Methods for measuring sheet resistance and calculating the effect of fixed charge on it
By obtaining the dopant ion concentration distribution and solving the Poisson equation, combined with the four-probe testing method, the influence of surface fixed charge on the sheet resistance measurement of high-resistivity samples is quantified. This solves the problem that the influence of surface charge cannot be effectively eliminated in the existing technology, and improves the accuracy of the measurement.
Patent Information
- Application Number
- CN202510633951.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-16
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing technology, the influence of surface fixed charge on the sheet resistance measurement of high-resistivity samples is difficult to quantitatively characterize, especially in high-resistivity samples where its influence cannot be effectively eliminated.
By obtaining the doped ion concentration distribution of the sample to be tested, assuming the fixed amount and positive or negative charge on the surface, the Poisson equation is solved to obtain the carrier concentration distribution, and the conductivity is integrated in the depth direction to calculate the sheet resistance. The influence of surface charge is offset by the four-probe testing method, and its influence on the measurement is quantified.
The quantitative calculation of the influence of surface fixed charge on the measurement of block resistance was realized, which improved the accuracy and reliability of high-resistivity sample measurement.
Smart Images

Figure CN123112486A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor integrated circuit measurement, and in particular to a method for measuring sheet resistance and a method for calculating the effect of fixed charge on it. Background Technology
[0002] Sheet resistance measurement is an important indicator for characterizing thin film quality. Currently, sheet resistance is obtained by four-probe testing. The introduction of four probes eliminates the influence of contact resistance. However, the influence of surface fixed charge still exists, such as environmental factors causing the accumulation of positive or negative charges on the surface. For samples with conventional resistivity, the influence of surface fixed charge is negligible, but for high-resistivity samples, the influence of surface fixed charge is significant and cannot be ignored. It should be noted that the term "high-resistivity" in this invention is a relative concept; the influence of surface charge varies for different samples. For example, for epitaxial wafers, surface charge may have an effect when the resistivity is above 40 ohm-cm, while for polished wafers, surface charge may only have an effect when the resistivity is greater than 1000 ohm-cm.
[0003] Therefore, how to quantitatively characterize the effect of fixed charge on the measurement of block resistance has become one of the problems that urgently need to be solved by those skilled in the art.
[0004] It should be noted that the above description of the technical background is only for the purpose of providing a clear and complete explanation of the technical solutions of the present invention and facilitating understanding by those skilled in the art. It should not be assumed that the above technical solutions are known to those skilled in the art simply because they have been described in the background section of this invention. Summary of the Invention
[0005] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a method for measuring sheet resistance and a method for calculating the influence of fixed charge on it, so as to solve the problem of the influence of surface fixed charge on sheet resistance measurement in the prior art.
[0006] To achieve the above and other related objectives, the present invention provides a method for calculating the influence of a fixed charge on the resistance measurement of a square block, wherein the method for calculating the influence of a fixed charge on the resistance measurement of a square block includes at least:
[0007] S1) Provide a sample to be tested and obtain the concentration distribution of dopant ions in the sample to be tested, wherein the dopant ions are donor impurities and / or acceptor impurities;
[0008] S2) Assuming a fixed surface charge and charge sign, and based on the concentration distribution of the doped ions, solve the Poisson equation under equilibrium distribution to obtain the carrier concentration distribution;
[0009] S3) Obtain the thickness of the sample to be tested, and integrate the inverse of the conductivity in the depth direction to calculate the sheet resistance;
[0010] S4) Re-assume the fixed surface charge and charge sign, return to step S2) to obtain the sheet resistance value under different fixed surface charge and charge sign, compare the change in sheet resistance value under different fixed surface charge and charge sign, and quantify the influence of fixed surface charge on sheet resistance measurement.
[0011] Optionally, when the sample to be tested is a polished sheet, the concentration of doped ions in the sample to be tested is uniformly distributed; the thickness of the sample to be tested is the thickness of the polished sheet.
[0012] Optionally, when the sample to be tested is an epitaxial wafer, the diffusion equation is solved based on the temperature and thermodynamic history of the epitaxial process to obtain the concentration distribution of the doped ions; the thickness of the sample to be tested is the measured thickness of the epitaxial layer in the epitaxial wafer or the calculated equivalent thickness of the epitaxial layer.
[0013] Alternatively, the diffusion equation satisfies:
[0014]
[0015] Among them, C A t represents the concentration distribution of donor or acceptor impurities; t represents time. For gradient; D eff The diffusion coefficient in Arrhenius form is related to the thermodynamic history of the temperature.
[0016] Alternatively, the method for calculating the equivalent thickness of the epitaxial layer includes:
[0017] S31) Calculate the width of the space charge region where the carriers are depleted based on the doping concentration of the epitaxial layer and the doping concentration of the substrate in the epitaxial wafer;
[0018] S32) Calculate the equivalent thickness of the epitaxial layer based on the measured thickness of the epitaxial layer, the depth of epitaxial diffusion into the substrate, and the width of the space charge region.
[0019] Alternatively, the width of the space charge region satisfies the following relationship:
[0020]
[0021] Among them, D space_charge ε is the width of the space charge region; ε0 is the vacuum permittivity; ε r is the relative permittivity of silicon; e is the elementary charge; N epi N represents the doping concentration of the epitaxial layer. subk represents the doping concentration of the substrate. B Boltzmann constant; T is Kelvin temperature; n i This represents the intrinsic carrier concentration at the current temperature.
[0022] Alternatively, the equivalent thickness of the epitaxial layer satisfies the following relationship:
[0023] D eff_epi =D orig_epi -D diff -D space_charge ;
[0024] Among them, D eff_epi D is the equivalent thickness of the epitaxial layer; orig_epi The measured thickness of the epitaxial layer; D diff D represents the depth of epitaxial diffusion into the substrate. space_charge The width of the space charge region.
[0025] Alternatively, the Poisson equation under the equilibrium distribution satisfies:
[0026]
[0027] The boundary conditions for surface charge satisfy:
[0028]
[0029] in, φ is the gradient; φ is the electrostatic potential; ε0 is the vacuum permittivity; ε r ρ is the relative permittivity of silicon; e is the elementary charge; k B Boltzmann constant; T is Kelvin temperature; n i N represents the intrinsic carrier concentration at the current temperature. d For the concentration distribution of donor impurities, N is the value when donor impurities are absent. d =0; N a The concentration distribution of acceptor impurities is given by N when acceptor impurities are absent. a =0; φ p For holes, the Fermi level, φ n For electrons, the Fermi level is equal to and constant under equilibrium distribution; p is the hole concentration distribution; n is the electron concentration distribution; Q sc This represents the fixed charge on the surface; a positive value indicates a positive charge, and a negative value indicates a negative charge.
[0030] Alternatively, the sheet resistance satisfies:
[0031]
[0032] Among them, R shσ(x) is the sheet resistance; h is the thickness of the sample under test; σ(x) is the conductivity; e is the elementary charge; n(x) is the electron concentration distribution; μ e (x) represents electron mobility; p(x) represents hole concentration distribution; μ p (x) represents the hole mobility.
[0033] To achieve the above and other related objectives, the present invention also provides a sheet resistance measurement method, which includes at least: obtaining an initial sheet resistance based on a four-probe testing method; evaluating the influence of the current surface charge on the sheet resistance measurement based on the above-mentioned method for calculating the influence of a fixed charge on the sheet resistance measurement; and canceling the influence of the surface charge on the sheet resistance measurement on the initial sheet resistance to obtain a compensated sheet resistance.
[0034] As described above, the sheet resistance measurement method and the method for calculating the effect of fixed charge on it according to the present invention have the following beneficial effects:
[0035] This invention combines process information (and equivalent thickness) to quantitatively calculate the influence of surface fixed charge on sheet resistance measurement, providing important guidance for high resistance measurement and improving the accuracy of sheet resistance measurement. Attached Figure Description
[0036] Figure 1 The diagram shows a flowchart of the method for calculating the effect of a fixed charge on the measurement of block resistance according to the present invention.
[0037] Figure 2 The diagram shown is a schematic representation of the concentration distribution curves of donor and acceptor impurities in an epitaxial wafer calculated in an example of the present invention.
[0038] Component designation explanation
[0039] Steps S1 to S4
[0040] Steps S31 to S32 Detailed Implementation
[0041] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0042] Please see Figures 1-2It should be noted that the illustrations provided in this embodiment are only schematic representations of the basic concept of the present invention. Therefore, the drawings only show the components related to the present invention and are not drawn according to the actual number, shape and size of the components in the actual implementation. In the actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.
[0043] like Figure 1 As shown, the present invention provides a method for calculating the influence of a fixed charge on the measurement of square block resistance. This method includes:
[0044] S1) Provide the sample to be tested and obtain the concentration distribution of doped ions in the sample to be tested.
[0045] Specifically, in this embodiment, the sample to be tested is set as a polished wafer or an epitaxial wafer (especially an inverse epitaxial wafer, i.e., the conductivity type of the epitaxial layer and the substrate is opposite). In practical use, any semiconductor medium that is suitable for this method can be used as the sample to be tested in this invention, and will not be elaborated here.
[0046] More specifically, when the sample to be tested is a polished sheet, since the concentration of doped ions on the polished sheet is uniformly distributed, the concentration distribution of doped ions can be directly measured, including but not limited to secondary ion mass spectrometry (SIMS), Hall effect measurement, and scanning capacitance microscopy (SCM). In practical use, any method that can obtain the concentration distribution of doped ions on the polished sheet is applicable to this invention and is not limited to this embodiment.
[0047] Specifically, when the sample to be tested is an epitaxial wafer, the diffusion equation is solved based on the thermal history of the epitaxial process (i.e., the sequence of temperature changes over time experienced by a semiconductor material or device during manufacturing), thereby obtaining the concentration distribution of doped ions. As an example, the diffusion equation satisfies:
[0048]
[0049] Among them, C A t represents the concentration distribution of donor or acceptor impurities; t represents time. For gradient; D eff The diffusion coefficient in the Arrhenius form related to the thermodynamic history of the stated temperature satisfies... D0 is a pre-exponential factor related to material, defect concentration, and diffusion mechanism, E a For diffusion activation energy, k B is Boltzmann's constant; T is Kelvin temperature.
[0050] It should be noted that the dopant ion in this invention can be a donor impurity, an acceptor impurity, or both, depending on the actual application scenario. Accordingly, in equation (1), when the dopant ion is a donor impurity, C... A =N d When the dopant ion is an acceptor impurity, C A =N a When the dopant ions include both donor and acceptor impurities, in the region where the dopant ions are only donor impurities, C A =N d In the region where the doped ions are only acceptor impurities, C A =N a In the region C where donor impurities and acceptor impurities overlap A =|N d -N a |(i.e., net doping concentration); where N d For the concentration distribution of donor impurities, N a This represents the concentration distribution of acceptor impurities.
[0051] like Figure 2 The figure shows the concentration distribution curves of donor and acceptor impurities in an epitaxial wafer calculated in an example of the present invention. The concentration of donor impurities remains essentially consistent within a depth range of 0-9 μm, consistently at 10. 14 cm -3 Acceptor impurities diffuse within a depth range of 8µm-8.5µm (depth D of epitaxial diffusion into the substrate). diff Approximately 0.5 μm), concentrations from 10 12 cm -3 Increase to 10 19 cm -3 .
[0052] S2) Assuming a fixed surface charge and charge sign, and based on the concentration distribution of doped ions, solve the Poisson equation under equilibrium distribution to obtain the carrier concentration distribution.
[0053] Specifically, in this embodiment, the Poisson equation under the equilibrium distribution satisfies:
[0054]
[0055] Where φ is the electrostatic potential; ε0 is the vacuum permittivity; ε r is the relative permittivity of silicon; e is the elementary charge; n i This represents the intrinsic carrier concentration distribution at the current temperature; N d For the concentration distribution of donor impurities, N is the value when donor impurities are absent. d =0; N aThe concentration distribution of acceptor impurities is given by N when acceptor impurities are absent. a =0; φ p For holes, the Fermi level, φ n denoted as Fermi level for electrons, both of which are equal and constant under equilibrium distribution; p is the hole concentration distribution, and n is the electron concentration distribution.
[0056] Assuming a fixed surface charge and its sign, where the fixed surface charge and its sign are reflected in the surface boundary conditions, satisfying:
[0057]
[0058] Among them, Q sc This represents the fixed charge on the surface; a positive value indicates a positive charge, and a negative value indicates a negative charge.
[0059] Solve the simultaneous equations (3), (4), (5), and (6) to obtain the carrier concentration distribution.
[0060] S3) Obtain the thickness h of the sample to be tested, and integrate the inverse of the conductivity in the depth direction to calculate the sheet resistance.
[0061] Specifically, when the sample to be tested is a polished sheet, the thickness of the sample to be tested is the thickness of the polished sheet, which can be obtained by measuring tools, including but not limited to laser interferometers, ellipsometers, etc., which will not be described in detail here.
[0062] Specifically, when the sample to be tested is an epitaxial wafer, as an example, the thickness of the sample is the measured thickness of the epitaxial layer in the epitaxial wafer. This measured thickness includes, but is not limited to, the thickness value obtained under Fourier Transform Infrared Spectroscopy (FTIR). Any method that can achieve the measurement of the epitaxial layer thickness is applicable to this invention, and will not be elaborated here. As another example, the thickness of the sample to be tested is the calculated equivalent thickness of the epitaxial layer in the epitaxial wafer; in this embodiment, the method for calculating the equivalent thickness of the epitaxial layer includes:
[0063] S31) Calculate the width of the space charge region after carrier depletion based on the doping concentration of the epitaxial layer and the doping concentration of the substrate in the epitaxial wafer. As an example, the width of the space charge region satisfies the following relationship:
[0064]
[0065] Among them, D space_charge V is the width of the space charge region. build For built-in potential; N epiN represents the doping concentration of the epitaxial layer (the donor impurity concentration is given when only donor impurities are included, the acceptor impurity concentration is given when only acceptor impurities are included, and the net doping concentration is given when both donor and acceptor impurities are included); sub The doping concentration is the substrate concentration; typically, the doping concentration of the epitaxial layer is lower than that of the substrate.
[0066] S32) Calculate the equivalent thickness of the epitaxial layer based on the measured thickness of the epitaxial layer, the depth of epitaxial diffusion into the substrate, and the width of the space charge region. As an example, the equivalent thickness of the epitaxial layer satisfies the following relationship:
[0067] D eff_epi =D orig_epi -D diff -D space_charge (9);
[0068] Among them, D eff_epi D is the equivalent thickness of the epitaxial layer. orig_epi For measuring the thickness of the epitaxial layer; D diff D represents the depth of epitaxial diffusion into the substrate. space_charge The width of the space charge region.
[0069] Specifically, the sheet resistance is obtained by substituting the thickness of the sample to be tested into the following equation (10) and integrating. In this embodiment, the sheet resistance satisfies:
[0070]
[0071] Among them, R sh σ(x) is the sheet resistance; h is the thickness of the sample; σ(x) is the conductivity; n(x) is the electron concentration distribution; μ e (x) represents electron mobility; p(x) represents hole concentration distribution; μ p (x) represents the hole mobility.
[0072] In this example, electron mobility μ e (x) and hole mobility μ p (x) satisfies the following relation:
[0073]
[0074] Where, μ min1 P c μ min2 C r μ1, C s α, β, μ Lξ and ξ are both user-defined parameters with no physical meaning. They can be obtained from empirical values based on Table 1 below, and the corresponding parameters can be substituted to calculate the value. It should be noted that in this example, the mobility model (11) considers the effect of scattering of doped elements. In actual use, other mobility models can also be used, which will not be elaborated here.
[0075]
[0076]
[0077] Table 1
[0078] S4) Reassume and adjust the amount and sign of the fixed surface charge, return to step S2), calculate the sheet resistance value under different amounts and signs of the fixed surface charge based on the updated amount and sign of the fixed surface charge, compare the changes in the sheet resistance value under different amounts and signs of the fixed surface charge, and quantify the influence of the fixed surface charge on the sheet resistance measurement.
[0079] Specifically, when the surface charge is 0, it is the sheet resistance value without surface charge. Then, the absolute change (in this example, the absolute change is the sheet resistance value under a certain fixed charge minus the sheet resistance without surface charge) and relative change (in this example, the relative change is the absolute change divided by the sheet resistance without surface charge) of the sheet resistance under different fixed surface charges can be compared. This quantifies the influence of the fixed surface charge on the sheet resistance measurement and provides important guidance for high resistance measurement.
[0080] In summary, this invention provides a method for measuring sheet resistance and a method for calculating the influence of fixed charge on it, comprising: S1) providing a sample to be tested and obtaining the concentration distribution of dopant ions in the sample, wherein the dopant ions are donor impurities and / or acceptor impurities; S2) assuming the amount and positivity of the fixed surface charge, and solving the Poisson equation under equilibrium distribution based on the concentration distribution of dopant ions to obtain the carrier concentration distribution; S3) obtaining the thickness of the sample to be tested, and integrating the inverse of the conductivity in the depth direction to calculate the sheet resistance; S4) reasserting the amount and positivity of the fixed surface charge, returning to step S2) to obtain the sheet resistance values under different amounts and positivity of the fixed surface charge, comparing the changes in the sheet resistance values under different amounts and positivity of the fixed surface charge, and quantifying the influence of the fixed surface charge on the sheet resistance measurement. This invention combines process information (and equivalent thickness) to achieve quantitative calculation of the influence of the fixed surface charge on the sheet resistance measurement, providing important guidance for high resistance measurement and effectively improving the accuracy of sheet resistance measurement. Therefore, this invention effectively overcomes the various shortcomings of the prior art and has high industrial application value.
[0081] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.
Claims
1. A method for calculating the influence of a fixed charge on the measurement of square block resistance, characterized in that, The method for calculating the effect of a fixed charge on the measurement of block resistance includes at least the following: S1) Provide a sample to be tested and obtain the concentration distribution of dopant ions in the sample to be tested, wherein the dopant ions are donor impurities and / or acceptor impurities; S2) Assuming a fixed surface charge and charge sign, and based on the concentration distribution of the doped ions, solve the Poisson equation under equilibrium distribution to obtain the carrier concentration distribution; S3) Obtain the thickness of the sample to be tested, and integrate the inverse of the conductivity in the depth direction to calculate the sheet resistance; S4) Re-assume the fixed surface charge and charge sign, return to step S2) to obtain the sheet resistance value under different fixed surface charge and charge sign, compare the change in sheet resistance value under different fixed surface charge and charge sign, and quantify the influence of fixed surface charge on sheet resistance measurement.
2. The method for calculating the influence of a fixed charge on the measurement of block resistance according to claim 1, characterized in that: When the sample to be tested is a polished sheet, the concentration of doped ions in the sample to be tested is uniformly distributed; the thickness of the sample to be tested is the same as the thickness of the polished sheet.
3. The method for calculating the influence of a fixed charge on the measurement of block resistance according to claim 1, characterized in that: When the sample to be tested is an epitaxial wafer, the diffusion equation is solved based on the temperature and thermodynamic history of the epitaxial process to obtain the concentration distribution of the doped ions; the thickness of the sample to be tested is the measured thickness of the epitaxial layer in the epitaxial wafer or the calculated equivalent thickness of the epitaxial layer.
4. The method for calculating the influence of a fixed charge on the measurement of block resistance according to claim 3, characterized in that: The diffusion equation satisfies: Among them, C A t represents the concentration distribution of donor or acceptor impurities; t represents time. For gradient; D eff The diffusion coefficient in Arrhenius form is related to the thermodynamic history of the temperature.
5. The method for calculating the influence of a fixed charge on the measurement of block resistance according to claim 3, characterized in that: The method for calculating the equivalent thickness of the epitaxial layer includes: S31) Calculate the width of the space charge region where the carriers are depleted based on the doping concentration of the epitaxial layer and the doping concentration of the substrate in the epitaxial wafer; S32) Calculate the equivalent thickness of the epitaxial layer based on the measured thickness of the epitaxial layer, the depth of epitaxial diffusion into the substrate, and the width of the space charge region.
6. The method for calculating the influence of a fixed charge on the measurement of block resistance according to claim 5, characterized in that: The width of the space charge region satisfies the following relationship: Among them, D space_charge ε is the width of the space charge region; ε0 is the vacuum permittivity; ε r is the relative permittivity of silicon; e is the elementary charge; N epi N represents the doping concentration of the epitaxial layer. sub k represents the doping concentration of the substrate. B Boltzmann constant; T is Kelvin temperature; n i This represents the intrinsic carrier concentration at the current temperature.
7. The method for calculating the influence of a fixed charge on the measurement of block resistance according to claim 5, characterized in that: The equivalent thickness of the epitaxial layer satisfies the following relationship: D eff_epi =D orig_epi -D diff -D space_charge ; Among them, D eff_epi D is the equivalent thickness of the epitaxial layer; orig_epi The measured thickness of the epitaxial layer; D diff D represents the depth of epitaxial diffusion into the substrate. space_charge The width of the space charge region.
8. The method for calculating the influence of a fixed charge on the measurement of block resistance according to any one of claims 1-7, characterized in that: The Poisson equation under the equilibrium distribution satisfies: The boundary conditions for surface charge satisfy: in, φ is the gradient; φ is the electrostatic potential; ε0 is the vacuum permittivity; ε r ρ is the relative permittivity of silicon; e is the elementary charge; k B Boltzmann constant; T is Kelvin temperature; n i N represents the intrinsic carrier concentration at the current temperature. d For the concentration distribution of donor impurities, N is the value when donor impurities are absent. d =0; N a The concentration distribution of acceptor impurities is given by N when acceptor impurities are absent. a =0; φ p For holes, the Fermi level, φ n For electrons, the Fermi level is equal to and constant under equilibrium distribution; p is the hole concentration distribution; n is the electron concentration distribution; Q sc This represents the fixed charge on the surface; a positive value indicates a positive charge, and a negative value indicates a negative charge.
9. The method for calculating the influence of a fixed charge on the measurement of block resistance according to any one of claims 1-7, characterized in that: The sheet resistance satisfies: Among them, R sh σ(x) is the sheet resistance; h is the thickness of the sample under test; σ(x) is the conductivity; e is the elementary charge; n(x) is the electron concentration distribution; μ e (x) represents electron mobility; p(x) represents hole concentration distribution; μ p (x) represents the hole mobility.
10. A method for measuring sheet resistance, characterized in that, The sheet resistance measurement method includes at least: obtaining an initial sheet resistance based on a four-probe testing method; evaluating the influence of the current surface charge on the sheet resistance measurement based on the method for calculating the influence of a fixed charge on the sheet resistance measurement as described in any one of claims 1-9; and canceling the influence of the surface charge on the sheet resistance measurement on the initial sheet resistance to obtain a compensated sheet resistance.