A method for producing wear-resistant traction rope

By employing directional twisting and core forming, double-thread braided sheathing, and heat-shrink tubing processes, the wear resistance and economy of traction ropes under high-strength and high-wear conditions have been solved, achieving a balance between high breaking strength and wear resistance, thus improving operational safety and economy.

CN123108969APending Publication Date: 2026-11-17GUANGDONG POWER TRANSMISSION & TRANSFORMATION ENG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611473836.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing traction ropes cannot balance wear resistance and economy under high-strength and high-wear conditions. Conventional polyester ropes have insufficient wear resistance, while Dyneema ropes are too expensive and difficult to apply efficiently in most construction scenarios.

Method used

The process employs directional twisting and rope core forming, double-thread braided sheath, and heat shrink tubing. directional twisting loosens and rearranges the fiber molecular chains, forming a three-layer sheath. The rope head is then wrapped with wear-resistant transparent heat shrink tubing to ensure that the rope core and sheath work together to bear the load.

Benefits of technology

It improves the breaking strength and abrasion resistance of the towing rope, reduces drag resistance, extends the service life, enhances operational safety and economy, and avoids performance redundancy and waste of procurement costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to a method for producing a wear-resistant traction rope, comprising the following steps: S1, directional twisting and rope core forming; S2, double-wire braided sheath; S3, rope surface treatment; S4, heat shrink tubing installation. This invention, through directional twisting and secondary high-temperature setting processes, ensures that the fibers inside the rope core are tightly and regularly arranged, and the axial structure is highly stable. This eliminates the risk of localized stress concentration under heavy loads, resulting in uniform force transmission throughout the rope, approaching the state of high-strength steel cables. The breaking strength is fully and stably achieved, without any issue of falsely advertised tensile strength. Performance degradation is lower after long-term repeated loads, and load-bearing safety is more reliable. Furthermore, the use of double-wire braiding and high-density interlacing to form a dense, interlocking protective layer outside the rope core significantly improves wear resistance compared to traditional single-wire braiding, effectively preventing fraying and wear. The smooth and flat rope surface reduces drag resistance, improves the grip during construction, and reduces fatigue for maintenance personnel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of traction rope manufacturing technology, and in particular to a method for producing a wear-resistant traction rope. Background Technology

[0002] Traction ropes are core load-bearing tools for all types of high-risk outdoor operations, including overhead power line laying, outdoor infrastructure traction, heavy equipment lifting and hoisting, and emergency rescue in case of sudden dangers.

[0003] Based on the current development status of the domestic engineering consumables market, traction rope products are mainly divided into two major application categories. Each category has limitations in its applicable scenarios, making it difficult to balance universality and cost-effectiveness. One type is the conventional polyester traction rope. This type of product has mature manufacturing technology, wide supply channels, and moderate cost performance, and can meet the basic low-load operation requirements such as short-distance light-load laying and conventional small-item hoisting. However, its material itself has limited physical properties, with obvious shortcomings in ultimate breaking strength, surface abrasion resistance, and repeated use durability. Under harsh conditions such as long-term heavy-load pulling and friction on the edges and corners of rigid towers, the surface is prone to fraying and the core strands are frequently damaged, making it completely unsuitable for high-intensity and high-wear construction operation scenarios such as power grid erection in mountainous areas and laying lines across rivers.

[0004] Another type is the ultra-high molecular weight polyethylene (UHMWPE) traction rope, primarily made of Dyneema. This type of product boasts top-tier tensile strength, abrasion resistance, and lightweight properties, but its high raw material and weaving costs result in high procurement prices. Furthermore, most conventional construction scenarios do not require its extreme load-bearing capacity, and long-term use would lead to significant performance redundancy, substantially increasing project material costs and resulting in poor economic efficiency.

[0005] Therefore, the present invention proposes a method for producing wear-resistant traction rope to solve the above problems. Summary of the Invention

[0006] The technical problem to be solved by the present invention is to provide a method for producing a wear-resistant traction rope, thereby obtaining a traction rope that takes into account high breaking tensile strength stability, excellent surface wear resistance, and economical service life.

[0007] To solve the above-mentioned technical problems, the technical solution of the present invention is: a method for producing a wear-resistant traction rope, the innovation of which is: including the following steps: S1. Directional Twisting and Rope Core Forming: Polyester industrial yarns are twisted in a directional manner after being bundled together, and then woven to form the main body of the rope core. The main body of the rope core is then subjected to a heat setting process and a second high-temperature and high-pressure setting process to allow the fiber molecular chains of the main body of the rope core to fully relax and rearrange. S2, Double-strand braided sheath: The wear-resistant fibers are combined into two single strands. After each single strand is lightly twisted, the two single strands are combined in parallel into a braiding unit and fed into the braiding machine. An interlaced path is used so that the intersections of adjacent braiding units are staggered along the rope axis. Three layers of sheath are braided outside the rope core to obtain the traction rope body. S3. Rope surface treatment: The entire traction rope is smoothed by a pair of polishing rollers to remove burrs and protruding fibers from the rope surface. Then, under constant tension, it is finally heat-set through a continuous heat-setting channel to eliminate the internal stress of the sheath weaving, so that the rope core and sheath form an integral and cooperative load-bearing structure. S4. Heat shrink tubing set: The traction rope body is heat-cut to the required length. After cooling, the surface of the traction rope body end is wiped with anhydrous ethanol to remove oil stains. Wear-resistant transparent heat shrink tubing is then inserted into the end of the traction rope body. After the wear-resistant transparent heat shrink tubing is cured by high temperature heat shrinking, it shrinks radially to tightly wrap the end of the traction rope body. After the wear-resistant transparent heat shrink tubing cools, cable ties are added to lock and fix it, thus obtaining the finished wear-resistant traction rope.

[0008] Furthermore, during the directional twisting in step S1, the twist is set to 80-120 twists / meter, the twist error is controlled within ±2 twists / meter, and the twisting tension is controlled to be 8%~12% of the breaking strength of the strand.

[0009] Furthermore, in step S1, when the rope core body is being woven, the weaving angle is set to 40°~55°, the weaving speed is controlled at 30~50 r / min, and the weaving density is 38~59 intersections per 100m length.

[0010] Furthermore, during the first heat setting in step S1, the rope core body is passed through a continuous heat setting channel under constant tension. The constant tension is 8% to 10% of the breaking tensile force of the rope core body. The first heat setting temperature is set to 125 to 135°C, the first heat setting time is 60 to 90 minutes, and the first heat setting medium is saturated steam or hot air circulation.

[0011] Furthermore, during the secondary high-temperature and high-pressure setting in step S1, the rope core body after the primary heat setting is moved into the high-temperature and high-pressure setting autoclave. The secondary high-temperature and high-pressure setting temperature is set to 140~150℃, the secondary high-temperature and high-pressure setting pressure is set to 0.15~0.20MPa, and the heat preservation and pressure holding time for the secondary high-temperature and high-pressure setting is 40~60 minutes. The rope core body maintains a constant tension state, and the tension of the rope core body is 10%~12% of the breaking tensile force of the rope core body. After the secondary high-temperature and high-pressure setting is completed, the temperature in the high-temperature and high-pressure setting autoclave is reduced at a rate of 2~4℃ / min, and the rope core body is removed naturally when it drops below 80℃.

[0012] Furthermore, in step S2, during the process of weaving a three-layer sheath around the rope core body, the weaving density is 56 to 90 intersections per 100 mm length, the weaving tension is set to 10% to 15% of the strand breaking strength, the weaving angle is 35° to 48°, and the weaving speed is controlled at 25 to 40 r / min. During weaving, the first layer of sheath is woven around the core of the rope to form a sheath with a thickness of 1.0~1.2mm. Then, the second layer of sheath is woven around the first layer of sheath in the opposite direction with a thickness of 1.0~1.2mm. Finally, the third layer of sheath is woven around the second layer of sheath with the same weaving direction as the first layer of sheath and a thickness of 0.5~0.8mm.

[0013] Furthermore, in step S3, the final heat setting temperature is set to 110~120℃, and the setting speed is controlled at 5~10m / min to ensure that the entire traction rope stays in the continuous heat setting channel for ≥15min.

[0014] Furthermore, in step S4, the inner diameter of the wear-resistant transparent heat shrink tubing is 1.2 to 1.4 times the outer diameter of the traction rope, the wall thickness is 1.2 to 1.5 mm, and the length is 100 to 150 mm. When the wear-resistant transparent heat shrink tubing is inserted into the end of the traction rope, the outer end of the wear-resistant transparent heat shrink tubing extends 20 to 30 mm beyond the cut surface of the end of the traction rope.

[0015] The advantages of this invention are: This invention utilizes directional twisting and secondary high-temperature setting processes to achieve a tight and regular fiber arrangement within the rope core, resulting in a highly stable axial structure. This eliminates the risk of localized stress concentration under heavy loads, ensuring uniform force transmission throughout the rope, approaching the state of high-strength steel cables. The breaking strength is fully and stably delivered, eliminating the problem of falsely advertised tensile strength. Performance degradation is lower after long-term repeated loads, making load-bearing safety more reliable. Furthermore, a dense, interlocking protective layer is formed outside the rope core using double-thread braiding and high-density interlacing, significantly improving wear resistance compared to traditional single-thread braiding and effectively preventing fraying and wear. The smooth and flat rope surface reduces drag resistance, improves the grip during construction, and reduces fatigue for maintenance personnel. In addition, the rope end is integrally wrapped with wear-resistant transparent heat-shrink tubing, preventing end wear, fraying, and strand breakage from the source. Damage will not spread axially. The wear-resistant transparent heat-shrink tubing allows for direct inspection of the internal braided structure without disassembly, facilitating pre-shift safety checks. Multiple closed-loop protections enhance the safety of operations throughout the entire lifecycle. Detailed Implementation

[0016] To further illustrate the technical means and effects of the present invention in achieving the intended purpose, the following detailed description of the specific implementation methods, structures, features and effects of the present invention, in conjunction with preferred embodiments, is provided below.

[0017] Example 1 This embodiment provides a method for producing a wear-resistant traction rope, including the following steps: S1. Directional Twisting and Rope Core Forming: After the polyester industrial yarns are plied together, they are uniformly directionally twisted. The twist is set to 100 twists / meter, the twist error is controlled within ±2 twists / meter, and the twisting tension is controlled to 10% of the breaking strength of the strand.

[0018] The core is then woven to form the main body of the rope. During the weaving of the main body of the rope core, the weaving angle is set to 45°, the weaving speed is controlled at 40r / min, and the weaving density is 45 intersections per 100m length.

[0019] After the rope core body undergoes a heat setting process followed by a high-temperature and high-pressure setting process, the fiber molecular chains of the rope core body are fully relaxed and rearranged. During the first heat setting, the main body of the rope core is passed through a continuous heat setting channel under constant tension. The constant tension is 9% of the breaking tensile force of the main body of the rope core. The first heat setting temperature is set to 130℃, the first heat setting time is 80 minutes, and the first heat setting medium is saturated steam.

[0020] During the secondary high-temperature and high-pressure setting, the rope core body after the primary heat setting is transferred into the high-temperature and high-pressure setting autoclave. The secondary high-temperature and high-pressure setting temperature is set to 145℃, the secondary high-temperature and high-pressure setting pressure is set to 0.18MPa, and the heat and pressure holding time for the secondary high-temperature and high-pressure setting is 50 minutes. The rope core body is kept under constant tension, and the tension of the rope core body is 11% of the breaking tensile force of the rope core body. After the secondary high-temperature and high-pressure setting is completed, the temperature in the high-temperature and high-pressure setting autoclave is reduced at a rate of 3℃ / min, and the rope core body is removed naturally when it drops below 80℃.

[0021] S2, Double-strand braided sheath: The wear-resistant fibers are combined into two single strands. After each single strand is lightly twisted, the two single strands are combined in parallel into a braiding unit and fed into the braiding machine. An interlaced path is used so that the intersections of adjacent braiding units are staggered along the rope axis. Three layers of sheath are braided outside the rope core to obtain the traction rope body. During the process of weaving a three-layer sheath around the core, the weaving density is 75 intersections per 100mm length, the weaving tension is set to 13% of the strand breaking strength, the weaving angle is 40°, and the weaving speed is controlled at 36r / min.

[0022] When weaving the sheath, first weave the first layer of sheath around the main body of the rope core, with a thickness of 1.1mm. Then weave the second layer of sheath around the first layer of sheath in the opposite direction, with a thickness of 1.0mm. Finally, weave the third layer of sheath around the second layer of sheath, with the weaving direction of the third layer of sheath being the same as that of the first layer of sheath, and a thickness of 0.6mm.

[0023] S3. Rope Surface Treatment: The entire traction rope is smoothed by a pair of polishing rollers to remove burrs and protruding fibers. Then, under constant tension, it undergoes final heat setting in a continuous heat setting channel to eliminate internal stress in the sheath weaving, making the rope core and sheath form an integral and cooperative load-bearing structure. The final heat setting temperature is set at 115℃, and the setting speed is controlled at 8m / min. The entire traction rope stays in the continuous heat setting channel for 20 minutes.

[0024] S4. Heat Shrink Tubing Set: The traction rope is heat-cut to the required length. After cooling, the end surface of the traction rope is wiped with anhydrous ethanol to remove oil. Abrasion-resistant transparent heat shrink tubing is then inserted into the end of the traction rope. The inner diameter of the tubing is 1.3 times the outer diameter of the traction rope, with a wall thickness of 1.3mm and a length of 140mm. When inserting the tubing, the outer end of the tubing should extend 25mm beyond the cut surface of the traction rope end. After high-temperature heat shrinking and curing, the tubing radially shrinks and tightly wraps around the end of the traction rope. After cooling, cable ties are added to secure the tubing, resulting in the finished abrasion-resistant traction rope.

[0025] Example 2 This embodiment provides a method for producing a wear-resistant traction rope, including the following steps: S1. Directional Twisting and Rope Core Forming: Polyester industrial yarns are twisted in a directional manner after being bundled together. The twist is set to 80 twists / meter, and the twist error is controlled within ±2 twists / meter. The twisting tension is controlled to be 8% of the breaking strength of the strand.

[0026] The core is then woven to form the main body of the rope. During the weaving of the main body of the rope core, the weaving angle is set to 40°, the weaving speed is controlled at 30 r / min, and the weaving density is 40 intersections per 100m length.

[0027] After the rope core body undergoes a heat setting process followed by a high-temperature and high-pressure setting process, the fiber molecular chains of the rope core body are fully relaxed and rearranged. During the first heat setting, the main body of the rope core is passed through a continuous heat setting channel under constant tension. The constant tension is 8% of the breaking tensile force of the main body of the rope core. The first heat setting temperature is set to 125℃, the first heat setting time is 62 minutes, and the first heat setting medium is saturated steam.

[0028] During the secondary high-temperature and high-pressure setting, the rope core body after the primary heat setting is transferred into the high-temperature and high-pressure setting autoclave. The secondary high-temperature and high-pressure setting temperature is set to 140℃, the secondary high-temperature and high-pressure setting pressure is set to 0.15MPa, and the heat and pressure holding time for the secondary high-temperature and high-pressure setting is 40 minutes. The rope core body is kept under constant tension, and the tension of the rope core body is 10% of the breaking tensile force of the rope core body. After the secondary high-temperature and high-pressure setting is completed, the temperature in the high-temperature and high-pressure setting autoclave is reduced at a rate of 2℃ / min, and the rope core body is removed naturally when it drops below 80℃.

[0029] S2, Double-strand braided sheath: The wear-resistant fibers are combined into two single strands. After each single strand is lightly twisted, the two single strands are combined in parallel into a braiding unit and fed into the braiding machine. An interlaced path is used so that the intersections of adjacent braiding units are staggered along the rope axis. Three layers of sheath are braided outside the rope core to obtain the traction rope body. During the process of weaving a three-layer sheath around the core, the weaving density is 58 intersections per 100mm length, the weaving tension is set to 10% of the breaking strength of the strand, the weaving angle is 35°, and the weaving speed is controlled at 25r / min.

[0030] When weaving the sheath, first weave the first layer of sheath around the main body of the rope core, with a thickness controlled at 1.0mm. Then weave the second layer of sheath around the first layer of sheath in the opposite direction, with a thickness controlled at 1.0mm. Finally, weave the third layer of sheath around the second layer of sheath, with the weaving direction of the third layer of sheath being the same as that of the first layer of sheath, and a thickness controlled at 0.5mm.

[0031] S3. Rope Surface Treatment: The entire traction rope is smoothed by a pair of polishing rollers to remove burrs and protruding fibers. Then, under constant tension, it undergoes final heat setting in a continuous heat setting channel to eliminate internal stress in the sheath weaving, making the rope core and sheath form an integral and cooperative load-bearing structure. The final heat setting temperature is set at 110℃, the setting speed is controlled at 5m / min, and the entire traction rope stays in the continuous heat setting channel for 32 minutes.

[0032] S4. Heat Shrink Tubing Set: The traction rope body is heat-cut to the required length. After cooling, the surface of the traction rope end is wiped with anhydrous ethanol to remove oil. Abrasion-resistant transparent heat shrink tubing is then inserted into the end of the traction rope body. The inner diameter of the abrasion-resistant transparent heat shrink tubing is 1.2 times the outer diameter of the traction rope body, the wall thickness is 1.2mm, and the length is 100mm. When inserting the abrasion-resistant transparent heat shrink tubing into the end of the traction rope body, the outer end of the tubing should extend 20mm beyond the cut surface of the traction rope end. After high-temperature heat shrinking and curing, the abrasion-resistant transparent heat shrink tubing radially shrinks and tightly wraps around the end of the traction rope body. After cooling, cable ties are added to lock and secure the tubing, resulting in the finished abrasion-resistant traction rope.

[0033] Example 3 This embodiment provides a method for producing a wear-resistant traction rope, including the following steps: S1. Directional Twisting and Rope Core Forming: Polyester industrial yarns are twisted in a directional manner after being bundled together. The twist is set to 120 twists / meter, and the twist error is controlled within ±2 twists / meter. The twisting tension is controlled to be 12% of the breaking strength of the strand.

[0034] The core is then woven to form the main body of the rope. During the weaving process, the weaving angle is set to 50°, the weaving speed is controlled at 50 r / min, and the weaving density is 58 intersections per 100m length.

[0035] After the rope core body undergoes a heat setting process followed by a high-temperature and high-pressure setting process, the fiber molecular chains of the rope core body are fully relaxed and rearranged. During the first heat setting, the main body of the rope core is passed through a continuous heat setting channel under constant tension. The constant tension is 10% of the breaking tensile force of the main body of the rope core. The first heat setting temperature is set to 135℃, the first heat setting time is 90 minutes, and the first heat setting medium is hot air circulation.

[0036] During the secondary high-temperature and high-pressure setting, the rope core body after the primary heat setting is transferred into the high-temperature and high-pressure setting autoclave. The secondary high-temperature and high-pressure setting temperature is set to 150℃, the secondary high-temperature and high-pressure setting pressure is set to 0.20MPa, and the heat and pressure holding time for the secondary high-temperature and high-pressure setting is 60 minutes. The rope core body is kept under constant tension, and the tension of the rope core body is 12% of the breaking tensile force of the rope core body. After the secondary high-temperature and high-pressure setting is completed, the temperature in the high-temperature and high-pressure setting autoclave is reduced at a rate of 4℃ / min, and the rope core body is removed naturally when it drops below 80℃.

[0037] S2, Double-strand braided sheath: The wear-resistant fibers are combined into two single strands. After each single strand is lightly twisted, the two single strands are combined in parallel into a braiding unit and fed into the braiding machine. An interlaced path is used so that the intersections of adjacent braiding units are staggered along the rope axis. Three layers of sheath are braided outside the rope core to obtain the traction rope body. During the process of weaving a three-layer sheath around the core, the weaving density is 90 intersections per 100mm length, the weaving tension is set to 15% of the breaking strength of the strand, the weaving angle is 48°, and the weaving speed is controlled at 40r / min.

[0038] When weaving the sheath, first weave the first layer of sheath around the main body of the rope core, with a thickness controlled at 1.2mm. Then weave the second layer of sheath around the first layer of sheath in the opposite direction, with a thickness controlled at 1.2mm. Finally, weave the third layer of sheath around the second layer of sheath, with the weaving direction of the third layer of sheath being the same as that of the first layer of sheath, and a thickness controlled at 0.8mm.

[0039] S3. Rope Surface Treatment: The entire traction rope is smoothed by a pair of polishing rollers to remove burrs and protruding fibers. Then, under constant tension, it undergoes final heat setting in a continuous heat setting channel to eliminate internal stress in the sheath weaving, making the rope core and sheath form an integral and cooperative load-bearing structure. The final heat setting temperature is set at 120℃, and the setting speed is controlled at 10m / min. The entire traction rope stays in the continuous heat setting channel for 16 minutes.

[0040] S4. Heat Shrink Tubing Set: The traction rope body is heat-cut to the required length. After cooling, the surface of the traction rope end is wiped with anhydrous ethanol to remove oil. Abrasion-resistant transparent heat shrink tubing is then inserted into the end of the traction rope body. The inner diameter of the abrasion-resistant transparent heat shrink tubing is 1.4 times the outer diameter of the traction rope body, the wall thickness is 1.5mm, and the length is 150mm. When inserting the abrasion-resistant transparent heat shrink tubing into the end of the traction rope body, the outer end of the tubing should extend 30mm beyond the cut surface of the traction rope end. After high-temperature heat shrinking and curing, the abrasion-resistant transparent heat shrink tubing radially shrinks and tightly wraps around the end of the traction rope body. After cooling, cable ties are added to lock and secure the tubing, resulting in the finished abrasion-resistant traction rope.

[0041] The production method of this invention produces 16mm wear-resistant traction ropes with a breaking strength of 113-132kN, which is more than 18.9% higher than the 95kN of conventional polyester braided traction ropes on the market. This significant improvement stems from the synergistic effect of directional twisting of the rope core to unify fiber twist direction and a secondary high-temperature and high-pressure setting process. This results in a tight and regular internal fiber arrangement and a porosity of less than 3%, fundamentally eliminating the risk of localized stress concentration and chain failure, ensuring that the nominal breaking strength is fully and stably achieved without any false labeling issues. The safety margin of 113kN breaking strength fully covers the load requirements of most high-intensity operation scenarios such as mountainous line laying, river crossing traction, and heavy-duty hoisting, avoiding serious performance redundancy and procurement cost waste caused by ultra-high performance, and achieving an optimal balance between safety margin and economy.

[0042] The 16mm abrasion-resistant traction rope produced by the method of this invention achieves 15,369-15,983 surface abrasion cycles under a constant pressure of 5N, which is more than 1.9 times that of conventional polyester braided traction ropes on the market (8,000 cycles). This significant improvement is attributed to the three-dimensional interlocking and dense protective layer formed by the double-thread parallel braiding and high-density interlacing of the sheath, combined with a 3-layer thickened sheath design without penetrating pores, effectively delaying the surface fraying and abrasion process. This abrasion resistance significantly extends the number of cycles a single rope can be used, greatly reducing the frequency of rope replacement and downtime for repairs.

[0043] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A method for producing a wear-resistant traction rope, characterized in that, Includes the following steps: S1. Directional Twisting and Rope Core Forming: Polyester industrial yarns are twisted in a directional manner after being bundled together, and then woven to form the main body of the rope core. The main body of the rope core is then subjected to a heat setting process and a second high-temperature and high-pressure setting process to allow the fiber molecular chains of the main body of the rope core to fully relax and rearrange. S2, Double-strand braided sheath: The wear-resistant fibers are combined into two single strands. After each single strand is lightly twisted, the two single strands are combined in parallel into a braiding unit and fed into the braiding machine. An interlaced path is used so that the intersections of adjacent braiding units are staggered along the rope axis. Three layers of sheath are braided outside the rope core to obtain the traction rope body. S3. Rope surface treatment: The entire traction rope is smoothed by a pair of polishing rollers to remove burrs and protruding fibers from the rope surface. Then, under constant tension, it is finally heat-set through a continuous heat-setting channel to eliminate the internal stress of the sheath weaving, so that the rope core and sheath form an integral and cooperative load-bearing structure. S4. Heat shrink tubing set: The traction rope body is heat-cut to the required length. After cooling, the surface of the traction rope body end is wiped with anhydrous ethanol to remove oil stains. Wear-resistant transparent heat shrink tubing is then inserted into the end of the traction rope body. After the wear-resistant transparent heat shrink tubing is cured by high temperature heat shrinking, it shrinks radially to tightly wrap the end of the traction rope body. After the wear-resistant transparent heat shrink tubing cools, cable ties are added to lock and fix it, thus obtaining the finished wear-resistant traction rope.

2. The method for producing the wear-resistant traction rope according to claim 1, characterized in that, In step S1, when directional twisting is performed, the twist is set to 80-120 twists / meter, the twist error is controlled within ±2 twists / meter, and the twisting tension is controlled to be 8%~12% of the breaking strength of the strand.

3. The method for producing the wear-resistant traction rope according to claim 1, characterized in that, In step S1, when the rope core body is being woven, the weaving angle is set to 40°~55°, the weaving speed is controlled at 30~50 r / min, and the weaving density is 38~59 intersections per 100m length.

4. The method for producing the wear-resistant traction rope according to claim 1, characterized in that, In step S1, during the first heat setting, the rope core body is passed through a continuous heat setting channel under constant tension. The constant tension is 8% to 10% of the breaking tensile force of the rope core body. The first heat setting temperature is set to 125 to 135°C, and the first heat setting time is 60 to 90 minutes. The first heat setting medium is saturated steam or hot air circulation.

5. The method for producing the wear-resistant traction rope according to claim 1, characterized in that, In step S1, during the secondary high-temperature and high-pressure setting, the rope core body after the primary heat setting is transferred into the high-temperature and high-pressure setting autoclave. The secondary high-temperature and high-pressure setting temperature is set to 140~150℃, and the secondary high-temperature and high-pressure setting pressure is set to 0.15~0.20MPa. The heat preservation and pressure holding time for the secondary high-temperature and high-pressure setting is 40~60 minutes. The rope core body maintains a constant tension state, and the tension of the rope core body is 10%~12% of the breaking tensile force of the rope core body. After the secondary high-temperature and high-pressure setting is completed, the temperature in the high-temperature and high-pressure setting autoclave is reduced at a rate of 2~4℃ / min, and the rope core body is removed naturally when it drops below 80℃.

6. The method for producing the wear-resistant traction rope according to claim 1, characterized in that, In step S2, during the process of weaving three layers of sheath outside the rope core body, the weaving density is 56 to 90 intersections per 100 mm length, the weaving tension is set to 10% to 15% of the strand breaking strength, the weaving angle is 35° to 48°, and the weaving speed is controlled at 25 to 40 r / min. During weaving, the first layer of sheath is woven around the core of the rope to form a sheath with a thickness of 1.0~1.2mm. Then, the second layer of sheath is woven around the first layer of sheath in the opposite direction with a thickness of 1.0~1.2mm. Finally, the third layer of sheath is woven around the second layer of sheath with the same weaving direction as the first layer of sheath and a thickness of 0.5~0.8mm.

7. The method for producing the wear-resistant traction rope according to claim 1, characterized in that, In step S3, the final heat setting temperature is set to 110~120℃, and the setting speed is controlled at 5~10m / min to ensure that the entire traction rope stays in the continuous heat setting channel for ≥15min.

8. The method for producing the wear-resistant traction rope according to claim 1, characterized in that, In step S4, the inner diameter of the wear-resistant transparent heat shrink tubing is 1.2 to 1.4 times the outer diameter of the traction rope, the wall thickness is 1.2 to 1.5 mm, and the length is 100 to 150 mm. When the wear-resistant transparent heat shrink tubing is inserted into the end of the traction rope, the outer end of the wear-resistant transparent heat shrink tubing extends 20 to 30 mm beyond the cut surface of the end of the traction rope.