A method for preparing PAN / PI composite core-sheath structured pre-oxidized filaments
By simultaneously completing the polymerization, cyclization, pre-oxidation, and imidization of PAN and PI through dry spinning process, combined with a condensation recovery device, the problems of insufficient thermal conductivity and radiation protection properties of PAN fiber and high cost of PI fiber are solved, realizing efficient and low-cost composite fiber production that meets green production standards.
Patent Information
- Application Number
- CN202611355371.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, PAN fibers have high thermal conductivity and poor radiation protection performance, PI fibers have high synthesis costs and are difficult to produce, composite methods have problems such as poor compatibility and complicated processes, dry spinning cannot achieve simultaneous polymerization, cyclization, pre-oxidation and imidization during the spinning process, and the solvent recovery problem has not been effectively solved.
A dry spinning process is adopted, in which the spinning solutions of the skin and core are prepared, and ZrO2 nanoparticles and cyclization catalysts are used to simultaneously complete the polymerization, cyclization, pre-oxidation and imidization of PAN and PI. The solvent is recycled by combining a condensation recovery device to form a PAN and PI composite skin-core structured pre-oxidized filament.
It achieves synergistic optimization of fiber performance, significantly shortens the process, increases production efficiency by 35%, reduces costs by 25%, and achieves a solvent recovery rate of 98%, meeting the requirements of green production. The fiber has excellent high temperature resistance, low thermal conductivity, and radiation protection properties.
Smart Images

Figure CN123108768A_ABST
Abstract
Description
Technical Field
[0001] This application relates to a method for preparing a PAN and PI composite core-sheath structured pre-oxidized filament, belonging to the field of polyacrylonitrile fiber technology. Background Technology
[0002] Polyacrylonitrile (PAN) fiber is widely used in flame-retardant materials, carbon fiber precursors, and other fields. However, pure PAN-based pre-oxidized fibers have drawbacks such as high thermal conductivity, poor radiation protection, and insufficient strength, which limits their application in high-end high-temperature protection and special filtration fields. Polyimide (PI) fiber has excellent high-temperature resistance, extremely low thermal conductivity, and outstanding radiation protection, but its monomer synthesis and spinning costs are high, and large-scale production is difficult, making it difficult to replace PAN fiber on a large scale.
[0003] In existing technologies, in order to make compatible use of the advantages of PAN and PI, the common composite methods are mostly physical blending or surface coating. These composite methods have problems such as poor compatibility between the two phases, weak interfacial bonding, and limited performance improvement. Furthermore, the use of PAN and PI in the core-sheath structure requires wet spinning process, which requires coagulation baths, washing tanks, etc. during the production process. Solvent recovery is difficult, and pre-oxidation and cyclization reactions must be carried out separately after spinning. The process is lengthy, complicated, and has low production efficiency.
[0004] Dry spinning of PAN / PI composites allows for solvent recovery via a conduit, making it easier to achieve green production compared to wet spinning. However, existing dry spinning technologies for preparing PAN / PI composite fibers cannot overcome the technical bottleneck of simultaneously completing polymerization, cyclization, pre-oxidation, and imidization during the spinning process. Therefore, it cannot significantly shorten the process and lacks an efficient solvent recovery system design for dry spinning, resulting in high solvent loss rates and hindering the realization of environmental and cost advantages. Summary of the Invention
[0005] In view of this, this application provides a method for preparing a PAN and PI composite core-shell structured pre-oxidized filament.
[0006] Specifically, this application is implemented through the following scheme: A method for preparing a PAN / PI composite core-sheath structured pre-oxidized filament, comprising the following steps: Step 1: Prepare the spinning solution for the outer layer and the spinning solution for the core layer separately.
[0007] The skin spinning solution is prepared as follows: acrylonitrile (AN) is used as the main monomer, itaconic acid (IA) is used as the comonomer, an initiator, a cyclization catalyst and a solvent are added and mixed to obtain a reaction system with a total monomer (acrylonitrile and itaconic acid) concentration of 18-22 wt%. ZrO2 nanoparticles (accounting for 7-11 wt% of the solid content of the solution) are added, ultrasonically dispersed evenly, heated to 60-70°C, and while stirring the polymerization reaction, a partial cyano cyclization reaction is completed simultaneously to obtain a skin spinning solution with a viscosity of 3000-6000 mPa·s.
[0008] The core spinning solution is prepared as follows: using pyromellitic dianhydride (PMDA) and 4,4'-diaminodiphenyl ether (ODA) as monomers, a solvent is added to prepare a polyamic acid (PAA) solution with a solid content of 12~18wt%; a cyclization accelerator is added, and the mixture is stirred to obtain a core spinning solution with a viscosity of 5000~8000 mPa·s.
[0009] Step 2: The sheath spinning solution and the core spinning solution pass sequentially through the spinning assembly and spinning channel. The spinning temperature (i.e. the temperature of the sheath spinning solution and the core spinning solution) is controlled at 70~90℃ and the spinning speed is 300~700m / min. Simultaneous cyclization and pre-oxidation are carried out during dry spinning to obtain composite precursor fibers.
[0010] The spinneret in the spinning assembly is a core-sheath composite spinneret.
[0011] Hot nitrogen gas is introduced into the spinning channel as a protective medium, and the temperature is controlled in three sections: the first section is the solvent evaporation section, with the temperature controlled at 80~120℃, so that the filaments can quickly remove the solvent; the second section is the synchronous cyclization and pre-oxidation section, with the temperature controlled at 180~230℃, so that the PAN skin layer completes the remaining cyano cyclization and pre-oxidation, and the polyamic acid core layer completes the imidization and cyclization; the third section is the curing and shaping section, with the temperature controlled at 220~260℃, so as to form a stable skin-core structure.
[0012] The total residence time of the filaments formed by the spinning assembly in the spinning channel is 1.5 to 3 minutes.
[0013] Step 3: After the composite filament exits the spinning channel, it is drawn and heat-set to obtain a pre-oxidized filament with a PAN and PI composite core-sheath structure.
[0014] The above-mentioned scheme not only achieves the compatibility of PAN and PI in terms of performance, but also realizes the simultaneous completion of polymerization, cyclization, pre-oxidation and imidization in the preparation process, eliminating the need for a separate pre-oxidation process, greatly reducing the process flow and significantly improving production efficiency; in the dry spinning process, it also realizes the efficient recovery and recycling of solvents, reducing production costs and environmental pressure.
[0015] Furthermore, as a preferred option: In step one: The initiator is azobisisobutyronitrile (AIBN).
[0016] The cyclization catalyst is pyridine.
[0017] The mass ratio of acrylonitrile, itaconic acid, initiator, and cyclization catalyst is 97~99:0.5~2.0:0.2~0.5:0.1~0.3, and preferably 98:1.5:0.3:0.2.
[0018] The cyclization accelerator is a mixture of acetic anhydride and pyridine.
[0019] The content of the cyclization accelerator is 0.5~2.0wt%, and preferably 1wt%.
[0020] The solvent is N,N-dimethylformamide (DMF).
[0021] In step two, The diameter of the spinneret holes on the spinneret plate is 0.15~0.25mm.
[0022] A condensation recovery device is installed at the top of the spinning channel to recover the solvent. The recovered DMF is purified by a distillation column to a purity of ≥99.5%, and can be recycled for the preparation of the skin layer spinning solution and the core layer spinning solution, with a solvent recovery rate of ≥98%. More preferably, the condensation temperature of the condensation recovery device is set to -10~0℃.
[0023] The spinning channel is divided into three temperature control sections: 100℃ (solvent evaporation section) → 220℃ (synchronous cyclization pre-oxidation section) → 240℃ (curing and shaping section).
[0024] In step three, The stretching ratio is 1.1 to 1.3.
[0025] The stretching temperature is 180~220℃ to achieve hot stretching.
[0026] The pre-oxidized filament prepared by the above method has a structure including a skin layer and a core layer, with a mass ratio of skin layer to core layer of 7:3 to 9:1. The skin layer is a polyacrylonitrile-based copolymer pre-oxidized structure, with acrylonitrile as the main component and containing a small amount of copolymer modification units. The core layer is a polyimide resin obtained by imidization of polyamic acid.
[0027] The mass ratio of the cortex to the core can be controlled by the ratio of the cross-sectional area of the cortex to the core channel on the spinneret. For example, if the mass ratio of the cortex to the core is 8:2, then the ratio of the cross-sectional area of the cortex to the core channel is 8:2.
[0028] The pre-oxidized filaments prepared by the above method have the following properties: limiting oxygen index ≥32%, breaking strength ≥4.5cN / dtex, thermal conductivity ≤0.035W / (m·K), and operating temperature ≥350℃.
[0029] Compared with the prior art, the beneficial effects of this application are summarized as follows: (1) The process is greatly shortened and the efficiency is significantly improved. The present invention completes solvent evaporation, PAN polymerization / cyclization / pre-oxidation, and PI precursor imidization and cyclization simultaneously in the dry spinning channel, eliminating the separate pre-oxidation and cyclization processes after spinning in the traditional process. The production cycle is shortened by more than 40%, the production efficiency is increased by 35%, and the production cost is reduced by 25%.
[0030] (2) The performance of the pre-oxidized filament is synergistically optimized. The preparation method of this application takes into account both cost and functional core-sheath structure design, giving full play to the advantages of the two materials: the sheath PAN provides low-cost high-temperature insulation, mature spinning process and large specific surface area; the core PI endows the fiber with excellent temperature resistance, low thermal conductivity and radiation protection performance. The resulting fiber has a limiting oxygen index ≥32%, thermal conductivity ≤0.035W / (m·K), and breaking strength ≥4.5cN / dtex, with no core-sheath delamination.
[0031] (3) Solvent recovery during dry spinning. This application sets up a condensation recovery device at the top of the spinning channel to form a condensation-distillation recovery system adapted to dry spinning. The DMF solvent recovery rate is ≥98%, and the purity of the recycled solvent is ≥99.5%, which greatly reduces solvent loss and environmental treatment costs and meets the requirements of green production.
[0032] The above solution is based on a mature PAN dry spinning process with modifications, exhibiting strong industrial adaptability and ease of large-scale promotion. It requires no large-scale equipment modifications and can be directly adapted to existing production lines; simultaneously, it solves the problem of high cost of pure PI fiber, possessing the potential for large-scale application. Attached Figure Description
[0033] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application.
[0034] Figure 1 This is a SEM image of the pre-oxidized filaments prepared in this application.
[0035] Figure 2 The image shows the EDS diagram of the pre-oxidized filaments prepared in this application. Part (a) of the image shows the overall morphology, and part (b) shows the elemental analysis, where red represents C, purple represents N, yellow represents O, blue represents Si, and orange represents Zr.
[0036] Figure 3 A quantitative bar chart of the elemental composition of the pre-oxidized filaments prepared in this application. Detailed Implementation
[0037] To make the technical problems, technical solutions, and beneficial effects to be solved by this application clearer, the technical solutions in the embodiments of this application will be further described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain this application and are not intended to limit the technical solutions of this application. All other embodiments obtained by those skilled in the art based on the embodiments in this application without creative effort are within the scope of protection of this application.
[0038] Example 1
[0039] This embodiment provides a method for preparing a PAN / PI composite core-sheath structured pre-oxidized filament, the steps of which are as follows: Step 1: Prepare the spinning solution for the outer layer and the spinning solution for the core layer.
[0040] (1) Preparation of the skin spinning solution: Take 98 parts by mass of AN monomer, 1.5 parts by mass of IA monomer, 0.3 parts by mass of AIBN and 0.2 parts by mass of pyridine, add DMF solvent to prepare a reaction system with a total monomer (acrylonitrile and itaconic acid) concentration of 20wt%, add ZrO2 nanoparticles accounting for 9wt% of the solid content of the solution, and disperse evenly by ultrasonication; heat the reaction system to 65℃ and stir for 2.5h to obtain a skin spinning solution with a viscosity of 4500mPa·s.
[0041] (2) Preparation of core spinning solution: PMDA and ODA were added at a molar ratio of 1:1.01, and DMF was added as a solvent to prepare a PAA solution with a solid content of 15wt%; 1wt% acetic anhydride / pyridine (volume ratio 1:1) was added as a cyclization promoter, and the mixture was stirred for 1h to obtain a core spinning solution with a viscosity of 6500mPa·s.
[0042] Step 2: Dry spinning.
[0043] The sheath spinning solution and core spinning solution prepared by the above method are sequentially passed through the spinning assembly and spinning channel to obtain composite raw yarn.
[0044] The spinning temperature (i.e. the temperature of the sheath spinning solution and the core spinning solution) is 80℃, and the spinning speed is 500m / min.
[0045] The spinneret in the spinning assembly is a sheath-core composite spinneret, with a channel cross-sectional area ratio of 8:2 between the sheath and the core, and a spinneret diameter of 0.2 mm.
[0046] A condensation recovery device is installed at the top of the spinning channel to recover the solvent. The condensation temperature is set to -5℃. The recovered DMF has a solvent purity of 99.7% after passing through a distillation column, and the solvent recovery rate is 98.5%.
[0047] Hot nitrogen gas is introduced into the spinning tunnel as a protective medium. The spinning tunnel is divided into three temperature control sections: 100℃ (solvent evaporation section) → 220℃ (synchronous cyclization pre-oxidation section) → 240℃ (curing and shaping section).
[0048] The total residence time of the filaments formed by the spinning assembly in the spinning channel is 2 minutes.
[0049] Step 3: After the composite filament exits the spinning tunnel, it is first hot-drawn at 200℃ and a draw ratio of 1.2, and then heat-set at 110℃ to obtain pre-oxidized filament.
[0050] (1) The microstructure of the obtained pre-oxidized filaments is as follows Figure 1 As shown, its structure exhibits a distinct core-skin type structure.
[0051] (2) The obtained pre-oxidized filaments were subjected to EDS analysis, and the results are as follows: Figure 2 As shown: the C content is approximately 73%, the N content is approximately 4%, the O content is approximately 11%, the Si content is approximately 2%, and the Zr content is approximately 9%. The Zr element originates from ZrO2 nanoparticles added to the cortex spinning solution. The ZrO2 remains structurally stable at the pre-oxidation temperature (220~260℃) and does not decompose. Figure 3 EDS quantitative analysis revealed that the pre-oxidized filament contained 64.6 wt% (73.3 at%) C, 13.2 wt% (12.8 at%) N, and 14.8 wt% (12.6 at%) O, constituting the framework elements of the PAN / PI composite matrix. The Si content was 0.5 wt% (0.3 at%), representing trace impurities. The Zr content was 6.9 wt% (1.0 at%), originating from ZrO2 nanoparticles introduced into the core spinning solution. The O / N atomic ratio was approximately 0.98, close to the theoretical ratio of carbonyl oxygen to imide nitrogen in the PI imide ring (1:1), indicating a relatively complete imidization reaction. Zr was detected as a Zr L-line, consistent with the EDS detection characteristics for heavy elements, and its content was largely consistent with the amount added. The above elemental composition and EDS surface scanning (…) Figure 2 The qualitative results were consistent with those of the above process, confirming the success of PI modification and confirming that the prepared pre-oxidized filament was indeed a PAN-PI composite matrix.
[0052] (3) The performance of the obtained oxidized filaments was tested: breaking strength 5.2 cN / dtex, limiting oxygen index 33.5%, thermal conductivity 0.032 W / (m·K), long-term operating temperature 360℃, and solvent loss rate 1.5%.
[0053] Comparative Example 1
[0054] The setup of this comparative example is the same as that of Example 1, except that: the spinning adopts the traditional wet spinning method (prepared with coagulation agent and water washing), and after spinning, it undergoes separate pre-oxidation (220℃×1h) and PI imidization (300℃×0.5h) treatment.
[0055] Results: The performance indicators were similar to those of Example 1, but the production cycle was longer, the solvent recovery rate was only 75%, the production cost was 30% higher, and the core-shell separation was more likely to occur.
[0056] Comparative Example 2
[0057] This comparative example demonstrates the preparation of pure PAN-based pre-oxidized fibers, i.e., using only the sheath spinning solution without core layer PI modification, and the other parameters are the same as in Example 1.
[0058] Results: The fracture strength is 2.5 cN / dtex, the limiting oxygen index is 28.3%, the thermal conductivity is 0.045 W / (m·K), the long-term operating temperature is only 300℃, and the radiation protection performance is poor.
[0059] The above-described embodiments are merely illustrative of several feasible implementations of the present invention, and their descriptions are relatively specific and detailed. However, they should not be construed as limiting the scope of the present invention, nor are the embodiments intended to limit the scope of protection in the claims of the present invention. For those skilled in the art, various modifications and improvements can be made without departing from the concept of the present invention. All equivalent implementations or changes that do not depart from the present invention should be included in the technology of the present invention.
Claims
1. A method for preparing a PAN / PI composite core-sheath structured pre-oxidized filament, characterized in that, The steps are as follows: Step 1: Prepare the spinning solution for the outer layer and the spinning solution for the core layer separately. The skin spinning solution is prepared as follows: acrylonitrile and itaconic acid are used as monomers, and an initiator, cyclization catalyst, and solvent are added to obtain a reaction system with a total monomer concentration of 18-22 wt%. The system is heated to 60-70°C to carry out the reaction, resulting in a skin spinning solution with a viscosity of 3000-6000 mPa·s. ZrO2 nanoparticles are then added, with a content of 7-11 wt% of the solid content of the skin spinning solution. The core spinning solution is prepared as follows: using pyromellitic dianhydride and 4,4'-diaminodiphenyl ether as monomers, a solvent is added to prepare a polyamic acid solution with a solid content of 12~18wt%; a cyclization accelerator is added, and the mixture is stirred to obtain a core spinning solution with a viscosity of 5000~8000mPa·s. Step two: The sheath spinning solution and the core spinning solution are sequentially passed through the spinning assembly and spinning channel. The spinning temperature is controlled at 70~90℃ and the spinning speed at 300~700m / min. Simultaneous cyclization and pre-oxidation occur during dry spinning to obtain composite precursor fibers. The spinneret in the spinning assembly is a core-sheath composite spinneret. Hot nitrogen gas is introduced into the spinning tunnel as a protective medium, and the temperature is controlled in three sections: 80~120℃, 180~230℃, and 220~260℃. The total residence time in the spinning tunnel is 1.5~3 minutes. Step 3: After the composite filament exits the spinning channel, it is drawn and heat-set to obtain a pre-oxidized filament with a PAN and PI composite core-sheath structure.
2. The method for preparing a PAN / PI composite core-sheath structured pre-oxidized filament according to claim 1, characterized in that: The cyclization catalyst is pyridine, and the cyclization promoter is a mixture of acetic anhydride and pyridine.
3. The method for preparing a PAN / PI composite core-sheath structured pre-oxidized filament according to claim 1, characterized in that: In step one, the mass ratio of acrylonitrile, itaconic acid, initiator, and cyclization catalyst is 97~99:0.5~2.0:0.2~0.5:0.1~0.
3.
4. The method for preparing a PAN / PI composite core-sheath structured pre-oxidized filament according to claim 1, characterized in that: The content of the cyclization accelerator is 0.5~2.0 wt%.
5. The method for preparing a PAN / PI composite core-sheath structured pre-oxidized filament according to claim 1, characterized in that: A condensation and recovery device is installed at the top of the spinning channel to recover the solvent.
6. The method for preparing a PAN / PI composite core-sheath structured pre-oxidized filament according to claim 5, characterized in that: The condensation temperature of the condensation recovery device is set to -10~0℃.
7. The method for preparing a PAN / PI composite core-sheath structured pre-oxidized filament according to claim 1, characterized in that: The stretching ratio is 1.1 to 1.
3.
8. The method for preparing a PAN / PI composite core-sheath structured pre-oxidized filament according to claim 1, characterized in that: The stretching temperature is 180~220℃.
9. The pre-oxidized filament prepared by the method according to any one of claims 1 to 8, characterized in that: It consists of a skin layer and a core layer, with a mass ratio of 7:3 to 9:
1. The skin layer is a pre-oxidized polyacrylonitrile copolymer structure, with acrylonitrile as the main component and containing copolymer modification units. The core layer is a polyimide resin obtained by imidization of polyamic acid.
10. The pre-oxidized filament according to claim 9, characterized in that: The limiting oxygen index of the pre-oxidized filament is ≥32%, the breaking strength is ≥4.5cN / dtex, the thermal conductivity is ≤0.035W / (m·K), and the service temperature is ≥350℃.