A Co-Cu spinel nanocatalyst with a heterogeneous interface, its preparation method, and its application in lignin electrocatalysis.

Co-Cu spinel nanocatalysts were synthesized by sol-gel method. By utilizing the heterostructure of CuO and Cu0.92Co2.08O4 interface, the problem of low electrocatalytic efficiency of lignin in the existing technology was solved, and efficient lignin depolymerization and high-value product generation were achieved.

CN123108627APending Publication Date: 2026-11-17GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611277861.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing non-precious metal catalysts have low efficiency, complex synthesis steps, unstable active components, and long reaction times in the electrocatalytic conversion of lignin, making it difficult to achieve efficient depolymerization and the generation of high-value products.

Method used

Co-Cu spinel nanocatalysts were synthesized using the sol-gel method. By calcining a copper-cobalt Prussian blue analog precursor in air at low temperature, a heterogeneous interface structure of CuO and Cu0.92Co2.08O4 was formed, which promoted the selective breaking of CO and C-C bonds.

Benefits of technology

The electrocatalytic conversion rate and selectivity of lignin were improved, while energy consumption and cost were reduced. A catalyst with uniform morphology and high specific surface area was obtained, achieving a conversion rate of over 88% for lignin model compounds and a benzaldehyde yield of over 53%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108627A_ABST
    Figure CN123108627A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of catalytic materials technology, and discloses a Co-Cu spinel nanocatalyst with a heterogeneous interface, its preparation method, and its application in lignin electrocatalysis. This invention uses copper acetate and potassium cobalt cyanide as metal sources, synthesizing a copper-cobalt Prussian blue analog precursor via room temperature co-precipitation, followed by in-situ conversion into a cubic Co-Cu spinel nanocatalyst with a Cu-O-Co heterogeneous interface through low-temperature calcination. This heterogeneous interface promotes the electrocatalysis of Co-Cu spinel nanocatalyst. 2+ / Co 3+ With Cu + / Cu 2+ The reversible cycle of the two redox pairs significantly enhances lattice oxygen mobility. This invention offers a mild and low-cost process with promising prospects for industrial application. When applied to the electrocatalytic conversion of lignin, at a current density of 30, the conversion rate of the model compound reached over 88%, and the benzaldehyde yield reached 53%, exhibiting excellent selectivity for aromatic monomers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalytic materials technology, and particularly relates to a Co-Cu spinel nanocatalyst with a heterogeneous interface, its preparation method, and its application in lignin electrocatalysis. Background Technology

[0002] Lignin, the most abundant aromatic natural polymer in nature, is widely found in plant cell walls and, along with cellulose and hemicellulose, constitutes the main components of lignocellulose biomass. Its structure is primarily composed of three phenylpropane units (p-coumarol, coniferyl alcohol, and sinapyl alcohol) linked by CO bonds (such as β-O-4) and C / C bonds (such as 5-5, β-1, β-5), making it an important potential source of renewable aromatic compounds. However, the high complexity of lignin's structure, its chemical inertness, and its susceptibility to condensation side reactions during depolymerization often lead to problems in traditional thermochemical conversion methods (such as pyrolysis and gasification) or catalytic hydrogenation, including poor product selectivity, high energy consumption, the need for high-pressure hydrogen or precious metal catalysts, and the tendency to produce coke. These issues severely restrict the high-value utilization of lignin resources. Therefore, developing mild, controllable, green, and efficient strategies for lignin depolymerization and directional conversion has become a research hotspot in the field of biomass conversion.

[0003] Electrocatalysis can achieve lignin depolymerization at ambient temperature and pressure, precisely controlling the reaction path by adjusting the electrode potential, thus avoiding the use of high-pressure hydrogen or strong oxidants. In recent years, various electrocatalysts have been used for the electrochemical conversion of lignin and its model compounds. In noble metal systems, Pd-based catalysts exhibit good CO bond cleavage activity for β-O-4 model compounds in alkaline media, with monophenol selectivity exceeding 85%; Pt electrodes can generate aromatic aldehydes such as vanillin and syringin during lignin oxidative depolymerization. In non-noble metal systems, Ni-Cu bimetallic supported nickel foam can significantly reduce overpotential, achieving efficient depolymerization of lignin sulfonates at 1.6 V vs. RHE, with a total monophenol yield of approximately 38%; Co-Fe layered double hydroxide (LDH), as an electrocatalyst, exhibits high selectivity for lignin β-O-4 bond cleavage in alkaline electrolytes, mainly generating guaiacol and acetophenone. Furthermore, Ni-Co spinel oxide can achieve C20 ... α -C βBond breaking. Although the aforementioned transition metal catalysts exhibit advantages in product selectivity regulation during the electrocatalytic conversion of lignin, they still face common problems such as easy dissolution of active catalyst components, low current efficiency, and long reaction times, with the overall lignin conversion rate mostly limited to the 50%-60% range. Therefore, developing highly active and stable non-noble metal electrocatalysts has become crucial. Spinel-structured materials have attracted attention due to their tunable metal ion occupancy, abundant redox pairs, and excellent conductivity. Among them, Co-Cu spinel nanocatalysts combine the high catalytic activity of cobalt with the promoting effect of copper on the selective breaking of C-C bonds, and are expected to achieve efficient depolymerization and high-value product generation in the electrocatalytic conversion of lignin. Summary of the Invention

[0004] In order to overcome the shortcomings and deficiencies of the existing technologies, such as low efficiency of non-precious metal catalysts, complex synthesis steps, unstable active components, and excessively long reaction time in the electrocatalytic conversion of lignin, the primary objective of this invention is to provide a method for preparing Co-Cu spinel nanocatalysts with heterogeneous interfaces. This method synthesizes the precursor of Co-Cu spinel catalyst by sol-gel method, and then calcines the precursor in air to obtain the final product.

[0005] Another objective of this invention is to provide a Co-Cu spinel nanocatalyst with a heterogeneous interface prepared by the above-described preparation method; the catalyst is a uniformly distributed, loosely porous nanoparticle or a nanocubic structure composed of small-sized nanoparticles.

[0006] Another object of the present invention is to provide an application of the above-mentioned Co-Cu spinel nanocatalyst with heterogeneous interface; the catalyst can be applied to the electrocatalytic conversion of lignin into high-value aromatic chemicals, and has excellent lignin conversion rate and monomer selectivity.

[0007] The objective of this invention is achieved through the following technical solution: A method for preparing a Co-Cu spinel nanocatalyst with a heterogeneous interface includes the following steps: (1) Dissolve potassium cobalt cyanide in deionized water to prepare solution A; dissolve copper acetate and sodium citrate in deionized water to prepare solution B; add solution A dropwise to solution B under magnetic stirring, stir and mix evenly, and allow to stand at room temperature for co-precipitation reaction. After the reaction is completed, wash and centrifuge, and dry the precipitate to obtain copper-cobalt Prussian blue analog precursor; the molar ratio of copper acetate to potassium cobalt cyanide is (3-1):(1-3), and the sodium citrate is used as a complexing agent, and the amount of sodium citrate used is 5 mmol when the total molar amount of copper acetate and potassium cobalt cyanide is 15 mmol. (2) Grind the copper-cobalt Prussian blue analog precursor obtained in step (1) into powder, place it in a muffle furnace and calcine it at low temperature in air atmosphere, raise the temperature to 300-500℃ at a rate of 1-3℃ / min and hold for 1-3 h, and after the reaction is completed, cool it naturally to room temperature to obtain Co-Cu spinel nanocatalyst with heterostructure interface.

[0008] In step (1), the molar volume ratio of potassium cobalt cyanide to deionized water in solution A is (2-10) mmol:50 mL, and the molar volume ratio of copper acetate to deionized water in solution B is (10-2) mmol:50 mL; the molar ratio of copper acetate to potassium cobalt cyanide is 2:1; the drying is carried out at 65-120℃ for 24-32 h.

[0009] Preferably, in step (1), the molar volume ratio of potassium cobalt cyanide to deionized water in solution A is 5 mmol: 50 mL; the molar volume ratio of copper acetate to deionized water in solution A is 10 mmol: 50 mL; and the drying is performed at 80°C for 24 h.

[0010] The coprecipitation reaction in step (1) is to let it stand for 24 hours at room temperature; the washing and centrifugation is to wash with deionized water and anhydrous ethanol in sequence and then centrifuge, repeating the washing and centrifugation operation 3 to 5 times.

[0011] The calcination in step (2) involves heating to 350°C at a rate of 1°C / min and holding for 2 hours.

[0012] A Co-Cu spinel nanocatalyst with a heterogeneous interface, prepared by the above-described method, wherein the Co-Cu spinel nanocatalyst has a nanocube morphology assembled from nanoparticles, and its interior forms CuO and CuO / Cu. 0.92 Co 2.08 A heterogeneous interface structure with O4 coexistence. This heterogeneous interface structure constructs a Co-Cu interface through a bimetallic synergistic effect between Co and Cu. 2+ / Co 3+ With Cu + / Cu 2+ A double redox pair is used to enhance the lattice oxygen migration rate and the regeneration capacity of reactive oxygen species. In the Co-Cu spinel nanocatalyst, the molar ratio of Co to Cu is (1-3):(3-1).

[0013] In the Co-Cu spinel nanocatalyst, the molar ratio of Co to Cu is 2:1.

[0014] The above-mentioned application of Co-Cu spinel nanocatalysts with heterogeneous interfaces in lignin electrocatalysis is carried out according to the following steps: Co-Cu spinel nanocatalysts with heterogeneous interfaces are loaded onto pretreated nickel foam as the anode working electrode, and a graphite rod is used as the cathode counter electrode; at a concentration... A potassium hydroxide solution was used as the cathode electrolyte, and lignin or lignin model compounds were added to a solution of a certain concentration. A potassium hydroxide solution was used as the anolyte; the working anode and the counter cathode were immersed in the corresponding electrolytes, and an electric current was applied while stirring to carry out an electrocatalytic reaction; the Cu-O-Co heterostructure in the Co-Cu spinel nanocatalyst was used to promote the selective breaking of CO and CC bonds in lignin or lignin model compounds to generate aromatic monomer products; the mass ratio of the lignin or lignin model compound to the Co-Cu spinel nanocatalyst with the heterostructure was 3:1.

[0015] The lignin model compound is 2-phenoxy-1-phenylethanol (PPE); when 2-phenoxy-1-phenylethanol is used as a substrate for electrocatalytic conversion, at 30... At the specified current density, the conversion rate of 2-phenoxy-1-phenylethanol reached over 88%, and the yield of benzaldehyde reached over 53%.

[0016] The present invention has the following advantages and beneficial effects compared with the prior art: (1) Compared with existing noble metal catalyst systems (such as Pb and Pt systems), the Co-Cu spinel nanocatalyst material of the present invention has the advantages of low raw material cost and easy access, and exhibits better electrocatalytic stability in the electrocatalytic conversion of lignin.

[0017] (2) Traditional methods for preparing catalysts usually rely on high temperatures (e.g., 800℃) or a protective atmosphere of H2, which leads to high energy consumption, complex processes, and inherent defects in the synthesized materials, such as uneven morphology, excessively large particle size, and low specific surface area. This invention adopts a sol-gel method with low-temperature sintering, reducing the calcination temperature to 300-500℃. On the one hand, this simplifies the process and reduces energy consumption and cost; on the other hand, it effectively controls the nucleation and growth of nanomaterials, resulting in catalyst products with uniform morphology and high specific surface area.

[0018] (3) The synthesis process of the Co-Cu spinel nanocatalyst material of the present invention is simple. Different nanocatalyst materials can be obtained by changing the ratio of potassium cobalt cyanide and copper acetate, which has good potential for industrial production.

[0019] (4) This invention can prepare Co-Cu spinel nanocatalyst materials with excellent electrochemical performance by controlling the metal ratio and the time and temperature of air calcination. Furthermore, this nanocatalyst material is a porous and loosely packed nanoparticle with a large specific surface area and more active sites, effectively improving the conversion rate and selectivity of lignin electrocatalytically converted into aromatic chemicals. This invention provides a novel and highly efficient spinel catalyst system for the high-value electrocatalytic conversion of lignin, and has significant application value in the field of biomass resource utilization.

[0020] (5) The Co-Cu spinel nanocatalyst material of this invention can be used at 30 At a current density of 88%, the conversion rate of lignin model compounds was achieved, with a phenol yield of 27% and a benzaldehyde yield of 53%. Compared with other non-precious metal catalysts, the selectivity was improved by 5%-10%, and the Co-Cu spinel nanocatalyst material of this invention has better catalytic performance. Attached Figure Description

[0021] Figure 1 This is the XRD pattern of the Co-Cu spinel nanocatalyst prepared in Example 1 of this invention.

[0022] Figure 2 These are SEM (a) and TEM (b) images of the Co-Cu spinel nanocatalyst prepared in Example 1 of this invention.

[0023] Figure 3 To utilize the Co-Cu spinel nanocatalyst prepared in Example 1 of this invention to catalyze the lignin model compound 2-phenoxy-1-phenylethanol, the liquid chromatogram of the liquid product after the reaction (the horizontal axis is time in minutes, and the vertical axis is the peak intensity) and the calculation of yield and selectivity are obtained.

[0024] Figure 4 The chromatogram is a gas chromatography-mass spectrometry (GC-MS) analysis of the liquid products after the enzymatic hydrolysis of lignin by the Co-Cu spinel nanocatalyst prepared in Example 1 of this invention (the horizontal axis is time in minutes, and the vertical axis is the peak intensity).

[0025] Figure 5 The image shows a chromatogram (x-axis: time in minutes, y-axis: peak intensity) of the liquid products after the enzymatic hydrolysis of lignin by the Co3O4 spinel nanocatalyst prepared in Comparative Example 1 of this invention.

[0026] Figure 6 The chromatogram is a gas chromatography-mass spectrometry (GC-MS) analysis of the liquid products after the enzymatic hydrolysis of lignin by the CuO spinel nanocatalyst prepared in Comparative Example 2 of this invention (the horizontal axis is time in minutes, and the vertical axis is the peak intensity).

[0027] Figure 7 The graph shows the LSV test results of the catalysts prepared in Examples 1-4 and Comparative Examples 1-2.

[0028] Figure 8 The images show the Tafel test results of the catalysts prepared in Examples 1-4 and Comparative Examples 1-2.

[0029] Figure 9 The overpotential results are shown in the graphs for the catalysts prepared in Examples 1-4 and Comparative Examples 1-2. Detailed Implementation

[0030] The present invention will be further described in detail below with reference to embodiments, but the implementation of the present invention is not limited thereto.

[0031] All raw materials used in the examples are commercially available; unless otherwise specified, the reagents, methods and equipment used in this invention are conventional reagents, methods and equipment in this technical field.

[0032] Example 1 (1) Weigh 1.66 g CoK3(CN)6 and dissolve it in 50 mL of deionized water to prepare solution A. Weigh 1.82 g Cu(CH3COO)2 and 1.29 g C6H5Na3O7 and dissolve them in 50 mL of deionized water to prepare solution B. Add solution A dropwise to solution B under magnetic stirring and stir for 30 min to mix evenly. Let it stand at room temperature for 24 h to carry out co-precipitation reaction. After the reaction is completed, wash it with deionized water and anhydrous ethanol in sequence and centrifuge. Repeat the washing and centrifugation operation 3 to 5 times. The precipitate obtained is dried at 80℃ for 24 h to obtain copper-cobalt Prussian blue analog precursor. (2) The copper-cobalt Prussian blue analog precursor obtained in step (1) was ground into powder, placed in a muffle furnace and calcined at low temperature in air atmosphere. The temperature was increased to 350℃ at a rate of 1℃ / min and held for 2 h. After the reaction was completed, it was naturally cooled to room temperature, and the product was collected to obtain the Co-Cu spinel nanocatalyst with heterogeneous interface, named CuO / Cu 0.92 Co 2.08 O4-1.

[0033] See Figure 1 CuO / Cu prepared according to the method described in Example 1 0.92 Co 2.08 X-ray powder diffraction (XRD) spectra of the O4 catalyst material. The peak positions in the figure correspond one-to-one with all diffraction planes of JCPDF standard cards (72-0629) and (37-0878), and no impure diffraction peaks were found.

[0034] See Figure 2 , Figure 2 In this context, 'a' represents the CuO / Cu prepared according to the method described in Example 1. 0.92 Co 2.08 Scanning electron microscope (SEM) images of O4 catalyst materials. Figure 2 In this context, 'b' represents the CuO / Cu prepared according to the method described in Example 1. 0.92 Co 2.08 Transmission electron microscopy (TEM) image of the O4 catalyst. The CuO / Cu ratio can be seen from the image. 0.92 Co 2.08 O4 catalyst is a nanocube catalyst material assembled from nanoparticles of varying sizes.

[0035] Example 2 (1) Weigh 3.32 g CoK3(CN)6 and dissolve it in 50 mL of deionized water to prepare solution A. Weigh 0.91 g Cu(CH3COO)2 and 1.29 g C6H5Na3O7 and dissolve them in 50 mL of deionized water to prepare solution B. Add solution A dropwise to solution B under magnetic stirring and stir for 30 min to mix evenly. Let it stand at room temperature for 24 h to carry out coprecipitation reaction. After the reaction is completed, wash it with deionized water and anhydrous ethanol in sequence and centrifuge. Repeat the washing and centrifugation operation 3 to 5 times. The precipitate obtained is dried at 80℃ for 24 h to obtain copper-cobalt Prussian blue analog precursor. (2) The copper-cobalt Prussian blue analog precursor obtained in step (1) was ground into powder, placed in a muffle furnace and calcined at low temperature in air atmosphere. The temperature was increased to 350℃ at a rate of 1℃ / min and held for 2 h. After the reaction was completed, it was naturally cooled to room temperature, and the product was collected to obtain the Co-Cu spinel nanocatalyst with heterogeneous interface, named CuO / Cu 0.92 Co 2.08 O4-2.

[0036] CuO / Cu prepared by the method described in Example 2 0.92 Co 2.08 The O4-2 catalyst material was observed to have a nanocubic structure in SEM and TEM tests.

[0037] Example 3 (1) Weigh 1.99 g CoK3(CN)6 and dissolve it in 50 mL of deionized water to prepare solution A. Weigh 0.36 g Cu(CH3COO)2 and 0.689 g anhydrous C6H5Na3O7 and dissolve them in 50 mL of deionized water to prepare solution B. Add solution A dropwise to solution B under magnetic stirring and stir for 30 min to mix evenly. Allow the mixture to stand at room temperature for 24 h to carry out coprecipitation reaction. After the reaction is completed, wash the mixture with deionized water and anhydrous ethanol in sequence and centrifuge. Repeat the washing and centrifugation operation 3 to 5 times. Dry the precipitate at 80℃ for 24 h to obtain the copper-cobalt Prussian blue analog precursor. (2) The copper-cobalt Prussian blue analog precursor obtained in step (1) was ground into powder, placed in a muffle furnace and calcined at low temperature in air atmosphere. The temperature was increased to 350℃ at a rate of 1℃ / min and held for 2 h. After the reaction was completed, it was naturally cooled to room temperature, and the product was collected to obtain the Co-Cu spinel nanocatalyst with heterogeneous interface, named CuO / Cu 0.92 Co 2.08 O4-3.

[0038] Example 4 (1) Weigh 0.66 g CoK3(CN)6 and dissolve it in 50 mL of deionized water to prepare solution A. Weigh 1.10 g Cu(CH3COO)2 and 1.29 g C6H5Na3O7 and dissolve them in 50 mL of deionized water to prepare solution B. Add solution A dropwise to solution B under magnetic stirring and stir for 30 min to mix evenly. Let it stand at room temperature for 24 h to carry out coprecipitation reaction. After the reaction is completed, wash it with deionized water and anhydrous ethanol in sequence and centrifuge. Repeat the washing and centrifugation operation 3 to 5 times. The precipitate obtained is dried at 80℃ for 24 h to obtain copper-cobalt Prussian blue analog precursor. (2) The copper-cobalt Prussian blue analog precursor obtained in step (1) was ground into powder, placed in a muffle furnace and calcined at low temperature in air atmosphere. The temperature was increased to 350℃ at a rate of 1℃ / min and held for 2 h. After the reaction was completed, it was naturally cooled to room temperature, and the product was collected to obtain the Co-Cu spinel nanocatalyst with heterogeneous interface, named CuO / Cu 0.92 Co 2.08 O4-4.

[0039] Comparative Example 1 (1) Weigh 3.32 g CoK3(CN)6 and dissolve it in 50 mL of deionized water to prepare solution A. Weigh 0.89 g Co(CH3COO)2 and 1.29 g C6H5Na3O7 and dissolve them in 50 mL of deionized water to prepare solution B. Add solution A dropwise to solution B under magnetic stirring and stir for 30 min to mix evenly. Allow the mixture to stand at room temperature for 24 h to carry out co-precipitation reaction. After the reaction is completed, wash the mixture with deionized water and anhydrous ethanol in sequence and centrifuge. Repeat the washing and centrifugation operation 3 to 5 times. Dry the precipitate at 80℃ for 24 h to obtain the precursor of cobalt Prussian blue analogue. (2) Grind the cobalt Prussian blue analog precursor obtained in step (1) into powder, place it in a muffle furnace and calcine it at low temperature in an air atmosphere. Increase the temperature to 350℃ at a rate of 1℃ / min and hold for 2 h. After the reaction is completed, cool it naturally to room temperature and collect the product to obtain the nanocatalyst, named Co3O4.

[0040] Comparative Example 2 Cu(CH3COO)2 was placed in a muffle furnace and calcined. The temperature was increased to 350℃ at a rate of 1℃ / min and held for 2 h. After the reaction was completed, the mixture was naturally cooled to room temperature, and the product was collected to obtain the nanocatalyst, which was named CuO.

[0041] Example 5 A solvent was prepared by mixing Nafion 117 solution, ethanol, and deionized water in a volume ratio of 3:40:40 and sonicating for 30 min. 0.05 g of the CuO / Cu prepared in Example 1 was then used. 0.92 Co 2.08 O4-1 nanocatalyst was dispersed in 1.5 mL of the solvent and sonicated for 10 min to obtain a catalyst dispersion. Nickel foam pretreated with acetone, ethanol, and deionized water was then sprayed onto the obtained catalyst dispersion, resulting in a catalyst loading of approximately 5.56 g / L. Nickel foam with supported catalyst was obtained. An H-type electrolytic cell was used, with the obtained nickel foam with supported catalyst as the working electrode and a graphite rod as the counter electrode. The anolyte was 50 mL of a solution containing 0.15 g of enzymatically hydrolyzed lignin. KOH solution, cathode electrolyte is 50 mL with a concentration of 1 KOH solution. At 25°C The reaction was stirred at a certain current density for 12 h. After the reaction, the electrolyte was neutralized with hydrochloric acid and centrifuged. The supernatant was extracted with dichloromethane, and the organic phase was qualitatively analyzed using an Agilent 7890B-7000C gas chromatograph-tandem mass spectrometer. (See also...) Figure 4The results showed that most of the liquid products obtained within the detection range were aromatic compounds, mainly including monophenols (vanillin, acetylvanillin, p-hydroxyacetophenone, p-hydroxybenzaldehyde, etc.) and aromatic monomers such as G-type (isoeugenol) and H-type (4-isopropylbenzyl alcohol, 4-methylbenzoic acid) derivatives. After neutralizing the reaction solution, the unreacted solid residue was collected, washed, dried, and weighed. 0.0385 g remained after the reaction, indicating a lignin conversion rate of 74.3%.

[0042] Example 6 The solvent was prepared by mixing Nafion 117 solution, ethanol, and deionized water in a volume ratio of 3:40:40 and sonicating for 30 min. 0.05 g of the CuO / Cu prepared in Example 2 was then used. 0.92 Co 2.08 O4-2 nanocatalyst was dispersed in 1.5 mL of the solvent and sonicated for 10 min to obtain a catalyst dispersion. Nickel foam pretreated with acetone, ethanol, and deionized water was then sprayed onto the obtained catalyst dispersion, resulting in a catalyst loading of approximately 5.56 g / L. Nickel foam with supported catalyst was obtained. An H-type electrolytic cell was used, with the obtained nickel foam with supported catalyst as the working electrode and a graphite rod as the counter electrode. The anolyte was 50 mL of a solution containing 0.15 g of enzymatically hydrolyzed lignin. KOH solution, cathode electrolyte 50 mL, concentration 1 KOH solution. At 25°C The reaction was stirred at a current density for 12 h. After the reaction was completed, the reaction solution was neutralized and filtered. Unreacted solid residue was collected, washed, dried and weighed. The filtrate was extracted with dichloromethane and the organic phase was subjected to GC-MS qualitative analysis. The composition of the obtained product was basically the same as that in Example 5. 0.0463 g remained after the reaction, and the lignin conversion rate was 69.1%.

[0043] Example 7 The solvent was prepared by mixing Nafion 117 solution, ethanol, and deionized water in a volume ratio of 3:40:40 and sonicating for 30 min. 0.05 g of the CuO / Cu prepared in Example 3 was then used. 0.92 Co 2.08 O4-3 nanocatalyst was dispersed in 1.5 mL of the solvent and sonicated for 10 min to obtain a catalyst dispersion. Nickel foam pretreated with acetone, ethanol, and deionized water was then sprayed onto the obtained catalyst dispersion, resulting in a catalyst loading of approximately 5.56 g / L. Nickel foam with supported catalyst was obtained. An H-type electrolytic cell was used, with the obtained nickel foam with supported catalyst as the working electrode and a graphite rod as the counter electrode. The anolyte was 50 mL of a solution containing 0.15 g of enzymatically hydrolyzed lignin. KOH solution, cathode electrolyte is 50 mL with a concentration of 1 KOH solution. At 25°C The reaction was stirred at a current density for 12 h. After the reaction was completed, the reaction solution was neutralized and filtered. Unreacted solid residue was collected, washed, dried and weighed. The filtrate was extracted with dichloromethane and the organic phase was subjected to GC-MS qualitative analysis. The composition of the obtained product was basically the same as that in Example 5. 0.0489 g remained after the reaction, and the lignin conversion rate was 67.4%.

[0044] Example 8 The solvent was prepared by mixing Nafion 117 solution, ethanol, and deionized water in a volume ratio of 3:40:40 and sonicating for 30 min. 0.05 g of the CuO / Cu prepared in Example 4 was then used. 0.92 Co 2.08 O4-4 nanocatalyst was dispersed in 1.5 mL of the solvent and sonicated for 10 min to obtain a catalyst dispersion. Nickel foam pretreated with acetone, ethanol, and deionized water was then sprayed onto the obtained catalyst dispersion, resulting in a catalyst loading of approximately 5.56 g / L. Nickel foam with supported catalyst was obtained. An H-type electrolytic cell was used, with the obtained nickel foam with supported catalyst as the working electrode and a graphite rod as the counter electrode. The anolyte was 50 mL of a solution containing 0.15 g of enzymatically hydrolyzed lignin. KOH solution, cathode electrolyte is 50 mL with a concentration of 1 KOH solution. At 25°C The reaction was stirred at a current density for 12 h. After the reaction was completed, the reaction solution was neutralized and filtered. Unreacted solid residue was collected, washed, dried and weighed. The filtrate was extracted with dichloromethane and the organic phase was subjected to GC-MS qualitative analysis. The composition of the obtained product was basically the same as that in Example 5. 0.0447 g remained after the reaction, and the lignin conversion rate was 70.2%.

[0045] Example 9 The solvent was prepared by mixing Nafion 117 solution, ethanol, and deionized water in a volume ratio of 3:40:40 and sonicating for 30 min. 0.05 g of the CuO / Cu prepared in Example 1 was then used. 0.92 Co 2.08 O4-1 nanocatalyst was dispersed in 1.5 mL of the solvent and sonicated for 10 min to obtain a catalyst dispersion. Nickel foam pretreated with acetone, ethanol, and deionized water was then sprayed onto the obtained catalyst dispersion, resulting in a catalyst loading of approximately 5.56 g / L. An H-type electrolytic cell was used, with the aforementioned catalyst-supported nickel foam as the working electrode and a graphite rod as the counter electrode. The anolyte was 50 mL of a solution containing 0.15 g of enzymatically hydrolyzed lignin. KOH solution, cathode electrolyte is 50 mL with a concentration of 1 KOH solution. At 25°C The reaction was stirred at the current density for 6 h. After the reaction was completed, the reaction solution was neutralized and filtered. The unreacted solid residue was collected, washed, dried and weighed. The filtrate was extracted with dichloromethane and the organic phase was subjected to GC-MS qualitative analysis. The composition of the obtained product was basically the same as that in Example 5. 0.0649 g remained after the reaction, and the lignin conversion rate was 56.7%.

[0046] Example 10 The solvent was prepared by mixing Nafion 117 solution, ethanol, and deionized water in a volume ratio of 3:40:40 and sonicating for 30 min. 0.05 g of the CuO / Cu prepared in Example 1 was then used. 0.92 Co 2.08 O4-1 nanocatalyst was dispersed in 1.5 mL of the solvent and sonicated for 10 min to obtain a catalyst dispersion. Nickel foam pretreated with acetone, ethanol, and deionized water was then sprayed onto the obtained catalyst dispersion, resulting in a catalyst loading of approximately 5.56 g / L. An H-type electrolytic cell was used, with the aforementioned catalyst-supported nickel foam as the working electrode and a graphite rod as the counter electrode. The anolyte was 50 mL of a solution containing 0.15 g of enzymatically hydrolyzed lignin. KOH solution, cathode electrolyte is 50 mL with a concentration of 1 KOH solution. At 25°C The reaction was stirred at a current density for 18 hours. After the reaction was completed, the reaction solution was neutralized and filtered. Unreacted solid residue was collected, washed, dried and weighed. The filtrate was extracted with dichloromethane and the organic phase was subjected to GC-MS qualitative analysis. The composition of the obtained product was basically the same as that in Example 5. 0.0416 g remained after the reaction, and the lignin conversion rate was 72.3%.

[0047] Example 11 The solvent was prepared by mixing Nafion 117 solution, ethanol, and deionized water in a volume ratio of 3:40:40 and sonicating for 30 min. 0.05 g of the CuO / Cu prepared in Example 1 was then used. 0.92 Co 2.08 O4-1 nanocatalyst was dispersed in 1.5 mL of the solvent and sonicated for 10 min to obtain a catalyst dispersion. Nickel foam pretreated with acetone, ethanol, and deionized water was then sprayed onto the obtained catalyst dispersion, resulting in a catalyst loading of approximately 5.56 g / L. An H-type electrolytic cell was used, with the aforementioned catalyst-supported nickel foam as the working electrode and a graphite rod as the counter electrode. The anolyte was 50 mL of electrolyte containing 0.15 g of enzymatically hydrolyzed lignin. KOH solution, cathode electrolyte 50 mL 1 KOH solution. At 25°C The reaction was stirred at a current density for 24 h. After the reaction was completed, the reaction solution was neutralized and filtered. Unreacted solid residue was collected, washed, dried and weighed. The filtrate was extracted with dichloromethane and the organic phase was subjected to GC-MS qualitative analysis. The composition of the obtained product was basically the same as that in Example 5. 0.0394 g remained after the reaction, and the lignin conversion rate was 73.7%.

[0048] Example 12 The solvent was prepared by mixing Nafion 117 solution, ethanol, and deionized water in a volume ratio of 3:40:40 and sonicating for 30 min. 0.05 g of the CuO / Cu prepared in Example 1 was then used. 0.92 Co 2.08 O4-1 nanocatalyst was dispersed in 1.5 mL of the solvent and sonicated for 10 min to obtain a catalyst dispersion. Nickel foam pretreated with acetone, ethanol, and deionized water was then sprayed onto the above catalyst dispersion, resulting in a catalyst loading of approximately 5.56%. An H-type electrolytic cell was used, with the aforementioned catalyst-supported nickel foam as the working electrode and a graphite rod as the counter electrode. The anolyte was 50 mL of a solution containing 0.15 g of enzymatically hydrolyzed lignin. KOH solution, cathode electrolyte is 50 mL with a concentration of 1 KOH solution. At 50 The reaction was stirred at the current density for 6 h. After the reaction was completed, the reaction solution was neutralized and filtered. Unreacted solid residue was collected, washed, dried and weighed. The filtrate was extracted with dichloromethane and the organic phase was subjected to GC-MS qualitative analysis. The composition of the obtained product was basically the same as that in Example 5. 0.0405 g remained after the reaction, and the lignin conversion rate was 73%.

[0049] Comparative Example 3 A solvent was prepared by mixing Nafion 117 solution, ethanol, and deionized water at a volume ratio of 3:40:40 and sonicating for 30 min. 0.05 g of the Co3O4 nanocatalyst prepared in Comparative Example 1 was dispersed in 1.5 mL of this solvent and sonicated for 10 min to obtain a catalyst dispersion. Nickel foam pretreated with acetone, ethanol, and deionized water was then sprayed onto the above-obtained catalyst dispersion, resulting in a catalyst loading of approximately 5.56 g. An H-type electrolytic cell was used, with the aforementioned catalyst-supported nickel foam as the working electrode and a graphite rod as the counter electrode. The anolyte was 50 mL of a solution containing 0.15 g of enzymatically hydrolyzed lignin. KOH solution, cathode electrolyte is 50 mL with a concentration of 1 KOH solution. At 25°C The reaction was stirred at a certain current density for 12 h. After the reaction, the electrolyte was neutralized with hydrochloric acid and centrifuged. The supernatant was extracted with dichloromethane, and the organic phase was qualitatively analyzed using an Agilent 7890B-7000C gas chromatograph-tandem mass spectrometer. (See also...) Figure 5 The gas chromatography-mass spectrometry (GC-MS) results showed that the liquid products obtained within the detection range were mainly long-chain alkanes, with only a small amount of aromatic compounds detected, namely 4-ethylbenzaldehyde, 2,5-di-tert-butylphenol, and 3,5-diisopropylphenol. After neutralizing the reaction solution, the unreacted solid residue was collected, washed, dried, and weighed. 0.0632 g remained after the reaction, indicating a lignin conversion rate of 57.9%. In summary, when using the single Co3O4 nanomaterial prepared in the comparative example as a catalyst for the enzymatic hydrolysis of lignin, its conversion efficiency was significantly lower than that of the catalyst in Example 1. The presumed reason is that single Co3O4 lacks the bimetallic synergistic electronic effect between Cu and Co, resulting in a low surface oxygen vacancy concentration and lattice oxygen mobility, making it difficult to effectively activate the CO ether bonds in lignin. Simultaneously, the Co3O4 surface has a single type of active sites, resulting in weak adsorption capacity for complex lignin macromolecules, and it is prone to aggregation or surface reconstruction during the reaction, reducing the effective active area and thus lowering the catalytic cracking performance.

[0050] Comparative Example 4 A solvent was prepared by mixing Nafion 117 solution, ethanol, and deionized water at a volume ratio of 3:40:40 and sonicating for 30 min. 0.05 g of the CuO nanocatalyst prepared in Comparative Example 2 was dispersed in 1.5 mL of this solvent and sonicated for 10 min to obtain a catalyst dispersion. Nickel foam pretreated with acetone, ethanol, and deionized water was then sprayed onto the above catalyst dispersion, resulting in a catalyst loading of approximately 5.56 g. An H-type electrolytic cell was used, with the aforementioned catalyst-supported nickel foam as the working electrode and a graphite rod as the counter electrode. The anolyte was 50 mL of a solution containing 0.15 g of enzymatically hydrolyzed lignin. KOH solution, cathode electrolyte is 50 mL with a concentration of 1 KOH solution. At 25°C The reaction was stirred at a certain current density for 12 h. After the reaction, the electrolyte was neutralized with hydrochloric acid and centrifuged. The supernatant was extracted with dichloromethane, and the organic phase was qualitatively analyzed using an Agilent 7890B-7000C gas chromatograph-tandem mass spectrometer. (See also...) Figure 6The gas chromatography-mass spectrometry (GC-MS) chromatogram showed that long-chain alkanes were the main component of the liquid product obtained within the detection range, with extremely low levels of aromatic compounds; only 2,5-di-tert-butylphenol was detected. After neutralizing the reaction solution, the unreacted solid residue was collected, washed, dried, and weighed. 0.0729 g remained after the reaction, indicating a lignin conversion rate of 51.4%. This demonstrates that the conversion efficiency of lignin catalyzed by the single CuO nanomaterial prepared in the comparative example was significantly lower than that of CuO / Cu... 0.92 Co 2.08 O4-1 catalyst. This is because Cu in single CuO is mainly in the form of Cu... 2+ While existing in this form, CuO has limited redox cycling capacity, making it difficult to continuously provide highly reactive oxygen species to break lignin C-C bonds and ether bonds. Simultaneously, the excessively strong Lewis acidity of the CuO surface easily induces non-selective condensation, generating coke byproducts that cover active sites and inhibit the formation of target products. Furthermore, CuO / Cu... 0.92 Co 2.08 The introduction of Co into the O4 catalyst modulates the electronic environment of Cu, leading to the formation of Cu. + / Cu 2+ With Co 2+ / Co 3+ The reversible redox pair significantly enhances the lattice oxygen migration rate and the regeneration capacity of reactive oxygen species, thereby greatly improving the catalytic depolymerization efficiency.

[0051] As shown in Table 1, from the effective examples 5-12 and comparative examples 3-4, according to the technical solution of the invention, adjusting the raw material ratio, selecting a suitable dispersant, or changing the reaction time and current density can all achieve the electrocatalytic conversion of lignin and obtain aromatic chemical products.

[0052] Table 1. Electrocatalytic conversion reaction conditions and conversion rates of Co-Cu spinel nanocatalyst materials prepared in Examples 1-12 and Comparative Examples 3-4 Verification Example 1 Electrochemical performance tests were conducted on the Co-Cu spinel nanocatalyst materials prepared in Examples 1-4 and the catalyst materials prepared in Comparative Examples 1-2 to examine their performance in the model compound 2-phenoxyphenylethanol (PPE). Electrochemical performance tests were performed on a GamryInterface 1010 electrochemical workstation using a traditional three-electrode system. A spectroscopically pure graphite rod (99.999% purity) was used as the counter electrode, and Hg / HgO was used as the reference electrode. The working electrode was prepared using a drop-coating method, mixing Nafion 117 solution, ethanol, and deionized water in a volume ratio of 3:40:40 and sonicating for 30 min to obtain the solvent. 0.05 g of the CuO nanocatalyst prepared in Comparative Example 2 was dispersed in 1.5 mL of this solvent and sonicated for 10 min to obtain the catalyst dispersion. Nickel foam pretreated with acetone, ethanol, and deionized water was sprayed onto the above catalyst dispersion, resulting in a catalyst loading of approximately 5.56 g. .

[0053] Electrochemical performance tests were performed in a 1 mmol PPE KOH electrolyte solution. Polarization curves were measured using linear sweep voltammetry, with the reaction starting at 0 V and ending at 2 V. The rate was scanned up to 1 V. The electrocatalytic activity of the catalyst was determined in a standard three-electrode system. To eliminate the potential gain effect of Pt on the catalyst, the auxiliary electrode was replaced with a spectroscopically pure graphite rod.

[0054] Table 2 Electrochemical performance test results of Examples 1-4 and Comparative Examples 1-2 The electrochemical test results are shown in Table 2. In the presence of organic substrates (represented by PPE), the polarization curves of all catalysts generally shifted towards lower potentials, indicating that the anolyte current has shifted from the traditional oxygen evolution reaction (OER) competing channel to the substrate oxidation channel. Figure 7 As shown, when the molar ratio of Co to Cu is 1:2 (i.e., the sample prepared in Example 1), it exhibits the lowest onset potential and the highest current response. This result indicates that the introduction of Cu forms a CuO / Cu matrix. 0.92 Co 2.08 The O4 heterointerface generates abundant Cu-O-Co bridging active sites. This indicates that this specific ratio is most favorable for substrate-related electron transfer sequences within the reaction potential window, macroscopically achieving a "conduction" effect on the anodic reaction pathway and laying the kinetic foundation for subsequent highly selective bond breaking. Further Tafel analysis reveals improvements in the rate-controlling steps, such as... Figure 8 As shown, the Tafel slope of the catalyst in Example 1 is 75. The efficiency was significantly lower than that of the comparative catalyst, indicating that the construction of the heterointerface effectively optimized the electron transfer efficiency in the rate-controlling step. Particularly noteworthy is the fact that... Figure 9 As shown, the catalyst in Example 1 was at 10 The required overpotential at the current density is only 134 mV, which is lower than that of the comparative example, and this advantage is more pronounced in the high current density region. These results fully demonstrate that the present invention, by constructing CuO / Cu... 0.92 Co 2.08 The O4 heterogeneous interface and optimized Co / Cu ratio significantly improved the substrate oxidation kinetics of the catalyst, providing strong experimental evidence for the superiority of the technical solution of this invention in the field of lignin electrocatalytic conversion.

[0055] In a standard H-type electrolyzer, the electrocatalytic depolymerization performance of Example 1 on the model compound 2-phenoxy-1-phenylethanol (PPE) was systematically evaluated. HPLC chromatograms ( Figure 3 a) shows that the main products of PPE depolymerization are benzaldehyde and phenol, confirming C α –C β Selective bond breaking. Electrocatalytic depolymerization exhibits a volcanic eruption-like trend. Figure 3 (b) Under optimal current conditions, 130 mA achieved a PPE conversion rate of 88% after 6 h of electrolysis, with benzaldehyde and phenol yields of 53% and 27%, respectively. Further increasing the current intensifies competition in the oxygen evolution reaction (OER) and limits mass transfer, thus reducing conversion efficiency. The system constructed in this invention achieves efficient bond-breaking conversion of PPE and scale-up of the target product under alkaline and mild conditions, demonstrating promising application prospects.

[0056] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A method for preparing a Co-Cu spinel nanocatalyst with a heterogeneous interface, characterized in that... The following steps are included: (1) Dissolve potassium cobalt cyanide in deionized water to prepare solution A, and dissolve copper acetate and sodium citrate in deionized water to prepare solution B; add solution A dropwise to solution B under magnetic stirring, stir and mix evenly, and allow to stand at room temperature for co-precipitation reaction. After the reaction is completed, wash and centrifuge, and dry the precipitate to obtain copper-cobalt Prussian blue analog precursor; the molar ratio of copper acetate to potassium cobalt cyanide is (3-1):(1-3), and the sodium citrate is used as a complexing agent, and the amount of sodium citrate used is 5 mmol when the total molar amount of copper acetate and potassium cobalt cyanide is 15 mmol. (2) Grind the copper-cobalt Prussian blue analog precursor obtained in step (1) into powder, place it in a muffle furnace and calcine it at low temperature in air atmosphere, raise the temperature to 300-500℃ at a rate of 1-3℃ / min and hold for 1-3 h, and after the reaction is completed, cool it naturally to room temperature to obtain Co-Cu spinel nanocatalyst with heterostructure interface.

2. The method for preparing a Co-Cu spinel nanocatalyst with a heterogeneous interface according to claim 1, characterized in that: In step (1), the molar volume ratio of potassium cobalt cyanide to deionized water in solution A is (2-10) mmol:50 mL, and the molar volume ratio of copper acetate to deionized water in solution B is (10-2) mmol:50 mL; the molar ratio of copper acetate to potassium cobalt cyanide is 2:1; the drying is carried out at 65-120℃ for 24-32 h.

3. The method for preparing a Co-Cu spinel nanocatalyst with a heterogeneous interface according to claim 2, characterized in that: The molar volume ratio of potassium cobalt cyanide to deionized water in solution A is 5 mmol: 50 mL; the molar volume ratio of copper acetate to deionized water in solution A is 10 mmol: 50 mL; the drying is carried out at 80 °C for 24 h.

4. The method for preparing a Co-Cu spinel nanocatalyst with a heterogeneous interface according to claim 1, characterized in that: The coprecipitation reaction in step (1) is to let it stand for 24 hours at room temperature; the washing and centrifugation is to wash with deionized water and anhydrous ethanol in sequence and then centrifuge, repeating the washing and centrifugation operation 3 to 5 times.

5. The method for preparing a Co-Cu spinel nanocatalyst with a heterogeneous interface according to claim 1, characterized in that: The calcination in step (2) involves heating to 350°C at a rate of 1°C / min and holding for 2 hours.

6. A Co-Cu spinel nanocatalyst with a heterogeneous interface prepared by the preparation method according to any one of claims 1-5, characterized in that: The Co-Cu spinel nanocatalyst with heterogeneous interfaces is a nanocube morphology assembled from nanoparticles, with CuO and CuO / Cu forming inside. 0.92 Co 2.08 A heterogeneous interface structure with O4 coexistence; this heterogeneous interface structure constructs Co through a bimetallic synergistic effect between Co and Cu. 2+ / Co 3+ With Cu + / Cu 2+ Two redox pairs are used to enhance the lattice oxygen migration rate and the regeneration capacity of reactive oxygen species.

7. The Co-Cu spinel nanocatalyst with a heterogeneous interface according to claim 6, characterized in that: In the Co-Cu spinel nanocatalyst, the molar ratio of Co to Cu is (1-3):(3-1).

8. The Co-Cu spinel nanocatalyst with a heterogeneous interface according to claim 7, characterized in that: In the Co-Cu spinel nanocatalyst, the molar ratio of Co to Cu is 2:

1.

9. The application of the Co-Cu spinel nanocatalyst with heterogeneous interface according to claim 6 in lignin electrocatalysis, characterized in that: The application is carried out according to the following steps: a Co-Cu spinel nanocatalyst with a heterogeneous interface is loaded onto pretreated nickel foam as the anode working electrode, and a graphite rod is used as the cathode counter electrode; at a concentration of 1... A potassium hydroxide solution was used as the cathode electrolyte, and lignin or a lignin model compound was added to a solution of 1% concentration. A potassium hydroxide solution was used as the anolyte; the anolyte and cathode electrodes were immersed in the corresponding anolyte and cathode electrolytes, respectively, and a current density was applied while stirring was started to carry out the electrocatalytic reaction; the Cu-O-Co heterostructure in the Co-Cu spinel nanocatalyst was used to promote the selective breaking of CO and CC bonds in lignin or lignin model compounds to generate aromatic monomer products; the mass ratio of the lignin or lignin model compound to the Co-Cu spinel nanocatalyst with the heterostructure was 3:

1.

10. The application according to claim 9, characterized in that: The lignin model compound is 2-phenoxy-1-phenylethanol; when 2-phenoxy-1-phenylethanol is used as a substrate for electrocatalytic conversion, at 30... At the specified current density, the conversion rate of 2-phenoxy-1-phenylethanol reached over 88%, and the yield of benzaldehyde reached over 53%.