A method and product for treating valve surfaces with an environmentally friendly, corrosion-resistant zirconium-based chemical conversion film.

By using the synergistic effect of components such as fluorozirconic acid on the valve surface, the problems of uneven film formation and environmental pollution of zirconium-based chemical conversion films on the valve surface are solved, realizing efficient and environmentally friendly zirconium-based conversion film treatment, and improving the corrosion resistance and film adhesion of the valve.

CN123108544APending Publication Date: 2026-11-17QINGTIAN YONGTUO METAL SURFACE TREATMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611503139.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing zirconium-based chemical conversion films lack uniformity and density when treating carbon steel/cast iron valves, and the passivation film on the stainless steel surface hinders the formation of zirconium-based conversion films, resulting in discontinuous or non-formable film layers. Traditional chemical conversion technologies also pose environmental pollution problems.

Method used

By employing the synergistic effect of fluorozirconic acid, film-forming promoters, metal complexing agents, pH buffers, and surfactants, combined with spraying or immersion processes, a uniform and dense zirconium-based chemical conversion film is formed on the valve surface, and a silane coupling agent is used for sealing treatment to improve adhesion.

Benefits of technology

It has achieved the formation of uniform and dense zirconium-based conversion films on the surfaces of various valve materials, which improves corrosion resistance, meets environmental protection requirements, reduces processing costs, and improves the adhesion between the film and organic coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention discloses an environmentally friendly and corrosion-resistant zirconium-based chemical conversion film treatment method and product for valve surfaces. The treatment solution comprises the following components at the following concentrations: fluorozirconic acid (calculated as Zr molar mass) 1.0–3.0 g / L, film-forming promoter 0.5–3.0 g / L, metal complexing agent 0.5–1.5 g / L, pH buffer 0.5–2.0 g / L, nonionic surfactant 0.1–0.3 g / L, with the balance being water. The treatment method includes: sequentially degreasing the valve workpiece, washing it with water (cast iron / carbon steel substrates require surface conditioning treatment); then placing the workpiece in the treatment solution and performing chemical conversion treatment at room temperature; finally, sequentially washing the converted workpiece with water, sealing it with a silane coupling agent, and washing and drying it with water to obtain a valve workpiece with a zirconium-based chemical conversion film on its surface. The treatment solution of this invention does not contain harmful substances such as chromium and phosphorus, making it environmentally friendly and safe. It is suitable for various valve materials such as cast iron, carbon steel, and stainless steel. The resulting conversion film is uniform and dense, with excellent corrosion resistance and strong adhesion to subsequent organic coatings. It can replace traditional phosphating and chromate passivation processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal surface treatment technology, and relates to an environmentally friendly and corrosion-resistant zirconium-based chemical conversion film treatment method and product for valve surfaces, and particularly to an environmentally friendly and corrosion-resistant zirconium-based chemical conversion film treatment solution with fluorozirconic acid as the main salt, suitable for industrial valve surface treatment and its application method. Background Technology

[0002] Ball valves are valves that use a ball as their opening and closing element. They are widely used in industries such as petroleum refining, long-distance pipelines, chemicals, papermaking, pharmaceuticals, water conservancy, power, municipal engineering, and steel, playing a crucial role in the national economy. Due to the nature of their installation and operation environments, ball valves are often exposed to corrosive environments, especially those used in the gas, petroleum, and coal chemical industries, where the transported materials typically contain corrosive gaseous and liquid media. Furthermore, metal hard-seal ball valves are generally made of carbon steel or stainless steel. Due to the inherent limitations of these materials (lower corrosion resistance or lower hardness), the ball and seat of carbon steel or stainless steel are prone to rapid wear and corrosion under harsh operating conditions. Severe corrosion can lead to leakage in-service valves, causing sudden and serious production accidents; at the very least, it can result in significant economic losses due to frequent valve replacement or repair, leading to downtime and maintenance. Therefore, implementing reasonable and effective anti-corrosion treatments for large ball valves is of paramount importance.

[0003] Chemical conversion treatment is the most commonly used, effective, and widely adopted surface treatment method in industry. Currently, traditional chemical conversion technologies mainly include chromate conversion coating technology and phosphate conversion coating technology. Among these, the coating layer of chromate conversion technology mainly contains hexavalent chromium compounds, and the conversion solution contains highly toxic and carcinogenic chromium. 6+ Phosphate production and wastewater discharge pose significant risks to the environment and human health. In 2003, the European Union issued the RoHS directive, banning the use of substances containing hexavalent chromium. Despite continuous improvements and optimizations in the phosphate conversion membrane technology, the problem of large-scale phosphate wastewater discharge during phosphate production remains unresolved, requiring expensive treatment.

[0004] Due to its economic and environmental advantages, zirconium-based chemical conversion coatings are becoming a mainstream pretreatment technology for metal surfaces, particularly in the automotive coating industry. Based on fluorozirconic acid, zirconium-based chemical conversion coatings form a nano-conversion film on a clean metal surface. This film, composed of amorphous zirconium oxide, has a dense structure, strong barrier properties, and excellent adhesion to the metal surface and subsequent organic coatings, significantly improving the corrosion resistance of the metal coating. Zirconium-based chemical conversion coatings are highly adaptable to treating zinc, iron, aluminum, and their alloys, with film thicknesses ranging from 20 to 400 nm. The amount of chemicals required for film formation is relatively low, resulting in minimal byproduct sediment. However, existing zirconization processes still suffer from insufficient film uniformity and density when treating carbon steel / cast iron valves. Uneven surface activity in carbon steel / cast iron can easily lead to "white rust" or colored interference patterns in the film. Simultaneously, the dense Cr2O3 passivation film on the surface of stainless steel valves hinders the formation of the zirconium-based conversion film, resulting in discontinuous or non-formation of the film.

[0005] To address the aforementioned issues, this invention provides an environmentally friendly and corrosion-resistant zirconium-based chemical conversion film treatment method and product suitable for valve surfaces. By introducing film-forming promoters, metal complexing agents, pH buffers, and surfactants into the treatment solution, a uniform, dense, and highly corrosion-resistant zirconium-based conversion film is formed on the surfaces of various valve materials such as cast iron, carbon steel, and stainless steel. This method can replace traditional phosphating and chromate passivation processes. Summary of the Invention

[0006] The purpose of this invention is to address the shortcomings of existing technologies by providing an environmentally friendly zirconium-based chemical conversion film treatment solution and its treatment method for valve surfaces.

[0007] In one aspect, the present invention provides an environmentally friendly and corrosion-resistant zirconium-based chemical conversion film treatment solution for valve surfaces. The method is simple, the reaction conditions are mild, the application range is wide, and it is efficient, economical, and environmentally friendly.

[0008] After degreasing, the valve is treated with a zirconium-based chemical conversion coating solution at room temperature through spraying or immersion to form a zirconium-based chemical protective film. The valve is then washed with water to remove any residual solution. To improve corrosion resistance, the valve can be sealed after zirconization treatment. Finally, it is washed with clean water and dried to obtain a valve with excellent corrosion resistance.

[0009] Preferably, the degreasing treatment uses a medium-temperature (50-60℃) alkaline degreasing agent, which is sprayed or soaked for 3-15 minutes to thoroughly remove oil and grease from the valve surface.

[0010] Preferably, valves made of cast iron / carbon steel can undergo surface conditioning treatment; a surface conditioning agent containing titanium salts or a special organic polymer is used to form uniform activation points on the clean surface, preparing it for subsequent zirconization treatment.

[0011] The zirconium-based chemical conversion membrane treatment solution comprises the following raw material components: Fluorozyric acid (calculated as Zr molar mass) 1.0–3.0 g / L; Film-forming accelerator: 0.5–3.0 g / L; Metal complexing agent 0.5–1.5 g / L; pH buffer 0.5–2.0 g / L; Nonionic surfactants: 0.1–0.3 g / L; The remainder is water.

[0012] Preferably, the film-forming promoter is a compound of nitrate and molybdate (such as NaNO3, 1.0 - 2.0 g / L; Na2MoO4·2H2O, 0.5 - 3.0 g / L), which accelerates the reaction and improves the film color.

[0013] Preferably, the metal complexing agent is citric acid, tartaric acid, or hydroxycarboxylic acid. Its function is to stabilize the solution, especially to prevent excessive corrosion during the treatment of stainless steel.

[0014] Preferably, the pH buffer is boric acid or an organic acid, which serves to maintain the pH of the treatment solution within a stable range of 3.8 to 4.5.

[0015] Preferably, the nonionic surfactant is fatty alcohol polyoxyethylene ether (AEO) and its derivatives or block polyether (PO-EO copolymer), which reduces surface tension and improves wettability and uniformity.

[0016] Preferably, the treatment time for the spraying or soaking process is adjusted according to the material and requirements. Generally, the spraying process takes 1 to 5 minutes, and the soaking process takes 3 to 10 minutes.

[0017] Preferably, the sealing treatment involves immersion or spraying with a 0.5%-1.0% aqueous solution of a silane coupling agent (such as GPTMS, BTSE) for 30-60 seconds.

[0018] Secondly, the present invention provides a valve workpiece with a zirconium-based chemical conversion film on its surface, which is prepared by the above method.

[0019] The beneficial effects of this invention are mainly reflected in: The zirconium-based chemical conversion film prepared by this invention uniformly and densely covers the surface of the valve workpiece. The film layer is a uniform rainbow-colored or blue-purple interference film, without defects such as dust or white spots.

[0020] The treatment solution of this invention does not contain harmful substances such as chromium and phosphorus, nor does it contain pollutants such as heavy metal nickel and nitrite. It is environmentally friendly and safe, and complies with the RoHS directive.

[0021] The treatment solution of this invention is suitable for various valve materials such as cast iron, carbon steel, and stainless steel. Through the synergistic effect of metal complexing agents and fluoride ions, it can effectively solve the problem of passivation film hindering film formation on stainless steel surfaces.

[0022] The treatment solution of this invention has a simple and low-cost formulation, can be operated at room temperature, has a short treatment time and low energy consumption, and is suitable for large-scale industrial applications.

[0023] This invention significantly improves the adhesion, water resistance, and corrosion resistance of zirconium-based conversion films to subsequent organic coatings through silane coupling agent sealing treatment. Attached Figure Description

[0024] Figure 1 This is a comparison of the performance of Example 1 and Comparative Example 1 using Tafel curve testing.

[0025] Figure 2 The performance of the Tafel curve was tested in Examples 1-3.

[0026] Figure 3 The images are SEM images of Example 1 and Comparative Example 1. Detailed Implementation

[0027] The present invention will be further illustrated below through specific embodiments: Example

[0028] The preparation of a zirconium-based chemical conversion film for a carbon steel substrate valve is carried out according to the following steps: Preparation of zirconium-based chemical conversion membrane treatment solution Fluorozyric acid 2 g / L, accelerator is a compound of NaNO3 1 g / L and Na2MoO4·1H2O 1 g / L, complexing agent is citric acid 1 g / L, buffer is boric acid 1.3 g / L, and nonionic surfactant is AEO 0.2 g / L.

[0029] The carbon steel valve substrate is immersed in an alkaline degreasing agent at 50°C for 10 minutes to thoroughly remove oil and grease from the valve surface. Then, a special organic polymer surface conditioner is used to condition the surface, creating uniform activation points on the clean surface.

[0030] The carbon steel substrate valve treated in step (2) is immersed in the zirconium-based chemical conversion film treatment solution prepared in step (1) for 5 minutes. After the reaction, it is taken out and rinsed with clean water to remove the residual treatment solution on the surface of the valve.

[0031] The valve treated in step (3) was immersed in a 0.5% BTSE aqueous solution for 30 seconds. Finally, it was washed with clean water and dried to obtain a carbon steel base valve with excellent corrosion resistance, and a Tafel curve test was performed.

[0032] Comparative Example 1 The valve treated in step (2) of Example 1 was used as Comparative Example 1 and its corrosion resistance was compared with that of Example 1 by Tafel curve testing.

[0033] The comparative results show that after treatment with zirconium-based chemical conversion coating solution, a zirconium-based chemical conversion coating is formed, which significantly enhances the corrosion resistance of the valve. Example

[0034] Preparation of zirconium-based chemical conversion membrane treatment solution The active ingredient is fluorozirconic acid 3 g / L, the accelerator is a compound of NaNO3 2 g / L and Na2MoO4·2H2O 1 g / L, the complexing agent is tartaric acid 1.2 g / L, the buffer is boric acid 2 g / L, and the nonionic surfactant is AEO 0.2 g / L.

[0035] The cast iron valve substrate is immersed in a 50°C alkaline degreasing agent for 10 minutes to thoroughly remove oil and grease from the valve surface. Then, a special organic polymer surface conditioner is used to condition the surface, creating uniform activation points on the clean surface.

[0036] The cast iron substrate valve treated in step (2) is immersed in the zirconium-based chemical conversion coating treatment solution prepared in step (1) for 3 minutes. After the reaction, it is taken out and rinsed with clean water to remove the residual treatment solution on the valve surface.

[0037] The valve treated in step (3) was immersed in a 1% GPTMS aqueous solution for 30 seconds. Finally, it was washed with clean water and dried to obtain a carbon steel base valve with excellent corrosion resistance. Example

[0038] Preparation of zirconium-based chemical conversion membrane treatment solution The active ingredient is fluorozirconic acid 3 g / L, the accelerator is a compound of NaNO3 2 g / L and Na2MoO4·2H2O 1 g / L, the complexing agent is tartaric acid 1 g / L, the buffer is citric acid 1.5 g / L, and the nonionic surfactant is BASF block polyether 0.15 g / L.

[0039] Immerse the stainless steel valve in a 50°C alkaline degreasing agent for 10 minutes to thoroughly remove oil and grease from the valve surface.

[0040] The cast iron substrate valve treated in step (2) is immersed in the zirconium-based chemical conversion coating treatment solution prepared in step (1) for 10 minutes. After the reaction, it is taken out and rinsed with clean water to remove the residual treatment solution on the valve surface.

[0041] The valve treated in step (3) was sprayed with a 1% GPTMS aqueous solution for 60 seconds. Finally, it was washed with clean water and dried to obtain a stainless steel valve with a glossy surface and excellent corrosion resistance.

Claims

1. A method for treating valve surfaces with an environmentally friendly, corrosion-resistant zirconium-based chemical conversion film and the product thereof, characterized in that... The method specifically involves: applying a zirconium-based chemical conversion coating solution to the degreased valve via spraying or immersion at room temperature to form a zirconium-based chemical protective film; washing away any residual solution with water; and sealing the valve after zirconization treatment to improve corrosion resistance. Finally, the valve is washed with clean water and dried to obtain a valve with excellent corrosion resistance. The zirconium-based chemical conversion membrane treatment solution comprises the following raw material components: Fluorozyric acid (calculated as Zr molar mass) 1.0–3.0 g / L; Film-forming accelerator: 0.5–3.0 g / L; Metal complexing agent 0.5–1.5 g / L; pH buffer 0.5–2.0 g / L; Nonionic surfactants: 0.1–0.3 g / L; The remainder is water.

2. The method according to claim 1, characterized in that... Zirconium-based chemical conversion membranes use fluoric acid as the main salt and ZrO2 as the main salt. 2+ It serves as the core for film formation.

3. The method according to claim 1, characterized in that... The film-forming accelerator is a compound of nitrate and molybdate.

4. The method according to claim 1, characterized in that... The metal complexing agent is citric acid, tartaric acid, or hydroxycarboxylic acid.

5. The method according to claim 1, characterized in that... The pH buffer is boric acid or an organic acid.

6. The method according to claim 1, characterized in that... The nonionic surfactant is fatty alcohol polyoxyethylene ether (AEO) and its derivatives or block polyether (PO-EO copolymer).

7. The treatment time for the spraying or soaking process according to claim 1 is adjusted according to the material and requirements. Generally, the spraying process is 1 to 5 minutes, and the soaking process is 3 to 10 minutes.

8. A valve with a corrosion-resistant zirconium-based chemical conversion film on its surface, prepared by the method described in any one of claims 1-7.