A method for sacrificial site treatment of porous substrates containing inorganic particles and organic solvents for alkaline water electrolysis composite membranes, modified substrates, and composite membranes.

By forming a soluble sacrificial occupant layer within the pores of a porous substrate, the problems of air retention and interface separation within the pores of the composite membrane are solved, achieving uniform composite and stable interfacial bonding of high-solids slurry and improving the performance of the alkaline water electrolysis device.

CN123108939APending Publication Date: 2026-11-17HEFEI MEMBRANE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610947858.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing composite membranes are prone to problems such as air retention in pores, lack of wetting, bubbles, voids, interface separation, and uneven filling in pores during the composite process of high solids content inorganic particles and organic solvent slurries. Existing treatment methods cannot effectively solve these problems.

Method used

The sacrificial occupant layer treatment method is adopted. By forming a soluble, swollen and migratable occupant layer on the inner wall of the pores, the edge of the pores and the fiber intersection area of ​​the porous substrate, the mass increase and pore volume ratio are controlled to ensure that no permanent pore-blocking layer is formed during the composite process and is replaced in subsequent processing, thereby promoting the entry of high solids slurry into the pores.

Benefits of technology

It reduces air retention and bubble residue in the pores, improves wetting and interfacial bonding in the pores, enhances the pore connectivity and interfacial bonding stability of the composite diaphragm, is suitable for continuous roll-to-roll processes, and improves bubble point pressure and peel strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108939A_ABST
    Figure CN123108939A_ABST
Patent Text Reader

Abstract

This invention discloses a method for sacrificial site treatment of porous substrates containing high-solids inorganic particles and organic solvents for composite membranes in alkaline water electrolysis, a sacrificial site-modified porous substrate, and a composite membrane. The method includes: providing an alkali-resistant porous substrate with interconnected channels; introducing a site-modifying treatment liquid containing a liquid medium and a layering component into the channels of the alkali-resistant porous substrate; removing excess site-modifying treatment liquid; and, through drying and other treatments, forming a sacrificial site layer on the inner walls of the pores, the edges of the channels, and / or the fiber cross-sections within the pores; composite with a high-solids inorganic particle-containing organic solvent slurry; and, during the composite process, dissolving, swelling, migrating, displacing, dissociating, or removing at least partially the sacrificial site layer, and allowing at least partially of the slurry to enter the channels of the alkali-resistant porous substrate. This invention can reduce air retention, bubbles, voids, unwetting, and interface separation defects within the pores, improving the interfacial bonding stability, bubble point pressure, and particle retention stability of the composite membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical fields of alkaline water electrolysis membrane materials, functional composite membranes, porous substrate interface modification and organic solvent-containing slurry composites. Specifically, it relates to a method for sacrificial site treatment of porous substrates for high solids content inorganic particle organic solvent slurry composites for alkaline water electrolysis composite membranes, the sacrificial site modified porous substrate obtained by the method, and the composite membrane containing the modified porous substrate. Background Technology

[0002] Alkaline water electrolysis hydrogen production devices typically require the use of diaphragm materials to separate the gases generated on the cathode and anode sides, while allowing ion conduction in the electrolyte. As alkaline electrolyzers develop towards higher current density, lower energy consumption, larger size, and longer lifespan, composite diaphragms need to simultaneously possess low sheet resistance, high bubble point pressure, good alkali resistance, and stable interfacial bonding capabilities.

[0003] Existing composite membranes typically use alkali-resistant, inert porous substrates such as polyphenylene sulfide, polytetrafluoroethylene, polyvinylidene fluoride, and polyetheretherketone as a support layer, and coat, impregnate, or composite a high-solids-content inorganic particulate functional slurry containing organic solvents onto the surface and / or channels of the porous substrate. The functional slurry typically contains inorganic particles such as zirconium oxide, titanium oxide, alumina, and barium sulfate, polymer binders, dispersants, and organic solvents such as N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, or dimethyl sulfoxide.

[0004] Because alkali-resistant inert porous substrates such as polyphenylene sulfide, polytetrafluoroethylene, and polyetheretherketone typically have low surface energy and few active sites, the process of high-solids-content inorganic particle organic solvent slurry entering and displacing air within the pores is easily hindered. In particular, problems such as gas retention, localized unwetting, voids, interfacial gaps, discontinuous particle distribution, and debonding of the functional composite layer from the substrate are prone to occur at the pore edges, fiber cross-sections within the pores, and in deep pores.

[0005] Existing cleaning, plasma treatment, hydrophilication treatment, coupling agent treatment, primer treatment, or direct pre-wetting treatment typically aim to improve the wettability of the outer surface or form a permanent modified layer. However, for high-solids slurries containing inorganic particles and organic solvents, simply improving the wettability of the outer surface cannot adequately solve the problems of gas retention and insufficient slurry displacement within the pores; while forming a permanent thick coating may cause pore blockage, reducing the slurry's ability to enter the pores. Therefore, a treatment method is needed that can both temporarily regulate the intrapore interface before slurry lamination and make way for functional slurry components during subsequent slurry lamination or post-treatment. Summary of the Invention

[0006] Furthermore, the sacrificial occupant layer in this invention is not a permanent pore-blocking layer, but rather a layer that can be at least partially dissolved, swollen, migrated, replaced, dissociated, or removed during the processes of compounding, solidification, washing, solvent replacement, or drying. It is distinguished from ordinary permanent pre-coating or pore-filling layers by limiting the increase in mass of the sacrificial occupant layer, the proportion of pore volume it occupies, and the final residual proportion.

[0007] This invention aims to solve the problems of air retention, lack of wetting, bubbles, voids, interface separation, and uneven filling in the pores that easily occur during the composite process of alkali-resistant inert porous substrates and high-solids inorganic particle organic solvent slurries. It provides a method for sacrificial site treatment of porous substrates for composite slurries containing high-solids inorganic particles and organic solvents in alkaline water electrolysis, a sacrificial site modified porous substrate, and an alkaline water electrolysis composite diaphragm.

[0008] To achieve the above objectives, the present invention provides a method for sacrificial site treatment of porous substrates for alkaline water electrolysis composite membranes containing high-solids inorganic particles and organic solvent slurries, comprising the following steps:

[0009] (1) Provide an alkali-resistant porous substrate with interconnected channels; (2) Introduce a locating treatment liquid containing a liquid medium and a layering component into the pores of the alkali-resistant porous substrate, so that the locating treatment liquid contacts the inner wall of the pores, the edge of the pores and / or the fiber crossing area inside the pores. (3) Remove excess treatment liquid from the outer surface, orifice and / or outer side of the pore of the alkali-resistant porous substrate, so that the layering component remains in the inner wall of the pore, the edge of the pore and / or the fiber crossing area inside the pore; (4) The alkali-resistant porous substrate treated with the occupancy treatment liquid is dried, semi-dried, solvent replaced and / or shaped, so that the layered components form a sacrificial occupancy layer, and a sacrificial occupancy modified porous substrate is obtained. (5) The sacrificial site-modified porous substrate is combined with a high-solids-content inorganic particle organic solvent slurry with a solid content of 40 wt% to 90 wt%; (6) During the compounding, coagulation, washing, solvent replacement or drying process, at least part of the sacrificial occupant layer is dissolved, swollen, migrated, replaced, dissociated or removed, and at least part of the high solids content inorganic particle organic solvent slurry enters the pores of the alkali-resistant porous substrate.

[0010] After step (4), the sacrificial occupant layer does not form a permanent continuous plugging layer that closes the orifice, and the orifice blockage area ratio is not higher than 10%; after step (6), the residual ratio of the sacrificial occupant layer relative to the sacrificial occupant layer before composite is 0 to 30%.

[0011] In a preferred embodiment, the alkali-resistant porous substrate is a PPS woven mesh, PPS nonwoven fabric, PTFE porous membrane, PEEK porous membrane, or PVDF porous support membrane.

[0012] In a preferred embodiment, the liquid phase medium is selected from one or more of N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, or γ-butyrolactone; the layering component is selected from one or more of polyvinylpyrrolidone, polyethylene glycol, polyvinyl butyral, polyether, polyetheramine, soluble polysulfone, or soluble polyethersulfone.

[0013] In a preferred embodiment, the layered component can remain on the inner wall of the pores after step (4) and can be at least partially dissolved, swollen or replaced by a high-solids organic solvent slurry containing inorganic particles, organic solvent, coagulant, washing liquid or solvent replacement liquid in step (5) or step (6).

[0014] In a preferred embodiment, the occupancy treatment liquid in step (2) is introduced into the pores of the alkali-resistant porous substrate by dip coating, roller coating, vacuum-assisted wetting, pressure-assisted wetting, circulating wetting or a combination thereof; in step (3), excess occupancy treatment liquid is removed by roller pressing, scraping, squeezing, air knife blowing, negative pressure suction, centrifugal slinging, metering roller control or a combination thereof.

[0015] In a preferred embodiment, the mass increase of the sacrificial occupant layer is 0.2 wt% to 5 wt% of the mass of the alkali-resistant porous substrate, and the sacrificial occupant layer occupies 5% to 30% of the pore volume of the alkali-resistant porous substrate.

[0016] In a preferred embodiment, the sacrificial occupant layer is a thin layer, a semi-continuous layer, an island layer, a dotted layer, a mesh layer, a gel layer, a swellable layer, or a discontinuous occupant layer, and is distributed on the inner wall of the pores, the edge of the pores, and / or the fiber crossing area within the pores.

[0017] In a preferred embodiment, the high-solids-content inorganic particle-organic solvent slurry comprises inorganic particles, a polymer binder, and an organic solvent; the inorganic particles are selected from one or more of zirconium oxide, titanium oxide, aluminum oxide, barium sulfate, or magnesium hydroxide; the polymer binder is selected from polysulfone, polyethersulfone, polyvinylidene fluoride, polyphenylene sulfide, polybenzimidazole, or combinations thereof; and the organic solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, or γ-butyrolactone.

[0018] In a preferred embodiment, the drying, semi-drying, solvent replacement and / or shaping treatment in step (4) includes a multi-stage drying process at 40 °C to 140 °C.

[0019] In a preferred embodiment, the method is implemented in a continuous roll form, wherein the alkali-resistant porous substrate sequentially passes through a pretreatment zone, a immersion zone for site treatment liquid, a liquid control zone, a multi-stage drying zone, a slurry composite zone, a coagulation or solvent replacement zone, a washing zone, a drying zone, and a winding zone.

[0020] The present invention also provides a sacrificial site modified porous substrate, which is prepared by steps (1) to (4) of the above method.

[0021] The present invention also provides an alkaline electrolytic water composite membrane, comprising a porous support layer prepared by the above method and a functional composite layer formed by the high solids content inorganic particle organic solvent slurry, wherein the functional composite layer at least partially enters the pores of the alkali-resistant porous substrate.

[0022] Compared with the prior art, the present invention has at least the following beneficial effects: (1) The present invention pre-occupies the inner wall of the pore, the edge of the pore and / or the fiber crossing area in the pore by sacrificing the occupant layer, which can reduce the air retention and bubble residue in the pore during the subsequent high solids content inorganic particle organic solvent slurry composite process; (2) The sacrificial occupant layer in this invention can be at least partially dissolved, swollen, migrated, replaced, dissociated or removed during the composite, coagulation, washing, solvent replacement or drying process, thereby avoiding the formation of a permanent pore-blocking layer and facilitating the entry of high solids content inorganic particle organic solvent slurry into the pores; (3) By controlling the mass increase of the sacrificial occupant layer, the pore volume ratio, the pore blockage area ratio and the residual ratio, the present invention can maintain the pore connectivity of the porous substrate while improving the wetting and interfacial bonding in the pores. (4) The present invention can reduce pores, unwetted areas and interface separation defects in composite membranes, and improve the interfacial bonding stability between high solids content inorganic particle organic solvent slurry and alkali-resistant porous substrate. (5) This invention is applicable to continuous roll material implementation, which facilitates the connection with the continuous coating, coagulation, washing, drying and winding process of alkaline electrolytic water composite membrane. Attached Figure Description

[0023] Figure 1. Flowchart of the porous substrate sacrificial site treatment method and subsequent slurry composite process described in this invention; Figure 2. Schematic diagram of the formation and subsequent dynamic evolution of the sacrificial occupant layer in various regions of the porous substrate through-hole channel according to the present invention. Figure 3. Schematic diagram comparing the interface state of untreated porous substrate and sacrificial site modified porous substrate during the slurry composite process. Figure 3A shows the state without sacrificial site treatment, and Figure 3B shows the state after sacrificial site treatment. Figure 4. A comparative schematic diagram of the comprehensive performance and state evolution of composite membranes prepared from untreated porous substrates and sacrificial site modified porous substrates. In Figure 4A, the test curves related to interfacial bonding or bubble point pressure are shown. Figure 4B is a bar chart comparing various performances. Figure 4C is a schematic diagram of the sacrificial site layer replacement and composite structure formation process.

[0024] Explanation of reference numerals in the attached figures 1. Porous substrate; 11. Connecting channels; 12. Pore inner wall; 13. Pore opening; 14. Fiber cross-section area within the pore; 2. Placement treatment liquid; 21. Liquid phase medium; 22. Layered component; 3. Sacrificial placer layer; 31. Soluble placer layer; 32. Swellable placer layer; 33. Displaceable placer layer; 4. High solids content slurry containing inorganic particles and organic solvents; 41. Inorganic particles; 42. Polymer binder; 43. Organic solvent; 5. Functional composite layer; 6. Composite membrane; 7. Bubbles or unwetting defects; 8. Interface separation defects; 9. In-pore composite structure; 10. Treatment direction or composite direction; a. State without sacrificial placer treatment; b. State after sacrificial placer treatment; c. Sacrificial placer layer replacement and composite structure formation process. Detailed Implementation The present invention will be further described below with reference to the accompanying drawings and embodiments. It should be understood that the following embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Without departing from the core concept of the present invention, those skilled in the art can adjust the type of substrate, composition of the site treatment liquid, liquid control method, drying conditions, slurry composition, coagulation and washing conditions.

[0025] right Figure 1-4 Explanation: Figure 1 is a schematic diagram of the process of the porous substrate sacrificial occupancy treatment method and the subsequent high solids content inorganic particle organic solvent slurry composite process described in this invention. It is used to illustrate the process of first providing a porous substrate (1) with interconnected channels (11), then introducing an occupancy treatment liquid (2) to make the liquid phase medium (21) and the layered component (22) contact the inner wall (12), the pore opening (13) and the fiber crossing area (14) inside the pore, forming a sacrificial occupancy layer (3) after treatment, and finally composited with a high solids content inorganic particle organic solvent slurry (4) so ​​that the slurry at least partially enters the interconnected channels (11). Figure 2 is a schematic diagram of the structure of the sacrificial occupant layer (3) of the present invention in the pores of the porous substrate (1) and the dissolution, swelling, migration, displacement, dissociation or removal during the subsequent slurry composite process. It is used to show that the sacrificial occupant layer (3) is distributed in the form of a soluble occupant layer (31), a swellable occupant layer (32) or a displaceable occupant layer (33) on the inner wall (12), the pore opening (13) and the fiber cross region (14) in the pore, and is acted on by media such as organic solvent (43) along the processing direction or composite direction (10) to guide the inorganic particles (41) and polymer binder (42) into the pores and contact the pore wall. Figure 3 is a schematic diagram comparing the interface states of untreated porous substrate and sacrificial site modified porous substrate in the composite process of high solids content inorganic particle organic solvent slurry (4). Figure 3A shows the state without sacrificial site treatment (a), which shows the state of bubbles or unwetting defects (7), interface separation defects (8), uneven filling in the pores, and insufficient local interface continuity caused by residual gas in the pores. Figure 3B shows the state after sacrificial site treatment (b), which shows the state of reducing air retention and unwetting areas in the pores by using a replaceable sacrificial site layer (3), so that the slurry components form a more continuous pore composite structure (9) in the connected pores (11). Figure 4 is a schematic diagram comparing the interfacial bonding, bubble point pressure and pore defects of the composite membrane (6) prepared from the untreated porous substrate and the sacrificial occupant modified porous substrate. Figure 4A and Figure 4B respectively show the differences in interfacial bonding performance or bubble point pressure related test performance between the untreated sample and the sacrificial occupant treated sample. Figure 4C is a schematic diagram of the sacrificial occupant layer replacement and composite structure formation process (c), showing the overall transformation mechanism of the sacrificial occupant layer (3) from a temporary occupant state to a continuous pore composite structure (9) and finally solidified into a functional composite layer (5) in the subsequent high solids content inorganic particle organic solvent slurry (4) composite and post-treatment process, so as to reduce pores, bubbles (7), unwetting and interfacial separation defects (8).

[0026] Example 1: PVP / NMP Sacrificial Placement Processing for PPS Woven Net This embodiment includes the following steps: Step 1: A polyphenylene sulfide woven mesh with a thickness of about 300 μm and interconnected pores is provided as an alkali-resistant porous substrate. The mesh is then subjected to ethanol cleaning, deionized water cleaning, and drying at 80 °C in sequence.

[0027] Step 2: Prepare the PVP / NMP occupancy treatment solution by dissolving polyvinylpyrrolidone in N-methylpyrrolidone to achieve a PVP mass fraction of 1.5 wt%. Immerse the dried PPS woven mesh in the PVP / NMP occupancy treatment solution and vacuum-assisted wetting at -80 kPa for 20 min to allow the occupancy treatment solution to penetrate the pores, inner walls of the pores, and fiber cross-sections of the PPS woven mesh.

[0028] Step 3: After removing the PPS woven mesh, remove excess occupant treatment liquid from the outer surface, orifice, and outer side of the channel by air knife blowing and roller pressing, so that the PVP / NMP occupant treatment liquid is mainly retained in the inner wall of the pores, the edge of the channel, and the fiber crossing area.

[0029] Step four involves drying the PPS woven web treated with the spacer treatment solution at 80 °C for 30 min, allowing PPS to form a sacrificial spacer layer on the inner walls of the pores, the edges of the channels, and the fiber cross-sections, thus obtaining a sacrificial spacer modified PPS woven web. The mass increase of the treated sample was approximately 2.1 wt%, and the pore blockage area ratio was less than 8%.

[0030] Step 5: The obtained sacrificial site modified PPS woven web is combined with a high solids content inorganic particulate organic solvent slurry containing zirconium oxide, polysulfone and NMP, wherein the solids content of the slurry is about 75 wt%.

[0031] Step six: During the lamination, coagulation, and washing processes, the sacrificial occupant layer is at least partially dissolved or replaced by the NMP slurry and coagulation solution, allowing the slurry to at least partially enter the PPS woven mesh channels. Compared to the untreated sample, the sacrificial occupant treated sample exhibits reduced air bubbles and unwetted areas within the pores, increased the peel strength of the composite diaphragm from approximately 0.18 N / cm to approximately 0.55 N / cm to 0.65 N / cm, and increased the bubble point pressure from approximately 0.31 MPa to approximately 0.48 MPa to 0.55 MPa.

[0032] Example 2: PVB / NMP sacrificial site treatment on PPS nonwoven fabric This embodiment includes the following steps: Step 1: Provide polyphenylene sulfide nonwoven fabric as an alkali-resistant porous substrate, and perform cleaning, degreasing and drying treatment on it.

[0033] Step 2: Prepare the PVB / NMP site-filling treatment solution by dissolving polyvinyl butyral in a mixed solvent of NMP and ethanol, so that the PVB mass fraction is 0.5 wt% to 3 wt%. Apply the PVB / NMP site-filling treatment solution to the PPS nonwoven fabric via roller coating, and use pressure-assisted methods to force the treatment solution into the pores of the PPS nonwoven fabric.

[0034] Step 3: Remove excess plating solution from the outer surface, openings, and outer sides of the pores of the PPS nonwoven fabric by roller pressing or air knife blowing, so that the PVB / NMP plating solution is mainly retained on the inner wall of the pores and the fiber crossing area.

[0035] Step four: The PPS nonwoven fabric treated with the occupancy treatment liquid is dried with hot air, so that PVB forms a sacrificial occupancy layer in the pores of the PPS nonwoven fabric that can be swollen or replaced by the subsequent NMP slurry, thus obtaining the sacrificial occupancy modified PPS nonwoven fabric.

[0036] Step 5: Composite the obtained sacrificial site modified PPS nonwoven fabric with a zirconium oxide / polyethersulfone slurry containing NMP.

[0037] Step six: During the lamination process, at least part of the sacrificial occupant layer is swollen, migrated, or displaced by NMP, allowing at least part of the high-solids slurry to enter the pores of the PPS nonwoven fabric. After treatment, defects within the pores of the composite diaphragm are reduced, the bubble point pressure increases to approximately 0.46 MPa to 0.52 MPa, and the peel strength increases to approximately 0.45 N / cm to 0.60 N / cm.

[0038] Example 3: PEG oligomer sacrificial site treatment of PPS nonwoven fabric This embodiment includes the following steps: Step 1: Provide PPS nonwoven fabric as an alkali-resistant porous substrate, clean and dry it for later use.

[0039] Step two: Dissolve the polyethylene glycol oligomer in an NMP / ethanol mixed solvent to form a PEG occupancy treatment solution. Immerse the PPS nonwoven fabric in the PEG occupancy treatment solution, and use vacuum-assisted wetting to allow the treatment solution to enter the pores of the PPS nonwoven fabric and contact the inner walls of the pores.

[0040] Step 3: Use a roller pressing method to remove excess PEG occupant treatment liquid from the outer surface and orifice of the PPS nonwoven fabric, so that the PEG occupant treatment liquid is mainly retained in the pore walls and fiber cross-section areas.

[0041] Step 4: Dry the PPS nonwoven fabric treated with the occupancy treatment solution at 40 ℃ to 80 ℃, so that the PEG oligomers remain on the pore walls and fiber cross regions, forming a sacrificial occupancy layer that can be replaced by NMP slurry, and obtain sacrificial occupancy modified PPS nonwoven fabric.

[0042] Step 5: Composite the obtained sacrificial site modified PPS nonwoven fabric with ZrO2 / polysulfone / NMP slurry.

[0043] Step six involves the PEG occupancy layer migrating or dissolving at least partially during slurry compounding and subsequent coagulation or washing, allowing at least partial slurry penetration into the pores. This treatment reduces unwetted areas within the pores, resulting in more continuous slurry spreading and increased peel strength to approximately 0.42 N / cm to 0.58 N / cm.

[0044] Example 4: PES / NMP sacrificial site treatment of PTFE porous membrane This embodiment includes the following steps: Step 1: Provide a polytetrafluoroethylene porous membrane as an alkali-resistant porous substrate, which is then cleaned and dried with ethanol for later use.

[0045] Step 2: Prepare an NMP occupancy treatment solution containing polyethersulfone, and use a pressure-assisted impregnation method to allow the occupancy treatment solution to enter the pores of the PTFE porous membrane and contact the inner wall of the pores.

[0046] Step 3: Remove excess treatment liquid from the surface, pore openings, and outer sides of the PTFE porous membrane by air knife purging.

[0047] Step four: The PTFE porous membrane treated with the occupancy treatment solution is semi-dried to form a thin layer or discontinuous occupancy layer of polyethersulfone on the inner wall of the pores, thus obtaining a sacrificial occupancy modified PTFE porous membrane.

[0048] Step 5: Combine the obtained sacrificial site modified PTFE porous membrane with an inorganic particulate slurry containing NMP.

[0049] Step six: During the slurry lamination process, the occupant layer is at least partially compatible with or displaced by the polymer binder in the slurry, allowing at least partial entry of the functional slurry into the pores of the PTFE porous membrane. After treatment, the interfacial bonding between the PTFE substrate and the functional slurry is improved, and the peel strength increases from approximately 0.08 N / cm to 0.12 N / cm to approximately 0.35 N / cm to 0.48 N / cm.

[0050] Example 5: Low-crosslinking hydrogel-type sacrificial spacer layer treatment for PPS woven web This embodiment includes the following steps: Step 1: Provide PPS woven mesh as an alkali-resistant porous substrate, clean and dry it for later use.

[0051] Step two: Prepare a site-filling treatment solution containing monomers or polymers capable of forming hydrogels, wherein the components include acrylamide monomers, acrylic monomers, polyvinyl alcohol, or combinations thereof. Introduce the site-filling treatment solution into the pores of the PPS woven mesh, ensuring it contacts the inner walls of the pores, the edges of the pores, and the fiber crossing areas.

[0052] Step 3: Remove excess treatment liquid from the outer surface of the PPS woven mesh, the openings, and the outside of the channels.

[0053] Step four: Through free radical polymerization, ionic crosslinking or hydrogen bonding, the components retained in the pores form a low-crosslinking hydrogel-type sacrificial occupant layer, resulting in a sacrificial occupant modified PPS woven web.

[0054] Step 5: Combine the obtained sacrificial site modified PPS woven web with NMP-based high solids content inorganic particle organic solvent slurry.

[0055] Step six involves the subsequent NMP slurry lamination and coagulation process, during which the hydrogel-type sacrificial occupant layer swells, dehydrates, migrates, or is displaced, allowing at least a portion of the slurry to enter the PPS woven mesh pores. This treatment reduces air retention within the pores, decreases large pore defects, and increases the bubble point pressure of the composite diaphragm to approximately 0.48 MPa to 0.56 MPa.

[0056] Example 6: Multi-stage drying sacrificial space-occupying treatment for continuous roll materials This embodiment includes the following steps: Step 1: Provide continuous PPS nonwoven fabric rolls as alkali-resistant porous substrates and feed them into continuous processing equipment.

[0057] Step 2 involves passing the continuous PPS nonwoven fabric roll through the pre-cleaning zone and the immersion zone of the occupancy treatment liquid. The occupancy treatment liquid is a PVP / NMP or PVP / NMP / ethanol mixture system, which allows the occupancy treatment liquid to enter the pores of the PPS nonwoven fabric and contact the inner wall of the pores and the fiber crossing area.

[0058] Step 3: Pass the impregnated PPS nonwoven fabric roll through the roller pressing and squeezing zone to remove excess treatment liquid from the outer surface, orifices, and outside of the channels.

[0059] Step four involves placing the PPS nonwoven fabric roll after liquid control into a multi-stage drying zone, which includes a pre-drying section at 40°C to 60°C, a setting section at 60°C to 90°C, and a post-drying section at 80°C to 120°C. This allows the sacrificial occupant layer to gradually form on the inner wall of the pores, preventing rapid accumulation at the pore openings and resulting in a sacrificial occupant modified PPS nonwoven fabric roll.

[0060] Step 5: The obtained sacrificial site-modified PPS nonwoven fabric roll is continuously compounded with ZrO2 / polysulfone / NMP slurry.

[0061] Step six involves continuous lamination, coagulation, washing, and drying, during which at least a portion of the sacrificial occupant layer is replaced or removed, allowing at least a portion of the slurry to enter the pores of the PPS nonwoven fabric. The resulting composite membrane exhibits improved slurry penetration uniformity in the width direction, with a bubble point pressure stabilizing at approximately 0.45 MPa to 0.54 MPa and a peel strength stabilizing at approximately 0.50 N / cm to 0.66 N / cm.

[0062] Example 7: The effect of the proportion of sacrificial site layer residue on the composite effect This embodiment includes the following steps: Step 1: Provide PPS woven mesh as an alkali-resistant porous substrate.

[0063] Step 2: The PPS woven web is subjected to a sacrificial spacer treatment solution, and modified PPS woven webs with different sacrificial spacer contents are obtained by adjusting the PVP concentration, rolling pressure and drying time.

[0064] Step 3: Remove excess treatment liquid from the outer surface and pore openings of each group of samples, so that the layered components are mainly retained in the inner wall of the pores, the edge of the pores, and the fiber intersection area.

[0065] Step four: Dry or shape each group of samples to form a sacrificial occupant layer from the laminar components.

[0066] Step 5: Each group of sacrificial occupancy modified PPS woven webs is compounded with the same high solids content inorganic particle organic solvent slurry, and the residual proportion of the sacrificial occupancy layer after compounding is controlled to be in the range of 0 to 30%, 30% to 50%, and above 80%, respectively.

[0067] Step six involves evaluating the in-pore composite continuity, bubble point pressure, surface resistivity, and local defects of samples with different residual proportions. The results show that when the residual proportion of the sacrificial occupant layer after composite formation is 0% to 30%, the in-pore composite continuity and bubble point pressure are superior. When the residual proportion is 30% to 50%, some improvement can still be achieved, but stability decreases. When the residual proportion exceeds 80%, some pores exhibit non-replaceable occupant structures, reducing the slurry's ability to enter the pores and increasing the surface resistivity and risk of local defects in the composite membrane. These results indicate that the sacrificial occupant layer should have replaceable characteristics and should not be used as a permanent pore-blocking layer.

[0068] Example 8: Adaptability verification of high solids content slurry This embodiment includes the following steps: Step 1: Provide the sacrificial occupancy modified PPS woven web obtained in Example 1.

[0069] Step 2: Prepare ZrO2 / polysulfone / NMP slurries with solid contents of 40 wt%, 60 wt%, 75 wt%, and 85 wt%, respectively.

[0070] Step 3: The sacrificial occupancy modified PPS woven web is compounded with the above-mentioned slurries with different solid contents.

[0071] Step four involves dissolving, swelling, migrating, displacing, dissociating, or removing at least part of the sacrificial occupant layer during the compounding, coagulation, washing, solvent replacement, or drying process, and allowing at least part of the slurry to enter the PPS woven mesh channels.

[0072] Step 5: Evaluate the presence of air bubbles in the pores, unwetted areas, continuity of the composite within the pores, and the interfacial bonding state of the samples after composite with slurries of different solid contents.

[0073] Step six shows that in a high-solids slurry system of 60 wt% to 85 wt%, PPS woven mesh without sacrificial site treatment is more prone to air bubbles in the pores and local unwetted areas; while sacrificial site modified PPS woven mesh can maintain better intrapore composite continuity and interfacial bonding state, indicating that the present invention is particularly suitable for high-solids slurry composites containing inorganic particles and organic solvents.

[0074] Example 9: Applicability on different alkali-resistant porous substrates This embodiment includes the following steps: Step 1: Select PPS woven mesh, PPS nonwoven fabric, PTFE porous membrane, PVDF porous support mesh and PEEK porous membrane as alkali-resistant porous substrates respectively.

[0075] Step 2: The above-mentioned substrates are subjected to sacrificial occupancy treatment using PVP / NMP, PVB / NMP, PEG / NMP or PES / NMP occupancy treatment solutions respectively, so that the occupancy treatment solution enters the pores of each substrate and contacts the inner wall of the pores, the edge of the pores or the fiber crossing area inside the pores.

[0076] Step 3: Remove excess cleaning solution from the outer surface of each substrate, the openings, and the outside of the channels.

[0077] Step four involves drying, semi-drying, solvent replacement, and / or shaping the substrates treated with the occupant treatment solution to form a replaceable occupant layer on the inner wall of the pores, the edge of the pores, or the fiber cross-section area within the pores.

[0078] Step 5: The obtained porous substrates with different sacrificial occupancy modifications are respectively compounded with the corresponding high solids content inorganic particle organic solvent slurry.

[0079] Step six involves evaluating the defects of intrapore bubbles, voids, and interface separation in the composite sample. The results show that, after sacrificial placement treatment, the aforementioned substrates can all form replaceable occupant layers on the inner walls of pores, at the edges of pores, or in the fiber cross-section areas within the pores. Compared to the corresponding untreated substrates, the defects of intrapore bubbles, voids, and interface separation are reduced after composite treatment, indicating that this invention is applicable to a variety of alkali-resistant inert porous substrates.

[0080] Example 10: Comparison Experiment with Untreated Samples This embodiment includes the following steps: Step 1: Provide PPS woven mesh as an alkali-resistant porous substrate. One group is not subjected to sacrificial site treatment and serves as a control sample; the other group is prepared as a sacrificial site modified PPS woven mesh according to the method of Example 1 and serves as an experimental sample.

[0081] Step 2: The control sample is directly compounded with a high-solids slurry containing zirconium oxide, polysulfone, and NMP to obtain the control composite membrane; the experimental sample is compounded with the same slurry under the same compounding process to obtain the experimental composite membrane.

[0082] Step 3: Perform cross-sectional observation, pore defect statistics, bubble point test, peel strength test and surface resistivity test on the two types of composite diaphragms.

[0083] Step four, the test results showed that, compared with the control composite membrane, the experimental composite membrane had fewer air bubbles, pores and uncomposite areas in the pores, and the distribution of slurry in the PPS woven mesh was more continuous; the bubble point pressure increased from about 0.31 MPa to about 0.48 MPa to 0.55 MPa, the peel strength increased from about 0.18 N / cm to about 0.55 N / cm to 0.65 N / cm, and the sheet resistivity did not show a significant increase.

[0084] Comparative Example 1: Porous substrate without sacrificial site treatment This comparative example includes the following steps: Step 1: Take the same PPS woven web as in Example 1, and perform only cleaning and drying treatments without forming a sacrificial placeholder layer.

[0085] Step 2: The PPS woven mesh is directly composited with ZrO2 / polysulfone / NMP slurry.

[0086] Step 3: Cross-sectional observation of the composite sample. The results showed that some pores, voids, or unwetted areas existed in the composite channels, and the interfacial continuity between the functional composite layer and the substrate pore walls was insufficient in some areas.

[0087] Comparative Example 2: Pre-coating treatment to form a permanent pore-filling layer This comparative example includes the following steps: Step 1: Use PPS woven mesh as the porous substrate.

[0088] Step 2: Use a high-concentration insoluble film-forming solution to pre-coat the outer surface and allow it to dry and cure completely, so that a thicker continuous layer is formed at the orifice.

[0089] Step 3: The pre-coated PPS woven mesh is combined with a high-solids-content inorganic particle organic solvent slurry.

[0090] Step four involves evaluating the pore filling and interface condition of the composite sample. The results show that subsequent slurry entry into the pores is hindered, with some areas exhibiting surface accumulation and insufficient internal filling. Furthermore, the bubble point pressure and interfacial bonding stability did not improve further.

[0091] Comparative Example 3: Pre-wetting treatment with organic solvent only This comparative example includes the following steps: Step 1: Use PPS woven mesh as the porous substrate.

[0092] Step 2: Prewetting is performed using only NMP, without adding any layering components.

[0093] Step 3: The PPS woven web pre-wetted with NMP is combined with a high-solids-content inorganic particle organic solvent slurry.

[0094] Step four involves evaluating the defects within the pores and the interface state of the composite sample. The results show that although the organic solvent can enter the pores for a short time, it cannot form a replaceable temporary site interface during drying or composite processes, thus having limited effect on improving subsequent slurry composite defects.

[0095] Comparative Example 4: Treatment of non-displaceable layered components This comparative example includes the following steps: Step 1: Use PPS woven mesh as the porous substrate.

[0096] Step 2: A non-displaceable layering component that is insoluble, non-swellable, and incompatible with NMP slurry is used to form an internal pre-layer.

[0097] Step 3: The PPS woven mesh with pre-layered holes is combined with a high-solids-content inorganic particle organic solvent slurry.

[0098] Step four involves evaluating the continuity of pore filling in the composite sample. The results show that the pre-layer is difficult to give way to the slurry components during subsequent slurry composite and solidification processes, resulting in poor continuity of pore filling. This indicates that the dissolution, swelling, or compatibility replacement relationship between the sacrificial occupant layer and the subsequent slurry organic solvent is an important condition for achieving the effects of this invention.

[0099] Table 1

[0100] As can be seen from the above embodiments and comparative examples, the present invention, by forming a replaceable sacrificial occupant layer on the inner wall of the pores, the edge of the pores, and / or the fiber intersection area within the pores, can improve the process of high-solids-content inorganic particle-organic solvent slurry entering the pores and the interfacial composite state within the pores. This reduces defects such as bubbles, voids, lack of wetting, uneven filling within the pores, and interfacial separation, thereby improving the interfacial bonding stability and bubble point pressure of the composite membrane. Compared with untreated, solvent-pre-wetting, permanently plugged pore pre-coating, or non-replaceable pre-coating methods, the sacrificial occupant layer of the present invention has temporary occupancy and subsequent clearance characteristics, making it more suitable for high-solids-content slurry composite membranes for alkaline water electrolysis.

[0101] Those skilled in the art, upon considering the specification and practicing this disclosure, can make various modifications, uses, or adaptations to this disclosure without departing from the core concept of the invention. The specification and embodiments are merely exemplary, and the scope of protection of this invention is determined by the claims.

Claims

1. A method for sacrificial site treatment of porous substrates containing inorganic particles and organic solvent slurry for alkaline water electrolysis composite membranes, characterized in that, Includes the following steps: (1) Provide an alkali-resistant porous substrate with interconnected channels; (2) Introduce a locating treatment liquid containing a liquid medium and a layering component into the pores of the alkali-resistant porous substrate, so that the locating treatment liquid contacts the inner wall of the pores, the edge of the pores and / or the fiber crossing area inside the pores. (3) Remove excess treatment liquid from the outer surface, orifice and / or outer side of the pore of the alkali-resistant porous substrate, so that the layering component remains in the inner wall of the pore, the edge of the pore and / or the fiber crossing area inside the pore; (4) The alkali-resistant porous substrate treated with the occupancy treatment liquid is dried, semi-dried, solvent replaced and / or shaped, so that the layered components form a sacrificial occupancy layer, and a sacrificial occupancy modified porous substrate is obtained. (5) The sacrificial site-modified porous substrate is combined with a high-solids-content inorganic particle organic solvent slurry with a solid content of 40 wt% to 90 wt%; (6) During the compounding, coagulation, washing, solvent replacement or drying process, at least part of the sacrificial occupant layer is dissolved, swollen, migrated, replaced, dissociated or removed, and at least part of the high solids content inorganic particle organic solvent slurry enters the pores of the alkali-resistant porous substrate. After step (4), the mass increase of the sacrificial occupant layer is 0.2 wt% to 5 wt% of the mass of the alkali-resistant porous substrate, the sacrificial occupant layer occupies 5% to 30% of the pore volume of the alkali-resistant porous substrate, the sacrificial occupant layer does not form a permanent continuous pore-blocking layer that closes the pore opening, and the pore opening blockage area ratio is not higher than 10%; after step (6), the residual ratio of the sacrificial occupant layer relative to the sacrificial occupant layer before composite is 0 to 30%.

2. The method according to claim 1, characterized in that, The alkali-resistant porous substrate is a PPS woven mesh, PPS nonwoven fabric, PTFE porous membrane, PEEK porous membrane or PVDF porous support membrane.

3. The method according to claim 1, characterized in that, The liquid medium is selected from one or more of N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, or γ-butyrolactone; the layering component is selected from one or more of polyvinylpyrrolidone, polyethylene glycol, polyvinyl butyral, polyether, polyetheramine, soluble polysulfone, or soluble polyethersulfone; the layering component can remain on the inner wall of the pores after step (4), and can be at least partially dissolved, swollen, or replaced by the high-solids-content inorganic particle organic solvent slurry, organic solvent, coagulating liquid, washing liquid, or solvent replacement liquid in step (5) or step (6).

4. The method according to claim 1, characterized in that, In step (2), the occupancy treatment liquid is introduced into the pores of the alkali-resistant porous substrate by dip coating, roller coating, vacuum-assisted wetting, pressure-assisted wetting, circulating wetting or a combination thereof; in step (3), excess occupancy treatment liquid is removed by roller pressing, scraping, squeezing, air knife blowing, negative pressure suction, centrifugal slinging, metering roller control or a combination thereof.

5. The method according to claim 1, characterized in that, The mass increase of the sacrificial occupant layer is 0.2 wt% to 5 wt% of the mass of the alkali-resistant porous substrate, and the sacrificial occupant layer occupies 5% to 30% of the pore volume of the alkali-resistant porous substrate.

6. The method according to claim 1, characterized in that, The sacrificial occupant layer is a thin layer, a semi-continuous layer, an island layer, a dotted layer, a network layer, a gel layer, a swellable layer, or a discontinuous occupant layer, and is distributed on the inner wall of the pore, the edge of the pore, and / or the fiber crossing area inside the pore.

7. The method according to claim 1, characterized in that, The high-solids-content inorganic particle-organic solvent slurry comprises inorganic particles, a polymer binder, and an organic solvent; the inorganic particles are selected from one or more of zirconium oxide, titanium oxide, aluminum oxide, barium sulfate, or magnesium hydroxide; the polymer binder is selected from polysulfone, polyethersulfone, polyvinylidene fluoride, polyphenylene sulfide, polybenzimidazole, or combinations thereof; and the organic solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, or γ-butyrolactone.

8. The method according to claim 1, characterized in that, The drying, semi-drying, solvent replacement and / or shaping treatment in step (4) includes multi-stage drying treatment from 40 ℃ to 140 ℃; and / or, the method is carried out in a continuous roll form, wherein the alkali-resistant porous substrate passes sequentially through a pretreatment zone, a immersion zone for site treatment liquid, a liquid control zone, a multi-stage drying zone, a slurry composite zone, a coagulation or solvent replacement zone, a washing zone, a drying zone and a winding zone.

9. A sacrificial site-modified porous substrate, characterized in that, Prepared by steps (1) to (4) of the method according to any one of claims 1 to 8.

10. An alkaline water electrolysis composite membrane, characterized in that, It includes a porous support layer prepared by the method of any one of claims 1 to 8 and a functional composite layer formed by the high solids content inorganic particle organic solvent slurry, wherein the functional composite layer at least partially enters the pores of the alkali-resistant porous substrate.