by insufficient laser energy input, as well as problems such as material scattering, excessive ablation and irregular forming caused by excessive energy input.

[0020] Furthermore, the distance between the silver selenide film and the acceptor substrate is controlled by a micron-level precision electronically controlled displacement platform or a micron-level feeler gauge, with a preset distance of 20 μm.

[0021] Compared with the prior art, the present invention has the following significant advantages:

[0022] (1) The present invention provides a continuous induced molding process for silver selenide thermoelectric materials. By continuously scanning the silver selenide film along a preset path with a femtosecond laser, the material release, transfer and molding are completed in the same process. There is no need to re-prepare physical masks for different molding paths. Customized continuous molding of silver selenide can be achieved by controlling the laser scanning trajectory.

[0023] (2) This invention provides a continuous induced molding process for silver selenide thermoelectric materials. Before preparing silver selenide thin films by magnetron sputtering, the Se content in the target material is pre-compensated so that the silver selenide film has a certain Se enrichment, reducing the degree of material composition deviation after continuous molding, effectively ensuring the final silver selenide composition, and solving the composition deviation caused by instantaneous high heat of laser.

[0024] (3) This invention provides a continuous induced molding process for silver selenide thermoelectric materials. By coordinating the average laser power, scanning speed and defocusing distance, the energy input per unit area of ​​silver selenide film is controlled, and a continuous molding process window is established, thereby improving problems such as discontinuous molding, material scattering and irregular contours, and improving the stability of continuous molding of silver selenide.

[0025] The present invention will now be described in further detail with reference to the accompanying drawings. Attached Figure Description

[0026] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments and descriptions of this application are used to explain this application and do not constitute an undue limitation of this application. In the drawings:

[0027] Figure 1 This is a characterization diagram of single-point induced transfer of silver selenide under the amplifier frequency parameters of 500:2 kHz in Example 1;

[0028] Figure 2 The image shows the single-point induced transfer characterization of silver selenide under the condition that the amplifier frequency is 1000 kHz in Comparative Example 1.

[0029] Figure 3 The image shows the single-point induced transfer characterization of silver selenide under the amplifier frequency parameters of 333:3 kHz in Comparative Example 2.

[0030] Figure 4 The image shows the single-point induced transfer characterization of silver selenide under the amplifier frequency parameters of 250:4 kHz in Comparative Example 3.

[0031] Figure 5 The image shows the single-point induced transfer characterization of silver selenide under the amplifier frequency parameters of 200:5 kHz in Comparative Example 4.

[0032] Figure 6 This is a characterization diagram of continuous induced molding of silver selenide under the preferred process parameters in Example 2;

[0033] Figure 7 The image shows the characterization of continuous induced molding of silver selenide under the condition of an average laser power of 6.0 W in Example 3.

[0034] Figure 8 The image shows the characterization of continuous induced molding of silver selenide under the condition of an average laser power of 7.2 W in Example 4.

[0035] Figure 9 The image shows the characterization of continuous induced molding of silver selenide under the condition that the average laser power is less than 6.0 W in Comparative Example 5.

[0036] Figure 10The image shows the characterization of continuous induced molding of silver selenide under the condition that the average laser power is higher than 7.2 W in Comparative Example 6.

[0037] Figure 11 The image shows the characterization of continuous induced molding of silver selenide under the condition of a defocus distance of -0.5 mm in Example 5.

[0038] Figure 12 The image shows the characterization of continuous induced molding of silver selenide under the condition of a defocus distance of -0.1 mm in Example 6.

[0039] Figure 13 The image shows the characterization of continuous induced molding of silver selenide under the condition that the defocus distance is less than -0.5 mm in Comparative Example 7.

[0040] Figure 14 The image shows the characterization of continuous induced molding of silver selenide under the condition that the defocus distance is greater than -0.1 mm in Comparative Example 8.

[0041] Figure 15 This is a characterization diagram of continuous induced molding of silver selenide under a processing speed of 2000 mm / s in Example 7;

[0042] Figure 16 This is a characterization diagram of continuous induced molding of silver selenide under a processing speed of 3000 mm / s in Example 8;

[0043] Figure 17 This is a characterization diagram of continuous induced molding of silver selenide under processing speeds below 2000 mm / s in Comparative Example 9;

[0044] Figure 18 The image shows the characterization of continuous induced molding of silver selenide under processing speeds higher than 3000 mm / s in Comparative Example 10. Detailed Implementation

[0045] The present invention will be further described below with reference to specific embodiments and comparative examples. It should be noted that the following embodiments are only for explaining the present invention and are not intended to limit the scope of protection of the present invention. Equivalent substitutions or adjustments made by those skilled in the art to the relevant process parameters without departing from the concept of the present invention should be included within the scope of protection of the present invention.

[0046] Example 1: Single-point induced transfer molding of silver selenide under amplifier frequency parameters of 500:2 kHz

[0047] This embodiment illustrates the influence of different amplifier frequency parameters on the laser-induced transfer behavior of silver selenide thin films and determines the preferred amplifier frequency parameters for subsequent continuous induction molding. A femtosecond laser with a wavelength of 1056 nm and a pulse width of 300 fs was used in the experiment. The average laser power was set to 6.8 W, the defocus distance was set to -0.25 mm, and other basic processing conditions remained consistent. In this embodiment, the amplifier frequency parameter was set to 500:2 kHz. The laser pulses were output at a pulse cluster repetition frequency of 500 kHz, with each pulse cluster containing two consecutive pulses. This allowed two adjacent pulses to act continuously on the same area within a short time, thereby enhancing the accumulation of local transient energy. Figure 1 It can be seen that a relatively large main deposition area forms at the center of the transfer region, with the material mainly concentrated near the laser action center, surrounded by a small number of fine particles and molten debris distributed in a ring. Compared with the simple surface ablation morphology, there is obvious main material transfer under this condition, indicating that the 500:2 kHz condition can transform the silver selenide film from a state of gradual material removal to a state of more obvious melt release and overall transfer. After the first pulse, rapid energy deposition occurs in local areas of the silver selenide film, leading to a state of heating, softening, or local melting. Subsequently, the second pulse continues to act on the already excited and heated material area, further accumulating local energy and promoting the formation of molten material and its release from the donor substrate surface. At the same time, there is a relatively long time interval between adjacent pulse clusters, allowing local material to undergo a certain degree of heat dissipation and state relaxation, thereby reducing excessive ablation and disordered scattering caused by continuous high-intensity energy accumulation. Therefore, the 500:2 kHz condition achieves a suitable balance between the transient energy accumulation required for material melting and release and excessive ablation. The continuous action within the cluster of two pulses can effectively promote the local melting and release of the silver selenide film, while avoiding excessive material scattering caused by excessive energy accumulation within the pulse cluster. Considering the integrity of the main deposition, the degree of transfer concentration, and the surrounding scattering, this invention selects 500:2 kHz as the preferred amplifier frequency parameter for subsequent continuous induced molding of silver selenide.

[0048] Comparative Example 1: Single-point induced transfer molding of silver selenide under amplifier frequency parameters of 1000 kHz

[0049] This comparative example illustrates the laser-induced transfer behavior of silver selenide thin films at an amplifier frequency of 1000 kHz. The experiment used a femtosecond laser with a wavelength of 1056 nm and a pulse width of 300 fs. The average laser power was set to 6.8 W, and the defocus distance was set to -0.25 mm. All other basic processing conditions remained consistent. In this comparative example, the amplifier frequency was set to 1000 kHz, meaning the laser pulses were continuously output at a relatively high repetition rate.

[0050] Depend on Figure 2 It can be seen that at 1000 kHz, only a few scattered droplet-like deposits appeared on the surface of the copper acceptor substrate. At the corresponding laser-induced locations, noticeable localized ablation pits were observed, without the formation of the larger and more concentrated bulk transfer structures seen at 500:2 kHz. This indicates that while this frequency can induce localized material removal from the silver selenide film, the amount of material effectively transferred to the acceptor substrate surface is small, and the overall process is primarily gradual ablation. With a consistent average laser power, the 1000 kHz output mode allows the laser energy to continuously act on the silver selenide film at a higher frequency and more uniform time intervals. The pulses are distributed more evenly over time, lacking the short-term continuous energy accumulation within pulse clusters. Therefore, the material is more prone to gradual ablation, making it difficult to form a concentrated release of large volumes of molten material. Thus, the silver selenide film mainly exhibits localized ablation, with only a small amount of molten material detaching from the donor substrate and transferring to the copper acceptor surface, ultimately forming scattered droplets. Compared to the 500:2 kHz condition where two pulses act consecutively within a short period and create significant local energy accumulation, the material release process at 1000 kHz is more gradual, making it difficult to effectively form a concentrated mass transfer. Therefore, although 1000 kHz can induce localized ablation and a small amount of material transfer in the silver selenide film, the amount of transfer and the degree of deposition concentration are significantly insufficient, making it unsuitable as the preferred amplifier frequency parameter for subsequent continuous induced molding of silver selenide.

[0051] Comparative Example 2: Silver selenide single-point induced transfer molding under amplifier frequency parameters of 333:3 kHz

[0052] This comparative example illustrates the laser-induced transfer behavior of silver selenide thin films when the amplifier frequency parameters are 333:3 kHz. The basic processing conditions are the same as in Example 1, except that the amplifier frequency parameters are adjusted to 333:3 kHz.

[0053] Depend on Figure 3 It can be seen that, under the condition of 333:3 kHz, although obvious material transfer traces can still be observed on the surface of the acceptor substrate, relatively obvious ablation characteristics are observed in each interaction area. An irregular deposition structure forms in the center of the transfer area, accompanied by obvious annular ablation areas and a large number of fine particles scattered around it. The main deposit in some locations has been broken or missing, making it difficult to maintain a nearly spherical droplet morphology similar to that under the condition of 500:2 kHz. This indicates that although the material can melt and release under this frequency condition, the transfer process is strongly disturbed by ablation, and the integrity and deposition concentration of the main material are significantly reduced.

[0054] Compared to the 500:2 kHz condition, the 333:3 kHz parameter increases the number of consecutive pulses within each pulse cluster, further enhancing the energy accumulation effect over a short period. After the preceding pulse heats and locally melts the silver selenide film, subsequent pulses continue to act on areas already at high temperatures or in a molten state. This may cause the local energy input to exceed the range required for stable material release, thereby enhancing material ablation, scattering, and disturbance in the molten zone. The obvious ablation pits and fragmented, irregular deposition morphology observed at multiple sites in the figure indicate that this condition is insufficient to maintain relatively intact droplet-shaped material transfer.

[0055] Therefore, while 333:3 kHz can promote material release and transfer in silver selenide films, the strong energy accumulation within the pulse cluster easily leads to significant ablation and material scattering, making it difficult for the transferred structure to maintain a complete and concentrated droplet morphology. Its transfer stability is lower than that under the 500:2 kHz condition. Therefore, 333:3 kHz is not a preferred amplifier frequency parameter for subsequent continuous induced molding of silver selenide.

[0056] Comparative Example 3: Silver selenide single-point induced transfer molding under amplifier frequency parameters of 250:4 kHz

[0057] This comparative example illustrates the laser-induced transfer behavior of silver selenide thin films when the amplifier frequency parameter is 250:4 kHz. The basic processing conditions are the same as in Example 1, except that the amplifier frequency parameter is adjusted to 250:4 kHz.

[0058] Depend on Figure 4 It can be seen that, under the condition of 250:4 kHz, obvious material transfer traces can still be observed on the surface of the acceptor substrate, but the main deposition area in the center of the transfer region is further reduced, and the droplets are unable to form a relatively complete and fully spread main structure similar to that under the condition of 500:2 kHz. At the same time, a more obvious particulate dispersion area appears around the laser-acted area, with a large number of small, high-contrast droplets and broken particles distributed around the main deposition area, indicating that the concentration of the transferred material is further reduced.

[0059] Compared to the 333:3 kHz condition, the number of consecutive pulses within each pulse cluster increases to four under the 250:4 kHz parameter, resulting in a stronger cumulative laser effect on the silver selenide film within a shorter time. After the preceding pulse heats, softens, or melts the local material, subsequent pulses continue to act on the already high-temperature material region, potentially further enhancing the disturbance in the molten zone and the intensity of material release. When the accumulated local energy exceeds the range required for stable droplet transfer, some molten material no longer transfers in the form of a relatively intact main droplet, but is more prone to breakage and scattering, leading to a reduction in the central main deposition area and a significant increase in the number of surrounding fine droplets and broken particles.

[0060] Therefore, although silver selenide material release and transfer can be achieved at 250:4 kHz, the accumulation effect within the pulse cluster is further enhanced, causing the transferred material to gradually transform from a relatively concentrated bulk deposition to dispersed droplets and broken particles. This is manifested in a decrease in the spreading area of ​​the main droplets, an expansion of the peripheral scattering area, and an increase in the number of fine particles. This indicates that the material transfer stability and deposition concentration further decrease under this frequency condition. Therefore, 250:4 kHz is not suitable as the preferred amplifier frequency parameter for subsequent continuous induced molding of silver selenide.

[0061] Comparative Example 4: Silver selenide single-point induced transfer molding under amplifier frequency parameters of 200:5 kHz

[0062] This comparative example illustrates the laser-induced transfer behavior of silver selenide thin films when the amplifier frequency parameter is 200:5 kHz. The basic processing conditions are the same as in Example 1, except that the amplifier frequency parameter is adjusted to 200:5 kHz.

[0063] Depend on Figure 5 It can be seen that under the 200:5 kHz condition, the laser-affected sites on the acceptor substrate surface mainly exhibit relatively obvious annular transfer traces, with scattered small droplets and particles observed on the periphery. The central region, however, lacks a complete host deposition structure, and some areas even show significant material deficiencies. Compared to the formation of larger, more complete host droplets under the 500:2 kHz condition, the concentration of transferred material is significantly reduced under the 200:5 kHz condition, making it difficult to form a stable and complete host deposition.

[0064] As the amplifier frequency parameters were further adjusted to 200:5 kHz, the number of consecutive pulses within each pulse cluster increased to five. After the preceding pulse locally heated and melted the silver selenide film, subsequent pulses continued to act on the already high-temperature or even molten area, further enhancing the local energy accumulation in a short period. During this process, the molten material was subjected to stronger disturbance and release, making it prone to breakage, scattering, or localized material removal. This caused a large amount of material that should have formed the main droplets to disperse to the periphery of the action area, ultimately resulting in a lack of material in the central region, while only a small number of ring-shaped fine droplets and scattered particles remained around it.

[0065] Therefore, although the 200:5 kHz condition can still induce material release from the silver selenide film, the energy accumulation within the pulse cluster is too strong, and the material transfer process has significantly deviated from the stable overall droplet transfer state. The integrity of the main deposition and the degree of material concentration are significantly lower than under the 500:2 kHz condition, making it unsuitable as an amplifier frequency parameter for subsequent continuous silver selenide-induced molding.

[0066] Example 2: Continuous Induction Molding of Silver Selenide Thermoelectric Material under Optimal Process Parameters

[0067] This embodiment illustrates that the present invention can stably form a continuous silver selenide structure under preferred process parameters.

[0068] JGS1 transparent glass with a thickness of 5 mm was selected as the transparent substrate. After cleaning, a silver selenide film with a thickness of 1.5 μm and an atomic percentage of approximately Ag:Se = 63.5:36.5 at.% was prepared on one side to pre-compensate for the loss of Se volatilization during laser processing.

[0069] A copper substrate was selected as the acceptor substrate. Before processing, the surface of the copper substrate was polished to a surface finish of 3000 mesh. Subsequently, a plasma cleaner was used to clean the surface of the copper substrate. The working gas was a mixture of 95% argon and 5% hydrogen by volume, with a gas flow rate of 1.5 L / min and a plasma power of 3.4 W.

[0070] The thin film and its transparent substrate are positioned opposite to the copper substrate, with the thin film facing the copper substrate, and the preset distance between the thin film and the copper substrate is controlled to be 20 μm.

[0071] Continuous induced forming was performed using a femtosecond laser with a wavelength of 1056 nm and a pulse width of 300 fs. During the processing, the average laser power was 6.8 W, the defocus distance was -0.25 mm, the processing speed was 2400 mm / s, and the amplifier frequency parameters were set to 500:2 kHz.

[0072] Depend on Figure 6 As can be seen, the resulting molded structure exhibits good continuity along the scanning direction, with the main deposited structure continuously distributed without large-scale breaks or obvious periodic gaps. The silver selenide material is mainly concentrated in the preset scanning trajectory region, indicating that the process parameters can meet the energy requirements for continuous release and transfer of the silver selenide film. Simultaneously, a small amount of molten material accumulation and dispersed particles can be observed on both sides of the molded structure, but this does not affect the main continuous structure, and the overall continuous molding state is maintained well. Further EDS elemental scanning and quantitative analysis of the obtained silver selenide continuous molding region revealed that both Ag and Se elements are distributed within the continuous molding region. Point scanning results show that the atomic percentages of Ag and Se within the molding region are close to the theoretical stoichiometric composition of Ag₂Se, i.e., the Ag:Se atomic ratio is close to 2:1. These results indicate that under the preferred continuous molding parameters used in this embodiment, after femtosecond laser treatment and material transfer, the elemental composition of the resulting continuous molding structure can maintain a composition close to the target Ag₂Se.

[0073] Example 3: Silver selenide forming at an average laser power of 6.0 W

[0074] This embodiment illustrates the molding process when the average laser power is at the lower limit of the range defined in this invention. The difference between this embodiment and Embodiment 2 is that the average laser power is adjusted to 6.0 W, while the other process conditions are the same as in Embodiment 2.

[0075] Under these conditions, the silver selenide film can still undergo localized melting and release under continuous femtosecond laser scanning, and transfer along the scanning direction to the acceptor surface, forming a continuous silver selenide structure. Figure 7 It can be seen that the obtained structure remains continuous along the laser scanning direction, and no large-scale fractures occur in the main deposition area, indicating that the average laser power of 6.0 W can still meet the requirements for continuous release and transfer of silver selenide film. Compared with 6.8 W, the overall width of the continuous structure formed under the 6.0 W condition is reduced, the amount of material deposited is relatively reduced, and the morphology of the main area is more concentrated. However, there are still some undulations and contractions on both sides of the structure, and a small number of attached droplets and dispersed particles can be observed. However, the silver selenide film can still maintain continuous transfer, but the reduced input energy per unit time leads to a relative decrease in the amount of locally molten material formed and transferred. Therefore, this power can be used as the lower limit condition for the stable continuous forming range of this invention. EDS elemental analysis of the obtained continuous forming area shows that Se is slightly enriched relative to the theoretical composition of Ag2Se. The atomic ratio of Ag to Se is about 1.9, which is close to the atomic ratio of Ag2Se, but Se element is slightly relatively enriched. This result is consistent with the lower laser energy input at 6.0 W, suggesting that the loss of Se element during laser continuous forming may be relatively reduced at lower power, allowing the pre-compensated portion of Se element to be retained. Therefore, 6.0 W can be used as the lower power limit for the continuous forming process of this invention.

[0076] Example 4: Molding process when the average laser power is 7.2 W

[0077] This embodiment illustrates the molding process when the average laser power is at the upper limit of the range defined in this invention. The difference between this embodiment and Embodiment 2 is that the average laser power is adjusted to 7.2 W, while the remaining process conditions are the same as in Embodiment 2.

[0078] Under these conditions, the silver selenide film can still undergo localized melting and release under continuous femtosecond laser scanning, and continuously transfer along the scanning direction to the surface of the copper acceptor substrate, forming a continuous silver selenide structure. Figure 8It can be seen that the obtained structure still maintains good continuity along the laser scanning direction, and no large-scale fractures occur in the main deposition area, indicating that the average laser power of 7.2 W can still meet the requirements for continuous transfer molding of silver selenide material. Compared with the 6.8 W power condition, the width of the molding area increases under the 7.2 W condition, and the material spreading and edge undulations are more obvious. Larger holes, depressions, and irregular edges can be observed in some areas, and there are more granular and strip-shaped scattered materials distributed around the molded structure. The above morphology indicates that as the average laser power is further increased, the energy input to the silver selenide film per unit time increases, the amount of locally molten material formed and the disturbance are enhanced, making the material exhibit a more obvious tendency to spread laterally and scatter during continuous transfer. Although the main structure can still maintain continuity, its edge regularity and material distribution uniformity are lower than under the 6.8 W condition. Therefore, 7.2 W can be used as the upper limit condition of the stable continuous molding power range of this invention. EDS elemental analysis of the obtained continuously formed region showed that the atomic percentages of Ag and Se in the region were still close to the theoretical stoichiometric composition of Ag₂Se, but compared with the theoretical value, there was a slight relative enrichment of Ag and a relative deficiency of Se, with the Ag to Se atomic ratio ≈ 2.15. This indicates that with the increase of the average laser power, the loss of Se element during the continuous forming process increases.

[0079] Comparative Example 5: Molding conditions with average laser power below 6.0 W

[0080] This comparative example illustrates the adverse effects on the molding effect when the average laser power is below the range defined in this invention. The difference between this comparative example and Example 2 is that the average laser power is adjusted to 5.5 W, while the remaining process conditions are the same as in Example 2.

[0081] Under these conditions, silver selenide films can still undergo localized material release and transfer after femtosecond laser irradiation, but the transfer process is difficult to continue along the laser scanning direction. For example... Figure 9 As shown, only a few separate or partially connected strip-shaped deposition structures are formed on the surface of the copper substrate, with obvious discontinuities along the scanning direction. In some areas, no effective deposition is even formed, making it impossible to obtain a complete and continuous silver selenide molding structure. Compared to the 6.0 W condition, the laser energy input to the silver selenide film per unit time is further reduced under the 5.5 W condition. The energy obtained in some areas is insufficient to maintain the continuous melting, release, and transfer of the silver selenide film, making it impossible to continuously connect the deposition areas formed at adjacent scanning positions. Although a certain amount of transferred material and a small amount of particulate matter can still be observed in some local locations, these local transfers are insufficient to form a stable and continuous linear structure. Therefore, 5.5 W is not within the scope of the stable and continuous molding process defined in this invention.

[0082] Comparative Example 6: Molding results when the average laser power is higher than 7.2 W

[0083] This comparative example illustrates the adverse effects on the molding effect when the average laser power exceeds the range defined in this invention. The difference between this comparative example and Example 2 is that the average laser power is adjusted to 7.8 W, while the remaining process conditions are the same as in Example 2.

[0084] Under these conditions, the energy input to the laser-treated area increased significantly, and the silver selenide material failed to maintain a stable and continuous transfer and deposition state, exhibiting obvious over-melting and ablation phenomena. For example... Figure 10 As shown, areas where a continuous silver selenide structure should have formed exhibited significant material loss and ablation grooves. In some areas, a large amount of silver selenide material was removed, making it impossible to form a complete, continuous, and stable structure. Obvious periodic laser action marks and extensive surface damage were observed within the processed area, indicating that the laser energy significantly exceeded the suitable range required for stable and continuous forming of silver selenide material. After some silver selenide material was excessively ablated and removed, the laser energy continued to act on the underlying copper acceptor substrate, causing significant ablation and damage to the copper substrate surface as well. Therefore, when the average laser power exceeds 7.2 W, excessively high energy input significantly disrupts the continuous transfer and deposition process of silver selenide material, resulting in material loss and severe ablation in the formed area.

[0085] Example 5: Forming results at a defocus distance of -0.50 mm

[0086] This embodiment illustrates the forming process when the defocus distance is within one boundary of the range defined by this invention. The difference between this embodiment and Embodiment 2 is that the defocus distance is adjusted to -0.50 mm, while the remaining process conditions are the same as in Embodiment 2.

[0087] Under these conditions, the silver selenide film can still undergo localized melting and release under continuous femtosecond laser scanning, and continuously transfer towards the surface of the copper acceptor substrate along the scanning direction, forming a continuous silver selenide structure. Figure 11It can be seen that the obtained structure remains continuous along the laser scanning direction, with the main deposition area being relatively concentrated and no obvious large-scale fractures appearing. Compared with the preferred defocusing condition of -0.25 mm, the overall width of the continuous structure formed under the -0.5 mm condition is reduced, and the edge undulation and material scattering are relatively decreased. Only slight necking and a small amount of edge accumulation can be observed in local areas, indicating that this defocusing condition can still meet the basic requirements for continuous transfer and forming of silver selenide materials. Further EDS elemental analysis of the formed area obtained under the -0.5 mm condition shows that the relative content of Se element is slightly increased compared with the preferred condition of -0.25 mm, that is, the percentage content of Se atoms is slightly higher, and the Ag:Se atomic ratio is ≈1.93, showing slight Se enrichment. Under the larger negative defocusing condition, due to the reduced energy input per unit area, the amount of molten material formed and the degree of lateral spreading are reduced. Therefore, the continuous formed structure shows a smaller linewidth compared with the -0.25 mm condition. Therefore, stable continuous molding of silver selenide material can still be achieved when the defocus distance is -0.5 mm, but the amount of material transferred and the width of the continuous structure are reduced compared with the preferred condition of -0.25 mm.

[0088] Example 6: Forming results at a defocus distance of -0.1 mm

[0089] This embodiment illustrates the forming process when the defocus distance is at the boundary of the range defined by this invention. The difference between this embodiment and Embodiment 2 is that the defocus distance is adjusted to -0.1 mm, while the other process conditions are the same as in Embodiment 2.

[0090] The silver selenide film can still undergo localized melting and release under continuous femtosecond laser scanning, and continuously transfer towards the surface of the copper acceptor substrate along the scanning direction, forming a continuous silver selenide structure. Figure 12 It can be seen that the obtained structure remains continuous along the laser scanning direction without large-scale line breaks, indicating that the -0.1 mm defocus condition can still meet the basic requirements for continuous transfer and forming of silver selenide materials. However, compared with the preferred -0.25 mm defocus condition, the surface and edges of the formed structure are significantly more irregular, with more holes, depressions, and molten material protrusions in local areas. Simultaneously, many spherical and strip-shaped dispersed particles can be observed around the formed structure, indicating that the melting disturbance and scattering effects on the material during continuous transfer are enhanced. EDS elemental analysis of the continuously formed region shows that Ag and Se elements deviate slightly from the theoretical Ag:Se = 2:1, i.e., Ag is relatively enriched and Se is relatively deficient, with an Ag to Se atomic ratio ≈ 2.1. This result indicates that under the -0.1 mm defocus condition, the loss of Se element during laser continuous forming is increased compared to the preferred defocus condition, meaning that the pre-compensated Se element cannot completely offset the Se loss caused by laser processing.

[0091] Comparative Example 7: Forming results when the defocus distance is less than -0.50 mm

[0092] This comparative example illustrates the adverse effects on the molding effect when the defocus distance is less than the range defined in this invention. The difference between this comparative example and Example 2 is that the defocus distance is adjusted to -0.6 mm, while the other process conditions are the same as in Example 2.

[0093] Under these conditions, silver selenide films can still undergo localized melting, release, and material transfer after being irradiated by a femtosecond laser, but they cannot form a stable and continuous shaped structure along the scanning direction. For example... Figure 13 As shown, the transferred material on the copper acceptor substrate surface is mainly distributed as separate droplets. Some adjacent droplets are only locally connected through a narrow neck, resulting in significant large-scale discontinuities along the laser scanning direction, failing to form a complete and continuous silver selenide linear structure. Compared to the -0.5 mm defocus condition, when the defocus distance is further adjusted to -0.6 mm, the laser spot acting on the silver selenide film surface further increases, and the energy input per unit area decreases. At this point, although the local laser energy can still melt and transfer some of the silver selenide film, it is insufficient to maintain a continuous material release process in adjacent scanning areas. The transferred molten material tends to shrink under the action of surface tension and form independent droplets, gradually transforming the originally continuously distributed material along the scanning direction into intermittent droplets.

[0094] Comparative Example 8: Forming results when the defocus distance is greater than -0.1 mm

[0095] This comparative example illustrates the adverse effects on the molding effect when the defocus distance exceeds the range defined in this invention. The difference between this comparative example and Example 2 is that the defocus distance is adjusted to 0 mm, i.e., in a near-focus state, while the other process conditions are the same as in Example 2.

[0096] Under these conditions, the silver selenide film failed to form a continuous and stable structure along the scanning direction after being subjected to a femtosecond laser. For example... Figure 14As shown, the transferred material on the copper acceptor substrate surface mainly exhibits a localized granular deposition structure distributed along the laser scanning trajectory, with significant gaps between adjacent deposition areas, failing to form a continuous silver selenide structure. Simultaneously, obvious laser action trajectories can be observed near the locations of each deposition structure, indicating that the material transfer process under these conditions has significantly deviated from a stable, continuous forming state. Compared to the -0.1 mm and -0.25 mm defocusing conditions, when the defocusing distance is further adjusted to 0 mm, the laser beam approaches the focal point, further reducing the spot size acting on the silver selenide film surface and significantly increasing the local energy input per unit area. This excessively high local energy density makes the silver selenide film more susceptible to severe ablation and release, making it difficult for the material to form a stable, continuous transfer and connection between adjacent scanning positions. Instead, it tends to transfer to the acceptor substrate surface in a localized, concentrated release manner, ultimately forming discrete deposition structures that are separated from each other.

[0097] Example 7: Forming at a processing speed of 2000 mm / s

[0098] This embodiment illustrates the forming process when the processing speed is close to the lower limit of the range defined in this invention. The difference between this embodiment and Embodiment 2 is that the laser processing speed is adjusted to 2000 mm / s, while the other process conditions are the same as in Embodiment 2.

[0099] Under these conditions, the silver selenide film can still undergo localized melting and release under continuous femtosecond laser scanning, and continuously transfer towards the surface of the copper acceptor substrate along the scanning direction, forming a continuous silver selenide structure. Figure 15 It can be seen that the obtained structure remains continuous along the laser scanning direction, and there is no significant large-scale interruption in the main deposition area, indicating that the processing speed of 2000 mm / s can still meet the basic requirements for continuous transfer and forming of silver selenide material. Compared with the preferred processing speed of 2400 mm / s, the formed structure under the condition of 2000 mm / s is generally wider and thicker, with increased edge undulation and irregularity. More obvious pores, depressions, and molten material protrusions can be observed in local areas. At the same time, there are more spherical and irregular granular structures distributed around the continuous structure, indicating that the silver selenide material is subjected to enhanced melting disturbance during the transfer process. Although the main structure can still maintain continuity, the lateral spreading and local scattering of material are more obvious than under the preferred speed conditions. Further EDS elemental analysis of the obtained continuous forming area shows that the atomic ratio of Ag to Se is slightly higher than the theoretical stoichiometric ratio of Ag2Se 2:1, Ag:Se≈2:06, showing a certain degree of relative Se deficiency. This result indicates that the loss of Se element during the continuous forming process increases under lower scanning speed conditions.

[0100] Example 8: Forming at a processing speed of 3000 mm / s

[0101] This embodiment illustrates the forming process when the processing speed is at the upper limit of the range defined by this invention. The difference between this embodiment and Embodiment 2 is that the laser processing speed is adjusted to 3000 mm / s, while the other process conditions are the same as in Embodiment 2.

[0102] Under these conditions, the silver selenide film can still undergo localized melting and release under continuous femtosecond laser scanning, and continuously transfer towards the surface of the copper acceptor substrate along the scanning direction, forming a continuous silver selenide structure. Figure 16 It can be seen that the obtained structure remains continuous along the laser scanning direction, and no obvious large-scale fractures appear in the main deposition area, indicating that the processing speed of 3000 mm / s can still meet the basic requirements for continuous transfer and forming of silver selenide materials. Compared with the preferred processing speed of 2400 mm / s, the overall width of the continuous structure obtained under the condition of 3000 mm / s is reduced, the amount of material deposited is relatively reduced, and the distribution in the main area is more concentrated, but a small number of pores, edge protrusions, and granular structures can still be observed locally. EDS elemental analysis of the obtained continuous forming area shows that the atomic ratio of Ag to Se is still close to the theoretical stoichiometry of Ag₂Se 2:1, but slightly less than 2:1 compared to the theoretical ratio, showing a slight relative enrichment of Se. This result indicates that under higher scanning speed conditions, the loss of Se element in the femtosecond laser continuous forming process is reduced, allowing more of the pre-compensated Se element to be retained.

[0103] Comparative Example 9: Forming conditions at processing speeds below 2000 mm / s

[0104] This comparative example illustrates the adverse effects on the molding effect when the processing speed is less than the lower limit of the range defined in this invention. The difference between this comparative example and Example 2 is that the processing speed is set to 1500 mm / s, while the other process conditions are the same as in Example 2.

[0105] Under these conditions, silver selenide films can still undergo localized melting, release, and material transfer after continuous femtosecond laser treatment, but it is difficult to maintain a stable and continuous forming state along the scanning direction. For example... Figure 17As shown, several relatively wide silver selenide deposition areas can be observed on the surface of the copper acceptor substrate, but there are obvious discontinuities between adjacent deposition areas, with large-scale material loss in some locations, failing to form a complete and continuous silver selenide linear structure. Simultaneously, the edges of the formed structure exhibit obvious irregular undulations, accompanied by numerous spherical and irregular granular scattering particles, and pores and material removal traces can also be observed in localized areas. Reducing the scanning speed prolongs the laser's interaction time on a unit length of silver selenide film, significantly increasing the cumulative laser energy received per unit length area. When the processing speed is below 2000 mm / s, the excessively high cumulative energy input further enhances the local melting and release of the silver selenide film, making the material more prone to violent spreading, scattering, and localized ablation during transfer. This results in a large amount of material release or removal in some areas, while a stable and uniform material supply cannot be maintained between adjacent areas, ultimately interrupting the continuous deposition process.

[0106] Comparative Example 10: Forming conditions at processing speeds above 3000 mm / s

[0107] This comparative example illustrates the adverse effects on the molding effect when the processing speed exceeds the upper limit of the range defined in this invention. The difference between this comparative example and Example 2 is that the processing speed is set to 3500 mm / s, while the other process conditions are the same as in Example 2.

[0108] Under these conditions, silver selenide films can still undergo localized melting, release, and material transfer after being irradiated by a femtosecond laser, but it is difficult to maintain a stable and continuous forming state along the scanning direction. For example... Figure 18 As shown, the transferred material on the copper acceptor substrate surface is mainly distributed in discontinuous blocky or segmental shapes, with obvious gaps between adjacent deposition areas. Some areas only form local deposition structures that are close to each other but not completely connected, making it impossible to obtain a complete and continuous silver selenide linear structure. Compared with the 3000 mm / s condition, when the processing speed is further increased, the effective interaction time of the laser on the silver selenide film per unit length is shortened, and the cumulative number of pulses and average energy input per unit length area are further reduced. At this time, although the local laser energy can still melt and release part of the silver selenide film, the amount of material transferred is insufficient to form a continuous connection between adjacent scanning positions. The molten material after transfer is more likely to shrink into mutually separated local deposition units under the action of surface tension, thus causing the originally continuous linear structure to gradually transform into a discontinuous structure. In the figure, each deposition unit is still arranged along the laser scanning direction, indicating that the laser-induced transfer process has not completely stopped, but its continuity has decreased significantly. This shows that when the processing speed is too high, the main factor limiting continuous forming is not that the material cannot be transferred at all, but that the effective energy input and the amount of material transferred per unit length area are insufficient, resulting in an unstable connection between adjacent deposition areas.

Claims

1. A continuous induced molding process for silver selenide thermoelectric materials, characterized in that, Including specific steps: Step 1: Based on the target composition of silver selenide and the selenium loss, the Se element is pre-supplemented in the magnetron sputtering target used to prepare the silver selenide thin film, and the target is used to prepare the silver selenide thin film on the cleaned transparent substrate to form a silver selenide thin film / transparent substrate structure. Step 2: Perform surface pretreatment on the acceptor substrate by grinding, polishing and plasma cleaning. Set the silver selenide film and its transparent substrate opposite to the acceptor substrate, so that the silver selenide film faces the acceptor substrate, and control the silver selenide film and the acceptor substrate to maintain a preset distance. Step 3: Set the amplifier frequency parameters of the femtosecond pulse laser so that the femtosecond pulse laser passes through the transparent substrate and acts on the silver selenide film, and continuously scans according to the preset forming path; Step 4: By adjusting the average laser power, scanning speed, and defocusing distance, the silver selenide film in the laser-acting area is locally melted and released, and continuously transferred towards the acceptor substrate under laser induction. Step 5: As the laser scans continuously, silver selenide material is continuously deposited on the surface of the acceptor substrate and cooled and solidified to form a continuous silver selenide molding structure corresponding to the preset scanning path.

2. The continuous induced molding process for silver selenide thermoelectric materials according to claim 1, characterized in that, The magnetron sputtering target is based on Ag2Se and Se element is added. The pre-compensation amount of Se element is 3.2%, that is, Ag:Se≈63.5:36.5 at.%.

3. The continuous induced molding process for silver selenide thermoelectric materials according to claim 1, characterized in that, The total thickness of the silver selenide film is 1.5 μm.

4. The continuous induced molding process for silver selenide thermoelectric materials according to claim 1, characterized in that, The transparent substrate is one of a transparent glass substrate, a quartz glass substrate, or a fused silica substrate, preferably a JGS1 type glass substrate, and the thickness of the transparent substrate is 5 mm.

5. The continuous induced molding process for silver selenide thermoelectric materials according to claim 1, characterized in that, The pulsed laser is a femtosecond laser with a wavelength of 1056 nm and a pulse width of 300 fs.

6. The continuous induced molding process for silver selenide thermoelectric materials according to claim 1, characterized in that, The acceptor substrate is a copper substrate. Before pulsed laser-induced continuous molding, the acceptor substrate is subjected to polishing and plasma cleaning. The polishing process brings the surface of the acceptor substrate to a mesh size of 3000. The plasma cleaning process uses a mixture of argon and hydrogen as the working gas. Preferably, the mixture consists of 95% argon and 5% hydrogen by volume, with a gas flow rate of 1.5 L / min and a plasma power of 3.4 W.

7. The continuous induced molding process for silver selenide thermoelectric materials according to claim 1, characterized in that, The amplifier frequency parameters of the femtosecond laser used are 500:2 kHz.

8. The continuous induced molding process for silver selenide thermoelectric materials according to claim 1, characterized in that, During the pulsed laser-induced forming process, the average laser power is 6.0 W to 7.2 W, preferably 6.8 W; the defocus distance is -0.5 mm to -0.1 mm, preferably -0.25 mm; and the processing speed is 2000-3000 mm / s, preferably 2400 mm / s.

9. The continuous induced molding process for silver selenide thermoelectric materials according to claim 1, characterized in that, The preset distance between the thin film and the receptor substrate is achieved by a micrometer-level precision electronically controlled displacement platform or a micrometer-level feeler gauge, and the preset distance is 20 μm.