A sapphire FP cavity sensing chip for fiber optic vibration sensors and its fabrication method

By designing and fabricating a full sapphire FP cavity sensing chip, the problems of insufficient temperature resistance and lateral interference of vibration sensors in high-temperature environments have been solved, enabling accurate measurement and miniaturization at high temperatures, making it suitable for high-temperature in-situ detection of aero-engines.

CN123111445APending Publication Date: 2026-11-17NO 49 INST CHINESE ELECTRONICS SCI & TECH GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611287300.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing vibration sensors have insufficient temperature resistance in high-temperature environments, weak structural resistance to lateral interference, and are difficult to adapt to the confined space inside aero engines. Furthermore, the immature manufacturing process leads to large measurement errors and a high false alarm rate, making it impossible to achieve in-situ detection at high temperatures.

Method used

The sensor chip employs an all-sapphire FP cavity, using C-axis sapphire single crystal material and a four-beam-double-film-central mass block structure. The FP interference cavity is formed through sapphire direct bonding process. Combined with SiO2/Si3N4/Al composite mask system and deep and shallow trench ICP etching process, the chip achieves high-temperature stability and miniaturization.

Benefits of technology

It achieves stable operation in high-temperature environments of 800℃~1200℃, reduces measurement errors, improves installation adaptability and measurement accuracy, meets the requirements of high-temperature in-situ testing of aero-engines, and has the capability for high-yield mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123111445A_ABST
    Figure CN123111445A_ABST
Patent Text Reader

Abstract

This invention discloses an all-sapphire F-P cavity sensing chip for fiber optic vibration sensors and its fabrication method, belonging to the field of fiber optic MEMS sensing technology. The sensing chip is composed of three layers of C-oriented sapphire single-crystal components bonded together: an upper cover, a main chip, and a lower cover. The main chip adopts a four-beam-double-film-central mass block constraint structure, with elastic beams and elastic films collaboratively constraining the mass block to suppress lateral vibration and torsional interference. All components are fabricated using C-oriented sapphire wafers, which can withstand high temperatures up to 800~1200℃. The fabrication process employs an integrated process of SiO2 / Si3N4 / Al composite masking, step-by-step ICP deep and shallow trench etching, back-side microstructure release, and direct sapphire bonding. This invention solves the defects of traditional piezoelectric and silicon-based sensors, such as high-temperature failure and poor anti-interference. The structure is miniaturized, and the sensor can achieve wideband vibration detection of 0~3kHz with a measurement range of 1g~10g, suitable for in-situ vibration fault monitoring of high-temperature aero-engines.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of fiber optic sensing and MEMS (Micro-Electro-Mechanical Systems) technology, and particularly relates to an all-sapphire FP cavity sensing chip for fiber optic vibration sensors and its fabrication method. Background Technology

[0002] Vibration sensors are devices that can sense and detect vibration changes in a measured object and convert the physical quantity of vibration into an electrical signal that is easy to collect and process. In the field of aircraft engine health monitoring, statistics show that more than 70% of mechanical failures in aircraft engines manifest as vibration. Vibration signals can directly reflect the operating status of key components such as aircraft engine rotors and blades, providing important data for early fault identification and performance evaluation. Therefore, vibration monitoring is the most reliable technical means for aircraft engine fault diagnosis, and vibration sensors are the core key components for achieving in-situ vibration monitoring of aircraft engines.

[0003] Currently, piezoelectric vibration sensors are the mainstream vibration sensors used in aero-engine vibration detection applications. Piezoelectric sensors rely on the piezoelectric effect of piezoelectric materials to convert vibration into electrical signals. However, these sensors exhibit several inherent drawbacks under the harsh operating conditions inside high-temperature aero-engines. First, the piezoelectric materials themselves have limited high-temperature resistance; the piezoelectric effect significantly attenuates or even disappears at high temperatures, making in-situ vibration measurements impossible in environments above 800°C. This makes them unsuitable for direct detection inside high-temperature aero-engines, limiting their placement to relatively cooler outer shell areas and failing to capture true vibration information from hot-end components. Second, traditional piezoelectric sensor probes have a large overall structure, while the available installation space inside an aero-engine is extremely limited. Traditional probes suffer from insufficient miniaturization and poor installation adaptability, making them difficult to place in the confined cavities of the engine's hot end. Third, the signal output of piezoelectric sensors is susceptible to interference from lateral and non-target vibration inputs, as well as the torsional effect of the sensing components. Vibration inputs from non-target directions introduce additional measurement noise, leading to larger measurement errors, frequent false alarms, and reduced reliability of fault diagnosis results.

[0004] To achieve vibration detection in high-temperature environments, MEMS miniature vibration sensors have been developed in existing technologies. Silicon is the most commonly used substrate material for MEMS devices, but silicon-based MEMS vibration sensors have a significant upper limit to their operating temperature. At high temperatures, the silicon substrate is prone to softening and oxidation, leading to rapid degradation of its mechanical properties. This makes it unsuitable for long-term stable operation in environments above 800°C, and thus unsuitable for the hot-end applications in aero-engines. Sapphire, with its high melting point, stable high-temperature mechanical properties, and good chemical inertness, is an ideal candidate substrate material for high-temperature MEMS devices. Currently, some FP-cavity fiber optic vibration sensing schemes based on sapphire materials have emerged. However, most existing sapphire vibration-sensitive structures employ single-beam support structures or support forms without elastic membrane auxiliary constraints, resulting in insufficient resistance to lateral interference. When lateral acceleration is input, the mass block is prone to deflection and torsion, causing non-target disturbances in the FP interferometric cavity length, directly degrading the vibration measurement accuracy.

[0005] In addition, sapphire is a ceramic single-crystal material with high hardness and strong chemical stability, making it difficult to fabricate in MEMS micro-nano processes. C-axis sapphire wafers are commonly used substrates for high-temperature optics and MEMS devices. Current processing technologies lack a composite mask system specifically adapted to C-axis sapphire wafers, making it difficult to achieve an integrated processing flow of step-by-step ICP etching of deep and shallow trenches and back-side release. During chip fabrication, the controllability of etching morphology is poor, microstructure release is incomplete, and chip forming yield is low. The consistency of subsequent bonding and packaging processes is poor, and defects are prone to exist at the packaging interface, making it difficult to mass-produce stable all-sapphire FP cavity sensitive chips.

[0006] In summary, existing technologies suffer from four main bottlenecks: First, the sensors lack sufficient high-temperature resistance, making it difficult to withstand operating conditions of 800℃~1200℃ and thus unable to achieve in-situ vibration detection at the hot end of aero-engines. Second, the sensitive structure has weak resistance to lateral interference, and is susceptible to lateral vibration and mass block torsion, resulting in large measurement errors and a high false alarm rate. Third, it is difficult to balance the requirements of high-temperature use with device miniaturization, making it unsuitable for the confined installation space inside aero-engines. Fourth, there is a lack of complete MEMS fabrication processes compatible with C-axis sapphire wafers, leading to poor device processing yield and packaging consistency. Therefore, developing an all-sapphire FP-cavity sensitive chip that can operate in high-temperature environments of 800℃-1200℃, has strong resistance to lateral interference, and possesses a processing technology suitable for mass production has significant engineering application value. Summary of the Invention

[0007] This invention aims to solve the problems of existing vibration sensors being unable to withstand high-temperature conditions of 800℃~1200℃, thus being unsuitable for high-temperature in-situ vibration detection of aero-engines, and existing MEMS vibration-sensitive structures being subject to interference from lateral vibration and mass block torsion, resulting in large measurement errors and high false alarm rates. The invention proposes an all-sapphire FP cavity sensitive chip for fiber optic vibration sensors and its fabrication method.

[0008] A sapphire FP cavity sensing chip for fiber optic vibration sensors includes an upper cover (1), a main chip (2), and a lower cover (3). The upper cover (1), the main chip (2), and the lower cover (3) are stacked and packaged to form an FP interference cavity. The upper cover (1), the main chip (2), and the lower cover (3) are all made of sapphire single crystal material, and the processing substrate is uniformly sapphire single crystal wafer with a crystal orientation of C. The main chip (2) is an integrated structure of four beams-double film-central mass block, including a fixed frame (4), four elastic beams (5), two elastic films (6), and a mass block (7). Two elastic beams (5) are set on each of the opposite sides of the mass block (7), and the two ends of the elastic beams (5) are vertically connected to the fixed frame (4) and the mass block (7) respectively. An elastic film (6) is set between the two elastic beams (5) on the same side. The upper cover (1), the main chip (2), and the lower cover (3) are sealed together by sapphire direct bonding process.

[0009] The method for fabricating an all-sapphire FP cavity sensing chip for an optical fiber vibration sensor according to the present invention is carried out according to the following steps:

[0010] S1. Select a C-oriented sapphire single crystal wafer and use LPCVD process to prepare a SiO2 / Si3N4 composite mask layer on the wafer surface;

[0011] S2, photolithography, and RIE etching pattern the composite mask on the front side of the wafer, and ICP process is used to etch 5~10μm sapphire shallow trenches on the front side.

[0012] S3. An aluminum layer is deposited on the back side of the sapphire wafer using electron beam evaporation to form a three-layer composite mask of SiO2 / Si3N4 / Al. The back mask patterning is completed by photolithography and RIE.

[0013] S4. Using ICP process, 80~90μm sapphire penetration grooves are etched on the back of the wafer. Continue to etch the elastic beam (5) and elastic film (6) on the back to obtain the main chip (2).

[0014] S5. The same batch of sapphire wafers are used to prepare size-matched top cover (1) and bottom cover (3) by photolithography and wet etching.

[0015] S6. The upper cover (1), main chip (2), and lower cover (3) are bonded sequentially using sapphire direct bonding process to obtain a complete sensitive chip.

[0016] The beneficial effects of this invention are:

[0017] 1. Ultra-wide high temperature resistance: The entire structure is made of C-axis sapphire single crystal material, which has excellent melting point, high temperature mechanical and optical stability. It can work stably in high temperature environments of 800℃~1200℃, breaking through the upper temperature limit of piezoelectric and silicon-based sensors, and is suitable for high temperature in-situ detection of aero engines.

[0018] 2. High resistance to lateral interference and high measurement accuracy: The structure adopts a four-elastic beam + double-sided elastic membrane cooperative limiting structure. The mass block only moves in the direction of sensitive vibration, which completely suppresses the torsion and yaw caused by lateral acceleration, greatly reduces the measurement error caused by random vibration, and reduces false alarms from the sensor.

[0019] 3. Miniaturized integration and strong installation adaptability: The three-layer integrated bonded microstructure has an overall size controlled at the millimeter level. Its small size allows it to be directly placed inside the narrow cavity of the engine, meeting the requirements for miniaturization and lightweighting of airborne equipment.

[0020] 4. Excellent optical interference stability: The uniform use of C-direction (0001) sapphire wafers ensures consistent lattice orientation, high thermal expansion matching of the three-layer components at high temperatures, small temperature drift of the FP cavity length, and stable fiber interference signal at high temperatures.

[0021] 5. Good process adaptability and high batch yield: A SiO2 / Si3N4 / Al composite mask system was developed for C-oriented sapphire. The step-by-step deep and shallow trench ICP etching + back-side release integrated process has controllable etching contour and complete structure release. The sapphire direct bonding interface has no adhesive layer, does not delaminate at high temperature and has excellent airtightness.

[0022] 6. Complete and measurable performance indicators: The fiber optic vibration sensor equipped with this chip can achieve wideband detection of 0~3kHz, a measurement range of 1g~10g, good linearity across the entire temperature range, and meets the vibration monitoring standards for aero-engines. Attached Figure Description

[0023] Figure 1 This is a top view of the main chip structure of the present invention;

[0024] Figure 2 This is a cross-sectional view of the wafer after the deposition of the composite mask layer;

[0025] Figure 3 A top view after the front mask of the wafer is patterned;

[0026] Figure 4 A top view of the wafer after shallow trench etching using ICP on the front side;

[0027] Figure 5 A top view of the back side of a wafer after patterning a composite mask on the back side;

[0028] Figure 6 This is a top view of the back side of the wafer after etching through-holes on the back side;

[0029] Figure 7 This is a cross-sectional view of the back side of the wafer after etching through-holes on the back side;

[0030] Figure 8 A top view of the main chip after the elastic beam and elastic membrane have been released;

[0031] Figure 9 This is a cross-sectional view of the main chip after the release of the elastic beam and elastic membrane.

[0032] Figure 10 Graphical front top view of the top / bottom cover mask;

[0033] Figure 11 This is a cross-sectional view of the upper / lower cover after wet etching.

[0034] Figure 12 This is a cross-sectional view of the entire chip after the top cover, main chip, and bottom cover have been bonded together.

[0035] Reference numerals: 1-Top cover, 2-Main chip, 3-Lower cover, 4-Fixed frame, 5-Elastic beam, 6-Elastic membrane, 7-Mass block. Detailed Implementation

[0036] Specific Implementation Method 1: This implementation method provides an all-sapphire FP cavity sensitive chip for fiber optic vibration sensors, comprising an upper cover (1), a main chip (2), and a lower cover (3). The upper cover (1), the main chip (2), and the lower cover (3) are stacked and packaged to form an FP interference cavity. The upper cover (1), the main chip (2), and the lower cover (3) are all made of sapphire single crystal material, and the processing substrate is uniformly made of sapphire single crystal wafer with a crystal orientation of C. The main chip (2) is an integrated structure of four beams-double film-central mass block, comprising a fixed support frame (4), four elastic beams (5), two elastic films (6), and a mass block (7). Two elastic beams (5) are provided on each of the opposite sides of the mass block (7), and the two ends of the elastic beams (5) are vertically connected to the fixed support frame (4) and the mass block (7), respectively. An elastic film (6) is provided between the two elastic beams (5) on the same side. The upper cover (1), the main chip (2), and the lower cover (3) are sealed together by sapphire direct bonding process.

[0037] This implementation employs a four-beam-double-membrane-central mass block constraint system. Two elastic beams are arranged symmetrically on each opposite side of the mass block, for a total of four elastic beams. The elastic beams vertically connect the fixed frame and the mass block, providing the main flexible suspension for the mass block and allowing it to translate along the sensitive detection direction. An elastic membrane is added between the two elastic beams on the same side, forming a composite constraint boundary with the elastic beams. The elastic membrane is a planar thin-film structure with high in-plane stiffness: for the detection axis, the elastic membrane withstands out-of-plane bending with low stiffness, not hindering the vibration displacement of the mass block along the target detection direction, preserving the normal vibration response of the sensor; for lateral and torsional directions, the in-plane rigid constraint of the elastic membrane restricts the relative misalignment and rotation of the two elastic beams, suppressing the torsion of the mass block around the detection axis, and simultaneously suppressing the yaw motion caused by lateral acceleration. The four-beam symmetry and the double-sided elastic membrane together form an over-constraint limiting system: allowing the mass block to generate effective translational displacement only in the sensitive direction being measured; under lateral acceleration input, the mass block torque is balanced by the four beams and the two elastic membranes, with almost no torsion or lateral deflection, the FP cavity reflector surfaces remain parallel, and no false interference signals are generated, eliminating false outputs introduced by lateral vibration, reducing measurement errors and suppressing false alarms.

[0038] Specific Implementation Method Two: This implementation method differs from Specific Implementation Method One in that the upper cover (1) and the lower cover (3) have the same geometric dimensions. Everything else is the same as in Specific Implementation Method One.

[0039] Specific Implementation Method 3: This implementation method differs from Specific Implementation Method 2 in that the dimensions of the upper cover (1) and lower cover (3) are 9050μm in length, 7470μm in width, and 250μm in thickness. Everything else is the same as in Specific Implementation Method 2.

[0040] Specific Implementation Method Four: This implementation method differs from Specific Implementation Method One in that the main chip (2) has dimensions of 9050μm in length, 7470μm in width, and 300μm in thickness. Everything else is the same as in Specific Implementation Method One.

[0041] Specific Implementation Method Five: This implementation method differs from Specific Implementation Method One in that the C-axis sapphire single crystal wafer is a (0001) crystal plane double-polished sapphire substrate. Everything else is the same as in Specific Implementation Method One.

[0042] Specific Implementation Method Six: This implementation method describes a method for fabricating an all-sapphire FP cavity sensing chip for an optical fiber vibration sensor, which is carried out according to the following steps:

[0043] S1. Select a C-oriented sapphire single crystal wafer and use LPCVD process to prepare a SiO2 / Si3N4 composite mask layer on the wafer surface;

[0044] S2, photolithography, and RIE etching pattern the composite mask on the front side of the wafer, and ICP process is used to etch 5~10μm sapphire shallow trenches on the front side.

[0045] S3. An aluminum layer is deposited on the back side of the sapphire wafer using electron beam evaporation to form a three-layer composite mask of SiO2 / Si3N4 / Al. The back mask patterning is completed by photolithography and RIE.

[0046] S4. Using ICP process, 80~90μm sapphire penetration grooves are etched on the back of the wafer. Continue to etch the elastic beam (5) and elastic film (6) on the back to obtain the main chip (2).

[0047] S5. The same batch of sapphire wafers are used to prepare size-matched top cover (1) and bottom cover (3) by photolithography and wet etching.

[0048] S6. The upper cover (1), main chip (2), and lower cover (3) are bonded sequentially using sapphire direct bonding process to obtain a complete sensitive chip.

[0049] This implementation uses sapphire material α-Al2O3 single crystal with a melting point of approximately 2050℃. Within the 800~1200℃ range, its elastic modulus, Poisson's ratio, and other mechanical parameters remain highly stable, exhibiting no phase transformation or plastic creep. It is chemically inert, does not oxidize in high-temperature air environments, and does not suffer from high-temperature oxidation and corrosion problems similar to silicon. It also avoids the polarization-depolarization effect of piezoelectric materials, and the material itself does not lose its structural function due to high temperatures. The chip operates based on the FP optical interference principle, belonging to a passive optical measurement structure. It does not require functional materials to provide an electro-mechanical conversion effect, thus avoiding the high-temperature failure mechanism of piezoelectric materials. The top cover, main chip, and bottom cover are all taken from C-axis (0001) sapphire wafers, with consistent crystal orientation and perfectly matched anisotropic thermal expansion coefficients. Sapphire belongs to the hexagonal crystal system, and different crystal orientations have significantly different thermal expansion coefficients. If the crystal orientations of the three layers are disordered, the inconsistent thermal expansion and contraction of each layer during high-temperature operation will generate huge thermal stress at the bonding interface, leading to warping, bonding interface cracking, and undesirable drift of the FP cavity length with temperature. This invention uses C-axis wafers throughout, and the thermal expansion behavior of the three-layer components is consistent. The overall chip warpage is small at high temperatures, and the FP cavity geometry can be stably maintained, ensuring the stability of the interference optical signal and enabling in-situ detection at high temperatures of 800~1200℃.

[0050] This embodiment uses glue-free direct bonding, with the bonding interface being a single-crystal-to-single-crystal atomic-level bond. There is no organic matter present, and the interface will not decompose, flow, or detach at a high temperature of 1200℃, thus maintaining the airtightness and shape stability of the FP cavity.

[0051] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Method Six in that the total thickness of the SiO2 / Si3N4 composite mask layer prepared by LPCVD in step S1 is 300~360nm. Everything else is the same as in Specific Implementation Method Six.

[0052] Specific Implementation Method Eight: This implementation method differs from Specific Implementation Method Six in that the depth of the shallow trench in the front ICP etching in step S2 is 5 μm. Everything else is the same as in Specific Implementation Method Six.

[0053] Specific Implementation Method Nine: This implementation method differs from Specific Implementation Method Six in that the depth of the backside ICP etching penetration groove in step S4 is 80~90μm. Everything else is the same as in Specific Implementation Method Six.

[0054] Specific Implementation Method 10: This implementation method differs from Specific Implementation Method 6 in that the etching depth of the upper and lower covers prepared by wet etching in step S5 is 10 μm. Everything else is the same as in Specific Implementation Method 6.

[0055] The beneficial effects of the present invention are verified through the following embodiments:

[0056] This embodiment describes a method for fabricating an all-sapphire FP cavity sensing chip for an optical fiber vibration sensor, which specifically follows these steps:

[0057] S1. Select a C-direction ((0001) crystal plane) double-polished sapphire single crystal wafer, determine the wafer crystal orientation and position the cutting edge to ensure that the lattice orientation of all components is uniform; the wafer substrate is used to process the top cover, main chip and bottom cover respectively;

[0058] S2. SiO2 / Si3N4 composite hard masks are deposited on both sides of the sapphire wafer using LPCVD process, with the total mask thickness controlled at 300~360nm. The SiO2 and Si3N4 bilayer composite structure improves the selectivity of sapphire dry etching and avoids premature mask wear. The thickness of the SiO2 layer is 200~260nm, and the thickness of the Si3N4 layer is 80~100nm.

[0059] S3. Spin-coat photoresist on the front side of the wafer. After photolithography exposure and development, use RIE dry etching to pattern the composite mask layer. Use the patterned mask as a protective layer and use ICP dry etching to etch the uncovered area to a depth of 5μm to form a shallow groove for FP cavity positioning.

[0060] RIE: Etching power: 100W, gas ratio: CF4+Ar, etching rate: 300~400Å / min, etching time: 7min-10min;

[0061] ICP: Etching power: 1000W, gas ratio: SF6+C4F8+Ar, etching rate: 1μm / min, etching time: 5min.

[0062] S4. Electron beam evaporation is used to deposit a metal aluminum layer on the back of the wafer to form a three-layer composite mask of SiO2 / Si3N4 / Al. The back mask patterning is completed by photolithography and RIE etching. The aluminum layer improves the resistance to deep trench etching. The thickness of the Al metal mask on the back is [not specified].

[0063] RIE: Etching power: 100W, gas ratio: CF4+Ar, etching rate: 300-400Å / min, etching time: 7min~10min.

[0064] Backside Al metal mask thickness: 2500~3000Å.

[0065] S5. Photoresist-assisted mask is prepared by back-side photolithography. The back-side area is etched by ICP dry etching to a depth of 80~90μm to form a through groove. Using a three-layer composite hard mask as a shield, the back-side ICP etching continues until the four elastic beams and two elastic films are completely released, resulting in an integrated main chip with a fixed frame and a central mass block. The overall dimensions of the main chip are: length 9050μm, width 7470μm, and thickness 300μm.

[0066] ICP: Etching power: 1000W, Gas ratio: SF6+C4F8+Ar, Etching rate: 1μm / min.

[0067] The elastic beam has a width of 300μm, a length of 1200μm, and a thickness of 85~95μm; the elastic membrane has a length of 4000μm, a width of 1000μm, and a thickness of 80~90μm; the central mass block has a thickness of 300μm.

[0068] S6. Take C-oriented sapphire wafers from the same batch and repeat the LPCVD deposition mask and photolithography patterning process; use wet etching process to process the tank with an etching depth of 10μm; after forming, the upper and lower covers have completely consistent geometric dimensions: length 9050μm, width 7470μm, thickness 250μm.

[0069] Sapphire wet etching: Etching solution type: H2SO4+H3PO4, volume ratio 1:3; Temperature: 150℃~280℃; Time is determined according to the process based on the profilometer.

[0070] S7. Stack the top cover, main chip and bottom cover three layers of single crystal sapphire components in sequence. Use glue-free sapphire direct bonding process for high temperature bonding. The three layers are tightly bonded to form a closed FP interference cavity, and finally a complete all-sapphire FP cavity vibration sensitive chip is obtained.

[0071] Bonding parameters: Bonding pressure 25000N; Vacuum degree: less than 0.0001mbar; Temperature: 450℃; Bonding time: 2h45min; Post-bonding annealing: 5℃ per minute, raise to 800℃ and hold for 1 hour, 1000℃ and hold for 1 hour, then raise to 1200℃ and hold for 3 hours, then lower to 300℃ after 200 minutes.

[0072] The fiber optic vibration sensor assembled using the sensitive chip prepared in this embodiment exhibits the following measured performance:

[0073] Operating temperature range: 800℃~1200℃, no deformation, delamination or signal drift during long-term high-temperature operation; detection frequency range: 0~3kHz; vibration range: 1g~10g; lateral vibration interference suppression capability is improved by more than 90%, and there is no measurement jump caused by mass block torsion.

Claims

1. A sapphire FP cavity sensing chip for fiber optic vibration sensors, comprising an upper cover (1), a main chip (2), and a lower cover (3), wherein the upper cover (1), the main chip (2), and the lower cover (3) are stacked and packaged to form an FP interference cavity, characterized in that, The upper cover (1), main chip (2), and lower cover (3) are all made of sapphire single crystal material, and the processing substrate is uniformly sapphire single crystal wafer with C-direction crystal orientation; the main chip (2) is an integrated structure of four beams-double film-central mass block, including fixed frame (4), four elastic beams (5), two elastic films (6), and one mass block (7); two elastic beams (5) are set on each of the opposite sides of the mass block (7), and the two ends of the elastic beams (5) are vertically connected to the fixed frame (4) and the mass block (7); an elastic film (6) is set between the two elastic beams (5) on the same side; the upper cover (1), main chip (2), and lower cover (3) are sealed together by sapphire direct bonding process.

2. The all-sapphire FP cavity sensing chip for fiber optic vibration sensors according to claim 1, characterized in that, The upper cover (1) and the lower cover (3) have the same geometric dimensions.

3. The all-sapphire FP cavity sensing chip for fiber optic vibration sensors according to claim 2, characterized in that, The upper cover (1) and lower cover (3) are 9050μm long, 7470μm wide and 250μm thick.

4. The all-sapphire FP cavity sensing chip for fiber optic vibration sensors according to claim 1, characterized in that, The main chip (2) has dimensions of 9050μm in length, 7470μm in width, and 300μm in thickness.

5. The all-sapphire FP cavity sensing chip for fiber optic vibration sensors according to claim 1, characterized in that, The C-axis sapphire single crystal wafer is a (0001) crystal plane double-polished sapphire substrate.

6. The method for fabricating an all-sapphire FP-cavity sensing chip for an optical fiber vibration sensor as described in claim 1, characterized in that, The fabrication method of the all-sapphire FP cavity sensing chip for fiber optic vibration sensors is carried out according to the following steps: S1. Select a C-oriented sapphire single crystal wafer and use LPCVD process to prepare a SiO2 / Si3N4 composite mask layer on the wafer surface; S2, photolithography, and RIE etching pattern the composite mask on the front side of the wafer, and ICP process is used to etch 5~10μm sapphire shallow trenches on the front side. S3. An aluminum layer is deposited on the back side of the sapphire wafer using electron beam evaporation to form a three-layer composite mask of SiO2 / Si3N4 / Al. The back mask patterning is completed by photolithography and RIE. S4. Using ICP process, 80~90μm sapphire penetration grooves are etched on the back of the wafer. Continue to etch the elastic beam (5) and elastic film (6) on the back to obtain the main chip (2). S5. The same batch of sapphire wafers are used to prepare size-matched top cover (1) and bottom cover (3) by photolithography and wet etching. S6. The upper cover (1), main chip (2), and lower cover (3) are bonded sequentially using sapphire direct bonding process to obtain a complete sensitive chip.

7. The method for fabricating an all-sapphire FP-cavity sensing chip for an optical fiber vibration sensor according to claim 6, characterized in that, The total thickness of the SiO2 / Si3N4 composite mask layer prepared by LPCVD in step S1 is 300~360nm.

8. The method for fabricating an all-sapphire FP-cavity sensing chip for an optical fiber vibration sensor according to claim 6, characterized in that, In step S2, the depth of the shallow trench etched by the front ICP is 5 μm.

9. The method for fabricating an all-sapphire FP-cavity sensing chip for an optical fiber vibration sensor according to claim 6, characterized in that, In step S4, the depth of the ICP etching penetration groove on the back side is 80~90μm.

10. The method for fabricating an all-sapphire FP-cavity sensing chip for an optical fiber vibration sensor according to claim 6, characterized in that, In step S5, the wet etching process is used to prepare the upper and lower covers with an etching depth of 10 μm.