A partition-type crystal growth furnace structure and growth method for suppressing cracking in large-sized lanthanide halide crystals
By introducing a synergistic design of structures such as baffles, radiation-shaping heat shields, and thermally conductive cores into the VB crystal growth furnace, the contradiction between temperature gradient and stress slow cooling during the growth of large-size lanthanide halide crystals was resolved, achieving stable crystal growth and high integrity.
Patent Information
- Application Number
- CN202611252453.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to simultaneously balance the large temperature gradient at the pore opening of the separator and the slow cooling with low stress after solidification during the growth of large-size lanthanide halide crystals (VB), leading to easy crystal cracking and difficulty in maintaining stable control of the solid-liquid interface morphology.
By designing a synergistic structure in a traditional VB crystal growth furnace, including baffles, an upper radiation shaping heat shield, a lower radiation shaping heat shield, a lower heater, a concentric annular heat-spreading cavity, surface metallized quartz support components, and a thermally conductive inner core, a stable temperature gradient and a uniform thermal field are formed, ensuring a temperature gradient during the crystal development stage and low stress during the cooling stage.
It significantly reduces the tendency of large-size lanthanide halide crystals to crack during growth, cooling and subsequent processing, increases the length of transparent constant diameter segments and crystal integrity, and improves the yield of finished products.
Smart Images

Figure CN123108718A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of transparent scintillation crystal growth technology, specifically relating to a partition-type crystal growth furnace structure and growth method for suppressing cracking of large-size lanthanide halide crystals. Background Technology
[0002] Lanthanide halide crystals are important inorganic scintillation crystal materials, with LaBr3, LaBr3:Ce, CeBr3, and LaCl3:Ce being representative examples. They possess high light output, fast decay, good energy resolution, and good time response performance, making them valuable for applications in nuclear radiation detection, medical imaging, security and counter-terrorism, space exploration, nuclear facility monitoring, industrial non-destructive testing, and high-energy physics experiments. As applications demand increasingly higher detection efficiency, energy resolution, time response, and engineering reliability, lanthanide halide crystals are gradually evolving towards larger sizes, lower defects, and higher machinability.
[0003] The vertical Bridgman process, or VB process, is one of the important methods for preparing lanthanide halide scintillation crystals. This method typically involves sealing the lanthanide halide raw material in a quartz ampoule or other growth container, melting the raw material in a high-temperature zone at the top, and then slowly lowering the temperature field of the growth container relative to the furnace body, allowing the melt to pass through a temperature gradient zone and gradually solidify to form a crystal. However, for large-sized lanthanide halide crystals, due to their generally high hygroscopicity, sensitivity to thermal expansion and mechanical strength, and complex heat transfer between the crystal and the growth container, problems easily arise during VB growth, such as crystal cracking, short, defect-free transparent isodiameter segments, localized residual stress concentration, breakage during cutting and processing, and unstable performance after encapsulation.
[0004] Existing crystal growth furnaces typically control the temperature field by using insulation layers, multi-zone heaters, furnace baffles, cold-end heat dissipation structures, or overall annealing processes. However, for large-size lanthanide halide crystals, relying solely on overall temperature programming, conventional multi-zone heating, or standard insulation structures is insufficient to simultaneously meet the requirements of stable crystal growth, equal-diameter growth interface control, and low-stress slow cooling after solidification. Specifically:
[0005] 1. During the crystal growth and shoulder formation stages, a large axial temperature gradient needs to be maintained near the septum orifice or the solid-liquid interface to achieve stable crystal growth, interface advancement, and orientation selection. During the constant-diameter growth stage, the radial temperature difference around the crucible or ampoule needs to be reduced to avoid overcooling at the solid-liquid interface edge and reduce radial thermal stress. When the crystal solidifies and enters the lower region, it needs to be cooled slowly to avoid thermal stress and crack propagation caused by excessive temperature difference or rapid cooling. In traditional VB crystal growth furnaces, septums are usually used to isolate hot and cold zones, creating a large temperature gradient near the central through-hole of the septum. However, if a low-gradient slow cooling zone is set directly below the septum, it is easy to weaken the large temperature gradient near the central through-hole of the septum, leading to instability of the solid-liquid interface in the crystal growth zone, interface depression, or interface position drift. If only a large temperature gradient is maintained near the septum, the solidified crystal is prone to thermal shock and cracking after entering the lower cold end. Therefore, traditional furnace designs that employ either "heating at the top and cooling at the bottom" or "overall low-gradient slow cooling" are difficult to balance large temperature gradient crystal attraction, interface morphology maintenance, and low-stress slow cooling.
[0006] 2. The seeding stability of lanthanide halide crystal VB growth depends not only on the furnace temperature zone settings but also on the axial thermal boundary at the lower end of the growth container. Traditional quartz supports or ordinary ceramic supports mainly provide mechanical support, with limited thermal conductivity and uncontrollable surface radiation absorption and re-radiation characteristics. During the seeding stage, if a stable axial thermal channel is lacking at the lower end of the growth container, heat cannot be continuously transferred or released along the growth axis, easily leading to local overheating at the seed crystal end, fluctuations in the axial temperature gradient at the solid-liquid interface, seed crystal position drift, or unstable initial crystal morphology. For large-sized lanthanide halide crystals, the aforementioned axial thermal boundary instability further amplifies interface curvature changes and thermal stress concentration, increasing the risk of seeding failure, initial cracks, or subsequent cracking in the constant-diameter section.
[0007] 3. In the actual growth of large-size lanthanide halide crystals (VB), although the lower heater can raise the ambient temperature around the solidified crystal and thus reduce cooling stress, if its radiant heat flow acts directly upwards near the central through-hole of the partition, it will weaken the temperature gradient formed by the partition, and may even lead to the drift of the solid-liquid interface and loss of control of the interface curvature.
[0008] 4. During the growth of large-size lanthanide halide crystals, the axisymmetric temperature distribution around the crucible or ampoule is easily affected by multiple factors, including eccentricity, localized heat dissipation, thermal conductivity of the support components, cold-end structure, and atmosphere flow, resulting in a circumferential temperature difference. This circumferential temperature difference can further induce localized tensile and shear stresses within the crystal, increasing the risk of crystal cracking and subsequent breakage during processing.
[0009] 5. The existing support is made of quartz. Although it has good high-temperature stability and ease of processing, its surface radiation absorption and re-radiation characteristics are uncontrollable, easily becoming non-design thermal boundaries and causing deviations between the actual and designed thermal fields. Especially below the partition and in the crystal-driving support area, the support often simultaneously serves as the support and guide for the growth container, and its surface radiation characteristics directly affect the heat exchange between the lower heater and the growth container. If the support surface is not treated, localized heat absorption, localized re-radiation, or localized thermal short circuits may occur, further exacerbating the non-uniformity of the thermal field in the crystal-driving area and around the solidified crystal.
[0010] To address the aforementioned issues, existing technologies already offer solutions for cracking during lanthanum bromide crystal growth and temperature field control. For example:
[0011] Chinese patent application CN110592659A discloses a multi-crucible gradient condensation crystal growth apparatus and its method for growing large-size lanthanum bromide single crystals. The scheme reduces internal stress at the solid-liquid interface and alleviates cracking problems in large-size lanthanum bromide single crystals through a double heating layer and a central compensation thermal field. However, it primarily targets the overall compensation thermal field of multiple crucibles under static or quasi-static conditions, aiming to reduce the lateral temperature difference between crucibles and place them in a more uniform lateral temperature field. However, for single-crucible VB-down growth, the crucible needs to continuously pass through the central through-hole of the partition, experiencing a dynamically changing thermal environment. Existing multi-crucible overall compensation thermal field designs do not independently control the radiative thermal coupling on the upper and lower sides of the partition during the dynamic VB-down growth process, nor do they address the structural problem of the spatially adjacent and functionally contradictory large gradient region at the partition orifice and the lower slow-cooling region.
[0012] For example, Chinese patent CN107268068B discloses a method for preparing lanthanum bromide crystals using a fully enclosed crucible. This method designs a convex quartz cover plate to form a fully enclosed growth environment with the lanthanum bromide quartz crucible, and makes the solid-liquid interface slightly convex to facilitate stress release within the crystal. However, its interface control mainly relies on the convex cover plate structure inside the crucible, which is a static and passive interface control method. For the growth of large-size lanthanum bromide single crystals in VB, the optimal requirements for the solid-liquid interface morphology are not the same at different growth stages. A convex cover plate with a fixed curvature can only provide a single interface morphology constraint and cannot provide differentiated interface control at different growth stages. It is difficult to control the supercooling and radial temperature gradient at the edge of the solid-liquid interface of large-size crystals, which poses a risk of edge dendrite nucleation or grain boundary formation. In addition, the existing scheme does not involve the coordinated thermal field design between the partition, lower heater, upper radiation shaping hot screen, lower radiation shaping hot screen and cold zone slow cooling channel in the VB crystal growth furnace, nor does it pay attention to the influence of the lower support structure of the ampoule on the axial thermal stability during the crystal pulling stage.
[0013] For example, Chinese patent application CN107119315A discloses a method for preparing lanthanum cerium bromide crystals using a temperature-adjustable crystal growth apparatus. While it adapts the temperature field by adjusting the insulation material layer, it primarily addresses the issues of temperature field adaptation under static growth conditions and furnace replicability. It does not resolve the contradiction between high-gradient crystal attraction and low-stress slow cooling during the VB descent of large-size lanthanide halide crystals, nor does it disclose the radiation-shaping heat shield and axially guided heat-conducting core structure.
[0014] Therefore, although existing technologies have proposed ways to improve the growth quality of lanthanide halide crystals by compensating for the thermal field, optimizing the crucible structure, adjusting the insulation material layer, or performing post-crystal heat treatment, these solutions mainly focus on overall temperature field homogenization, crucible internal interface control, or static growth temperature field adaptation. They have not yet addressed the structural control of the radiative thermal coupling between the partition temperature gradient region and the lower slow cooling region during the VB descent process, nor have they addressed the non-axisymmetric cooling problem of the solidified crystal periphery by combining circumferential thermal homogenization and radial thermal insulation. Furthermore, they have not coordinated the design of the surface metallized quartz support and its internal thermally conductive core as key structures serving the axial thermal control during the crystallization stage. As a result, the growth of large-size lanthanide halide crystals (VB) presents technical problems such as easy cracking, difficulty in balancing the large temperature gradient at the partition orifice with low-stress slow cooling after solidification, difficulty in stabilizing the solid-liquid interface morphology, and disturbances in the temperature gradient at the partition orifice caused by the upper and lower thermal fields. Summary of the Invention
[0015] The purpose of this invention is to address the shortcomings of existing large-size lanthanide halide crystal VB growth processes, such as easy cracking, difficulty in balancing large temperature gradients at the diaphragm orifices with low-stress slow cooling after solidification, difficulty in maintaining stable control of the solid-liquid interface morphology, and disturbances to the temperature gradient at the diaphragm orifices caused by the upper and lower thermal fields. The invention provides a diaphragm-type crystal growth furnace structure that suppresses cracking in large-size lanthanide halide crystals.
[0016] The technical concept of this invention is as follows:
[0017] Analysis of existing technologies reveals that when growing large-size lanthanide halide crystals using a conventional VB crystal growth furnace, relying solely on the top heater, upper heater, lower heater, bottom heater, and ordinary insulation layer to create an axial temperature gradient is insufficient to achieve ideal crystal growth results, and the tendency for crystal cracking remains high. This is because cracking in large-size lanthanide halide crystals is not only related to the overall cooling rate but also closely related to the temperature gradient near the baffle orifice, the curvature of the solid-liquid interface, the radial temperature difference around the ampoule, the temperature abrupt change when the crystal enters the lower region after solidification, and the axial thermally conductive boundary at the support structure. If the temperature below the baffle is too low, the solidified crystal is prone to cracking due to cold-end thermal shock. Conversely, directly increasing the temperature below the baffle or setting up lower compensation heating can weaken the large temperature gradient near the baffle orifice due to upward radiation from the lower heat source, leading to unstable crystal growth, interface depression, or interface position drift. Therefore, to obtain large-size, low-defect, and high-integrity lanthanide halide crystals, it is necessary to simultaneously achieve large temperature gradient crystal attraction and growth, radiative heat flow shaping, low-stress slow cooling of solidified crystals, and axially symmetric isothermal cooling of the outer periphery of the crystal in the furnace structure.
[0018] Based on the above research and analysis, this invention, unlike traditional VB crystal growth furnaces, does not simply increase or decrease the temperature of a certain temperature zone. Instead, it integrates the partition, upper and lower radiative shaping hot screens, lower heater, bottom heater, concentric annular heat-spreading cavity, surface-metallized quartz support, and heat-conducting inner core into a single design. The partition is used to create a large temperature gradient near the central through-hole, suitable for crystal introduction and initial interface advancement. Both the upper and lower radiative shaping hot screens are used to restrict, weaken, or redirect the radiative heat flow from adjacent temperature zones into the vicinity of the partition opening. Their surface shape, radial spacing, axial position, shaping surface inclination angle, and material selection rules are consistent; the only difference is their opposite direction of action. The upper radiative shaping hot screen mainly controls the downward radiative heat flow from the high-temperature melting zone to below the partition opening, while the lower radiative shaping hot screen mainly controls the downward radiative heat flow from the lower slow-cooling zone to above the partition opening. The upward radiative heat flow decouples the temperature gradient near the diaphragm orifice from the compensating heating effect of the lower slow cooling zone. The concentric annular heat exchanger reduces the circumferential temperature difference and non-axisymmetric thermal disturbances around the growth vessel. The surface-metallized quartz support reduces the undesigned thermal boundary effects caused by heat absorption and re-radiation from ordinary quartz supports. The thermally conductive core inside the surface-metallized quartz support provides a stable thermal path along the crystal growth axis for the seed crystal segment or tapered crystal-guiding segment, enhancing axial thermal coupling and growth driving force during the crystal-guiding stage. Through the synergy of these structures, the large temperature gradient at the diaphragm orifice and the low-stress slow cooling after solidification can be balanced. While maintaining the large temperature gradient at the diaphragm orifice and the low curvature morphology of the solid-liquid interface, the solidified crystal is gradually cooled after entering the lower slow cooling zone, stabilizing and controlling the solid-liquid interface morphology. This avoids disturbances to the temperature gradient at the diaphragm orifice caused by the upper and lower thermal fields, thereby reducing the cracking tendency of large-sized lanthanide halide crystals during growth, cooling, and subsequent processing.
[0019] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0020] A partition-type crystal growth furnace structure for suppressing cracking of large-sized lanthanide halide crystals includes a furnace body and heating units, growth containers, upper radiation shaping heat shields, lower radiation shaping heat shields, surface metallized quartz support components, heat-conducting inner cores, partitions, and concentric annular heat-spreading cavities respectively disposed in the furnace body.
[0021] The furnace body is arranged vertically from top to bottom as follows: a high-temperature melting zone, a partition temperature gradient zone, and a lower slow cooling zone; the partition is located in the partition temperature gradient zone and has a central through hole; the top of the growth container is located in the high-temperature melting zone, and the bottom of the growth container passes through the central through hole and is located in the lower slow cooling zone; the bottom of the growth container is provided with a seed crystal segment or a conical crystal-guiding segment.
[0022] The upper radiative shaping heat screen is located above the partition and is used to regulate the downward radiative heat flow from the high-temperature melting zone to below the central through hole; the lower radiative shaping heat screen is located below the partition and is used to regulate the upward radiative heat flow from the lower slow cooling zone to above the central through hole; the upper and lower radiative shaping heat screens decouple the temperature gradient near the central through hole from the compensating heating effect of the lower slow cooling zone.
[0023] The surface-metallized quartz support is located below the growth container and connected to the bottom end of the growth container; the thermally conductive inner core is located inside the surface-metallized quartz support and is used to provide a stable axial thermal path to the bottom end of the growth container.
[0024] The concentric annular heat dissipation cavity is disposed on the outer periphery of the growth container and extends from the temperature gradient region of the partition below the partition to the lower slow cooling region; it is used to provide a uniform outer periphery thermal environment to the solidified crystal in the growth container and reduce the circumferential temperature difference and non-axisymmetric thermal disturbance on the outer periphery of the growth container.
[0025] The heating unit is used to provide the required reaction temperature to the high-temperature melting zone and the lower slow cooling zone, and to provide thermal compensation to the upper and lower ends of the growth vessel.
[0026] Further specified, the wall thickness of the growth container is 1.5mm to 8mm; the minimum inner diameter of the seed crystal segment or the conical crystal guide segment is 0.05 to 0.40 times the crystal diameter; and the cone angle of the conical crystal guide segment is 10° to 60°.
[0027] Further defined, the upper radiation shaping heat shield includes a partition shielding section, a radiation shaping section, and a transition section; the partition shielding section is located near the central through hole and is used to regulate the downward radiation heat flow from the high-temperature melting zone to below the central through hole; the radiation shaping section is located on the outer periphery of the growth container and is used to adjust the radial heat flow distribution near the solid-liquid interface; the transition section faces the high-temperature melting zone and is used to gradually transition the melt from the high-temperature melting zone to the partition temperature gradient zone.
[0028] Further specified, the diameter D1 of the central through hole, the outer diameter D2 of the growth container, and the inner diameter D of the furnace chamber of the furnace body are... f The radial distance g between the radiation shaping heat shield and the outer wall of the growth container, and the axial position h of the radiation shaping heat shield relative to the partition, satisfy the following:
[0029] The radial spacing g is 0.02 to 0.25 times D2; the axial position h is 0.05 to 0.50 times D2; D1 / D2 is 1.05 to 2.50; (D f -D2) / 2 is 0.05D2 to 1.20D2;
[0030] The tilt angle θ of the shaping surface of the radiation shaping section relative to the axis of the growth container is 10° to 80°; and the tilt angle θ decreases as the D1 / D2 ratio increases.
[0031] Further defined, the surface shape of the upper radiation shaping heat shield is annular, cylindrical, conical, inclined, stepped, arc-shaped, or composite surface shape; the composite surface shape is composed of any two or three of the inclined, arc-shaped, and stepped surfaces, or is composed of multiple similar surfaces with different geometric parameters in a continuous combination; the similar surfaces are inclined, arc-shaped, or stepped surfaces;
[0032] The surface shape of the upper radiation shaping heat shield is related to the inner diameter D of the furnace. f The outer diameter D2 of the growth container and the heat flow control requirements satisfy the following: when only axial shielding of the central through-hole is required, the surface shape of the upper radiative shaping heat shield is annular; when continuous axisymmetric shielding or guidance is required along the axial direction of the outer periphery of the growth container, the surface shape of the upper radiative shaping heat shield is cylindrical; when 0.05D2≤(D f When -D2) / 2≤0.25D2, the surface shape of the upper radiation shaping heat shield is inclined or conical; when 0.25D2<(D f When -D2) / 2≤0.60D2, the surface shape of the upper radiation shaping heat shield is a conical, arc-shaped, stepped, or cylindrical composite structure; when 0.60D2<(D f When -D2) / 2≤1.2D2, the surface shape of the upper radiation shaping heat shield is a composite surface structure;
[0033] The material of the upper radiation shaping heat shield is one or more of high-temperature resistant metals, high-temperature resistant alloys, and high-temperature resistant ceramic materials; wherein, the high-temperature resistant metal is one or more of molybdenum, tungsten, tantalum, niobium, rhenium, and platinum; the high-temperature resistant alloy is one or more of molybdenum-tungsten alloy, tungsten-rhenium alloy, molybdenum-rhenium alloy, tantalum-tungsten alloy, nickel-based high-temperature alloy, cobalt-based high-temperature alloy, and iron-chromium-aluminum alloy; and the high-temperature resistant ceramic material is one or more of silicon carbide, boron nitride ceramic, aluminum nitride ceramic, alumina ceramic, zirconium oxide ceramic, mullite ceramic, and magnesium oxide ceramic.
[0034] Further defined, the structure of the lower radiation shaping heat shield is the same as that of the upper radiation shaping heat shield, and is mirrored in the horizontal direction about the partition; for the lower radiation shaping heat shield, the partition shielding section is located near the central through hole, used to regulate the upward radiation heat flow from the lower slow cooling zone to the center through hole; the radiation shaping section is located on the outer periphery of the growth container, used to adjust the radial heat flow distribution near the solid-liquid interface; the transition section faces the lower slow cooling zone, used to allow the solidified crystal to gradually transition from the partition temperature gradient zone to the lower slow cooling zone.
[0035] Further defined, the concentric annular heat-spreading cavity comprises, from the inside out, an inner thermally conductive and heat-spreading layer, an annular buffer gap layer, and an outer thermal insulation layer; the inner thermally conductive and heat-spreading layer is close to the growth container; the thickness of the inner thermally conductive and heat-spreading layer is 2mm to 20mm, and the thickness increases with the increase of the crystal diameter; the thickness of the outer thermal insulation layer is 1 to 5 times the thickness of the inner thermally conductive and heat-spreading layer;
[0036] The inner heat-conducting and temperature-equalizing layer is made of one or more of molybdenum, tungsten, tantalum, boron nitride, silicon carbide, and high-temperature resistant alloy materials. The high-temperature resistant alloy materials include one or more of molybdenum-tungsten alloy, tungsten-rhenium alloy, molybdenum-rhenium alloy, tantalum-tungsten alloy, nickel-based high-temperature alloy, cobalt-based high-temperature alloy, and iron-chromium-aluminum alloy. The outer thermal insulation layer is made of one or more of alumina fiber, zirconium oxide fiber, mullite, boron nitride ceramic, alumina ceramic, aluminum silicate fiber, magnesium oxide ceramic, porous alumina ceramic, calcium oxide-stabilized zirconium oxide ceramic, and other high-temperature resistant insulation materials.
[0037] Further defined, the surface-metallized quartz support includes a quartz substrate and a metal film layer disposed on the surface of the quartz substrate; the metal film layer is used to reduce the undesigned thermal boundary disturbance caused by heat absorption and re-radiation on the surface of the quartz substrate; the metal film layer is a molybdenum film, tungsten film, platinum film, gold film, nickel film, tantalum film, or a composite film layer formed by various metals; the thickness of the metal film layer is 0.1 μm to 200 μm;
[0038] The thermally conductive core is made of one or more of the following materials: molybdenum, tungsten, tantalum, silicon carbide, aluminum nitride, boron nitride, aluminum oxide, sapphire, and high-temperature alloys; the diameter of the thermally conductive core is 2mm to 30mm.
[0039] Further defined, the heating unit includes a top heater, an upper heater, a lower heater, and a bottom heater; the top heater is located above the growth container and is used to provide thermal compensation to the upper end of the growth container; the bottom heater is located at the bottom of the growth container and is used to provide thermal compensation to the lower end of the growth container; the upper heater is located above the partition and is used to provide the required reaction temperature to the high-temperature melting zone; the lower heater is located below the partition and is used to provide the required reaction temperature to the lower slow cooling zone.
[0040] A lowering mechanism is provided on the outside of the furnace body. The lowering mechanism is connected to the growth container through a surface metallized quartz support and is used to drive the growth container to descend vertically inside the furnace body.
[0041] A method for growing large-size lanthanide halide crystals, formed by the aforementioned partition-type crystal growth furnace structure for suppressing cracking in large-size lanthanide halide crystals, includes the following steps:
[0042] Step 1: Load the lanthanide halide raw material into the growth container and seal it under vacuum or inert atmosphere;
[0043] Step 2: Place the sealed growth container inside the furnace. The top of the growth container is located in the high-temperature melting zone, and the bottom of the growth container passes through the central through hole and is located in the lower slow cooling zone. At the same time, the seed crystal segment or conical crystal-guiding segment at the bottom of the growth container is connected to the top of the surface metallized quartz support.
[0044] Step 3: The melting temperature of the lanthanide halide feedstock is T. m The heating unit is activated to raise the temperature of the high-temperature melting zone to T. m + (5℃~100℃) to fully melt the raw materials in the growth container; the upper temperature of the temperature gradient zone of the partition is T. m ~T m +50℃, the lower end temperature of the temperature gradient zone of the partition is T. m - (10℃~120℃); The upper temperature of the lower slow cooling zone is T m - (50℃~200℃), the lower end temperature of the lower slow cooling zone is T m - (150℃~350℃);
[0045] Step 4: Adjust the size of the upper and lower radiation shaping hot screens to form a temperature gradient zone near the central through hole; at the same time, adjust the output power of the heating unit so that the axial temperature gradient of the partition temperature gradient zone is 5℃ / cm~80℃ / cm, and the temperature difference between the central and edge regions of the solid-liquid interface in the growth container is controlled within 20℃.
[0046] Step 5: The control unit controls the lowering mechanism to drive the growth container to descend relative to the furnace body, so that the melt in the growth container enters the temperature gradient zone of the partition plate from the high temperature melting zone. Crystal introduction, shoulder formation and initial solidification are completed near the central through hole of the partition plate, and crystals are gradually formed.
[0047] Step 6: As the growth container continues to descend, the solidified crystals enter the lower slow cooling zone, where they undergo circumferential homogenization and low-stress slow cooling under the combined action of the concentric annular heat exchanger, heating unit, and surface metallized quartz support; at the same time, the axial heat-conducting boundary of the seed crystal segment or conical crystal guide segment is stabilized by the thermally conductive inner core.
[0048] Step 7: After the crystal has completely solidified, perform heat preservation annealing in the lower slow cooling zone. The annealing temperature is 150℃~350℃ lower than the melting temperature of the lanthanide halide raw material, and the heat preservation time is 12h~72h. Then, slowly reduce the temperature to 50℃~120℃ or room temperature at a cooling rate of 5℃ / h~30℃ / h. Stop heating and remove the growth container to obtain large-sized lanthanide halide crystals.
[0049] A large-size lanthanide halide crystal is prepared using the aforementioned large-size lanthanide halide crystal growth method, and the diameter of the large-size lanthanide halide crystal is 38 mm or more.
[0050] Application of large-size lanthanide halide crystals as crystal elements in the fabrication of lanthanide halide scintillation crystal detectors.
[0051] Compared with existing technologies, the advantages of this invention are: The invention utilizes a heating unit, growth container, upper radiation shaping heat shield, lower radiation shaping heat shield, surface metallized quartz support, heat-conducting inner core, partition, and concentric annular heat-spreading cavity within the furnace body. Through multi-structure synergy, it avoids the weakening of the crystal-attracting temperature gradient near the central through-hole by upward radiation from the lower heat source, reduces the circumferential temperature difference and asymmetric cooling disturbance around the growth container, and ensures that the axial temperature gradient of the central through-hole of the partition, the radial temperature difference at the solid-liquid interface, and the lower slow-cooling temperature gradient are all within a controlled range. This improves the repeatability of the solid-liquid interface position and morphology during the crystal-attracting stage and reduces the cold-end thermal shock when the solidified crystal enters the lower region. It significantly reduces the cracking tendency of large-size lanthanide halide crystals during growth, cooling, cutting, and subsequent packaging, ultimately increasing the length of the transparent constant-diameter section, crystal integrity, and subsequent processing yield. Specifically, this is manifested in:
[0052] 1. The furnace body of this invention is vertically divided into a high-temperature melting zone, a partition temperature gradient zone, and a lower slow cooling zone. The high-temperature melting zone not only provides the main melting heat source but also compensates for heat loss at the upper end of the melt within the growth container, ensuring sufficient melting and stable heat preservation of the raw materials, and providing ample melt supply to the solid-liquid interface. In the partition temperature gradient zone, a large local temperature gradient is formed at the central through-hole, and the upper / lower radiative shaping heat shields respectively block the upward / downward radiative heat flow, preventing direct radiation interference from the upper and lower temperature zones. In the lower slow cooling zone, the solidified crystal is compensated with heating, and a concentric annular heat exchanger cavity achieves slow cooling, preventing excessively rapid cooling and the generation of thermal stress. Through the synergistic effect of these three thermal field structures, the fundamental contradiction of achieving both large gradient crystal growth and low-stress slow cooling in conventional furnaces is resolved, effectively suppressing cracking of large-size lanthanide halide crystals and improving their performance.
[0053] 2. The structure of the lower radiation shaping heat shield of this invention is the same as that of the upper radiation shaping heat shield, both containing a partition shielding section, a radiation shaping section, and a transition section; and they are mirror images of each other in the horizontal direction of the partition. The partition shielding section of the upper radiation shaping heat shield is close to the central through hole, directly blocking the downward radiation from the high-temperature melting zone to the area below the central through hole, preventing the high heat flow from weakening the axial temperature gradient at the orifice; the partition shielding section of the lower radiation shaping heat shield blocks the upward radiation heat flow generated by the lower slow cooling zone, so that the lower compensating heating heat will not disturb the temperature gradient field near the orifice in the opposite direction. The radiation shaping sections of the two radiation shaping heat shields are respectively surrounding the outer periphery of the growth container, and by adjusting the radial heat flow distribution near the solid-liquid interface, the radial temperature at the interface is made more uniform; at the same time, the transition section of the upper radiation shaping heat shield allows the melt to gradually enter the partition temperature gradient zone from the high-temperature melting zone, and the transition section of the lower radiation shaping heat shield allows the solidified crystal to gradually enter the lower slow cooling zone from the partition temperature gradient zone, avoiding sudden temperature changes. The structure and arrangement of the lower and upper radiation-shaping thermal shields enable complete thermal decoupling between the large temperature gradient near the central through-hole of the partition and the compensating heating in the lower slow-cooling zone. This thermal decoupling design not only stabilizes the interface driving force and morphology controllability during the crystal-leading stage but also avoids cold-end thermal shock and stress concentration caused by sudden temperature changes, thus suppressing cracking in large-size lanthanide halide crystals.
[0054] 3. In this invention, the diameter D1 of the central through hole, the outer diameter D2 of the growth container, and the inner diameter D of the furnace chamber of the furnace body are... f The radial distance *g* between the radiation-shaping heat shield and the outer wall of the growth container, and the axial position *h* of the radiation-shaping heat shield relative to the partition, satisfy the following conditions: the radial distance *g* is 0.02–0.25 times D2; the axial position *h* is 0.05–0.50 times D2; and D1 / D2 is 1.05–2.50. f -D2) / 2 is 0.05D2 to 1.20D2; the tilt angle θ of the shaping surface of the radiation shaping section relative to the axis of the growth container is 10° to 80°; and the tilt angle θ decreases as the ratio of D1 / D2 increases. The multi-geometric parameter collaborative design of the radiation shaping heat shield ensures, on the one hand, that the radiation heat transfer between the radiation shaping heat shield and the growth container is within the optimal range, ensuring that the radiation shaping effect of the heat shield is precisely applied to the region near the solid-liquid interface, so that the heat flow control effect is precisely presented, thereby avoiding interface position drift; on the other hand, it ensures that the solid-liquid interface can maintain a low curvature and flat shape under different furnace configurations, avoiding distortion of the interface morphology, thereby improving the quality of large-size lanthanide halide crystals.
[0055] 4. The concentric annular homogenizing cavity of this invention consists of, from the inside out, an inner heat-conducting homogenizing layer, an annular buffer gap layer, and an outer thermal insulation layer. The inner heat-conducting homogenizing layer is close to the growth container, which can homogenize the circumferential temperature difference caused by uneven circumferential temperature in the furnace or eccentricity of the container. The annular buffer gap layer provides a buffer space. The outer thermal insulation layer reduces radial heat loss, providing a gentle cooling environment for the solidified crystal. In addition, the thickness of the inner layer increases with the crystal diameter, ensuring the radial heat conduction capacity required for large-sized crystals. This eliminates the circumferential temperature difference and asymmetric thermal disturbances around the growth container, achieving axisymmetric homogenization cooling. This fundamentally reduces radial thermal stress concentration and significantly lowers the risk of large-sized crystals cracking due to radial temperature differences.
[0056] 5. The surface-metallized quartz support of this invention includes a quartz substrate and a metal film layer disposed on the surface of the quartz substrate. The metal film layer has high reflectivity, which significantly reduces the absorption and re-emission of thermal radiation by the quartz, eliminates the undesigned thermal boundary disturbance caused by the support structure, and significantly improves the controllability and repeatability of the overall thermal field. The thermally conductive core located inside the surface-metallized quartz support provides a stable low thermal resistance thermal conduction path along the crystal growth axis for the seed crystal segment or tapered crystal-guiding segment at the bottom of the growth container, enhancing the thermal extraction efficiency of the seed crystal end. In addition, a large gradient is maintained above the partition through two radiation-shaping thermal screens, and the thermally conductive core provides a heat dissipation outlet below, forming a complete axial heat flow loop. The thermally conductive core and the partition work together to greatly improve the axial thermal coupling capability and thermal driving force during the crystal-guiding stage, ensuring that the seed crystal segment is successfully guided and stably transitions to constant diameter growth, thereby improving the crystal-guiding success rate.
[0057] 6. The heating unit of this invention includes a top heater, an upper heater, a lower heater, and a bottom heater; the upper and lower heaters independently control the reference temperatures of the high-temperature zone and the slow-cooling zone, respectively, and together with two radiation-shaping heat shields and a concentric annular heat-spreading cavity, realize a dual temperature field control strategy of passive structural shaping and active heating closed loop; the top heater compensates for the temperature loss caused by radiation heat dissipation at the upper end of the melt, preventing crystallization or component volatilization on the melt surface; the bottom heater compensates for the overcooling caused by excessive heat passing through the heat-conducting inner core heat-conducting heat at the lower end of the crystal, preventing the crystal from cracking due to excessively low bottom temperature.
[0058] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0059] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0060] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:
[0061] Figure 1 This is a schematic diagram illustrating the structure and quantitative relationship of a partition-type VB crystal growth furnace for suppressing cracking of large-sized lanthanide halide crystals according to the present invention; wherein, 1-top heater; 2-upper heater; 3-growth container; 4-upper radiation shaping heat shield; 5-lower radiation shaping heat shield; 6-lower heater; 7-surface metallized quartz support; 8-thermal conductive core; 9-insulation frame; 10-partition; 11-concentric annular heat dissipation cavity; 12-bottom heater;
[0062] Figure 1 The crystal diameter D, the outer diameter D2 of the growth container 3, the wall thickness t of the growth container 3, the diameter D1 of the central through hole, and the inner diameter D of the furnace chamber are also indicated. f Radial spacing g, axial position h, tilt angle θ of the radiation-shaping heat shield, temperature Tc at the center of the solid-liquid interface, and temperature Te at the edge of the solid-liquid interface;
[0063] Figure 2 The gold-plated quartz support used in Embodiment 1 of the present invention;
[0064] Figure 3 This is a schematic diagram of cracking in a 3-inch LaBr3 crystal grown in a conventional partitioned VB crystal growth furnace, as shown in Comparative Example 1. Detailed Implementation
[0065] The embodiments of the present invention are described in detail below. These embodiments are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0066] In this invention, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the relative positions of the corresponding components in the direction of gravity when they are in use, while "inner" and "outer" refer to their relative positions to the contours of the corresponding components themselves. Furthermore, the terms "first," "second," etc., used in this invention are for distinguishing one element from another and do not indicate sequence or importance. In the following description, when referring to the accompanying drawings, unless otherwise explained, the same reference numerals in different drawings denote the same or similar elements.
[0067] The research team of this invention analyzed the structure and cracking problems of existing large-size lanthanide halide crystal VB crystal growth furnaces and found that conventional VB crystal growth furnaces typically rely on top heating, upper heating, lower heating, bottom heating, and ordinary heat preservation structures to form an axial temperature gradient. Although this type of structure can achieve raw material melting and crystal solidification, it is still prone to problems such as unstable crystal attraction, excessive curvature of the solid-liquid interface, significant circumferential temperature difference around the crucible or ampoule, large thermal shock when the solidified crystal enters the lower region, and cracking of the crystal during cooling, cutting, or packaging.
[0068] To address the aforementioned problems, this invention proposes a baffled VB crystal growth furnace structure to suppress cracking in large-sized lanthanide halide crystals. This structure does not simply improve crystal quality by raising or lowering the temperature in a specific zone. Instead, it divides the furnace thermal field into a high-temperature melting zone, a baffled temperature gradient zone, and a lower slow-cooling zone, and achieves coordinated control through baffles, an upper and lower radiative shaping heat shield, a concentric annular heat-spreading cavity, surface-metallized quartz supports, and a thermally conductive inner core. The system comprises: a partition plate to form a large temperature gradient region near the central through-hole; upper and lower radiation shaping heat shields to regulate the radiative heat flow path between the high-temperature melting zone, the partition plate temperature gradient region, and the lower slow cooling zone; a concentric annular heat exchanger to reduce the circumferential temperature difference around the crucible or ampoule; surface-metallized quartz supports to reduce undesigned radiation boundary disturbances caused by ordinary quartz supports; and a thermally conductive core to provide a stable axial heat conduction path for the seed crystal segment or conical crystal-guiding segment, thereby improving the repeatability of the solid-liquid interface position and morphology during the crystal-guiding stage. This addresses the technical problems encountered in the growth of large-size lanthanide halide crystals (VB), such as easy cracking, difficulty in balancing the large temperature gradient at the partition plate orifice with low-stress slow cooling after solidification, difficulty in maintaining stable control of the solid-liquid interface morphology, and disturbances to the temperature gradient at the partition plate orifice caused by the upper and lower thermal fields.
[0069] See Figure 1 The present invention discloses a partition-type VB crystal growth furnace structure for suppressing cracking of large-sized lanthanide halide crystals, comprising a furnace body, a top heater 1, an upper heater 2, a growth container 3, a partition 10, an upper radiation shaping heat shield 4, a lower radiation shaping heat shield 5, a lower heater 6, a bottom heater 12, a concentric annular heat-spreading cavity 11, a surface-metallized quartz support 7, a heat-conducting inner core 8, a heat-insulating frame 9, a temperature measuring element, a control unit, and a lowering mechanism.
[0070] The large-size lanthanide halide crystals referred to in this invention include LaBr3 crystals, LaBr3:Ce crystals, CeBr3 crystals, LaCl3:Ce crystals, LaBr3-LaCl3 mixed halide crystals, or other halide scintillation crystals containing lanthanide elements; the diameter D of the large-size lanthanide halide crystals is 38 mm or more, preferably 50 mm or more, and more preferably 76 mm or more.
[0071] In one embodiment of the present invention, a high-temperature melting zone, a partition temperature gradient zone, and a lower slow cooling zone are sequentially formed vertically inside the furnace body. The high-temperature melting zone is located at the upper part of the furnace body and is used to melt, heat-hold, and homogenize the lanthanide halide raw material in the growth container 3. Preferably, the temperature of the high-temperature melting zone is 5°C to 100°C higher than the melting point of the grown lanthanide halide crystal, and more preferably 10°C to 50°C higher than the melting point, to ensure that the lanthanide halide raw material is fully melted and the melt temperature is kept stable. The partition temperature gradient zone is located between the high-temperature melting zone and the lower slow cooling zone and is used to form a large temperature gradient zone when the growth container 3 passes through the central through-hole of the partition, and to shape the radiative heat flow near the solid-liquid interface. The axial temperature gradient Gz of the partition temperature gradient zone is 5°C / cm to 80°C / cm, preferably 10°C / cm to 50°C / cm. The partition temperature gradient zone can achieve stable crystal attraction, shoulder formation, and initial solid-liquid interface advancement, so that the solid-liquid interface is maintained in an approximately straight, slightly convex, or low-curvature shape. The lower slow cooling zone is located below the temperature gradient zone of the partition plate. It is used for compensating heating, axial thermal regulation, and low-stress slow cooling of the solidified crystal, seed crystal segment, or conical crystal-guiding segment, and to allow the solidified crystal to cool slowly at a set rate after leaving the temperature gradient zone of the partition plate. The axial temperature gradient of the lower slow cooling zone is 0.5℃ / cm to 20℃ / cm, preferably 1℃ / cm to 10℃ / cm.
[0072] In a possible embodiment of the present invention, the growth container 3 is a crucible or ampoule, specifically one of the following: a quartz crucible, a quartz ampoule, a low-hydroxyl quartz ampoule, a quartz ampoule with an inner wall coating, or a sandblasted quartz crucible. The type and material of the growth container 3 are selected according to the target large-size lanthanide halide crystal. Specifically, for LaBr3 crystal, LaBr3:Ce crystal, and CeBr3 crystal, quartz ampoules, low-hydroxyl quartz ampoules, or quartz ampoules with an inner wall coating are preferred. For LaCl3:Ce crystal or LaBr3-LaCl3 mixed halide crystal, low-hydroxyl quartz ampoules, quartz ampoules with an inner wall coating, or sandblasted quartz crucibles are preferred to reduce the reaction, adhesion, and thermal stress concentration between the halide melt and the inner wall of the crucible or ampoule.
[0073] In a possible embodiment of the present invention, the wall thickness t of the growth container 3 is 1.5 mm to 8 mm, and increases with the increase of the crystal diameter D. For crystals with a diameter D of 38 mm to 50 mm, the wall thickness t is preferably 1.5 mm to 4 mm; for crystals with a diameter D of 50 mm to 76 mm, the wall thickness t is preferably 2 mm to 6 mm; for crystals with a diameter D of 76 mm or more, the wall thickness t is preferably 3 mm to 8 mm. When the inner diameter of the growth container 3 is approximately equal to the diameter D of the crystal being grown, the outer diameter D2 of the growth container 3 is D+2t.
[0074] In one embodiment of the present invention, the outer diameter D2 of the growth container 3 is matched with the central through hole of the partition, the upper radiation shaping heat shield 4 and the lower radiation shaping heat shield 5; when the crystal diameter D increases, the outer diameter D2 of the growth container 3, the aperture D1 of the central through hole and the radial distance g between the radiation shaping heat shield and the outer wall of the growth container 3 all increase synchronously to avoid mechanical interference and maintain a stable temperature gradient near the central through hole of the partition.
[0075] In an embodiment of the present invention, a seed crystal segment or a conical crystal-guiding segment is provided at the bottom of the growth container 3. The minimum inner diameter of the seed crystal segment or the conical crystal-guiding segment is 0.05 to 0.40 times the crystal diameter D, preferably 0.10 to 0.25 times. When a conical crystal-guiding segment is provided at the bottom of the growth container 3, the cone angle of the conical crystal-guiding segment is 10° to 60°, preferably 20° to 45°.
[0076] In one embodiment of the present invention, the top heater 1 and the upper heater 2 are disposed on the upper part of the furnace body and located within or corresponding to the high-temperature melting zone. The top heater 1 is used to compensate for heat loss at the upper end of the growth container 3, and the upper heater 2 is used to maintain the temperature stability of the main melting zone of the growth container 3, so that the lanthanide halide raw material is fully melted and the melt temperature is kept stable. The lower heater 6 is disposed below the partition 10 and is located within or corresponding to the lower slow cooling zone. The bottom heater 12 is disposed near the lower end of the growth container 3 and is used to compensate for heating the solidified crystal or the lower end of the growth container 3, so that the solidified crystal is slowly cooled when it enters the lower slow cooling zone after passing through the temperature gradient zone of the partition, thereby reducing cold-end thermal shock and residual thermal stress.
[0077] In one embodiment of the present invention, the insulation frame 9 is disposed inside the furnace body, and the top heater 1, upper heater 2, lower heater 6, bottom heater 12, growth container 3, partition 10, upper radiative shaping heat shield 4, lower radiative shaping heat shield 5, concentric annular heat-spreading cavity 11, surface metallized quartz support 7, and heat-conducting inner core 8 are all disposed within the insulation frame 9. The insulation frame 9 is used to construct the basic insulation boundary of the furnace body, and together with the top heater 1, upper heater 2, lower heater 6, and bottom heater 12, forms a temperature field distributed along the vertical direction. The growth container 3 is disposed within the insulation frame 9 along the axial direction of the furnace body, and is used to hold lanthanide halide raw materials or lanthanide halide melt. The top heater 1 is disposed above the growth container 3 to compensate for heat loss at the upper end of the growth container 3; the upper heater 2 is disposed on the upper outer periphery of the growth container 3 to maintain a stable temperature in the main melting zone of the growth container 3, so that the lanthanide halide raw materials are fully melted and the melt temperature is kept stable. The top heater 1 and the upper heater 2 together form a high-temperature melting zone.
[0078] In one embodiment of the present invention, a partition 10 is disposed between the upper heater 2 and the lower heater 6, and a central through hole is provided in the center of the partition 10 for the growth container 3 to pass through; an annular radiation channel is formed between the central through hole and the growth container 3, allowing the growth container 3 to pass through the partition temperature gradient region near the partition 10 during its descent, and forming a partition temperature gradient region near the central through hole for crystal attraction and initial solidification. This partition temperature gradient region is used to achieve stable crystal attraction, shoulder formation, and initial solid-liquid interface advancement, keeping the solid-liquid interface in an approximately flat, slightly convex, or low-curvature shape.
[0079] In a possible embodiment of the present invention, the partition 10 is an annular partition, a disc-shaped partition, or a composite heat-insulating partition with a central through hole; the thickness of the partition 10 is 5mm to 80mm, preferably 10mm to 50mm. The aperture D1 of the central through hole on the partition is matched with the outer diameter D2 of the growth container 3, and the ratio D1 / D2 is 1.05 to 2.50, preferably 1.10 to 1.80; if D1 / D2 is too small, mechanical interference is easily generated when the growth container 3 passes through the central through hole, and the annular radiation channel is too narrow, resulting in insufficient thermal compensation at the solid-liquid interface edge; if D1 / D2 is too large, the thermal isolation effect of the partition 10 between the high-temperature melting zone and the lower slow cooling zone is weakened, and the upward radiation generated by the lower heat source is easily introduced into the vicinity of the central through hole of the partition, weakening the large temperature gradient required for crystal growth.
[0080] In one embodiment of the present invention, the upper radiative shaping heat shield 4 is disposed above the partition 10 or on the side of the partition 10 near the high-temperature melting zone, and the lower radiative shaping heat shield 5 is disposed below the partition 10 or on the side of the partition 10 near the lower slow cooling zone; the upper radiative shaping heat shield 4 is used to limit, weaken or redirect the direct radiative heat flow from the top heater 1 and the upper heater 2 to the area below the partition 10, and the lower radiative shaping heat shield 5 is used to block, weaken or redirect the upward radiative heat flow from the lower heater 6 and the bottom heater 12 to the vicinity of the central through hole on the partition.
[0081] In one embodiment of the present invention, the upper radiation shaping heat shield 4 includes a partition shielding section, a radiation shaping section, and a transition section; the partition shielding section is located near the central through hole and is used to regulate the downward radiation heat flow from the high-temperature melting zone to below the central through hole; the radiation shaping section is located on the outer periphery of the growth container 3 and is used to adjust the radial heat flow distribution near the solid-liquid interface; the transition section faces the high-temperature melting zone and is used to gradually transition the melt from the high-temperature melting zone to the partition temperature gradient zone.
[0082] In one embodiment of the present invention, the structure of the lower radiation shaping heat shield 5 is the same as that of the upper radiation shaping heat shield 4, and is mirrored in the horizontal direction with respect to the partition 10; for the lower radiation shaping heat shield 5, the partition shielding section is located near the central through hole, which is used to regulate the upward radiation heat flow from the lower slow cooling zone to the center through hole; the radiation shaping section is located on the outer periphery of the growth container 3, which is used to adjust the radial heat flow distribution near the solid-liquid interface; the transition section faces the lower slow cooling zone, which is used to allow the solidified crystal to gradually transition from the partition temperature gradient zone to the lower slow cooling zone.
[0083] Both the upper and lower radiation shaping heat shields 4 and 5 include a partition shielding section, a radiation shaping section, and a transition section. The partition shielding section is positioned near the central through-hole to reduce direct radiation from adjacent heating zones to the central through-hole. The radiation shaping section is located on the outer periphery of the growth container 3 to adjust the radial heat flow distribution near the solid-liquid interface. The transition section is positioned towards adjacent temperature zones to allow the melt or solidified crystal to gradually transition from one temperature zone to another. The upper and lower radiation shaping heat shields 4 and 5 of this invention are not simply heat-insulating components, but rather serve to change the radiation angle relationship between the heater, furnace wall, central through-hole, and the outer periphery of the growth container 3, so that the radiant heat flow is distributed in a predetermined direction.
[0084] In a possible embodiment of the present invention, both the upper radiative shaping heat shield 4 and the lower radiative shaping heat shield 5 are solid heat shield structures. The solid heat shield structure can be annular, cylindrical, conical, inclined, stepped, arc-shaped, or a composite surface. Among them, the annular heat shield is mainly used for axial shielding near the central through hole, and the cylindrical heat shield is mainly used for forming continuous axisymmetric shielding or guidance along the outer periphery of the growth container 3.
[0085] As a preferred embodiment of the present invention, the composite surface is composed of any two or three of the following: inclined surface, curved surface, and stepped surface, or a continuous combination of multiple similar surfaces with different geometric parameters, wherein the similar surfaces are inclined surface, curved surface, or stepped surface.
[0086] In a more preferred embodiment of the present invention, when the composite surface is composed of any two or three of the inclined surface, arc surface and stepped surface, the inclined surface, arc surface or stepped surface can be multiple identical surface shapes or multiple different surface shapes.
[0087] As a more preferred embodiment of the present invention, the composite surface is composed of a continuous combination of multiple inclined surfaces with different inclination angles, a continuous combination of multiple arc surfaces with different curvatures, or a continuous combination of multiple stepped surfaces with different heights.
[0088] In this invention, the surface shape, radial spacing, axial position, shaping surface tilt angle, and material selection of the upper radiating shaping heat shield 4 and the lower radiating shaping heat shield 5 follow the same collaborative design.
[0089] In a preferred embodiment of the present invention, the diameter D1 of the central through hole, the outer diameter D2 of the growth container 3, and the inner diameter D of the furnace chamber of the furnace body are specified. f The radial distance g between the radiation shaping heat shield and the outer wall of the growth container 3, and the axial position h of the radiation shaping heat shield relative to the partition 10, satisfy the following: the radial distance g is 0.02 to 0.25 times D2, more preferably 0.05 to 0.15 times; the axial position h is 0.05 to 0.50 times D2, more preferably 0.10 to 0.30 times; (D f -D2) / 2 is 0.05D2 to 1.20D2, preferably (D f-D2) / 2 is 0.10D2 to 0.80D2. Through the above dimensional relationship, the upper radiative shaping heat shield 4 and the lower radiative shaping heat shield 5 can avoid mechanical interference with the growth container 3, and effectively shield and redirect the radiative heat flow generated in adjacent temperature zones. In a preferred embodiment of the present invention, the tilt angle θ of the shaping surface of the corresponding radiative shaping section of the upper radiative shaping heat shield 4 and the lower radiative shaping heat shield 5 relative to the axis of the growth container 3 is 10° to 80°, more preferably 30° to 70°. The inclination angle θ of the radiation shaping section is not chosen in isolation. The synergistic selection relationship between the aperture D1 of the central through-hole, the outer diameter D2 of the growth container 3, and the inclination angle θ of the radiation shaping section is as follows: When D1 / D2 is 1.05 to 1.20, the annular radiation channel between the central through-hole and the growth container 3 is relatively narrow, and the baffle has a strong shielding effect on the radiative heat flow of adjacent temperature zones, but the heat compensation at the solid-liquid interface edge is relatively insufficient. At this time, the inclination angle θ of the radiation shaping section is preferably 50° to 70° to guide part of the radiative heat flow to the outer periphery of the growth container 3 to compensate for the heat at the solid-liquid interface edge; when D1 / D2 is 1... When D1 / D2 is between 20 and 1.60, the annular radiation channel is at a medium opening, and the shielding effect of the baffle and the edge compensation effect are relatively balanced. At this time, the inclination angle θ of the radiation shaping section is preferably 35° to 60° to take into account the large temperature gradient at the baffle orifice and the low curvature control of the solid-liquid interface. When D1 / D2 is between 1.60 and 2.50, the annular radiation channel is wider, and the radiation coupling from adjacent temperature zones to the baffle orifice is enhanced. At this time, the inclination angle θ of the radiation shaping section is preferably 10° to 45°, and the axial length or radial shielding width of the baffle shielding section is increased accordingly to reduce the proportion of radiative heat flow directly entering the central through hole.
[0090] In a preferred embodiment of the present invention, the surface shape of the radiation shaping heat shield is related to the inner diameter D of the furnace. f The outer diameter D2 of the growth container 3 and the heat flow control requirements should satisfy the following: when only axial shielding of the central through hole is required and the radial compensation requirement of the solid-liquid interface is weak, the radiation shaping heat shield preferably adopts a ring structure; when continuous axisymmetric shielding or guidance is required along the axial direction of the outer periphery of the growth container 3, the radiation shaping heat shield preferably adopts a cylindrical structure; when the inner diameter D2 of the furnace is... f The radial space between D2 and D2 is small, i.e., 0.05D2≤(D f When -D2) / 2≤0.25D2 (preferably 0.10D2≤(D f -D2) / 2≤0.25D2), the radiation shaping heat shield preferably adopts a sloped or conical structure to achieve radiation shielding within a limited radial space; when 0.25D2<(D f When -D2) / 2≤0.60D2, the radiation shaping heat shield preferably adopts a conical, arc-shaped, stepped, or cylindrical composite structure to simultaneously achieve orifice shielding, peripheral compensation, and thermal field transition; when 0.60D2<(D fWhen -D2) / 2≤1.2D2 (preferably 0.60D2<(D f -D2) / 2≤0.80D2), the radiation shaping heat shield preferably adopts a composite surface structure, and the radiation heat flow is controlled by partitioning the partition shielding section, radiation shaping section and heat field transition section to avoid local radiation heat flow concentration under wide furnace conditions.
[0091] It should be noted that both the upper radiative shaping heat shield 4 and the lower radiative shaping heat shield 5 are radiative heat flow shaping structures. The surface shape, radial spacing, axial position, shaping surface inclination angle, and material selection of the upper radiative shaping heat shield 4 and the lower radiative shaping heat shield 5 follow the same collaborative design, based on D1 / D2, D... f / D2, radial spacing g, axial position h of each radiative shaping heat shield relative to the partition 10, and inclination angle θ of the radiative shaping section on each radiative shaping heat shield are selected in a coordinated manner. The only difference is that the directions of action are opposite: the upper radiative shaping heat shield 4 mainly acts on the downward radiative heat flow from the high-temperature melting zone, while the lower radiative shaping heat shield 5 mainly acts on the upward radiative heat flow from the lower slow cooling zone. Through the coordinated action of the upper radiative shaping heat shield 4 and the lower radiative shaping heat shield 5, the radiative heat flow between the high-temperature melting zone, the partition temperature gradient zone, and the lower slow cooling zone is distributed according to a set path, avoiding the weakening of the large temperature gradient near the central through hole on the partition by the compensating heating of the lower slow cooling zone.
[0092] In a preferred embodiment of the present invention, the solid-liquid interface morphology is related to the axial temperature gradient Gz, the radial temperature difference ΔTr, and the radiative heat flux distribution caused by the radiation-shaping heat shield. The radial temperature difference is represented by the temperature Tc at the center near the solid-liquid interface and the temperature Te at the edge, where ΔTr = Te - Tc; the axial temperature gradient Gz is represented by the ratio of the temperature difference to the distance between the upper and lower temperature measuring points near the solid-liquid interface. Preferably, by adjusting D1 / D2, the inclination angle θ of the radiation-shaping section, the radial spacing g, the axial position h, and the output power of each heater, |ΔTr| is controlled within 20°C, and more preferably within 10°C. This is because: when ΔTr is -10 to 0℃, the solid-liquid interface edge is slightly colder than the center, and the interface can remain approximately straight or slightly advance towards the edge; when ΔTr is 0℃ to 10℃, the solid-liquid interface edge receives moderate thermal compensation, and the interface can maintain a slightly convex or low-curvature shape; when ΔTr is greater than 20℃, the edge compensation is too strong, which can easily lead to local overheating or interface depression; when ΔTr is less than -20℃, the tendency for edge undercooling is enhanced, which can easily induce edge stress concentration and cracking. Therefore, this invention limits ΔTr to a range suitable for low-curvature advancement of the interface by synergistically selecting the aperture ratio, tilt angle, and lower compensation thermal field of the partition. In addition, when |ΔTr| is greater than 0, the solid-liquid interface control factor K=Gz·R / |ΔTr| is not less than 3, preferably not less than 5, where R is the inner radius of the growth container 3. Through the above control relationship, the axial solidification driving force can be made dominant, and the radial temperature difference will not cause obvious interface bending, thereby maintaining the solid-liquid interface in an approximately straight, slightly convex, or low-curvature shape.
[0093] This invention, through the synergistic limitation of D1 / D2 and the tilt angle θ of the radiation shaping section, maintains an axial temperature gradient of 5℃ / cm to 80℃ / cm, preferably 10℃ / cm to 50℃ / cm, near the central through-hole, while keeping the temperature difference between the central and edge regions of the solid-liquid interface within a controllable range. This avoids the temperature gradient decrease caused by simply increasing the diameter of the central through-hole, and also avoids localized radiative heat flow concentration caused by simply increasing the tilt angle of the radiation shaping section on the radiation shaping heat shield, thereby reducing the risks of solid-liquid interface depression, edge undercooling, localized overheating, and crystal cracking.
[0094] In a feasible embodiment of the present invention, the materials of the upper radiative shaping heat shield 4 and the lower radiative shaping heat shield 5 should meet the requirements of high temperature resistance, low volatility, low gas evolution, dimensional stability, thermal shock stability, and compatibility with the halide atmosphere in the furnace, and should maintain morphological stability within the set temperature range of the high-temperature melting zone, the partition temperature gradient zone, and the lower slow cooling zone. Preferably, both the upper radiative shaping heat shield 4 and the lower radiative shaping heat shield 5 are made of one or more of high-temperature resistant metals, high-temperature resistant alloys, and high-temperature resistant ceramic materials; wherein, the high-temperature resistant metal is one or more of molybdenum, tungsten, tantalum, niobium, rhenium, and platinum; the high-temperature resistant alloy is one or more of molybdenum-tungsten alloy, tungsten-rhenium alloy, molybdenum-rhenium alloy, tantalum-tungsten alloy, nickel-based high-temperature alloy, cobalt-based high-temperature alloy, and iron-chromium-aluminum alloy; and the high-temperature resistant ceramic material is one or more of silicon carbide, boron nitride ceramic, aluminum nitride ceramic, alumina ceramic, zirconium oxide ceramic, mullite ceramic, and magnesium oxide ceramic. Their surfaces can be polished, sandblasted, coated, oxidized, or treated with composite coatings to adjust surface emissivity and reflection characteristics. When the long-term operating temperature of the two radiation shaping heat shields is below 700℃, it is preferable to use a composite structure of molybdenum, tantalum, platinum, molybdenum-tungsten alloy, nickel-based high-temperature alloy or cobalt-based high-temperature alloy to obtain a more stable radiation boundary; when the long-term operating temperature is above 700℃, it is preferable to use molybdenum, tungsten, tantalum, molybdenum-tungsten alloy, tungsten-rhenium alloy, silicon carbide, boron nitride ceramic or alumina ceramic materials to improve the high-temperature structural stability and resistance to thermal deformation.
[0095] In one embodiment of the present invention, the concentric annular heat exchanger 11 is disposed on the outer periphery of the growth container 3 and is located in the lower slow cooling zone or at the transition position between the temperature gradient zone of the partition and the lower slow cooling zone. The concentric annular heat exchanger 11 is used to reduce the circumferential temperature difference and non-axisymmetric cooling disturbance on the outer periphery of the growth container 3, so that the solidified crystal can obtain a more uniform outer peripheral thermal environment during the descent and slow cooling process.
[0096] In this invention, a concentric annular heat homogenizing cavity 11 is disposed on the outer periphery of the growth container 3. The concentric annular heat homogenizing cavity 11 includes an inner thermally conductive homogenizing layer, an outer thermal insulation layer, and an annular buffer gap layer disposed between the two. The inner thermally conductive homogenizing layer is disposed close to the outer periphery of the growth container 3 and is used to rapidly homogenize heat along the circumference. The outer thermal insulation layer is used to reduce the non-axisymmetric influence of local heat dissipation in the furnace or the lower cold end structure on the outer periphery of the crystal. The annular buffer gap layer is used to weaken local thermal short circuits and thermal shock.
[0097] Preferably, the inner heat-conducting and temperature-equalizing layer is made of one or more of molybdenum, tungsten, tantalum, boron nitride, silicon carbide, and high-temperature resistant alloy materials. The high-temperature resistant alloy materials include one or more of molybdenum-tungsten alloy, tungsten-rhenium alloy, molybdenum-rhenium alloy, tantalum-tungsten alloy, nickel-based high-temperature alloy, cobalt-based high-temperature alloy, and iron-chromium-aluminum alloy. The outer thermal insulation layer is made of one or more of alumina fiber, zirconium oxide fiber, mullite, boron nitride ceramic, alumina ceramic, aluminum silicate fiber, magnesium oxide ceramic, porous alumina ceramic, calcium oxide-stabilized zirconium oxide ceramic, and other high-temperature resistant thermal insulation materials.
[0098] Preferably, the materials selected for the inner thermally conductive homogenizing layer and the outer thermal insulation layer should match the crystal size, the temperature gradient of the lower slow cooling zone, and the circumferential temperature difference around the growth container 3. For lanthanide halide crystals with a crystal diameter D of 38 mm to 50 mm, the inner thermally conductive homogenizing layer is preferably made of boron nitride, silicon carbide, or high-temperature resistant alloy materials (including molybdenum-tungsten alloy, tungsten-rhenium alloy, molybdenum-rhenium alloy, tantalum-tungsten alloy, nickel-based high-temperature alloy, cobalt-based high-temperature alloy, or iron-chromium-aluminum alloy), with a thickness of 2 mm to 10 mm. For lanthanide halide crystals with a crystal diameter D of 50 mm to 76 mm and above, the inner thermally conductive homogenizing layer is preferably made of molybdenum, tungsten, tantalum, silicon carbide, or high-temperature resistant alloy materials (including molybdenum-tungsten alloy, tungsten-rhenium alloy, molybdenum-rhenium alloy, tantalum-tungsten alloy, nickel-based high-temperature alloy, cobalt-based high-temperature alloy, or iron-chromium-aluminum alloy), with a thickness of 5 mm to 20 mm, to improve the circumferential heat diffusion capability. The thickness of the outer thermal insulation layer is preferably 1 to 5 times that of the inner thermally conductive and heat-equalizing layer, which limits rapid heat loss in the radial direction and reduces the temperature difference in the circumferential direction in conjunction with the inner thermally conductive and heat-equalizing layer. By making the equivalent thermal conductivity of the inner thermally conductive and heat-equalizing layer higher than that of the outer thermal insulation layer, a composite thermal boundary of "uniform heat distribution in the inner circumference and radial insulation on the outer side" can be formed, thereby avoiding thermal short circuits or insufficient insulation caused by simple material replacement. In this invention, the concentric annular heat-spreading cavity 11 is located below the partition 10 and extends from the partition temperature gradient region below the partition 10 to the lower slow cooling region. The concentric annular heat-spreading cavity 11 includes, from top to bottom along the axial direction, an upper thermal field transition section, a middle circumferential temperature uniformization section, and a lower slow cooling insulation section. The upper thermal field transition section is used to connect the partition temperature gradient region and the lower slow cooling region. The middle circumferential temperature uniformization section is used to reduce the circumferential temperature difference around the growth container 3. The lower slow cooling insulation section is used to slow down the cooling rate of the solidified crystal in the lower slow cooling region.
[0099] In one embodiment of the present invention, the surface-metallized quartz support 7 is disposed below the growth container 3 for supporting, positioning, or guiding the growth container 3. See also... Figure 2 The surface-metallized quartz support 7 includes a quartz substrate and a metal film layer disposed on the surface of the quartz substrate. The metal film layer is used to reduce the non-designed thermal boundary disturbance caused by heat absorption and re-radiation on the surface of the quartz substrate, so that the surface-metallized quartz support 7 has both mechanical support and radiation boundary control functions.
[0100] Preferably, the metal film is a molybdenum film, tungsten film, platinum film, gold film, nickel film, tantalum film, or a composite film formed from the above metals; the thickness of the metal film is 0.1 μm to 200 μm, preferably 1 μm to 50 μm; the metal film can be formed on the surface of the quartz support by magnetron sputtering, vapor deposition, chemical plating, thermal spraying, metal foil covering, metal sleeve fitting, or high-temperature sintering.
[0101] In one embodiment of the present invention, the thermally conductive inner core 8 is disposed inside the surface metallized quartz support 7 and arranged along the crystal growth axis. The upper end of the thermally conductive inner core 8 is close to the seed crystal segment or conical crystal-guiding segment of the growth container 3, and the lower end of the thermally conductive inner core 8 is thermally coupled with the area near the lower slow cooling zone and the bottom heater 12. This provides a stable axial thermal path for the seed crystal segment or conical crystal-guiding segment, facilitating axial heat flow control during the crystal-guiding stage. The thermally conductive inner core 8 can enhance the axial thermal coupling between the seed crystal segment or conical crystal-guiding segment and the lower thermal field, improve the repeatability of the solid-liquid interface position and interface morphology near the central through hole of the partition 10, reduce local overheating or local undercooling of the seed crystal segment, and thus improve the crystal-guiding success rate.
[0102] Preferably, the thermally conductive inner core 8 is made of one or more of the following materials: molybdenum, tungsten, tantalum, silicon carbide, aluminum nitride, boron nitride, alumina, sapphire, or high-temperature resistant alloys. The high-temperature resistant alloys include one or more of the following: molybdenum-tungsten alloy, tungsten-rhenium alloy, molybdenum-rhenium alloy, tantalum-tungsten alloy, nickel-based high-temperature alloy, cobalt-based high-temperature alloy, or iron-chromium-aluminum alloy. The diameter of the thermally conductive inner core is 2mm to 30mm, preferably 5mm to 20mm. The thermally conductive inner core and the surface metallized quartz support 7 are in close contact, with a clearance fit, or connected by a high-temperature resistant insulation material. The high-temperature resistant insulation material is alumina-silica fiber paper, high-alumina fiber paper, quartz wool, etc. Furthermore, the materials and dimensions of the metal film layer and the thermally conductive inner core 8 are selected in a synergistic relationship. When the long-term operating temperature near the lower slow cooling zone or the surface metallized quartz support 7 is below 700℃, the metal film layer is preferably made of gold or platinum to obtain a lower surface emissivity and stable chemical compatibility. When the operating temperature is above 700℃, the metal film layer is preferably made of molybdenum, tungsten, or tantalum to improve high-temperature stability. For crystals with a diameter D of 38mm to 50mm, the diameter of the thermally conductive core 8 is preferably 5mm to 10mm; for crystals with a diameter D of 50mm to 76mm and above, the diameter of the thermally conductive core 8 is preferably 10mm to 20mm. If the thermally conductive core is made of a high thermal conductivity material such as molybdenum, tungsten, tantalum, silicon carbide, or aluminum nitride, a smaller diameter can be selected to avoid excessive local heat conduction; if a medium thermal conductivity or insulating high-temperature resistant material such as boron nitride, aluminum oxide, or sapphire is used, the diameter can be appropriately increased to maintain the axial thermal stability of the seed crystal segment or the tapered crystal guide segment. Thus, the surface metallized quartz support 7 adjusts the radiation boundary through the metal film layer, and the heat-conducting core 8 adjusts the axial heat conduction capacity through the material and diameter. The two work together to the seed crystal segment or the conical crystal guide segment, avoiding the seed crystal segment or the conical crystal guide segment from being too cold, too hot or having the interface position drifted due to the selection of a single material parameter.
[0103] In one embodiment of the present invention, temperature sensing elements are respectively disposed in the high-temperature melting zone, the partition temperature gradient zone, the lower slow cooling zone, the area near the bottom heater 12, and the area near the surface metallized quartz support 7, for real-time acquisition of furnace body axial and local thermal field information.
[0104] In one embodiment of the present invention, the control unit independently adjusts the output power of the four heaters—top heater 1, upper heater 2, lower heater 6, and bottom heater 12—based on the temperature signal fed back by the temperature sensing element, so that the high-temperature melting zone maintains the temperature required for melting the lanthanide halide raw material, the partition temperature gradient zone maintains a large temperature gradient, and the lower slow cooling zone maintains a relatively slow cooling rate.
[0105] During the crystal-leading stage, the control unit prioritizes ensuring a stable heat supply to the upper part while limiting the direct upward radiation of the lower heater 6 and the bottom heater 12 to the central through hole of the partition 10. During the slow cooling stage, the power of the top heater 1 and the upper heater 2 is gradually reduced while the compensation heating of the lower heater 6 and the bottom heater 12 is maintained to reduce the temperature jump when the solidified crystal enters the lower region.
[0106] In one embodiment of the present invention, the descent mechanism is used to drive the growth container 3 to descend vertically relative to the furnace body temperature field, with a descent rate of 0.05 mm / h to 5 mm / h, preferably 0.1 mm / h to 2 mm / h. During the crystal pulling stage, a low-speed descent can be used, during the constant-diameter growth stage, a constant-speed descent can be used, and after the crystal has completely solidified, a slow cooling or in-situ annealing method can be used to reduce residual thermal stress.
[0107] To facilitate the description of the thermal field effect, the circumferential temperature difference at the same height on the outer periphery of growth container 3 is defined as ΔTθ, where ΔTθ = Tθ,max - Tθ,min, and Tθ,max is the highest temperature among multiple circumferential temperature measurement points at the same height, and Tθ,min is the lowest temperature among multiple circumferential temperature measurement points at the same height. The equivalent cooling rate when the solidified crystal enters the lower slow cooling zone is defined as Vc, in °C / min, used to characterize the strength of the cold-end thermal shock experienced by the crystal when it enters the lower slow cooling zone from the temperature gradient region of the partition. The smaller Vc is, the weaker the temperature abrupt change and the smaller the thermal shock when the crystal enters the lower region.
[0108] It should be noted that the control unit and the lowering mechanism adopt the temperature control and lifting mechanism in existing VB crystal growth equipment, and their structure and working process are mature and known technologies in existing VB crystal growth.
[0109] It should be noted that the furnace structure of the present invention can be used to grow LaBr3, LaBr3:Ce, CeBr3, LaCl3:Ce and other lanthanide halide crystals; when used to grow LaBr3 or LaBr3:Ce crystals, the raw materials are sealed in a quartz ampoule, and a seed crystal segment or a conical crystal-guiding segment is provided at the bottom of the quartz ampoule. The upper end of the heat-conducting inner core 8 is arranged corresponding to the seed crystal segment or the conical crystal-guiding segment to stabilize the axial heat-conducting boundary of the crystal-guiding end.
[0110] For different lanthanide halide crystals, the set temperatures of the high-temperature melting zone, the partition temperature gradient zone, and the lower slow cooling zone are based on the melting point T of the corresponding crystal. m Adjustments are made based on a benchmark. For example, the temperature of the high-temperature melting zone is set higher than T. m 10℃~50℃; the upper temperature of the temperature gradient zone of the partition is T. m Up to T m At 30℃, the lower end of the temperature gradient zone of the partition is below T. m10℃~80℃; the inlet temperature of the lower slow cooling zone is lower than T. m 50℃~200℃. For crystals with a large coefficient of thermal expansion or a large diameter, the descent rate should be reduced, the circumferential heat conduction capacity of the concentric annular heat spreader should be increased, and the compensation temperature of the lower slow cooling zone should be appropriately increased. For crystals with a high melting point, molybdenum, tungsten, tantalum, silicon carbide, aluminum nitride, or other high-temperature resistant alloy materials should be preferred as radiation-shaping heat shields, concentric annular heat spreaders, or heat-conducting inner core materials to maintain the stability of heat shield shaping and axial heat conduction.
[0111] The present invention also provides a method for growing large-size lanthanide halide crystals using the above-mentioned partitioned VB crystal growth furnace structure, comprising the following steps;
[0112] Step 1: The lanthanide halide raw material is loaded into the growth container 3 and sealed under vacuum or inert atmosphere. Preferably, the growth container 3 is a quartz ampoule.
[0113] Step 2: Place the sealed growth container 3 into the furnace body of the partition-type VB crystal growth furnace, so that the growth container 3 corresponds to the high-temperature melting zone, the partition temperature gradient zone and the lower slow cooling zone in the furnace body in sequence, and arrange the seed crystal segment or conical crystal guiding segment at the lower end of the growth container 3 in correspondence with the surface metallized quartz support 7 and its internal heat-conducting core 8.
[0114] Step 3: Start the top heater 1 and the upper heater 2 to raise the temperature of the high-temperature melting zone to above the melting temperature of the lanthanide halide raw materials and to fully melt the raw materials in the growth container 3; at the same time, adjust the lower heater 6 and the bottom heater 12 to maintain the compensation temperature in the lower slow cooling zone.
[0115] Among them, each temperature zone is based on the melting point T of the lanthanide halide crystals grown therein. m The baseline setting is: the temperature of the high-temperature melting zone is higher than T. m 5℃~100℃, preferably higher than T m 10℃~50℃; the upper temperature of the temperature gradient zone of the partition is T. m Up to T m At 50℃, the lower end of the temperature gradient zone of the partition plate is below T. m 10℃~120℃, preferably below T m The axial temperature gradient in the partition temperature gradient zone is 5℃ / cm to 80℃ / cm, preferably 10℃ / cm to 50℃ / cm; the inlet temperature of the lower slow cooling zone is lower than T. m The temperature ranges from 50℃ to 200℃, and the temperature of the bottom slow cooling section is lower than T. m The axial temperature gradient of the lower slow cooling zone is 0.5℃ / cm to 20℃ / cm, preferably 1℃ / cm to 10℃ / cm, and ranges from 150℃ to 350℃.
[0116] Taking LaBr3 crystal as an example, the temperature of the high-temperature melting zone is set to 790℃~850℃, the temperature near the central through hole is set to 720℃~820℃, the inlet temperature of the lower slow cooling zone is set to 580℃~730℃, and the temperature of the bottom slow cooling section is set to 430℃~650℃.
[0117] Step 4: Adjust the output power of the top heater 1, upper heater 2, lower heater 6 and bottom heater 12 of the heating unit by controlling the control unit, and adjust the radiative heat flow path by adjusting the size of the upper radiative shaping heat shield 4 and the lower radiative shaping heat shield 5 to form a large temperature gradient zone near the central through hole. At the same time, make the axial temperature gradient of the partition temperature gradient zone 5℃ / cm~80℃ / cm, and the axial temperature gradient of the lower slow cooling zone 0.5℃ / cm~20℃ / cm. Control the temperature difference between the central region and the edge region of the solid-liquid interface in the growth container 3 within 20℃.
[0118] Specifically, during the melting stage, the output power of the top heater 1 and the upper heater 2 are increased to stabilize the high-temperature melting zone at a level higher than T. m 10℃~50℃; During the crystallization stage, the output power of the upper heater 2 is made higher than that of the lower heater 6, and the output power of the lower heater 6 is made higher than or close to that of the bottom heater 12, thereby forming a temperature distribution that decreases from top to bottom near the central through hole; When the temperature gradient at the baffle orifice is insufficient, the output power of the top heater 1 or the upper heater 2 is increased, the output power of the lower heater 6 or the bottom heater 12 is decreased, or the shielding ratio of the upper radiation shaping heat shield 4 and the lower radiation shaping heat shield 5 to the direct radiation heat flow is increased simultaneously; When the solid-liquid interface edge is too cold, the output power of the lower heater 6 is appropriately increased or the tilt angle θ of the radiation shaping section of the upper radiation shaping heat shield 4 or the tilt angle θ of the radiation shaping section of the lower radiation shaping heat shield 5 is adjusted so that some of the radiation heat flow is redirected to the outer periphery of the growth container 3; When the solid-liquid interface edge is overheated, the output power of the lower heater 6 or the bottom heater 12 is decreased, or the tilt angle of the radiation shaping section is reduced, and the shielding of the radiation heat flow by the baffle shielding section is increased. Through the above adjustments, the axial temperature gradient near the central through hole on the partition plate is maintained at 5℃ / cm to 80℃ / cm, preferably 10℃ / cm to 50℃ / cm; and the axial temperature gradient in the lower slow cooling zone is maintained at 0.5℃ / cm to 20℃ / cm, preferably 1℃ / cm to 10℃ / cm; at the same time, the temperature difference between the central region and the edge region of the solid-liquid interface in the growth container 3 is controlled within 20℃.
[0119] Step 5: The growth container 3 is slowly lowered relative to the furnace body temperature field by the lowering mechanism, so that the melt in the growth container 3 enters the temperature gradient zone of the partition plate from the high temperature melting zone. Crystal introduction, shoulder formation and initial solidification are completed near the central through hole of the partition plate, and crystals are gradually formed.
[0120] Step 6: As the growth container 3 continues to descend, the solidified crystal enters the lower slow cooling zone, where circumferential homogenization and low-stress slow cooling are achieved through the combined action of the concentric annular heat exchanger 11, the lower heater 6, the bottom heater 12, and the surface metallized quartz support 7. At the same time, the axial thermal boundary of the seed crystal segment or the conical crystal guide segment is stabilized by the thermally conductive inner core 8 set inside the surface metallized quartz support 7.
[0121] Step 7: After the crystals have completely solidified, perform heat treatment in the lower slow cooling zone or in-situ annealing temperature zone. The preferred annealing temperature is below T. m The temperature is maintained at 150℃~350℃ for 12h~72h; then the temperature is slowly reduced to 50℃~120℃ or room temperature at a cooling rate of 5℃ / h~30℃ / h. The heater is then turned off and the growth container 3 is removed to obtain large-sized lanthanide halide crystals.
[0122] Taking LaBr3 crystal as an example, it is annealed at a temperature of 430℃~630℃ for 24h~48h, and then slowly cooled to below 80℃ according to the cooling rate before being taken out.
[0123] The present invention also provides a large-size lanthanide halide crystal, which is prepared by the above-described partitioned VB crystal growth furnace structure or the above-described method.
[0124] A crystal element for a lanthanide halide scintillation crystal detector, the raw material of which is a large-size lanthanide halide crystal prepared by the above method.
[0125] Preferably, a method for preparing a crystal element for a lanthanide halide scintillation crystal detector involves cutting, grinding, polishing, encapsulating, or optically coupling a large-size lanthanide halide crystal, and selecting a region with low cracks and low stress to obtain the crystal.
[0126] The embodiments of the present invention are described in detail below. These embodiments are exemplary and intended to explain the present invention, and should not be construed as limiting the scope of protection of the present invention.
[0127] It should be noted that, unless otherwise specified, the equipment, pharmaceuticals, reagents, etc. used in the following embodiments are all products known in the art and can be obtained commercially.
[0128] Comparative Example 1
[0129] LaBr3 crystals were grown using a conventional baffled VB crystal growth furnace. This conventional baffled VB crystal growth furnace includes an insulation structure (top heater), an upper heater, a lower heater, a bottom heater, and baffles (with a central through-hole on the baffles); however, it lacks the upper radiation shaping heat shield 4, the lower radiation shaping heat shield 5, the concentric annular heat dissipation cavity 11, the surface-metallized quartz support 7, and the heat-conducting inner core 8. The specific steps are as follows:
[0130] Step 1: Load the LaBr3 raw material into growth container 3 (quartz ampoule) and seal it under vacuum or inert atmosphere.
[0131] Step 2: Place the sealed quartz ampoule in a conventional partitioned VB crystal growth furnace. The raw material is melted by the upper heater, and a lower heat field is formed by the lower heater and the bottom heater.
[0132] Step 3: The quartz ampoule is slowly lowered using a descending mechanism, allowing the melt to pass through the temperature gradient zone near the partition and gradually solidify, resulting in a 3-inch LaBr3 crystal, denoted as Comparative Example 1. Its crack structure is as follows: Figure 3 As shown.
[0133] In Comparative Example 1, the lack of effective blocking and shaping of the upward radiative heat flow generated by the lower heater and bottom heater easily weakens the temperature gradient near the central through hole of the partition. At the same time, the growth container 3 lacks a concentric annular heat equalization cavity for circumferential temperature equalization, and the surface radiation boundary of the quartz support is also lacking control. During the growth and cooling process, the crystal is prone to local thermal stress concentration and cracking tendency.
[0134] Under thermal field simulation and multi-point temperature measurement verification conditions, the circumferential temperature difference ΔTθ at four points at the same height on the outer periphery of growth container 3 in Comparative Example 1 is approximately 12℃~18℃; the equivalent cooling rate Vc when the solidified crystal enters the lower region is approximately 2℃ / min~5℃ / min. After cooling and exiting the furnace, the crystal is prone to through-cracks, edge cracks, or local crack propagation, and the integrity of the transparent constant-diameter section is poor, resulting in a high risk of breakage during subsequent cutting and processing.
[0135] Example 1
[0136] This embodiment uses the partition-type VB crystal growth furnace structure described in this invention to grow 3-inch LaBr3 crystals.
[0137] Step 1: Load the LaBr3 raw material into the growth container 3. The bottom of the growth container 3 is provided with a tapered crystal-guiding section and sealed under vacuum or inert atmosphere.
[0138] Step 2: Place the sealed growth container 3 in the partition-type VB crystal growth furnace of the present invention, so that the upper part of the growth container 3 corresponds to the high-temperature melting zone formed by the top heater 1 and the upper heater 2, the middle part of the growth container 3 corresponds to the partition temperature gradient zone near the partition 10, and the lower part of the growth container 3 corresponds to the lower slow cooling zone formed by the lower heater 6 and the bottom heater 12; and make the bottom conical crystal-leading section of the growth container 3 correspond to the surface metallized quartz support 7 and its internal heat-conducting core 8.
[0139] Step 3: Activate the top heater 1 and upper heater 2 to raise the temperature of the high-temperature melting zone above the melting temperature of the LaBr3 raw material, ensuring complete melting of the raw material within the growth container 3; simultaneously activate the lower heater 6 and bottom heater 12 to create a compensated heating environment in the lower slow cooling zone. In this embodiment, the temperature of the high-temperature melting zone is controlled at 800℃~830℃, the temperature near the central through-hole of the partition 10 is controlled at 730℃~800℃, the inlet temperature of the lower slow cooling zone is controlled at 620℃~700℃, and the temperature of the bottom slow cooling section is controlled at 500℃~620℃.
[0140] Step 4: Adjust the position of the upper radiation shaping heat shield 4 and the lower radiation shaping heat shield 5 and their radiation shaping surfaces to form a stable temperature gradient zone near the central through hole of the partition 10, while avoiding direct disturbance of the temperature gradient at the partition orifice by the downward radiation from the high-temperature melting zone and the upward radiation from the lower slow cooling zone.
[0141] In this embodiment, the ratio D1 / D2 of the aperture D1 of the central through hole of the partition 10 to the outer diameter D2 of the growth container 3 is controlled to be 1.20 to 1.45; the radial spacing g is 0.02 to 0.25 times D2, and the axial position h is 0.05 to 0.50 times D2. f -D2) / 2 is 0.10D2~0.80D2. Both the upper radiation shaping heat shield 4 and the lower radiation shaping heat shield 5 adopt a conical or inclined structure. The tilt angle θ of the shaping surface relative to the axis of the growth container 3 is controlled to be 45°~60°, so that the radiative heat flow on the high temperature side and the low temperature side acts on the central through hole and the outer periphery of the growth container 3 according to the set path, rather than directly causing the temperature gradient at the central through hole to run out of control.
[0142] Step 5: The growth container 3 is slowly lowered at a set rate by the lowering mechanism, so that the lanthanide halide melt passes through the temperature gradient zone near the central through hole of the partition 10 to complete crystal introduction and initial solidification, and continues to pass through the lower slow cooling zone for low-stress slow cooling.
[0143] Step 6: After the crystal has completely solidified, it is annealed at 500℃~620℃ for 24h~48h, and then slowly cooled to below 80℃ at a rate of 10℃ / h~25℃ / h. The growth container 3 is then removed to obtain a 3-inch crack-free LaBr3 crystal, which is referred to as Example 1.
[0144] Compared with Comparative Example 1, in Example 1, the decoupling of radiative heat flow between the partition temperature gradient region and the lower slow cooling region was achieved through the upper radiative shaping heat shield 4 and the lower radiative shaping heat shield 5; the circumferential temperature difference on the outer periphery of the growth container 3 was reduced through the concentric annular heat dissipation cavity 11; and the circumferential temperature difference on the outer periphery of the growth container 3 was reduced through... Figure 2 The surface metallized quartz support 7 of the gold-plated film reduces the undesigned thermal boundary disturbance introduced by the support structure; the axial thermal boundary of the tapered crystal section is improved by the thermally conductive inner core 8 disposed inside the surface metallized quartz support 7.
[0145] In a thermal field simulation and multi-point temperature measurement verification of this embodiment, the circumferential temperature difference ΔTθ at four points at the same height on the outer periphery of the growth container 3 decreased from approximately 12℃ to 18℃ in Comparative Example 1 to approximately 3℃ to 6℃; the equivalent cooling rate Vc when the solidified crystal enters the lower region decreased from 2℃ / min to 5℃ / min in Comparative Example 1 to 0.2℃ / min to 1℃ / min, and the equivalent thermal shock intensity decreased by approximately 60% to 90%. After cooling and exiting the furnace, the crystal in Comparative Example 1 was prone to through-cracks or obvious edge cracks, while the 3-inch LaBr3 crystal obtained in Example 1 showed no through-cracks, significantly reduced edge cracks, and improved integrity of the transparent constant-diameter section, exhibiting better overall integrity and adaptability for subsequent cutting and processing.
[0146] Example 2
[0147] This embodiment is basically the same as embodiment 1, except that: the metal film layer on the surface of the surface metallized quartz support 7 is a molybdenum film or a tungsten film, and the heat-conducting inner core 8 is made of molybdenum, tungsten, silicon carbide or aluminum nitride.
[0148] Step 1: Load the LaBr3 raw material into the growth container 3, which has a tapered seed section at the bottom, and seal it under vacuum or inert atmosphere.
[0149] Step 2: Place the growth container 3 in the partitioned VB crystal growth furnace so that the conical crystal-leading segment corresponds to the surface metallized quartz support 7 and the heat-conducting inner core 8.
[0150] Step 3: The raw material is melted by the top heater 1 and the upper heater 2, and a lower slow cooling zone is formed by the lower heater 6 and the bottom heater 12.
[0151] Step 4: Adjust the radiative heat flow path by using the upper radiative shaping heat shield 4 and the lower radiative shaping heat shield 5 to maintain a stable temperature gradient near the central through hole of the partition 10.
[0152] Step 5: The growth container 3 is slowly lowered by the lowering mechanism to complete the crystal introduction, solidification and slow cooling process, and LaBr3 crystal is obtained, which is recorded as Example 2.
[0153] This embodiment illustrates that the metal film layer of the surface metallized quartz support 7 is not limited to gold; it can also be a molybdenum film, tungsten film, or other high-temperature resistant metal film layer. The material of the thermally conductive core 8 is also not limited to a single material; it can be one or more of molybdenum, tungsten, tantalum, silicon carbide, aluminum nitride, boron nitride, alumina, sapphire, or high-temperature resistant alloy materials. As long as a stable axial heat conduction path can be provided during the crystal pulling stage and the temperature environment inside the furnace can be adapted, the technical effects of this invention can be achieved. Under one verification condition in this embodiment, the circumferential temperature difference ΔTθ around the growth container 3 can be controlled at approximately 4°C to 8°C, and no obvious through-cracks are observed after the crystal cools.
[0154] Example 3
[0155] This embodiment is basically the same as Embodiment 1, except that the crystals grown are CeBr3 crystals, LaBr3:Ce crystals, or LaCl3:Ce crystals, and the set temperatures of the high-temperature melting zone, the partition temperature gradient zone, and the lower slow cooling zone inside the furnace are adjusted according to the melting point of the lanthanide halide crystals grown.
[0156] Step 1: Load CeBr3 raw material, LaBr3:Ce raw material or LaCl3:Ce raw material into growth container 3 and seal it under vacuum or inert atmosphere.
[0157] Step 2: Place the sealed growth container 3 into the partition-type VB crystal growth furnace of the present invention, so that the growth container 3 corresponds sequentially to the high-temperature melting zone, the partition temperature gradient zone and the lower slow cooling zone.
[0158] Step 3: Based on the melting point of the lanthanide halide crystals being grown, adjust the output power of the top heater 1, upper heater 2, lower heater 6 and bottom heater 12 so that the raw material is melted in the high-temperature melting zone, a suitable temperature gradient for crystal development is formed in the partition temperature gradient zone, and a low-stress slow cooling environment is formed in the lower slow cooling zone.
[0159] Step 4: The growth container 3 is slowly lowered by the lowering mechanism, allowing the melt to pass through the temperature gradient zone of the partition to complete crystal introduction and solidification, and then gradually cooled in the lower slow cooling zone to obtain large-size CeBr3 crystals, LaBr3:Ce crystals or LaCl3:Ce crystals.
[0160] This embodiment illustrates that the partition-type VB crystal growth furnace structure of the present invention is not only applicable to LaBr3 crystals, but also to LaBr3:Ce crystals, CeBr3 crystals, LaCl3:Ce crystals, and other lanthanide halide scintillation crystals. For different crystal materials, only by adjusting the set temperature of each temperature zone, the partition aperture, the angle of the radiation-shaping heat shield, and the descent rate according to their melting point, thermal expansion characteristics, and ampoule structure, the same or similar low-stress growth effect can be achieved. Under one verification condition, after adopting the structure of the present invention, the circumferential temperature difference ΔTθ around the growth container 3 can be controlled within 10°C, and the equivalent cooling rate Vc when the solidified crystal enters the lower slow cooling zone can be controlled within about 1°C / min. The tendency of crystal cracking is significantly lower than that of conventional partition-type VB furnaces.
[0161] Example 4
[0162] This embodiment is basically the same as embodiment 1, except that the upper radiating shaping heat shield 4 and the lower radiating shaping heat shield 5 adopt the same or mirror images of different solid structural forms, including conical, inclined, stepped or arc-shaped structures.
[0163] Step 1: Load the LaBr3 raw material into growth container 3 and seal it.
[0164] Step 2: Place the growth container 3 in the partitioned VB crystal growth furnace, and conduct growth experiments using conical, inclined, stepped, or arc-shaped upper radiation shaping heat shield 4 and lower radiation shaping heat shield 5 respectively.
[0165] Step 3: Adjust the output power of the top heater 1, upper heater 2, lower heater 6 and bottom heater 12 to form a temperature gradient region suitable for crystal introduction near the central through hole of the partition plate 10.
[0166] Step 4: The growth container 3 is slowly lowered by the lowering mechanism to complete the crystal introduction, solidification and slow cooling process, and obtain LaBr3 crystals.
[0167] This embodiment illustrates that the specific morphology, materials, and installation dimensions of the upper radiative shaping heat shield 4 and the lower radiative shaping heat shield 5 can be adjusted according to the dimensions of the growth container 3, the inner diameter of the furnace, the position of the heater, and the desired solid-liquid interface morphology. Let the outer diameter of the growth container 3 be D2, the diameter of the central through-hole of the partition 10 be D1, and the inner diameter of the furnace be D... f The tilt angle of the shaping surface of the radiation shaping heat shield relative to the axis of the growth container 3 is θ. The quantitative design rules for the upper radiation shaping heat shield 4 and the lower radiation shaping heat shield 5 are consistent: when D1 / D2 is 1.05~1.20 and (D f -D2) / 2 is 0.05D2 to 1.20D2 of D fWhen D1 / D2 is small, the radiation channel is narrow, and θ is preferably 50° to 70°. The radiative heat flow is mainly guided to the outer periphery of the growth container 3, which is beneficial to obtaining a slightly convex or nearly flat interface. When D1 / D2 is 1.20 to 1.60, θ is preferably 35° to 60°. The radiative heat flow is balanced between the shielding of the partition orifice and the compensation of the outer periphery, which is beneficial to obtaining a low curvature interface. When D1 / D2 is 1.60 to 2.50, θ is preferably 10° to 45°, and the length of the partition shielding section of the radiation shaping heat screen is increased to reduce the proportion of radiative heat flow directly entering the central through hole of the partition 10, so as to avoid overheating or positional drift of the solid-liquid interface center.
[0168] The interface morphology can be characterized by the radial temperature difference ΔTr between the edge temperature Te and the center temperature Tc near the solid-liquid interface, where ΔTr = Te - Tc. When ΔTr is -10 to 0℃, the interface can remain approximately straight or the edge can advance slightly ahead. When ΔTr is 0 to 10℃, the interface edge receives moderate thermal compensation, and the interface can maintain a slightly convex or low curvature morphology. When ΔTr is greater than 20℃, the edge compensation is too strong, which can easily lead to local overheating or interface depression. When ΔTr is less than -20℃, the tendency for edge undercooling is enhanced, which can easily induce edge stress concentration and cracking. By controlling the combination relationship between D1 / D2, Df / D2, and θ, the radiative heat flow distribution near the central through-hole of the partition 10 and the periphery of the growth container 3 can be matched with the target interface morphology, thereby reducing the tendency for interface edge undercooling and crystal cracking.
[0169] Therefore, it can be determined that the partition-type VB crystal growth furnace structure provided by this invention can establish a stable, controllable, and decoupled thermal field relationship between the high-temperature melting zone, the partition temperature gradient zone, and the lower slow cooling zone. Compared with Comparative Example 1, under a preferred embodiment, the circumferential temperature difference ΔTθ around the growth container 3 can be reduced from 12℃~18℃ to 3℃~6℃, and the equivalent cooling rate Vc when the solidified crystal enters the lower slow cooling zone can be reduced from 2℃ / min~5℃ / min to 0.2℃ / min~1℃ / min, and the equivalent thermal shock intensity is reduced by about 60%~90%. The probability of crystal penetration cracks or edge cracks is significantly reduced, and the integrity of the transparent constant diameter section and the yield of subsequent cutting and processing are improved. These results show that this invention can improve the crystal-attracting stability of large-size lanthanide halide crystals, reduce the circumferential temperature difference around the growth container 3, reduce the thermal shock when the solidified crystal enters the lower region, and reduce the tendency of crystals to crack during growth, cooling, cutting, and subsequent packaging.
[0170] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the scope of the technology disclosed in the present invention to make other changes and modifications to the technical solution of the present invention, and such modifications or substitutions should be covered within the scope of protection of the present invention.
Claims
1. A partition-type crystal growth furnace structure for suppressing cracking in large-sized lanthanide halide crystals, characterized in that, It includes a furnace body and heating units, growth container (3), upper radiation shaping heat shield (4), lower radiation shaping heat shield (5), surface metallized quartz support (7), heat-conducting inner core (8), partition (10) and concentric annular heat-spreading cavity (11) respectively installed in the furnace body; The furnace body is arranged vertically from top to bottom as follows: a high-temperature melting zone, a partition temperature gradient zone, and a lower slow cooling zone; the partition (10) is located in the partition temperature gradient zone, and a central through hole is provided on the partition (10); the top of the growth container (3) is located in the high-temperature melting zone, and the bottom of the growth container (3) passes through the central through hole and is located in the lower slow cooling zone; a seed crystal segment or a conical crystal-guiding segment is provided at the bottom of the growth container (3); The upper radiation shaping heat shield (4) is located above the partition (10) and is used to regulate the downward radiation heat flow from the high-temperature melting zone to the center through hole; the lower radiation shaping heat shield (5) is located below the partition (10) and is used to regulate the upward radiation heat flow from the lower slow cooling zone to the center through hole. The upper radiation shaping heat shield (4) and the lower radiation shaping heat shield (5) decouple the temperature gradient near the central through hole from the compensating heating effect of the lower slow cooling zone; The surface metallized quartz support (7) is located below the growth container (3) and connected to the bottom end of the growth container (3); the heat-conducting inner core (8) is located inside the surface metallized quartz support (7) and is used to provide a stable axial heat-conducting path for the bottom end of the growth container (3). The concentric annular heat dissipation cavity (11) is disposed on the outer periphery of the growth container (3) and extends from the temperature gradient region of the partition (10) to the lower slow cooling region; it is used to provide a uniform outer periphery thermal environment to the solidified crystal in the growth container (3) and reduce the circumferential temperature difference and non-axisymmetric thermal disturbance on the outer periphery of the growth container (3). The heating unit is used to provide the required reaction temperature to the high-temperature melting zone and the lower slow cooling zone, and to provide thermal compensation to the upper end and the lower end of the growth container (3).
2. The partition-type crystal growth furnace structure for suppressing cracking of large-size lanthanide halide crystals according to claim 1, characterized in that, The wall thickness of the growth container (3) is 1.5 mm to 8 mm; the minimum inner diameter of the seed crystal segment or the conical crystal guide segment is 0.05 to 0.40 times the crystal diameter; the cone angle of the conical crystal guide segment is 10° to 60°.
3. The partition-type crystal growth furnace structure for suppressing cracking of large-size lanthanide halide crystals according to claim 1, characterized in that, The upper radiation shaping heat shield (4) includes a partition shielding section, a radiation shaping section and a transition section; the partition shielding section is located near the central through hole and is used to regulate the downward radiation heat flow from the high-temperature melting zone to below the central through hole; the radiation shaping section is located on the outer periphery of the growth container (3) and is used to adjust the radial heat flow distribution near the solid-liquid interface; the transition section faces the high-temperature melting zone and is used to gradually transition the melt from the high-temperature melting zone to the partition temperature gradient zone.
4. The partition-type crystal growth furnace structure for suppressing cracking of large-size lanthanide halide crystals according to claim 3, characterized in that, The diameter D1 of the central through hole, the outer diameter D2 of the growth container (3), and the inner diameter D of the furnace chamber of the furnace body are all specified. f The radial distance g between the radiation shaping heat shield and the outer wall of the growth container (3) and the axial position h of the radiation shaping heat shield relative to the partition (10) satisfy the following: The radial spacing g is 0.02 to 0.25 times D2; the axial position h is 0.05 to 0.50 times D2; D1 / D2 is 1.05 to 2.50; (D f -D2) / 2 is 0.05D2 to 1.20D2; The tilt angle θ of the shaping surface of the radiation shaping section relative to the axis of the growth container (3) is 10° to 80°; and the tilt angle θ decreases as the ratio of D1 / D2 increases.
5. The partition-type crystal growth furnace structure for suppressing cracking of large-size lanthanide halide crystals according to claim 4, characterized in that, The surface shape of the upper radiation shaping heat shield (4) is annular, cylindrical, conical, inclined, stepped, arc-shaped or composite; the composite surface is composed of any two or three of the inclined, arc and stepped surfaces, or multiple similar surfaces with different geometric parameters are continuously combined; the similar surfaces are inclined, arc or stepped. The surface shape of the upper radiation shaping heat shield (4) is related to the inner diameter D of the furnace. f The outer diameter D2 of the growth container (3) and the heat flow control requirements satisfy the following: when only axial shielding of the central through hole is required, the surface shape of the upper radiation shaping heat shield (4) is annular; when continuous axisymmetric shielding or guidance is required along the axial direction of the outer periphery of the growth container (3), the surface shape of the upper radiation shaping heat shield (4) is cylindrical; when 0.05D2≤(D f When -D2) / 2≤0.25D2, the surface shape of the upper radiation shaping heat shield (4) is a sloping or conical shape; when 0.25D2<(D f When -D2) / 2≤0.60D2, the surface shape of the upper radiation shaping heat shield (4) is a conical, arc-shaped, stepped, or cylindrical composite structure; when 0.60D2<(D f When -D2) / 2≤1.2D2, the surface shape of the upper radiation shaping heat shield (4) is a composite surface structure; The material of the upper radiation shaping heat shield (4) is one or more of high-temperature resistant metals, high-temperature resistant alloys, and high-temperature resistant ceramic materials; wherein, the high-temperature resistant metal is one or more of molybdenum, tungsten, tantalum, niobium, rhenium, and platinum; the high-temperature resistant alloy is one or more of molybdenum-tungsten alloy, tungsten-rhenium alloy, molybdenum-rhenium alloy, tantalum-tungsten alloy, nickel-based high-temperature alloy, cobalt-based high-temperature alloy, and iron-chromium-aluminum alloy; and the high-temperature resistant ceramic material is one or more of silicon carbide, boron nitride ceramic, aluminum nitride ceramic, alumina ceramic, zirconium oxide ceramic, mullite ceramic, and magnesium oxide ceramic.
6. The partition-type crystal growth furnace structure for suppressing cracking of large-size lanthanide halide crystals according to claim 3, characterized in that, The structure of the lower radiation shaping heat shield (5) is the same as that of the upper radiation shaping heat shield (4), and is mirrored in the horizontal direction of the partition (10). For the lower radiation shaping heat shield (5), the partition shielding section is set close to the central through hole to regulate the upward radiation heat flow from the lower slow cooling zone to the center through hole. The radiation shaping section is set on the outer periphery of the growth container (3) to adjust the radial heat flow distribution near the solid-liquid interface. The transition section faces the lower slow cooling zone to allow the solidified crystal to gradually transition from the partition temperature gradient zone to the lower slow cooling zone.
7. The partition-type crystal growth furnace structure for suppressing cracking of large-size lanthanide halide crystals according to claim 1, characterized in that, The concentric annular heat-spreading cavity (11) includes, from the inside out, an inner heat-conducting and heat-spreading layer, an annular buffer gap layer, and an outer heat-insulating layer; the inner heat-conducting and heat-spreading layer is close to the growth container (3); the thickness of the inner heat-conducting and heat-spreading layer is 2mm~20mm, and the thickness increases with the increase of the crystal diameter; the thickness of the outer heat-insulating layer is 1 to 5 times the thickness of the inner heat-conducting and heat-spreading layer. The inner heat-conducting and temperature-equalizing layer is made of one or more of molybdenum, tungsten, tantalum, boron nitride, silicon carbide, and high-temperature resistant alloy materials. The high-temperature resistant alloy materials include one or more of molybdenum-tungsten alloy, tungsten-rhenium alloy, molybdenum-rhenium alloy, tantalum-tungsten alloy, nickel-based high-temperature alloy, cobalt-based high-temperature alloy, and iron-chromium-aluminum alloy. The outer thermal insulation layer is made of one or more of alumina fiber, zirconium oxide fiber, mullite, boron nitride ceramic, alumina ceramic, aluminum silicate fiber, magnesium oxide ceramic, porous alumina ceramic, calcium oxide-stabilized zirconium oxide ceramic, and other high-temperature resistant insulation materials.
8. The partition-type crystal growth furnace structure for suppressing cracking of large-size lanthanide halide crystals according to claim 1, characterized in that, The surface-metallized quartz support (7) includes a quartz substrate and a metal film layer disposed on the surface of the quartz substrate; the metal film layer is used to reduce the non-designed thermal boundary disturbance caused by heat absorption and re-radiation on the surface of the quartz substrate; the metal film layer is a molybdenum film, tungsten film, platinum film, gold film, nickel film, tantalum film or a composite film layer formed by various metals; the thickness of the metal film layer is 0.1μm to 200μm; The thermally conductive core (8) is made of one or more of the following materials: molybdenum, tungsten, tantalum, silicon carbide, aluminum nitride, boron nitride, aluminum oxide, sapphire, and high-temperature resistant alloys. The high-temperature resistant alloys include one or more of the following: molybdenum-tungsten alloy, tungsten-rhenium alloy, molybdenum-rhenium alloy, tantalum-tungsten alloy, nickel-based high-temperature alloy, cobalt-based high-temperature alloy, and iron-chromium-aluminum alloy. The diameter of the thermally conductive core is 2 mm to 30 mm. The thermally conductive core (8) is connected to the surface metallized quartz support (7) by a high-temperature resistant insulation material, which is alumina-silica fiber paper, high-alumina fiber paper, or quartz wool.
9. The partition-type crystal growth furnace structure for suppressing cracking of large-size lanthanide halide crystals according to claim 1, characterized in that, The heating unit includes a top heater (1), an upper heater (2), a lower heater (6), and a bottom heater (12); the top heater (1) is located above the growth container (3) and is used to provide thermal compensation to the upper end of the growth container (3); the bottom heater (12) is located at the bottom of the growth container (3) and is used to provide thermal compensation to the lower end of the growth container (3); the upper heater (2) is located above the partition (10) and is used to provide the required reaction temperature to the high-temperature melting zone; the lower heater (6) is located at the lower part of the partition (10) and is used to provide the required reaction temperature to the lower slow cooling zone. A lowering mechanism is provided on the outside of the furnace body. The lowering mechanism is connected to the growth container (3) through a surface metallized quartz support (7) and is used to drive the growth container (3) to descend vertically inside the furnace body.
10. A method for growing large-size lanthanide halide crystals, comprising a partition-type crystal growth furnace structure for suppressing cracking of large-size lanthanide halide crystals as described in claim 1, characterized in that... Includes the following steps: Step 1: Load the lanthanide halide raw material into the growth container (3) and seal it under vacuum or inert atmosphere; Step 2: Place the sealed growth container (3) into the furnace body. The top of the growth container (3) is located in the high-temperature melting zone, and the bottom of the growth container (3) passes through the central through hole and is located in the lower slow cooling zone. At the same time, the seed crystal segment or conical crystal-leading segment at the bottom of the growth container (3) is connected to the top of the surface metallized quartz support (7). Step 3: The melting temperature of the lanthanide halide feedstock is T. m The heating unit is activated to raise the temperature of the high-temperature melting zone to T. m + (5℃~100℃) to fully melt the raw materials in the growth container (3); the upper temperature of the temperature gradient zone of the partition is T m ~T m +50℃, the lower end temperature of the temperature gradient zone of the partition is T. m - (10℃~120℃); The upper temperature of the lower slow cooling zone is T m - (50℃~200℃), the lower end temperature of the lower slow cooling zone is T m - (150℃~350℃); Step 4: Adjust the size of the upper radiation shaping heat shield (4) and the lower radiation shaping heat shield (5) to form a temperature gradient zone near the central through hole; at the same time, adjust the output power of the heating unit so that the axial temperature gradient of the partition temperature gradient zone is 5℃ / cm~80℃ / cm, and the temperature difference between the central region and the edge region of the solid-liquid interface in the growth container (3) is controlled within 20℃. Step 5: Drive the growth container (3) to descend along the vertical direction of the furnace body through the external descending mechanism, so that the melt in the growth container (3) enters the temperature gradient zone of the partition from the high temperature melting zone, and completes crystal introduction, shoulder formation and initial solidification near the central through hole of the partition, and gradually forms crystals; Step 6: As the growth container (3) continues to descend, the solidified crystal enters the lower slow cooling zone, where it undergoes circumferential temperature uniformity and low-stress slow cooling under the combined action of the concentric annular heat dissipation cavity (11), the heating unit, and the surface metallized quartz support (7); at the same time, the axial heat-conducting boundary of the seed crystal segment or the conical crystal-leading segment is stabilized by the heat-conducting inner core (8). Step 7: After the crystal has completely solidified, it is annealed in the lower slow cooling zone. The annealing temperature is 150℃~350℃ lower than the melting temperature of the lanthanide halide raw material, and the holding time is 12h~72h. Then, it is slowly cooled to 50℃~120℃ or room temperature at a cooling rate of 5℃ / h~30℃ / h. Heating is stopped and the growth container (3) is removed to obtain large-sized lanthanide halide crystals.
11. A large-size lanthanide halide crystal, prepared using the large-size lanthanide halide crystal growth method described in claim 10, characterized in that... The diameter of the large-sized lanthanide halide crystals is 38 mm or more.
12. The application of the large-size lanthanide halide crystal of claim 11 as a crystal element in the fabrication of lanthanide halide scintillation crystal detectors.
Citation Information
Patent Citations
Method for preparing cerium lanthanum bromide crystal by use of crystal growing device with adjustable temperature field
CN107119315A
Method for preparing lanthanum bromide crystal by using a fully enclosed crucible
CN107268068B
Multi-crucible gradient condensation crystal growth device and method for growing large-size lanthanum bromide single crystal by using same
CN110592659A