A method for shaping laser-induced forward transfer deposition of metal microsphere arrays

By employing a shaping laser-induced forward transfer deposition method, a phase holographic beam array is generated using a spatial light modulator. Energy deviations are monitored and compensated in real time, solving the problems of low transfer efficiency and poor array uniformity in metal microsphere arrays. This enables the efficient and flexible fabrication of metal microsphere arrays, adaptable to diverse substrates.

CN123108557APending Publication Date: 2026-11-17SHENZHEN ZHONGJI AUTOMATION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611027081.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for metal microsphere arrays suffer from low transfer efficiency, limited flexibility in array arrangement and microsphere size control, and poor array uniformity, making it difficult to meet the high-throughput requirements of mass transfer and adapt to diverse receiving substrates and application scenarios.

Method used

A shaping laser-induced forward transfer deposition method is adopted, which uses a spatial light modulator to modulate the phase of the incident laser to generate a phase holographic beam array of the target metal microsphere array. The energy deviation of the sub-beams is monitored and compensated in real time, enabling parallel transfer of multiple metal microspheres and flexible switching of array arrangement.

Benefits of technology

This improves the fabrication efficiency of metal microsphere arrays, enhances the uniformity and flexibility of the arrays, meets the requirements of high-throughput transfer, adapts to different substrate application scenarios, and reduces material costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108557A_ABST
    Figure CN123108557A_ABST
Patent Text Reader

Abstract

This application belongs to the field of semiconductor metal microsphere array fabrication technology, and more specifically, relates to a method for shaping laser-induced forward transfer deposition of metal microsphere arrays. This application uses a spatial light modulator to shape a single laser beam into a multi-sub-beam array corresponding to the target array, transferring tens to tens of thousands of metal microspheres in parallel with a single pulse. By updating the phase hologram in real time, the array arrangement and the energy distribution of each sub-beam are dynamically reconstructed. A closed-loop feedback mechanism compensates for the energy deviation of each sub-beam pulse by pulse, achieving high-efficiency, high-flexibility, and high-uniformity fabrication of the metal microsphere array. Simultaneously, by rationally designing the center distance of the sub-beams, the ineffective consumption of surrounding donor material by plasma plume crosstalk is effectively avoided, ensuring the donor layer in non-target areas on the donor substrate remains intact, significantly improving the utilization rate of the donor material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of semiconductor metal microsphere array fabrication technology, and more specifically, relates to a method for shaping laser-induced forward transfer deposition of metal microsphere arrays. Background Technology

[0002] Metal microspheres (typically with particle sizes ranging from tens to hundreds of micrometers) have broad application prospects in high-end manufacturing fields such as microelectronic packaging, biomedical detection, precision manufacturing, and aerospace. However, the efficient and high-quality array manufacturing technology of metal microspheres has always been a key technological bottleneck restricting their large-scale industrial application.

[0003] Currently, the fabrication of metal microsphere arrays is mainly achieved through techniques such as self-assembly, semiconductor processing, and printing transfer. Self-assembly utilizes the physicochemical forces between materials to guide the formation of microspheres into an array, which can achieve both high throughput and high efficiency, but defect control is difficult. Semiconductor processing uses photolithography equipment as the core and uses techniques such as photolithography and etching to fabricate metal microsphere arrays. This method has high positional accuracy and good consistency in batch manufacturing, but the equipment is expensive, the process is complex, and it has poor adaptability to curved surfaces or large-area applications.

[0004] Printing transfer methods use lasers, electric fields, or other energy fields to print materials onto a target substrate, achieving point-to-point deposition. This method features digital, non-contact deposition, high material utilization, and controllable fabrication processes. Laser-induced forward transfer (LIFT) is a typical example of this method. Using a laser as the driving force, it precisely transfers the donor material from a transparent substrate to a receiving substrate. It is a non-contact, maskless, high-resolution additive manufacturing method capable of supporting micro- and nano-scale transfer of various materials, including metals, polymers, and biomaterials, providing a feasible path for the mass transfer of metal microsphere arrays. However, in the LIFT process, the transfer of metal microspheres is typically accomplished using a point-by-point scanning method, where a single laser beam acts on each microsphere sequentially, processing only one target per transfer. This method is inefficient when transferring arrays of tens or even hundreds of thousands of microspheres, making it difficult to meet the high-throughput requirements of fields such as optoelectronic device packaging for mass transfer.

[0005] A few studies have attempted to use fixed beam-splitting diffractive optical elements (DOEs) to generate multiple beams to achieve parallel transfer of multiple metal microspheres, but the following shortcomings still exist: (1) the beam splitting pattern, dot spacing and energy distribution cannot be adjusted once the fabrication is completed, which limits the system's flexibility; (2) the energy deviation between each sub-beam cannot be compensated in real time, resulting in poor array uniformity; (3) it is difficult to quickly switch the array arrangement (such as rectangular, hexagonal, ring or irregular layout) for different receiving substrates; (4) the range of control over the microsphere diameter and array density is limited.

[0006] Therefore, there is an urgent need for a mass production method for metal microsphere arrays that combines high efficiency, high precision, and high flexibility. Summary of the Invention

[0007] To address the shortcomings of existing technologies, this application aims to provide a method for shaping laser-induced forward transfer deposition of metal microsphere arrays. This method addresses the problems of low transfer efficiency, limited flexibility in array arrangement and microsphere size control, poor array uniformity, difficulty in meeting the high-throughput requirements of mass transfer, and inability to adapt to diverse receiving substrates and application scenarios in existing metal microsphere array fabrication technologies.

[0008] To achieve the above objectives, in a first aspect, this application provides a method for shaping laser-induced forward transfer deposition of metal microsphere arrays, comprising the following steps: S1. A donor substrate and a receiver substrate are provided. A metal microsphere donor layer is provided on one side surface of the donor substrate. The receiver substrate is opposite to and spaced apart from the side surface of the donor substrate where the metal microsphere donor layer is provided. S2. Phase modulation of the incident laser is performed using a spatial light modulator to obtain a beam array corresponding to the phase hologram of the target metal microsphere array. The beam array includes multiple sub-beams. S3. Irradiate the above-mentioned beam array onto the side surface of the donor substrate facing away from the metal microsphere donor layer, so that the metal material of the metal microsphere donor layer is peeled off from the donor substrate and transferred to the corresponding position of the receiving substrate to form the target metal microsphere array.

[0009] Preferably, the above irradiation process further includes: The energy density of each sub-beam and the transfer state of the corresponding metal microspheres are monitored in real time. Based on the monitoring results, the phase hologram loaded by the spatial light modulator is modulated in real time to compensate for the energy deviation between the sub-beams.

[0010] Preferably, the above-mentioned spatial light modulator is a phase-type spatial light modulator.

[0011] Preferably, the distance between the donor substrate and the receiver substrate is 10 μm to 500 μm.

[0012] Preferably, the diameter of the metal microspheres in the above-mentioned target metal microsphere array is 0.5μm~100μm.

[0013] Preferably, the energy density of each of the above sub-beams is 10 mJ / cm². 2 ~5J / cm 2 .

[0014] Preferably, the center-to-center distance between adjacent metal microspheres in the above-mentioned target metal microsphere array is 15 μm to 500 μm.

[0015] Preferably, the number of the above-mentioned sub-beams is 25 to 10,000.

[0016] Secondly, this application provides a system for shaping laser-induced forward transfer deposition of metal microsphere arrays, comprising: Laser output module, used to output the first laser beam; A collimation and beam expansion module is disposed in the optical path of the first laser beam and is used to expand the original diameter of the first laser beam spot to a preset diameter to obtain a second laser beam. A spatial light modulation module is set in the optical path of the second laser beam to perform phase modulation on the second laser beam, load a phase hologram corresponding to the arrangement of the target metal microsphere array, and output a beam array containing multiple sub-beams. A projection optics module is disposed in the optical path of the aforementioned beam array and is used to image the aforementioned beam array onto the side surface of the donor substrate facing the laser incident surface. The aforementioned donor substrate is disposed downstream of the optical path of the aforementioned projection optical module, and a metal microsphere donor layer is provided on the side of its surface facing away from the laser incident. The receiving substrate is disposed opposite to and spaced apart from the side surface of the donor substrate on which the metal microsphere donor layer is provided, and is used to receive the metal microspheres transferred by laser-induced transfer to form a target metal microsphere array. The control module is communicatively connected to the aforementioned spatial light modulation module and is used to generate the aforementioned phase hologram and load it into the aforementioned spatial light modulation module.

[0017] Preferably, the system further includes a monitoring module; The aforementioned monitoring module is located in the optical path of the aforementioned beam array and is used to monitor the energy density of each sub-beam and the transfer state of the corresponding metal microspheres in real time, and to feed back the monitoring results to the aforementioned control module. The aforementioned control module is also used to adjust the phase hologram loaded onto the aforementioned spatial light modulation module in real time based on the aforementioned monitoring results, so as to compensate for the energy deviation between each sub-beam.

[0018] In summary, the technical solutions conceived in this application have the following main technical advantages compared with the prior art: (1) The metal microsphere array deposition method based on shaping laser and mask provided in this application shapes a single laser beam into a beam array containing multiple sub-beams corresponding to the target array through a spatial light modulator. Tens to tens of thousands of metal microspheres can be transferred in parallel in a single pulse. The array fabrication efficiency is several orders of magnitude higher than the point-by-point scanning LIFT process, which meets the high throughput requirements of mass transfer in fields such as optoelectronic device packaging.

[0019] (2) This application achieves dynamic reconstruction of the array arrangement and energy distribution of each sub-beam without replacing any hardware components by updating the phase hologram in real time, which significantly improves the process adaptability to different packaged device layouts. Furthermore, through optional real-time energy monitoring and closed-loop feedback mechanisms, the energy deviation of each sub-beam is dynamically compensated pulse by pulse, overcoming the problem of poor array consistency caused by the uneven energy between factor beams in the fixed DOE scheme.

[0020] (3) This application reduces the single-point energy density of each sub-beam by distributing the energy of a single high-energy laser beam to multiple sub-beams arranged in a spatially isolated manner, thereby effectively suppressing the generation intensity and lateral expansion range of the plasma. At the same time, by rationally designing the center distance of the sub-beams, the ineffective consumption of surrounding donor materials by plasma plume crosstalk is effectively avoided. Non-target areas on the donor substrate can remain intact, effectively reducing material costs.

[0021] (4) This application utilizes the flexible control capability of the spatial light modulator. By pre-calibrating the parallelism deviation between the donor substrate and the receiver substrate, the focal length and energy of each sub-beam can be compensated point by point, so that the laser parameters at each transfer position can be adapted to the local gap difference. Uniform and stable microsphere transfer can be achieved in the full range without relying on high-precision mechanical assembly, thus increasing the process window. Attached Figure Description

[0022] Figure 1 This is a schematic flowchart of the method for shaping laser-induced forward transfer deposition of metal microsphere arrays provided in this application; Figure 2 This is a comparison diagram of the alignment state of the beam array and the receiving substrate before and after compensation. In this diagram, (a) is before compensation and (b) is after compensation. Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0024] In the specification and claims of this application, the terms “first” and “second” are used to distinguish different objects, rather than to describe a specific order of objects, and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated.

[0025] In the description of the embodiments in this application, the words "exemplary" or "for example" are used to indicate that they are examples, illustrations, or descriptions. Any embodiment or design that is described as "exemplary" or "for example" in the embodiments of this application should not be construed as being more preferred or advantageous than other embodiments or design options. Specifically, the use of the words "exemplary" or "for example" is intended to present the relevant concepts in a specific manner.

[0026] In the description of the embodiments in this application, unless otherwise stated, "multiple" means two or more.

[0027] Spatial Light Modulators (SLMs) have attracted widespread attention in the field of laser micromachining. However, directly applying SLM beam splitting technology to the parallel transfer of metal microspheres in the LIFT process faces a series of technical obstacles. First, when transferring metal microspheres in the LIFT process, the total energy of the incident laser is subject to a dual constraint: the damage threshold of the SLM device and the transfer threshold requirement of the donor layer. If the beam splitting is too small, the energy of a single beam will exceed the tolerance limit of the SLM; if the beam splitting is too large, the energy of a single beam will be insufficient to trigger the transfer. At the same time, the actual beam splitting conditions are also coupled with multiple parameters such as the incident laser energy, the SLM diffraction efficiency, and the focused spot size at the donor layer, which together affect the effective energy density acting on the donor layer. This makes it difficult to directly determine the beam splitting conditions that can simultaneously meet the dual threshold constraints through conventional experimental methods. Second, due to the limitations of the phase modulation accuracy, pixelation structure, and optical path system errors of the SLM itself, the energy uniformity between the sub-beams after beam splitting is difficult to guarantee. The LIFT transfer of metal microspheres is extremely sensitive to laser energy density, and energy deviation will directly lead to inconsistent transfer rates of microspheres at different positions in the array and deterioration of array uniformity. Furthermore, zero-order light interference is unavoidable during SLM beam splitting, and non-target higher-order diffraction orders are spatially close to or overlap with target orders. These stray lights interfere with the precision of microsphere deposition. In addition, even if the initial beam splitting conditions are met, the optical system still faces dynamic deviations during long-term operation: thermal drift of optical components introduces phase fluctuations, leading to sub-beam position shifts and energy redistribution; energy fluctuations between laser pulses also cause fluctuations in the total energy of a single pulse, further exacerbating the degradation of deposition precision. These technical obstacles involve multiple levels, including device physics, intrinsic defects of the optical system, and inherent interferences in the process, which are mutually restrictive. How to overcome these technical obstacles while achieving the effective application of SLM beam splitting in the parallel transfer of LIFT metal microspheres is the technical problem this application aims to solve.

[0028] Specifically, this application provides a method for shaping laser-induced forward transfer deposition of metal microsphere arrays, such as... Figure 1 As shown, it includes the following steps: S1. A donor substrate and a receiver substrate are provided. A metal microsphere donor layer is provided on one side surface of the donor substrate. The receiver substrate is opposite to and spaced apart from the side surface of the donor substrate where the metal microsphere donor layer is provided. S2. Phase modulation of the incident laser is performed using a spatial light modulator to obtain a beam array corresponding to the phase hologram of the target metal microsphere array. The beam array includes multiple sub-beams. S3. Irradiate the above-mentioned beam array onto the side surface of the donor substrate facing away from the metal microsphere donor layer, so that the metal material of the metal microsphere donor layer is peeled off from the donor substrate and transferred to the corresponding position of the receiving substrate to form the target metal microsphere array.

[0029] In some embodiments, the spatial light modulator is a phase-type spatial light modulator, and phase modulation of the incident laser beam is achieved by loading a phase hologram onto the spatial light modulator. The phase hologram is obtained by iterative Fourier transform algorithm (such as the Gerchberg-Saxton algorithm), based on the arrangement of the target metal microsphere array, the microsphere size, the wavelength of the incident laser beam, and the pixel parameters of the spatial light modulator, through repeated iterative calculations between the modulation plane of the spatial light modulator and the irradiation plane of the donor substrate. This results in the beam array modulated by the spatial light modulator forming a multi-beam pattern on the surface of the donor substrate that corresponds to the position of the microspheres in the target metal microsphere array.

[0030] In some embodiments, the irradiation process further includes: real-time monitoring of the energy density of each sub-beam and the transfer state of the metal microspheres corresponding to each sub-beam, and real-time modulation of the phase hologram loaded by the spatial light modulator based on the monitoring results to compensate for the energy deviation between the sub-beams.

[0031] In some embodiments, the arrangement of the target metal microsphere array includes, but is not limited to, any one of a rectangular array, a hexagonal array, a ring array, and an irregular array. The array arrangement can be switched by changing the phase hologram loaded onto the spatial light modulator.

[0032] This application combines programmable spatial light modulator beam splitting technology with LIFT (Limited-In-Time) fabrication. A phase hologram is loaded onto the spatial light modulator, and the incident laser is shaped into sub-beams corresponding to the positions of the microspheres in the target metal microsphere array. Multiple metal microspheres are simultaneously transferred in a single irradiation. Compared to existing point-by-point scanning LIFT, this application replaces serial scanning with parallel transfer, significantly improving array fabrication efficiency. Compared to fixed-beam diffraction optical element schemes, this application allows for programmable switching of the array arrangement without changing hardware components. Furthermore, through optional real-time energy monitoring and closed-loop feedback mechanisms, the energy distribution of each sub-beam is dynamically compensated, maintaining transfer efficiency and flexibility while ensuring the consistency of microsphere deposition at various array positions. This achieves high-efficiency, high-flexibility, and high-uniformity fabrication of metal microsphere arrays.

[0033] In some embodiments, the receiving substrate is any one of a planar substrate, a flexible substrate, or a curved substrate. In some embodiments, the distance between the donor substrate and the receiving substrate is 10 μm to 500 μm.

[0034] In some embodiments, the energy density of each sub-beam is higher than the metal material transfer threshold in the donor layer and lower than the laser damage threshold of the spatial light modulator. In actual manufacturing, the number of sub-beams is determined based on the total energy of the incident laser, the diffraction efficiency of the spatial light modulator, the spot size of each sub-beam, and the energy density of each sub-beam, wherein the energy density of each sub-beam is not lower than the material transfer threshold of the metal microspheres.

[0035] In some embodiments, the diameter of the metal microspheres in the aforementioned target metal microsphere array is 0.5 μm to 100 μm. The microsphere diameter determines the minimum spot coverage area required for a single microsphere, thereby affecting the spot size of each sub-beam on the donor substrate surface, and ultimately, together with the energy density of each sub-beam, determines the effective energy of a single pulse acting on a single microsphere. Metal microspheres within the aforementioned diameter range are suitable for both small-diameter solder balls used in microelectronic packaging and medium-diameter functional microspheres used in biomedical detection and other fields.

[0036] In some embodiments, the energy density of each of the sub-beams is 10 mJ / cm². 2 ~5J / cm 2 When the energy density of each sub-beam approaches the lower limit, a larger number of beams can be obtained under a given total incident laser energy and diffraction efficiency, suitable for scenarios with high array flux requirements. When the energy density of each sub-beam approaches the upper limit, it is suitable for metal materials with high transfer thresholds (such as high-melting-point alloys) to ensure that each sub-beam can reliably trigger microsphere transfer. The selection of the above energy density is determined by the control module based on the material system and particle size of the microspheres, combined with the total incident laser energy and the diffraction efficiency of the spatial light modulator. The above energy density range covers the typical transfer thresholds of commonly used metal materials (including but not limited to gold, copper, silver, tin-based alloys, nickel and their alloys) in the LIFT process in fields such as microelectronic packaging, biomedical detection and precision manufacturing. Within this range, by adjusting the total incident laser energy and the number of beams, the transfer thresholds of different materials can be flexibly matched without replacing core optical components such as spatial light modulators or projection optical modules due to material changes.

[0037] In some embodiments, the center-to-center distance between adjacent metal microspheres in the aforementioned target metal microsphere array is 15 μm to 500 μm, preferably 15 μm to 150 μm. The center-to-center distance determines the spatial distribution density of the microspheres in the array. Controlling the center-to-center distance within the aforementioned range can effectively suppress the influence of crosstalk between the jet plumes of adjacent microspheres on the deposition accuracy under the conditions of the diameter of the metal microspheres and the energy density of each sub-beam.

[0038] In some embodiments, the number of sub-beams is 25 to 10,000 (5×5 to 100×100). When the energy density of the sub-beams is close to the material transfer threshold and the spot size is small, the energy consumption per beam is low, and a larger number of beams can be obtained for a given total incident laser energy, which is suitable for array manufacturing scenarios of small-particle-size, low-transfer-threshold materials. Conversely, when used for large-particle-size or high-transfer-threshold materials, the energy density required per beam increases, and the number of beams decreases accordingly. The specific number of beams within the above range can be flexibly adjusted according to the material system, particle size, and target array size of the target metal microspheres.

[0039] In some embodiments, depending on the application requirements of the metal microsphere array, the above method also includes post-treatment such as sintering or curing of the deposited metal microsphere array to enhance its adhesion, conductivity and mechanical stability.

[0040] In some embodiments, the sintering temperature is 200℃~600℃. Those skilled in the art can select a suitable sintering temperature according to actual application requirements. For example, sintering is performed at 200℃~300℃ to remove residual organic solvents and to achieve initial fusion between the metal microspheres; sintering is performed at 300℃~450℃ to achieve metallurgical bonding between microspheres and improve conductivity; and sintering is performed at 450℃~600℃ to achieve densification. In some embodiments, the sintering time is 10min~120min, the sintering heating rate is 2~10℃ / min, and the sintering atmosphere is nitrogen, hydrogen, argon, helium, or a mixture thereof.

[0041] In some embodiments, the deposited metal microsphere array is subjected to laser in-situ curing. The energy density of the laser in-situ curing process is lower than the energy density threshold for the transfer of the metal microsphere donor layer.

[0042] On the other hand, this application also provides a system for shaping laser-induced forward transfer deposition of metal microsphere arrays, comprising: Laser output module, used to output the first laser beam; A collimation and beam expansion module is disposed in the optical path of the first laser beam and is used to expand the original diameter of the first laser beam spot to a preset diameter to obtain a second laser beam. A spatial light modulation module is set in the optical path of the second laser beam to perform phase modulation on the second laser beam, load a phase hologram corresponding to the arrangement of the target metal microsphere array, and output a beam array containing multiple sub-beams. A projection optics module is disposed in the optical path of the aforementioned beam array and is used to image the aforementioned beam array onto the side surface of the donor substrate facing the laser incident surface. The aforementioned donor substrate is disposed downstream of the optical path of the aforementioned projection optical module, and a metal microsphere donor layer is provided on the side of its surface facing away from the laser incident. The receiving substrate is disposed opposite to and spaced apart from the side surface of the donor substrate on which the metal microsphere donor layer is provided, and is used to receive the metal microspheres transferred by laser-induced transfer to form a target metal microsphere array. The control module is communicatively connected to the aforementioned spatial light modulation module and is used to generate the aforementioned phase hologram and load it into the aforementioned spatial light modulation module.

[0043] In some implementations, the laser output module described above may employ a pulsed laser with a pulse width in the nanosecond to femtosecond range and a wavelength within the operating band of the spatial light modulation module. The total energy of a single pulse can be flexibly configured according to the number of target sub-beams and the energy density required by each sub-beam.

[0044] In some embodiments, the projection optics module is used to image the beam array onto the surface of the donor substrate facing the laser incident side at a preset scaling ratio. The preset scaling ratio is determined by the pixel pitch of the spatial light modulation module and the center distance between adjacent microspheres in the target metal microsphere array, so that the spot size of each sub-beam matches the corresponding microsphere particle size.

[0045] In some embodiments, the system further includes a monitoring module; the monitoring module is disposed in the optical path of the beam array and is used to monitor the energy density of each sub-beam and the transfer state of the metal microspheres corresponding to each sub-beam in real time, and to feed back the monitoring results to the control module. The aforementioned control module is also used to adjust the phase hologram loaded onto the aforementioned spatial light modulation module in real time based on the aforementioned monitoring results, so as to compensate for the energy deviation between each sub-beam and ensure the uniformity of array deposition.

[0046] It should be understood that the materials, reagents, and instruments used in the following embodiments, as long as they are of the same or similar type, model, quality, properties, or functions, can be used to implement this application. Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods. Unless otherwise specified, the materials and reagents used in the following embodiments are commercially available.

[0047] The following are examples and comparative examples: Example 1 This embodiment aims to prepare a rectangular array of gold microspheres (20×20 microspheres, 10 μm diameter, and 50 μm center-to-center distance between adjacent microspheres). The method provided includes the following steps: (1) Preparation of donor substrate and receiver substrate A fused silica transparent substrate was used as the supply substrate, and a 200 nm thick gold film was deposited as the donor layer by magnetron sputtering. A silicon-based chip packaging substrate was used as the receiving substrate. The surface of the substrate was made hydrophilic by O2 plasma treatment, and cross alignment marks were prepared on the edge of the receiving substrate by photolithography to assist in the alignment of the donor and receiver substrates.

[0048] (2) Shaping and arraying of laser beams A Q-switched Nd:YAG pulsed laser with a wavelength of 532nm and a pulse of 10ns is used as the light source. After the output laser beam is passed through a beam expansion and collimation system (5 times beam expansion), it uniformly illuminates a reflective liquid crystal SLM (1920×1080 pixels resolution, 8-bit phase modulation).

[0049] Using the pre-calibrated phase-grayscale response curve of the SLM, a 20×20 rectangular phase hologram (CGH) is designed and generated using a weighted iterative Fourier transform algorithm. The sampling point spacing on the target surface is 100 μm (corresponding to the angular spacing between adjacent diffraction orders in the angular spectrum), and the energy of each target point is uniformly distributed. The CGH is loaded onto the SLM, and the laser is phase-modulated by the SLM to generate a beam array containing 20×20 sub-beams.

[0050] (3) Projection of beam array The aforementioned beam array was projected onto the side of the supply substrate facing away from the metal microsphere donor layer using a 4f projection system (with a magnification M of 0.5× for the projection lens). After projection, the spot diameter of each sub-beam on the surface of the donor layer was 12 μm, and the center-to-center distance between adjacent spots was 50 μm, corresponding to the position of the microspheres in the target metal microsphere array.

[0051] (4) Laser-induced forward transfer deposition To ensure accurate alignment of each sub-beam with the target position on the receiving substrate, a low-energy alignment detection is performed before irradiation. A low-energy pulse (with a single pulse energy reduced to 10% of the processing energy; this low-energy detection pulse has the same temporal width and spatial distribution as the processing pulse, only the total energy is reduced) is emitted. The actual landing position of each sub-beam on the receiving substrate is obtained through the photodiode array detector of the monitoring module and compared with the preset position of the target array. For sub-beams with positional deviations, a phase tilt term is superimposed on the local region of the corresponding diffraction order in the CGH to correct the incident angle of the sub-beam, thus achieving alignment compensation. Figure 2 The image shows a comparison of the laser beam array and the receiving substrate before and after alignment compensation. It can be seen that... Figure 2 Content (a) is for compensating for the deviation of the front sub-beam from the target position. Figure 2 Content (b) shows the precise correspondence between the positions of each sub-beam and the target array after compensation.

[0052] After alignment, the single-pulse energy of the laser pulser is adjusted so that the energy density of each sub-beam reaching the gold thin film is approximately 250 mJ / cm². 2 The gap between the donor substrate and the receiver substrate is monitored in real time by a laser displacement sensor and controlled within 100μm±1μm by a closed-loop feedback system.

[0053] A real-time energy monitoring and feedback system operates simultaneously. A wedge-shaped beam splitter with a splitting ratio of 99:1 is inserted between the SLM and the 4f imaging system, with 1% of the split beam entering the monitoring branch. The monitoring branch is equipped with an auxiliary imaging lens (focal length 100mm) optically conjugate with the donor layer, imaging the beam array onto an InGaAs photodiode array detector (resolution 400×400), ensuring each detector pixel corresponds to a sub-beam. Before the initial irradiation, a low-energy detection pulse (single pulse energy reduced to 10% of the processing energy) is emitted, recording the initial energy of each sub-beam and setting a target uniformity value. During the processing pulse emission, the energy of each sub-beam is simultaneously acquired, and the deviation is calculated. For sub-beams with deviations exceeding ±2%, the diffraction efficiency of that order is fine-tuned by superimposing low spatial frequency phase perturbations in a local region corresponding to the original CGH diffraction order. After three pulse iterations, the energy non-uniformity of each sub-beam is corrected to within ±2%. Subsequently, a complete processing pulse simultaneously irradiates all 400 target locations. The gold film melts and is ejected instantaneously at the corresponding sub-beam position, forming gold microspheres and depositing them onto the corresponding positions on the receiving substrate. A single pulse completes the transfer of a 20×20 gold microsphere array.

[0054] (5) Post-processing of the target metal microsphere array The receiving substrate with the deposited gold microsphere array was sintered at 150°C for 30 minutes in a nitrogen atmosphere to enhance the adhesion between the microspheres and the substrate.

[0055] Example 2 This embodiment aims to prepare a rectangular array of copper microspheres (10×10 microspheres, 6μm diameter, and 50μm center-to-center distance between adjacent microspheres). The method provided includes the following steps: (1) Preparation of donor substrate and receiver substrate A fused silica transparent substrate was used as the supply substrate, and a 500 nm thick pure copper film (99.99% purity) was deposited as the donor layer by DC magnetron sputtering, with a base vacuum better than 5 × 10⁻⁶. -4 Pa, the film thickness uniformity was verified by a step tester to be 500±25nm. The receiving substrate is a glass substrate coated with a molybdenum layer (thickness of about 500nm), which is ultrasonically cleaned in sequence with acetone, ethanol and deionized water for 10min, treated with O2 plasma for 90s to make the surface hydrophilic, and cross alignment marks are prepared on the edge of the receiving substrate by photolithography to assist in the alignment of the donor substrate and the receiving substrate.

[0056] (2) Shaping and arraying of laser beams A Q-switched Nd:YAG pulsed laser with a wavelength of 532nm and a pulse of 10ns is used as the light source. After the output laser beam is passed through a beam expansion and collimation system (5 times beam expansion), it uniformly illuminates a reflective liquid crystal SLM (1920×1080 pixels resolution, 8-bit phase modulation).

[0057] Using the pre-calibrated phase-grayscale response curve of the SLM, a 10×10 rectangular phase hologram (CGH) is designed and generated using a weighted iterative Fourier transform algorithm. The sampling point spacing on the target surface is 100 μm (corresponding to the angular spacing between adjacent diffraction orders in the angular spectrum), and the energy of each target point is uniformly distributed. The CGH is loaded onto the SLM, and the laser is phase-modulated by the SLM to generate a beam array containing 10×10 sub-beams.

[0058] (3) Projection of beam array The aforementioned beam array was projected onto the surface of the donor substrate facing the laser incident side using a 4f projection system (with a magnification M of 0.5× for the projection lens). After projection, the spot diameter of each sub-beam on the donor layer surface was 8 μm (NA=0.3), and the center-to-center distance between adjacent spots was 50 μm, corresponding to the position of the microspheres in the target copper microsphere array.

[0059] (4) Laser-induced forward transfer deposition The single-pulse energy of the laser pulser was adjusted so that the energy density of each sub-beam reaching the copper film was approximately 0.88 J / cm². 2 (This value represents the optimized transfer energy density of a 500nm thick copper film under the action of a 532nm wavelength nanosecond laser). The gap between the donor substrate and the receiver substrate is controlled at 80μm±1μm.

[0060] A real-time energy monitoring and feedback system operates simultaneously. A wedge-shaped beam splitter with a splitting ratio of 99:1 is inserted between the SLM and the 4f imaging system, with 1% of the split beam entering the monitoring branch. The monitoring branch is equipped with an auxiliary imaging lens (focal length 100mm) optically conjugate with the donor layer, imaging the beam array onto an InGaAs photodiode array detector (resolution 400×400), ensuring each detector pixel corresponds to a sub-beam. Before the initial irradiation, a low-energy detection pulse (single pulse energy reduced to 10% of the processing energy) is emitted, recording the initial energy of each sub-beam and setting a target uniformity value. During the processing pulse emission, the energy of each sub-beam is simultaneously acquired, and the deviation is calculated. For sub-beams with deviations exceeding ±2%, the diffraction efficiency of that order is fine-tuned by superimposing low spatial frequency phase perturbations in a local region corresponding to the original CGH diffraction order. After three pulse iterations, the energy non-uniformity of each sub-beam is corrected to within ±2%. Subsequently, a complete processing pulse simultaneously irradiates all 100 target locations, and 10×10 copper microspheres are simultaneously transferred and deposited onto the molybdenum layer surface of the receiving substrate, completing the transfer of the copper microsphere array.

[0061] (5) Post-processing of the target metal microsphere array The receiving substrate with the deposited copper microsphere array was sintered at 200°C for 30 minutes in a nitrogen atmosphere to enhance the adhesion between the microspheres and the substrate.

[0062] Example 3 This embodiment aims to prepare a rectangular array of pure indium microspheres (10×10 microspheres, 3μm diameter, and 100μm center-to-center distance between adjacent microspheres). The method provided includes the following steps: (1) Preparation of donor substrate and receiver substrate A fused silica transparent substrate was used as the supply substrate, and a 30 nm thick pure indium thin film (99.999% purity) was deposited as the donor layer using a thermal evaporation deposition system. The evaporation rate was controlled at 0.2~0.5 nm / s, and the base vacuum was better than 1×10⁻⁶. -5 Pa, the film thickness was monitored online by a quartz crystal oscillator. The receiving substrate was a glass substrate coated with a molybdenum layer (approximately 500 nm thick), which was ultrasonically cleaned sequentially with acetone, ethanol, and deionized water for 10 min, and then dried with nitrogen for later use.

[0063] (2) Shaping and arraying of laser beams A Ti:Sapphire femtosecond pulsed laser (ultrashort pulse laser amplification system) with a wavelength of 790nm and a pulse width of 30fs is used as the light source. After the output laser beam is used, the beam diameter is expanded to 8mm by a beam expansion and collimation system to uniformly illuminate the reflective liquid crystal SLM (1920×1200 pixels, pixel pitch 7.8μm, 10-bit phase modulation).

[0064] Using the pre-calibrated phase-grayscale response curve of the SLM, a 10×10 rectangular phase hologram (CGH) is designed and generated using a weighted iterative Fourier transform algorithm. The sampling point spacing on the target surface is 100 μm (corresponding to the angular spacing between adjacent diffraction orders in the angular spectrum), and the energy of each target point is uniformly distributed. The CGH is loaded onto the SLM, and the laser is phase-modulated by the SLM to generate a beam array containing 10×10 sub-beams.

[0065] (3) Projection of beam array The aforementioned beam array was projected onto the side of the donor substrate facing the laser incident surface using a 4f projection system (with a magnification M of 1× for the projection lens). After projection, the spot diameter of each sub-beam on the donor layer surface was 4 μm (NA=0.2), and the center-to-center distance between adjacent spots was 10 μm, corresponding to the position of the microspheres in the target indium microsphere array.

[0066] (4) Laser-induced forward transfer deposition The single-pulse energy of the laser pulser is adjusted so that the energy density of each sub-beam reaching the indium film is approximately 0.2 J / cm². 2 The gap between the donor substrate and the receiver substrate is controlled at 50μm±1μm.

[0067] The real-time monitoring branch (splitting ratio 99:1) uses a cooled CCD camera (optically conjugate with the donor layer) to detect the energy of each sub-beam and feeds it back to the computer. After multiple pulse iterations, the energy non-uniformity is corrected to ±2%. Subsequently, a complete processing pulse simultaneously irradiates all 100 target locations, and 10×10 indium microspheres are simultaneously transferred and deposited onto the molybdenum layer surface of the receiving substrate, completing the transfer of the indium microsphere array.

[0068] (5) Post-processing of the target metal microsphere array The receiving substrate with the indium microsphere array deposited was sintered at 180°C for 10 min in a nitrogen atmosphere to enhance the adhesion between the microspheres and the substrate.

[0069] Comparative Example 1 This comparative example uses a single-beam LIFT point-by-point scanning method to transfer and deposit an array of metal microspheres.

[0070] The donor and receiver substrates were fabricated in the same manner as in Example 1. The laser system used a Q-switched Nd:YAG pulsed laser with a wavelength of 532 nm and a pulse width of 10 ns. The laser beam was focused by a focusing lens into a Gaussian spot with a diameter of 12 μm, and the single-pulse energy density was approximately 250 mJ / cm². 2 A high-precision translation stage was used to scan point by point, and laser pulses were triggered sequentially according to the 20×20 array trajectory, depositing one gold microsphere at each point. The post-processing method for the gold microsphere array was the same as in Example 1.

[0071] Comparative Example 2 This comparative example uses a fixed DOE beam splitting technique to transfer and deposit a metal microsphere array.

[0072] The donor and receiver substrates are fabricated in the same manner as in Example 1. The laser system is the same as in Example 1, but a fixed diffractive optical element (DOE) is used instead of a spatial light modulator (SLM) for beam splitting, generating 20×20 sub-beams, each with an energy density of approximately 250 mJ / cm². 2 No real-time energy monitoring or feedback compensation is performed. The post-processing method for the gold microsphere array is the same as in Example 1.

[0073] Comparative Example 3 The method for shaping laser-induced forward transfer deposition of metal microsphere arrays provided in this comparative example is the same as that in embodiment 1, except that in step (4), when laser-induced forward transfer deposition is performed, real-time energy monitoring and feedback compensation are not performed, that is, only SLM beam splitting technology is used to transfer and deposit metal microsphere arrays.

[0074] The microstructure of gold microspheres deposited on the receiving substrate was observed using SEM. Experiments revealed a large coefficient of variation in microsphere diameter within the array, with some sites missing. The reasons for this are likely due to optical path system errors and limitations in SLM phase modulation accuracy. The energy uniformity of the multifocal path is highly sensitive to incident laser quality, optical system defects, and external disturbances. Significant initial energy inhomogeneity was observed in each sub-beam. Sub-beams with higher energy resulted in excessive vaporization of the donor gold film, causing spatter; sub-beams with lower energy resulted in incomplete removal of the donor gold film, leading to microspheres with smaller diameters or failure to detach.

[0075] The donor substrates transferred in Examples 1-3 and Comparative Examples 1-3 were observed and imaged in their entirety using an optical microscope. After image binarization, the total area of ​​the donor layer consumed and the effective consumption area corresponding to the target position were calculated. The material utilization rate was estimated using the following formula: Material utilization rate = (Volume of donor material corresponding to successfully transferred microspheres / Volume of donor material in the donor layer in the area where material removal occurred due to laser irradiation) × 100%. The results are shown in Table 1.

[0076] Table 1. Utilization rate of metallic materials in the donor layer in Examples 1-3 and Comparative Examples 1-3

[0077] The above results demonstrate that the method for shaping laser-induced forward transfer deposition of metal microsphere arrays provided in this application, by employing SLM beam splitting technology and combining it with real-time energy monitoring and feedback adjustment processes to dynamically compensate for the energy distribution of each sub-beam, keeps the energy deviation of each sub-beam at an extremely low level. This avoids microsphere non-transfer due to excessively low sub-beam energy and excessive donor layer ablation due to excessively high sub-beam energy, thereby improving the effective utilization rate of the donor material. Simultaneously, phase holography optimization suppresses zero-order and high-order diffraction stray light, reducing the ineffective consumption of donor layer material in non-target areas. Compared with the traditional single-beam LIFT point-by-point scanning and fixed DOE beam splitting scheme, this application significantly improves the utilization rate of donor layer material under the same target array size.

[0078] Comparative Example 4 The method for shaping laser-induced forward transfer deposition of metal microsphere arrays provided in this comparative example is the same as in Example 1, except that the total laser energy (1 mJ) laser beam is split into 200 × 200 sub-beams, and the energy density of each sub-beam is approximately 32 mJ / cm². 2 .

[0079] The experimental results showed that the donor layer was only slightly heated, the gold film could not effectively melt the glass, and no microspheres were deposited on the receiving substrate.

[0080] Comparative Example 5 The method for shaping laser-induced forward transfer deposition of metal microsphere arrays provided in this comparative example is the same as in Example 1, except that the center-to-center distance between adjacent microspheres in the target gold microsphere array is set to 10 μm.

[0081] SEM was used to observe the morphology of the donor substrate and the microstructure of the gold microspheres deposited on the receiving substrate after irradiation. The experiment revealed localized melting and spattering marks in the non-target irradiated areas of the donor gold film. Some target locations on the receiving substrate did not have gold microspheres deposited, and the deposited microspheres deviated from the target point by more than 8 μm, resulting in decreased array regularity. The possible reason is that after a single laser pulse acts on the donor layer during the LIFT process, the plasma plume formed by the vaporization and ionization of the metal material expands outward in a direction perpendicular to the donor layer surface. The expansion regions of adjacent plumes overlap on the donor layer surface, causing interference in the exchange of momentum and heat between the plumes, thus affecting the directional deposition of the microspheres.

[0082] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A method of shaping a laser-induced forward transfer deposited metal microsphere array, the method comprising: providing a substrate having a plurality of metal microspheres deposited thereon; and irradiating the substrate with a laser beam to shape the metal microspheres into a desired pattern. Includes the following steps: S1. A donor substrate and a receiver substrate are provided. A metal microsphere donor layer is provided on one side surface of the donor substrate. The receiver substrate is opposite to and spaced apart from the side surface of the donor substrate where the metal microsphere donor layer is provided. S2. Phase modulation of the incident laser is performed using a spatial light modulator to obtain a beam array corresponding to the phase hologram of the target metal microsphere array, wherein the beam array includes multiple sub-beams; S3. Irradiate the beam array onto the side surface of the donor substrate facing away from the metal microsphere donor layer, so that the metal material of the metal microsphere donor layer is peeled off from the donor substrate and transferred to the corresponding position of the receiving substrate to form the target metal microsphere array.

2. The method according to claim 1, characterized in that, The irradiation process also includes: The energy density of each sub-beam and the transfer state of the corresponding metal microspheres are monitored in real time. Based on the monitoring results, the phase hologram loaded by the spatial light modulator is modulated in real time to compensate for the energy deviation between the sub-beams.

3. The method according to claim 1, characterized in that, The spatial light modulator is a phase-type spatial light modulator.

4. The method according to claim 1, characterized in that, The distance between the donor substrate and the receiver substrate is 10μm to 500μm.

5. The method according to claim 1, characterized in that, The diameter of the metal microspheres in the target metal microsphere array is 0.5μm~100μm.

6. The method according to claim 5, characterized in that, The energy density of each of the sub-beams is 10 mJ / cm 2 5 J / cm 2 .

7. The method according to claim 6, characterized in that, The center-to-center distance between adjacent metal microspheres in the target metal microsphere array is 15 μm to 500 μm.

8. The method according to claim 6, characterized in that, The number of sub-beams is 25 to 10,000.

9. A system for shaping laser-induced forward transfer deposition of metal microsphere arrays, characterized in that, include: Laser output module, used to output the first laser beam; A collimation and beam expansion module is disposed in the optical path of the first laser beam and is used to expand the original diameter of the first laser beam spot to a preset diameter to obtain a second laser beam. A spatial light modulation module is set in the optical path of the second laser beam to perform phase modulation on the second laser beam, load a phase hologram corresponding to the arrangement of the target metal microsphere array, and output a beam array containing multiple sub-beams; A projection optics module is disposed in the optical path of the beam array and is used to image the beam array onto the side surface of the donor substrate facing the laser incident surface. The donor substrate is disposed downstream of the optical path of the projection optical module, and a metal microsphere donor layer is provided on the side of its surface facing away from the laser incident. A receiving substrate is disposed opposite to and spaced apart from the side surface of the donor substrate on which a metal microsphere donor layer is provided, for receiving the metal microspheres transferred by laser-induced transfer to form a target metal microsphere array. The control module is communicatively connected to the spatial light modulation module and is used to generate the phase hologram and load it into the spatial light modulation module.

10. The system according to claim 9, characterized in that, It also includes a monitoring module; The monitoring module is located in the optical path of the beam array and is used to monitor the energy density of each sub-beam and the transfer state of the metal microspheres corresponding to each sub-beam in real time, and to feed back the monitoring results to the control module. The control module is also used to adjust the phase hologram loaded onto the spatial light modulation module in real time according to the monitoring results, so as to compensate for the energy deviation between each sub-beam.