A method, apparatus, and composite diaphragm for modifying the inner wall interface of alkali-resistant porous substrates driven by alternating bidirectional pressure differential.
By using an alternating bidirectional pressure differential driving method and heat treatment technology, the problem of uneven modification of the inner wall of porous substrate pores was solved, achieving uniformity of inner wall modification and stability of interface bonding, thus improving the performance of the composite membrane.
Patent Information
- Application Number
- CN202610952354.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-29
- Publication Date
- 2026-11-17
AI Technical Summary
The porous substrate of existing composite membranes has uneven pore wall modification, which leads to uneven pore filling, interface debonding, reduced bubble point pressure and insufficient long-term operational stability. Traditional unidirectional differential pressure treatment tends to result in more deposition on the inlet side and insufficient modification on the outlet side.
An alternating bidirectional pressure differential driving method is adopted to make the interface modification liquid pass through the pores of the alkali-resistant porous substrate multiple times in opposite directions. The pressure differential direction is switched by controlling the cumulative liquid permeation, flow rate decay and liquid level change. Combined with heat treatment and curing treatment, the surface modification components are fixed to the inner wall of the pores.
It improves the uniformity of pore wall modification and the penetration depth of functional slurry, enhances interfacial bonding stability and the bubble point retention ability of composite membrane, and reduces the risk of pore blockage.
Smart Images

Figure CN123108940A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of alkaline water electrolysis membrane materials, functional composite membranes, porous substrate interface modification and continuous processing equipment. Specifically, it relates to a method for modifying the interface of the pore inner wall of an alkali-resistant porous substrate driven by alternating bidirectional pressure difference, an apparatus for implementing the method, an interface-modified porous substrate obtained by the method, and a composite membrane containing the interface-modified porous substrate. Background Technology
[0002] Alkaline water electrolysis hydrogen production devices typically require the use of diaphragm materials to separate the gases on the cathode and anode sides while allowing ion conduction in the electrolyte. As electrolyzers develop towards higher current density, lower energy consumption, larger size, and longer lifespan, composite diaphragms need to simultaneously possess low sheet resistivity, high bubble point pressure, good alkali resistance, and stable interfacial bonding capabilities.
[0003] Existing composite membranes typically use alkali-resistant, inert porous substrates such as polyphenylene sulfide, polyetheretherketone, polytetrafluoroethylene, and polyvinylidene fluoride as the support layer, and then coat, impregnate, or laminate functional slurries containing organic solvents onto their surface and into the pores. Because these porous substrates have low surface energy and few polar sites on their pore walls, the wetting, spreading, and penetration of the functional slurry within the pores are often insufficient, leading to problems such as uneven pore filling, interfacial debonding, reduced bubble point pressure, and insufficient long-term operational stability.
[0004] Traditional immersion, simple surface coating, plasma treatment, or ordinary coupling agent treatment mainly act on the outer surface or shallow pores of porous substrates, making it difficult to ensure that surface modification components uniformly penetrate the inner walls of complex pores in the thickness direction. Although unidirectional pressure differential permeation can promote the entry of the treatment solution into the pores, the treatment solution mainly passes through the porous substrate in a single direction, which easily leads to more deposition on the inlet side, while the outlet side or the deep part of the pores is not sufficiently modified, and the uniformity of modification on the inner walls of the pores is still limited.
[0005] Therefore, there is an urgent need for a method and equipment that enables the interface modification liquid to pass through the pores of the alkali-resistant porous substrate multiple times in opposite directions and to stably fix the surface modification components to the inner wall of the pores after post-treatment, so as to improve the uniformity of the inner wall modification, the penetration depth of the functional slurry, the stability of the interface bonding and the bubble point retention ability of the composite membrane. Summary of the Invention
[0006] Furthermore, this invention combines the first differential pressure, the second differential pressure, the number of alternating cycles, and the bidirectional cumulative permeation volume balance control, which differs from ordinary unidirectional differential pressure wetting or backwashing treatment, and can reduce the problems of inlet-side deposition and outlet-side insufficient modification.
[0007] The purpose of this invention is to provide a method for modifying the interface of the pore inner wall of an alkali-resistant porous substrate driven by alternating bidirectional pressure difference, so as to solve the problems that the pore inner wall of the alkali-resistant inert porous substrate is difficult to be fully wetted by functional slurry containing organic solvent, the unidirectional pressure difference treatment easily leads to more deposition on the inlet side and insufficient modification on the outlet side, uneven modification of the pore inner wall, and insufficient subsequent composite stability.
[0008] To achieve the above objectives, the present invention provides a method for modifying the interface of the pore inner wall of an alkali-resistant porous substrate driven by alternating bidirectional pressure difference, comprising the following steps:
[0009] Step 1: Provide an alkali-resistant porous substrate with communicating channels, and seal and clamp the alkali-resistant porous substrate between a first processing chamber and a second processing chamber that are disposed opposite to each other, so that the alkali-resistant porous substrate constitutes a liquid penetration interface between the first processing chamber and the second processing chamber. Step 2: Introduce an interface modification liquid into the first processing chamber and / or the second processing chamber. The interface modification liquid includes an organic solvent and a surface modification component that can be fixed to the inner wall of the pores. Step 3: Establish a first pressure difference so that the pressure inside the first processing chamber is higher than the pressure inside the second processing chamber, and drive the interface modification liquid to pass through the connecting channels of the alkali-resistant porous substrate along the first direction and contact the inner wall of the pores. Step 4: Switch the pressure difference direction and establish a second pressure difference so that the pressure inside the second processing chamber is higher than the pressure inside the first processing chamber, and drive the interface modification liquid to pass through the connecting channels of the alkali-resistant porous substrate in a second direction opposite to the first direction and contact the inner wall of the pores. Step 5: Repeat steps 3 and 4 as an alternating bidirectional differential pressure cycle, and control the switching of differential pressure direction based on the permeation volume per unit area, flow rate decay, differential pressure decay, changes in liquid level in the treatment chamber, or online permeation volume monitoring signals. Step 6: Remove excess interface modification liquid from the outer surface, pore openings, and / or the outer side of the pores of the alkali-resistant porous substrate; Step 7: Perform heat treatment, crosslinking treatment, curing treatment, anti-solvent treatment, washing and / or drying on the treated alkali-resistant porous substrate to fix the surface modification components to the inner wall of the pores, thereby obtaining an interface-modified porous substrate.
[0010] In a preferred embodiment, the alkali-resistant porous substrate is selected from one or more of PPS, PTFE, PEEK, PVDF and their composite porous substrates.
[0011] In a preferred embodiment, the first pressure difference and the second pressure difference are 30 kPa to 180 kPa, the pressure difference in each direction is maintained for 30 s to 5 min, and the alternating bidirectional pressure difference cycle is repeated for 3 to 10 cycles.
[0012] In a preferred embodiment, the ratio of the cumulative permeation volume in the first direction to the cumulative permeation volume in the second direction is 0.5 to 2.0, and the cumulative permeation volume per unit area in each direction is 0.01 mL / cm² to 50 mL / cm²; and / or the pressure differential treatment is terminated or reduced when the rate of change of permeation volume per unit area in two adjacent alternating bidirectional pressure differential cycles is less than 50%.
[0013] In a preferred embodiment, after treatment, the signal intensity ratio of the surface modification components on the first and second sides of the pore wall in the thickness direction of the alkali-resistant porous substrate is 0.6 to 1.8, the pore blockage area ratio is not higher than 20%, and the liquid permeability retention rate after treatment is not lower than 70% of that before treatment.
[0014] In a preferred embodiment, the surface modification component of the interface modification liquid has a mass fraction of 0.05 wt% to 5 wt%, and the viscosity of the interface modification liquid at the treatment temperature is 2 mPa·s to 500 mPa·s.
[0015] In a preferred embodiment, the organic solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, or γ-butyrolactone; the surface modification component is selected from polysulfone, polyethersulfone, polyvinylpyrrolidone, polyethyleneimine, dopamine, tannic acid, silane coupling agent, or a combination thereof.
[0016] In a preferred embodiment, the method further includes unwinding, dynamic clamping and sealing, alternating bidirectional differential pressure treatment, liquid control, post-treatment, washing, drying and rewinding steps.
[0017] The present invention also provides an interface-modified porous substrate, which is prepared by the above method.
[0018] The present invention also provides an alkaline water electrolysis composite membrane, comprising the above-mentioned interface-modified porous substrate and a functional composite layer located on one or both sides of the interface-modified porous substrate, wherein the functional composite layer at least partially enters the communicating channels of the interface-modified porous substrate and combines with the surface modification components of the pore inner wall.
[0019] The present invention also provides an alternating bidirectional differential pressure interface modification device for implementing the above method, comprising a first processing chamber, a second processing chamber, a porous substrate clamping and sealing assembly, a liquid inlet, a liquid outlet, a pressure regulating system, a modification liquid circulation system, a differential pressure detection assembly, a cumulative liquid permeation monitoring assembly, and a flow direction switching valve group.
[0020] Compared with the prior art, the present invention has at least the following beneficial effects: First, the interface modification liquid can pass through the interconnecting channels of the alkali-resistant porous substrate multiple times in opposite directions, improving the sufficient contact between the inner wall of the pores and the interface modification liquid; Second, by controlling the switching through cumulative permeate volume, flow rate attenuation, pressure difference attenuation, liquid level change, or online permeate volume monitoring signals, it is beneficial to reduce inlet-side deposition and insufficient modification on the outlet side in unidirectional pressure difference treatment; Third, by controlling the liquid and fixing through post-treatment, the surface modification components are retained on the inner wall of the pores, while reducing the risk of pore blockage; Fourth, the resulting interface-modified porous substrate can improve the permeation uniformity, interfacial bonding stability, and bubble point pressure of the composite diaphragm for subsequent functional slurries containing organic solvents. Attached Figure Description
[0021] Figure 1 is a schematic diagram of the overall structure of the alkali-resistant porous substrate pore inner wall interface modification device driven by alternating bidirectional pressure difference according to the present invention.
[0022] Figure 2 is a cross-sectional structural diagram of the first processing cavity, the second processing cavity, and the porous substrate clamping and sealing assembly of the present invention.
[0023] Figure 3 is a schematic diagram of the interface modification liquid passing through the pores of the alkali-resistant porous substrate along the first direction in the first flow state of the present invention.
[0024] Figure 4 is a schematic diagram of the interface modification liquid passing through the pores of the alkali-resistant porous substrate in the second flow state of the present invention along the second direction.
[0025] Figure 5 is a schematic diagram of the process by which the interface modification liquid repeatedly passes through the pores and acts on the inner wall of the pores during the alternating bidirectional pressure differential treatment process of the present invention.
[0026] Figure 6 is a schematic diagram comparing the interface modification states of the pore inner wall of an untreated porous substrate, a porous substrate treated with unidirectional pressure difference, and a porous substrate treated with alternating bidirectional pressure difference according to the present invention.
[0027] Figure 7 is a schematic diagram of the composite membrane prepared using the interface-modified porous substrate of the present invention.
[0028] Figure 8 shows the trend of performance changes under different alternating bidirectional pressure differential cycles, where a represents the trend of permeation time, b represents the trend of peel strength, c represents the trend of interface density, and d represents the trend of bubble point pressure.
[0029] Explanation of reference numerals in the attached drawings: 1. First processing chamber; 2. Second processing chamber; 3. Alkali-resistant porous substrate; 4. Porous substrate clamping and sealing assembly; 5. Flow direction switching valve group; 6. Pressure regulating system; 7. Differential pressure detection assembly; 8. Online monitoring and control system; 9. Unwinding module; 10. Rewinding module; 11. Upper seal; 12. Lower seal; 13. Modifying liquid circulation system; 14. Support mesh plate; 15. Pressing plate; 16. Pressing assembly; 17. First interface; 18. Second interface; 19. High-pressure side; 20. Low-pressure side; 21. Functional composite layer; 22. Interface-modified porous substrate; 23. Pore inner wall interface modification layer; 24. Pore filling area. Detailed Implementation
[0030] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0031] The present invention will be further described below with reference to the accompanying drawings and embodiments. It should be understood that the following embodiments are only used to illustrate the technical solutions and effects of the present invention, and are not intended to limit the scope of protection of the present invention. Without departing from the core concept of the present invention, those skilled in the art can adjust or replace the substrate type, interface modification liquid composition, pressure difference, alternation cycle, post-treatment method, equipment structure, and functional slurry composition.
[0032] In this invention, the term "pore inner wall" refers to the internal channels, fiber gaps, mesh edges, and surfaces surrounding fiber intersections of an alkali-resistant porous substrate, as well as the inner surfaces formed by the interconnected channels. The term "alternating bidirectional pressure differential cycle" refers to a combined process in which the interface modification liquid passes through the channels once in a first direction and once in a second direction. The term "retainable surface modification component" refers to a component that can be retained on the pore inner wall through adsorption, entanglement, deposition, crosslinking, coordination, condensation, hydrogen bonding, polar interactions, or film formation.
[0033] I. Equipment Structure and Processing Procedure As shown in Figures 1 and 2, the alternating bidirectional differential pressure interface modification device of the present invention includes a first processing chamber 1, a second processing chamber 2, a porous substrate clamping and sealing assembly 4, a flow direction switching valve group 5, a pressure regulating system 6, a differential pressure detection assembly 7, an online monitoring and control system 8, an unwinding module 9, a winding module 10, and a modification liquid circulation system 13. The alkali-resistant porous substrate 3 is sealed and clamped between the first processing chamber 1 and the second processing chamber 2 by the porous substrate clamping and sealing assembly 4, such that the first processing chamber 1 and the second processing chamber 2 are located on opposite sides of the alkali-resistant porous substrate 3.
[0034] As shown in Figure 3, in the first flow state, the first processing chamber 1 is the high-pressure side 19, and the second processing chamber 2 is the low-pressure side 20. Under the action of the first pressure difference, the interface modification liquid enters the pores of the alkali-resistant porous substrate 3 from the first processing chamber 1 and passes through the pores along the first direction into the second processing chamber 2. As shown in Figure 4, in the second flow state, the second processing chamber 2 is the high-pressure side 19, and the first processing chamber 1 is the low-pressure side 20. Under the action of the second pressure difference, the interface modification liquid enters the pores of the alkali-resistant porous substrate 3 from the second processing chamber 2 and passes through the pores along the second direction opposite to the first direction into the first processing chamber 1.
[0035] As shown in Figure 5, through the alternating switching of the first and second flow states, the interface modification liquid forms a reciprocating penetration process within the pores. Compared with ordinary immersion treatment, this process can increase the probability of the treatment liquid entering the deep part of the pores; compared with unidirectional pressure difference treatment, this process can reduce the tendency of the modification component to be excessively deposited in the inlet region on one side, so that the inner wall of the pores at different depths can contact the interface modification liquid.
[0036] As shown in Figure 6, the inner walls of untreated porous substrates typically lack a continuous interface modification layer; unidirectional pressure differential treatment of porous substrates may result in excessive modification on the inlet side and insufficient modification on the outlet side; in the alternating bidirectional pressure differential treatment of porous substrates of the present invention, the interface modification layer 23 on the inner walls of the pores can form a relatively uniform distribution along the thickness direction. As shown in Figure 7, when preparing a composite membrane using the interface-modified porous substrate 22 of the present invention, the functional composite layer 21 can be located on one or both sides of the interface-modified porous substrate 22, and at least partially enter the pores to form the pore filling region 24.
[0037] II. Testing Methods Organic solvent contact angle test: The porous substrate before and after treatment is flattened and fixed on the sample stage. The corresponding organic solvent droplets are dropped, and the contact angle between the droplet and the substrate surface is recorded. At least five positions are tested for each sample, and the average value is taken.
[0038] Functional slurry penetration time test: A quantitative amount of functional slurry containing organic solvent is added dropwise to the surface of a porous substrate. The penetration time is defined as the time it takes for the droplet or liquid layer to completely penetrate the pores of the substrate and for no obvious residual liquid surface to form on the surface. Each sample is tested at least three times, and the average value is taken.
[0039] Peel strength test: After the functional composite layer is laminated with the porous substrate, it is cut into strip-shaped specimens and peel tests are performed using a tensile testing device. The peel strength is calculated by dividing the average force during the stable peeling stage by the specimen width.
[0040] Bubble point pressure test: After the composite diaphragm is fully wetted with the test solution, it is fixed in the bubble point test device. The gas pressure is gradually increased, and the pressure at which continuous bubbles appear is taken as the bubble point pressure.
[0041] Orifice blockage area ratio test: The proportion of orifice area that is continuously closed or obviously blocked to the total orifice area is obtained by binary analysis of optical microscopic images or scanning images and statistical processing.
[0042] III. Examples Example 1: NMP / PVP alternating bidirectional pressure difference interface modification of PPS nonwoven fabric Step 1: Provide polyphenylene sulfide nonwoven fabric as an alkali-resistant porous substrate, and seal and clamp the polyphenylene sulfide nonwoven fabric between the first processing chamber and the second processing chamber, so that the polyphenylene sulfide nonwoven fabric constitutes the liquid penetration interface between the first processing chamber and the second processing chamber.
[0043] Step two, prepare the interface modification solution. The interface modification solution includes N-methylpyrrolidone and polyvinylpyrrolidone, wherein the mass fraction of polyvinylpyrrolidone is 2 wt%. The interface modification solution is introduced into the first processing chamber and / or the second processing chamber.
[0044] Step 3: Establish a first pressure difference, making the pressure inside the first processing chamber higher than the pressure inside the second processing chamber. The first pressure difference is 80 kPa, and is maintained for 2 minutes. Drive the interface modification liquid through the connecting channels of the polyphenylene sulfide nonwoven fabric along the first direction and contact the inner wall of the pores.
[0045] Step 4: Switch the pressure difference direction and establish a second pressure difference, so that the pressure in the second processing chamber is higher than the pressure in the first processing chamber. The second pressure difference is 80 kPa, and it is maintained for 2 minutes. Drive the interface modification liquid through the connecting channels of the polyphenylene sulfide nonwoven fabric in a second direction opposite to the first direction and contact the inner wall of the pores.
[0046] Step 5: Repeat steps 3 and 4 as an alternating bidirectional differential pressure cycle for 5 cycles, and control the switching of differential pressure direction based on changes in liquid level and permeation rate in the processing chamber.
[0047] Step 6: Remove the treated polyphenylene sulfide nonwoven fabric and remove excess interface modification liquid from its outer surface, pores, and the outside of the pores.
[0048] Step 7: The polyphenylene sulfide nonwoven fabric obtained in Step 6 is subjected to heat treatment at 80 °C, washing and drying, so that the polyvinylpyrrolidone surface modification component is fixed on the inner wall of the pores, and an interface-modified PPS porous substrate is obtained.
[0049] The results showed that the contact angle of the untreated PPS nonwoven fabric with NMP was about 68°, about 41° after unidirectional pressure difference treatment, and about 23° after treatment in this embodiment; the penetration time of the functional slurry was shortened from about 110 s to about 38 s; the peel strength of the composite diaphragm was about 4.76 N / m, and the bubble point pressure was about 181 kPa.
[0050] Example 2: DMAc / polysulfone alternating bidirectional differential pressure interface modification of PPS mesh Step 1: Provide polyphenylene sulfide mesh as an alkali-resistant porous substrate, and seal and clamp the polyphenylene sulfide mesh between the first processing chamber and the second processing chamber.
[0051] Step 2: Prepare an interface modification solution containing N,N-dimethylacetamide and polysulfone, wherein the polysulfone mass fraction is 3wt%, and introduce the interface modification solution into the first processing chamber and / or the second processing chamber.
[0052] Step 3: Establish the first pressure difference, so that the interface modification liquid passes through the connecting channels of the polyphenylene sulfide mesh along the first direction. The first pressure difference is 100 kPa, and it is maintained for 2 minutes in each direction.
[0053] Step 4: Switch the pressure difference direction and establish a second pressure difference, so that the interface modification liquid passes through the connecting channel in the second direction opposite to the first direction. The second pressure difference is 100 kPa, and each direction is maintained for 2 min.
[0054] Step 5: Repeat the first and second differential pressures as an alternating bidirectional differential pressure cycle for 6 cycles, and control the switching of differential pressure direction based on changes in liquid level and permeation rate in the processing chamber.
[0055] Step 6: Remove excess interface modification liquid from the outer surface and orifices of the polyphenylene sulfide mesh.
[0056] Step 7: The polyphenylene sulfide mesh obtained in Step 6 is heated to 90 °C for shaping, washed with ethanol and dried to fix the polysulfone surface modification components on the inner wall of the pores, thus obtaining the interface-modified PPS mesh.
[0057] The results showed that the contact angle of the PPS mesh with DMAc decreased from about 64° to about 21° after treatment, the penetration time of the functional slurry was shortened from about 105 s to about 35 s, the peel strength of the composite diaphragm was about 4.92 N / m, and the bubble point pressure was about 188 kPa.
[0058] Example 3: DMSO / PEI alternating bidirectional differential pressure interface modification of PPS nonwoven fabric Step 1: Provide PPS nonwoven fabric as an alkali-resistant porous substrate, and seal and clamp the PPS nonwoven fabric between the first processing chamber and the second processing chamber.
[0059] Step 2: Prepare an interface modification solution containing dimethyl sulfoxide and polyethyleneimine, wherein the mass fraction of polyethyleneimine is 1.5 wt%, and introduce the interface modification solution into the first processing chamber and / or the second processing chamber.
[0060] Step 3: Establish the first pressure difference, so that the interface modification liquid passes through the interconnecting channels of the PPS nonwoven fabric along the first direction. The first pressure difference is 60 kPa.
[0061] Step 4: Switch the pressure difference direction and establish a second pressure difference, so that the interface modification liquid passes through the interconnecting channels of the PPS nonwoven fabric in a second direction opposite to the first direction. The second pressure difference is 60 kPa.
[0062] Step 5: Repeat the first and second differential pressures as an alternating bidirectional differential pressure cycle for 4 cycles, and control the switching of differential pressure direction based on the change in liquid level in the processing chamber.
[0063] Step 6: Remove excess interface modification liquid from the outer surface, pores, and outer sides of the PPS nonwoven fabric.
[0064] Step 7: The PPS nonwoven fabric obtained in Step 6 is subjected to 70 °C heat treatment, washing and drying to fix the polyethyleneimine surface modification component on the inner wall of the pores, thus obtaining an interface-modified PPS porous substrate.
[0065] The results showed that the contact angle of the treated PPS nonwoven fabric with DMSO decreased from about 71° to about 28°, the peel strength of the composite diaphragm was about 4.08 N / m, and the bubble point pressure was about 162 kPa.
[0066] Example 4: NMP / Dopamine alternating bidirectional pressure difference interface modification of PPS fiber porous membrane Step 1: Provide a PPS fiber porous membrane as an alkali-resistant porous substrate, and seal and clamp the PPS fiber porous membrane between the first processing chamber and the second processing chamber.
[0067] Step 2: Prepare an interface modification solution containing NMP and dopamine, wherein the mass fraction of dopamine is 1 wt%, and introduce the interface modification solution into the first processing chamber and / or the second processing chamber.
[0068] Step 3: Establish the first pressure difference, so that the interface modification liquid passes through the interconnecting channels of the PPS fiber porous membrane along the first direction. The first pressure difference is 120 kPa.
[0069] Step 4: Switch the pressure difference direction and establish a second pressure difference, so that the interface modification liquid passes through the interconnecting channels of the PPS fiber porous membrane along the second direction. The second pressure difference is 120 kPa.
[0070] Step 5: Repeat the first and second pressure differentials as an alternating bidirectional pressure differential cycle for 8 cycles, and control the switching of the pressure differential direction based on the change in the liquid permeation rate.
[0071] Step 6: Remove excess interface modification solution from the outer surface, pore openings, and outer sides of the PPS fiber porous membrane.
[0072] Step 7: The PPS fiber porous membrane obtained in Step 6 is subjected to weak alkali curing, washing and drying to fix the dopamine surface modification component on the inner wall of the pores.
[0073] The results showed that the contact angle with NMP decreased from about 69° to about 20° after treatment, the peel strength of the composite diaphragm was about 5.18 N / m, and the bubble point pressure was about 196 kPa.
[0074] Example 5: Eutectic Solvent / NMP / PVP Alternating Bidirectional Pressure Difference Interface Modification of PPS Nonwoven Fabric Step 1: Provide PPS nonwoven fabric as an alkali-resistant porous substrate, and seal and clamp the PPS nonwoven fabric between the first processing chamber and the second processing chamber.
[0075] Step 2: Mix choline chloride and urea in a molar ratio of 1:2 to form a eutectic solvent component, add NMP and PVP to form an interface modification solution, wherein the mass fraction of PVP is 2 wt%, and introduce the interface modification solution into the first processing chamber and / or the second processing chamber.
[0076] Step 3: Establish the first pressure difference, so that the interface modification liquid passes through the interconnecting channels of the PPS nonwoven fabric along the first direction. The first pressure difference is 80 kPa.
[0077] Step 4: Switch the pressure difference direction and establish a second pressure difference, so that the interface modification liquid passes through the interconnecting channels of the PPS nonwoven fabric in a second direction opposite to the first direction. The second pressure difference is 80 kPa.
[0078] Step 5: Repeat the first and second differential pressures as an alternating bidirectional differential pressure cycle for 5 cycles, and control the switching of differential pressure direction based on changes in liquid level and permeation rate in the processing chamber.
[0079] Step 6: Remove excess interface modification liquid from the outer surface, pores, and outer sides of the PPS nonwoven fabric.
[0080] Step 7: The PPS nonwoven fabric obtained in Step 6 is subjected to heat treatment at 80 ℃, washing and drying to fix the PVP surface modification components to the inner wall of the pores.
[0081] The results showed that the contact angle of the treated PPS substrate with NMP was approximately 21°, the peel strength of the composite diaphragm was approximately 5.36 N / m, and the bubble point pressure was approximately 203 kPa.
[0082] Example 6: DMF / dopamine-silane alternating bidirectional pressure difference interface modification of PTFE porous membranes Step 1: Provide a polytetrafluoroethylene porous membrane as an alkali-resistant porous substrate, and seal and clamp the polytetrafluoroethylene porous membrane between the first processing chamber and the second processing chamber.
[0083] Step 2: Prepare an interface modification solution containing DMF, dopamine and silane coupling agent, and introduce the interface modification solution into the first processing chamber and / or the second processing chamber.
[0084] Step 3: Establish the first pressure difference, so that the interface modification liquid passes through the interconnecting channels of the polytetrafluoroethylene porous membrane along the first direction. The first pressure difference is 150 kPa.
[0085] Step 4: Switch the pressure difference direction and establish a second pressure difference, so that the interface modification liquid passes through the interconnecting channels of the polytetrafluoroethylene porous membrane in a second direction opposite to the first direction. The second pressure difference is 150 kPa.
[0086] Step 5: Repeat the first and second pressure differentials as an alternating bidirectional pressure differential cycle for 10 cycles, and control the switching of the pressure differential direction based on the change in the liquid permeation rate.
[0087] Step 6: Remove excess interface modification solution from the outer surface, pore openings, and outer sides of the polytetrafluoroethylene porous membrane.
[0088] Step 7: The polytetrafluoroethylene porous membrane obtained in Step 6 is cured, washed, and dried to fix the dopamine-silane surface modification component to the inner wall of the pores.
[0089] The results showed that the contact angle of the untreated PTFE porous membrane with DMF was about 92°, which decreased to about 36° after treatment; the peel strength of the composite membrane increased from about 0.82 N / m to about 3.68 N / m, and the bubble point pressure increased from about 76 kPa to about 142 kPa.
[0090] Example 7: NMP / PAA-PVP alternating bidirectional differential pressure interface modification of PVDF porous membranes Step 1: Provide a polyvinylidene fluoride porous membrane as an alkali-resistant porous substrate, and seal and clamp the polyvinylidene fluoride porous membrane between the first processing chamber and the second processing chamber.
[0091] Step 2: Prepare an interface modification solution containing NMP, polyacrylic acid and polyvinylpyrrolidone, wherein the total mass fraction of polyacrylic acid and polyvinylpyrrolidone is 2.5 wt%, and introduce the interface modification solution into the first processing chamber and / or the second processing chamber.
[0092] Step 3: Establish the first pressure difference, so that the interface modification liquid passes through the interconnecting channels of the polyvinylidene fluoride porous membrane along the first direction. The first pressure difference is 100 kPa.
[0093] Step 4: Switch the pressure difference direction and establish a second pressure difference, so that the interface modification liquid passes through the interconnecting channels of the polyvinylidene fluoride porous membrane along the second direction. The second pressure difference is 100 kPa.
[0094] Step 5: Repeat the first and second differential pressures as an alternating bidirectional differential pressure cycle for 6 cycles, and control the switching of differential pressure direction based on the change in liquid level in the processing chamber.
[0095] Step 6: Remove excess interface modification solution from the outer surface, pore openings, and outer sides of the polyvinylidene fluoride porous membrane.
[0096] Step 7: The polyvinylidene fluoride porous membrane obtained in Step 6 is subjected to heat treatment, washing and drying to fix the polyacrylic acid and polyvinylpyrrolidone surface modification components to the inner wall of the pores.
[0097] The results showed that the contact angle of the PVDF porous membrane with NMP decreased from about 78° to about 26°, the peel strength of the composite membrane was about 3.96 N / m, and the bubble point pressure was about 153 kPa.
[0098] Example 8: γ-Butyrolactone / PES-PVP alternating bidirectional pressure difference interface modification of PEEK porous substrate Step 1: Provide a polyetheretherketone porous substrate as an alkali-resistant porous substrate, and seal and clamp the polyetheretherketone porous substrate between the first processing chamber and the second processing chamber.
[0099] Step 2: Prepare an interface modification solution containing γ-butyrolactone, polyethersulfone and polyvinylpyrrolidone, wherein the total mass fraction of polyethersulfone and polyvinylpyrrolidone is 3 wt%, and introduce the interface modification solution into the first processing chamber and / or the second processing chamber.
[0100] Step 3: Establish a first pressure difference, so that the interface modification liquid passes through the interconnecting channels of the polyether ether ketone porous substrate along the first direction. The first pressure difference is 120 kPa.
[0101] Step 4: Switch the pressure difference direction and establish a second pressure difference, so that the interface modification liquid passes through the interconnecting channels of the polyether ether ketone porous substrate along the second direction. The second pressure difference is 120 kPa.
[0102] Step 5: Repeat the first and second pressure differentials as an alternating bidirectional pressure differential cycle for 7 cycles, and control the switching of the pressure differential direction based on the change in liquid permeation.
[0103] Step 6: Remove excess interface modification liquid from the outer surface, pore openings, and outer sides of the polyetheretherketone porous substrate.
[0104] Step 7: Heat, shape, wash and dry the polyether ether ketone porous substrate obtained in Step 6 to fix the polyether sulfone and polyvinylpyrrolidone surface modification components to the inner wall of the pores.
[0105] The results showed that the contact angle of the PEEK porous substrate with γ-butyrolactone decreased from about 73° to about 30° after treatment, the peel strength of the composite membrane was about 3.84 N / m, and the bubble point pressure was about 151 kPa.
[0106] Example 9: The effect of alternating bidirectional pressure differential cycles on the pore wall modification effect Step 1: Provide PPS nonwoven fabric as an alkali-resistant porous substrate, and seal and clamp the PPS nonwoven fabric between the first processing chamber and the second processing chamber.
[0107] Step 2: Prepare an NMP / PVP interface modification solution, wherein the PVP mass fraction is 2 wt%, and introduce the interface modification solution into the first processing chamber and / or the second processing chamber.
[0108] Step 3: Establish the first pressure difference, so that the interface modification liquid passes through the interconnecting channels of the PPS nonwoven fabric along the first direction. The first pressure difference is 80 kPa.
[0109] Step 4: Switch the pressure difference direction and establish a second pressure difference, so that the interface modification liquid passes through the interconnecting channels of the PPS nonwoven fabric along the second direction. The second pressure difference is 80 kPa.
[0110] Step 5: Take the first pressure difference and the second pressure difference as an alternating bidirectional pressure difference cycle, and set the alternating bidirectional pressure difference cycle to 1, 3, 5 and 10 respectively, and control the switching of pressure difference direction based on the change of liquid permeation.
[0111] Step 6: Remove excess interface modification liquid from the outer surface, pores, and outer sides of the PPS nonwoven fabric.
[0112] Step 7: The PPS nonwoven fabric obtained in Step 6 is subjected to heat treatment at 80 ℃, washing and drying to fix the PVP surface modification components to the inner wall of the pores.
[0113] The results showed that as the alternating bidirectional pressure differential cycle increased, the penetration time of the functional slurry gradually shortened, while the interfacial bonding strength and bubble point pressure gradually increased. When the alternating bidirectional pressure differential cycle reached 5 cycles, the performance improvement tended to stabilize.
[0114] Table 1
[0115] Example 10: Continuous dual-chamber alternating bidirectional pressure differential treatment of PPS nonwoven fabric rolls Step 1: Provide PPS nonwoven fabric rolls as alkali-resistant porous substrates, and allow the PPS nonwoven fabric rolls to enter the dynamic clamping and sealing area between the first and second processing chambers via the unwinding module.
[0116] Step 2: Prepare an NMP / PVP interface modification solution, wherein the PVP mass fraction is 2 wt%, and introduce the interface modification solution into the first processing chamber and / or the second processing chamber.
[0117] Step 3: Establish the first pressure difference, so that the interface modification liquid passes through the connecting channels of the PPS nonwoven fabric roll along the first direction. The first pressure difference is 80 kPa.
[0118] Step 4: Switch the pressure difference direction and establish a second pressure difference, so that the interface modification liquid passes through the connecting channels of the PPS nonwoven fabric roll along the second direction. The second pressure difference is 80 kPa.
[0119] Step 5: Repeat the first and second differential pressures as an alternating bidirectional differential pressure cycle for 5 cycles, and control the switching of differential pressure direction based on the liquid level change in the processing chamber and the online liquid permeation monitoring signal.
[0120] Step 6: Control the liquid in the continuously output PPS nonwoven fabric rolls to remove excess interface modification liquid from the outer surface, orifices, and outside the channels.
[0121] Step 7: The PPS nonwoven fabric roll obtained in Step 6 is heat-set, washed, dried and wound up in sequence to fix the PVP surface modification components to the inner wall of the pores.
[0122] The results showed that the continuously treated PPS nonwoven fabric rolls exhibited good interface modification uniformity along both the width and length directions. The contact angles of samples with NMP at different locations ranged from approximately 22° to 28°, and the penetration times of the functional slurry ranged from approximately 36 s to 43 s.
[0123] Example 11: Comparison of Dual-Cavity Alternating Bidirectional Differential Pressure Treatment and Unidirectional Differential Pressure Treatment Step 1: Provide PPS nonwoven fabric as an alkali-resistant porous substrate, and seal and clamp the PPS nonwoven fabric between the first processing chamber and the second processing chamber.
[0124] Step 2: Prepare an NMP / PVP interface modification solution, wherein the PVP mass fraction is 2 wt%, and introduce the interface modification solution into the first processing chamber and / or the second processing chamber.
[0125] Step 3: Establish the first pressure difference, so that the interface modification liquid passes through the interconnecting channels of the PPS nonwoven fabric along the first direction. The first pressure difference is 80 kPa.
[0126] Step 4: Switch the pressure difference direction and establish a second pressure difference, so that the interface modification liquid passes through the interconnecting channels of the PPS nonwoven fabric along the second direction. The second pressure difference is 80 kPa.
[0127] Step 5: Repeat the first and second pressure differentials as an alternating bidirectional pressure differential cycle for 5 cycles, and control the switching of the pressure differential direction based on the change in liquid permeation. In contrast, the unidirectional pressure differential treatment is set to a pressure differential of 80 kPa, allowing the modifying liquid to pass through the substrate 5 times from the first treatment chamber to the second treatment chamber.
[0128] Step 6: Remove excess interface modification liquid from the outer surface, orifice, and outer side of the pores of the samples treated with alternating bidirectional and unidirectional pressure differential treatments.
[0129] Step 7: The sample obtained in Step 6 is subjected to heat treatment at 80 °C, washing and drying to fix the PVP surface modification components to the inner wall of the pores.
[0130] The results showed that the unidirectional pressure differential treatment sample had the problem of excessive deposition on one side and insufficient modification on the other side. The functional slurry penetration time was approximately 92 s, the peel strength was approximately 2.18 N / m, and the bubble point pressure was approximately 116 kPa. The dual-cavity alternating bidirectional pressure differential treatment sample had more uniform modification of the pore inner wall. The functional slurry penetration time was approximately 38 s, the peel strength was approximately 4.76 N / m, and the bubble point pressure was approximately 181 kPa.
[0131] Example 12: Preparation of alkaline water electrolysis composite membrane using interface-modified PPS porous substrate Step 1: Provide the interface-modified PPS porous substrate obtained in Example 1 as an alkali-resistant porous substrate.
[0132] Step 2: Prepare a functional slurry containing NMP, wherein the functional slurry comprises zirconium oxide inorganic particles, polysulfone film-forming polymer, binder and dispersant.
[0133] Step 3: Apply the functional slurry to one side of the interface-modified PPS porous substrate, so that the functional slurry enters at least part of the interconnecting channels of the interface-modified PPS porous substrate along the first direction.
[0134] Step four: Coating or additional wetting is performed on the other side of the interface-modified PPS porous substrate as needed, so that the functional slurry enters at least part of the connected channels of the interface-modified PPS porous substrate along the second direction.
[0135] Step 5: Control the amount and distribution of functional slurry in the interface-modified PPS porous substrate to enable the functional slurry to bond with the interface modification layer on the inner wall of the pores.
[0136] Step 6: Remove excess slurry from the outer surface and pores of the interface-modified PPS porous substrate.
[0137] Step 7: After drying and shaping, an alkaline electrolytic water composite membrane is obtained.
[0138] The results showed that the peel strength increased from about 1.35 N / m to about 4.80 N / m in the untreated substrate sample, the bubble point pressure increased from about 102 kPa to about 183 kPa, and the sheet resistivity remained at about 0.31 Ω·cm².
[0139] IV. Comparison and Summary of Implementation Results Comparative Example 1: Untreated PPS porous substrate. The contact angle of the untreated PPS nonwoven fabric with NMP is approximately 68°, the functional slurry penetration time is approximately 110 s, the peel strength of the resulting composite membrane is approximately 1.35 N / m, and the bubble point pressure is approximately 102 kPa.
[0140] Comparative Example 2: Standard Immersion Treatment. The same NMP / PVP interface modification solution was used for immersion at normal pressure without differential pressure treatment. Results showed that the functional slurry penetration time was approximately 96 s, the peel strength was approximately 1.62 N / m, and the bubble point pressure was approximately 108 kPa.
[0141] Comparative Example 3: Unidirectional pressure differential treatment. The treatment solution was allowed to penetrate the substrate pores in only one direction, with a pressure differential of 80 kPa and 5 penetration cycles. The results showed that the functional slurry penetration time was approximately 92 s, the peel strength was approximately 2.18 N / m, and the bubble point pressure was approximately 116 kPa.
[0142] Comparative Example 4: Treatment without surface modification components. NMP was used as the treatment solution, without the addition of PVP or other surface modification components. The results showed that the peel strength of the composite membrane was approximately 1.91 N / m, and the bubble point pressure was approximately 113 kPa.
[0143] Comparative Example 5: No post-treatment fixing step. No heat treatment or other post-treatment fixing steps were performed after treatment. The results showed that the peel strength of the composite diaphragm was approximately 2.46 N / m, and the bubble point pressure was approximately 128 kPa.
[0144] Table 2
[0145] As can be seen from the above embodiments and comparative examples, the alternating bidirectional pressure differential treatment of the present invention can significantly improve the uniformity of the modification of the pore inner wall of the alkali-resistant porous substrate and the stability of subsequent composites. Compared with untreated, ordinary immersion, unidirectional pressure differential, no modified components, and no post-treatment fixation schemes, the present invention shows significant improvements in functional slurry penetration time, peel strength, and bubble point pressure.
[0146] This invention can be used in combination with processes such as roller coating, blade coating, dip coating, slot coating, antisolvent deposition, heat setting, washing and drying. It is suitable for the pretreatment, pore wall interface modification and continuous preparation of alkali-resistant porous substrates for alkaline electrolytic water composite membranes, and has good industrial applicability.
Claims
1. An alkaline-resistant porous substrate pore inner wall interface modification method of an alternating bidirectional pressure differential drive, characterized by, Includes the following steps: Step 1: Provide an alkali-resistant porous substrate with communicating channels, and seal and clamp the alkali-resistant porous substrate between a first processing chamber and a second processing chamber that are disposed opposite to each other, so that the alkali-resistant porous substrate constitutes a liquid penetration interface between the first processing chamber and the second processing chamber. Step 2: Introduce an interface modification liquid into the first processing chamber and / or the second processing chamber. The interface modification liquid includes an organic solvent and a surface modification component that can be fixed to the inner wall of the pores. Step 3: Establish a first pressure difference so that the pressure inside the first processing chamber is higher than the pressure inside the second processing chamber, and drive the interface modification liquid to pass through the connecting channels of the alkali-resistant porous substrate along the first direction and contact the inner wall of the pores. Step 4: Switch the pressure difference direction and establish a second pressure difference so that the pressure inside the second processing chamber is higher than the pressure inside the first processing chamber, and drive the interface modification liquid to pass through the connecting channels of the alkali-resistant porous substrate in a second direction opposite to the first direction and contact the inner wall of the pores. Step 5: Repeat steps 3 and 4 as an alternating bidirectional differential pressure cycle, and control the switching of differential pressure direction based on the permeable volume per unit area, flow rate attenuation, differential pressure attenuation, liquid level change in the treatment chamber, or online permeable volume monitoring signal, so that the ratio of the cumulative permeable volume in the first direction to the cumulative permeable volume in the second direction is 0.5 to 2.
0. Step 6: Remove excess interface modification liquid from the outer surface, pore openings, and / or the outer side of the pores of the alkali-resistant porous substrate; Step 7: Perform heat treatment, crosslinking treatment, curing treatment, anti-solvent treatment, washing and / or drying on the treated alkali-resistant porous substrate to fix the surface modification components to the inner wall of the pores, thereby obtaining an interface-modified porous substrate.
2. The method of claim 1, wherein, The alkali-resistant porous substrate is selected from one or more of PPS, PTFE, PEEK, PVDF and their composite porous substrates.
3. The method of claim 1, wherein, The first pressure difference and the second pressure difference are 30 kPa to 180 kPa respectively; the pressure difference in each direction is maintained for 30 s to 5 min; the alternating bidirectional pressure difference cycle is repeated for 3 to 10 cycles.
4. The method of claim 1, wherein, The cumulative permeation volume per unit area in each direction ranges from 0.01 mL / cm² to 50 mL / cm²; and / or the change rate of permeation volume per unit area within two adjacent alternating bidirectional differential pressure cycles is less than 50%, at which point the differential pressure treatment is terminated or reduced.
5. The method of claim 1, wherein, After treatment, the signal intensity ratio of the surface modification components on the first and second sides of the pore wall in the thickness direction of the alkali-resistant porous substrate is 0.6 to 1.8, the pore blockage area ratio is not higher than 20%, and the liquid permeability retention rate after treatment is not lower than 70% of that before treatment.
6. The method of claim 1, wherein, The surface modification component of the interface modification liquid has a mass fraction of 0.05 wt% to 5 wt%, and the viscosity of the interface modification liquid at the treatment temperature is 2 mPa·s to 500 mPa·s.
7. The method of claim 1, wherein, The organic solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, or γ-butyrolactone; the surface modification component is selected from polysulfone, polyethersulfone, polyvinylpyrrolidone, polyethyleneimine, dopamine, tannic acid, silane coupling agent, or a combination thereof.
8. The method of claim 1, wherein, The alkali-resistant porous substrate is a continuous roll material, and the method further includes unwinding, dynamic clamping and sealing, alternating bidirectional pressure differential treatment, liquid control, post-treatment, washing, drying and rewinding steps.
9. An interface-modified porous substrate, characterized by, It is prepared by the method described in any one of claims 1 to 8.
10. An alkaline electrolyzed water composite separator, characterized by, The invention includes the interface-modified porous substrate as described in claim 9 and a functional composite layer located on one or both sides of the interface-modified porous substrate, wherein the functional composite layer at least partially enters the communicating channels of the interface-modified porous substrate and combines with the surface modification components of the pore inner wall.
11. An alternating bi-directional pressure differential interface modification device for implementing the method of any one of claims 1 to 8, characterized in that, It includes a first processing chamber, a second processing chamber, a porous substrate clamping and sealing assembly, a liquid inlet, a liquid outlet, a pressure regulating system, a modification liquid circulation system, a differential pressure detection assembly, a cumulative liquid permeation monitoring assembly, and a flow direction switching valve assembly.