Manufacturing method of opaque MoSi photomask

By measuring the critical dimensions of the chromium patterned layer after Cr etching and predicting the critical dimensions of the MoSi light-shielding layer, the MoSi etching time can be adjusted to achieve bidirectional precise compensation. This solves the problem that existing opaque MoSi mask manufacturing methods cannot accurately predict and compensate for critical dimensions, and significantly reduces the scrap rate of advanced nodes.

CN123113237APending Publication Date: 2026-11-17RUIJING SEMICON (NINGBO) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611611211.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for manufacturing opaque MoSi masks cannot accurately predict and compensate for critical dimensions after Cr etching, resulting in CD MTT exceeding specifications for advanced nodes, leading to a high scrap rate and failing to meet the accuracy requirements of 28nm and below nodes.

Method used

By measuring the critical dimensions of the chromium patterned layer after Cr etching, the critical dimensions of the final MoSi light-shielding layer are predicted using a preset MoSi etching deviation relationship. Bidirectional precise compensation is achieved by adjusting the MoSi etching time, thus forming an opaque MoSi mask.

Benefits of technology

It significantly reduces the scrap rate caused by CD MTT exceeding specifications for opaque MoSi masks at nodes of 28nm, 14nm, 7nm and below, improves process yield, and does not require additional equipment or process steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123113237A_ABST
    Figure CN123113237A_ABST
Patent Text Reader

Abstract

This invention provides a method for manufacturing an opaque MoSi mask, belonging to the field of integrated circuits. The method includes: providing a blank mask, which includes a light-transmitting substrate, a MoSi light-shielding material layer, and a chromium material layer; etching the chromium material layer to form a chromium pattern layer; measuring the critical dimension of the opening in the chromium pattern layer; obtaining a predicted value of the critical dimension of the opening in the MoSi light-shielding layer based on the measured value of the critical dimension and a preset MoSi etching deviation relationship; comparing the predicted value with a target value of the critical dimension of the opening in the MoSi light-shielding layer; if the predicted value is greater than the target value, reducing the basic MoSi etching time; if the predicted value is less than the target value, increasing the basic MoSi etching time; using the chromium pattern layer as a shielding layer, etching the MoSi light-shielding material layer according to the adjusted basic MoSi etching time to form a MoSi light-shielding layer; and removing the chromium pattern layer to form an opaque MoSi mask. This invention can predict the final critical dimension after chromium etching and compensate for it in a timely manner, significantly improving process yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of integrated circuits, and more particularly to a method for manufacturing an opaque MoSi mask. Background Technology

[0002] Opaque MoSi (OMOG) masks use an opaque MoSi thin film instead of a traditional chromium (Cr) layer as the light-shielding layer. Compared to traditional Cr masks, OMOG masks have become the mainstream choice for critical layer photomask fabrication at technology nodes of 28nm and below (including advanced nodes such as 14nm and 7nm) due to their superior optical performance and higher pattern resolution in the deep ultraviolet (DUV) and even extreme ultraviolet (EUV) lithography bands.

[0003] As integrated circuit manufacturing processes continue to evolve towards smaller dimensions, the requirements for mask pattern precision have reached unprecedented levels. Among these, the Critical Dimension Mean to Target (CD MTT) is one of the core indicators for measuring mask manufacturing precision. Specifically, the CD specification requirement for the 28nm node is controlled within ±4nm, for the 14nm node it is as stringent as ±2nm, and for the 7nm node, the CD specification is further tightened to ±1.4nm. It is foreseeable that with the development of more advanced nodes in the future, the CD MTT specification will further shrink, posing an extreme challenge to the controllability of the manufacturing process.

[0004] Against this backdrop, traditional OMOG mask manufacturing processes, lacking effective compensation mechanisms, face severe yield problems. Due to the lack of predictive and controllable methods for the final CD (Disc Mounting Time), various process fluctuations during manufacturing directly lead to the final product's CD MTT (Disc Mounting Time Tolerance) exceeding specifications (Out of Spec, or OOS). Statistics show that under uncompensated process conditions, the mask scrap rate (OOS rate) caused by CD MTT exceeding specifications rises sharply with node evolution. The OOS rate at the 28nm node has reached 5%-10%, further deteriorating to 10%-15% at the 14nm node, and reaching a staggering 15%-30% at the 7nm node. Such a high scrap rate not only results in huge waste of raw materials and processing costs but also severely restricts the mass production efficiency and economic benefits of advanced process chips.

[0005] To reduce the scrap rate caused by Critical Dimension Tolerance (CD) exceeding specifications, the industry typically compensates for CD deviations during the fabrication of opaque MoSi masks using over-etching with Cr. However, this method has significant limitations: First, it can only compensate for small deviations in critical dimensions; if the CD is large, it cannot be remedied, making it a one-way compensation mechanism. Second, the over-etching after Cr etching requires lateral etching to change the final CD, which alters the sidewall profile of Cr, leading to changes in CD linearity, pattern density dependence, and other CD behaviors, resulting in a decrease in mask quality. Therefore, it is only suitable for mask fabrication at nodes above 55nm and cannot meet the precision requirements of advanced nodes at 28nm and below. Furthermore, the over-etching of Cr indirectly alters the final CD by changing the sidewall profile of Cr, resulting in significant fluctuations and limited control precision, making it difficult to meet the stringent specifications of advanced nodes.

[0006] Therefore, developing a manufacturing method for opaque MoSi masks that can effectively predict and accurately compensate for CD deviations has become an urgent need to overcome the bottleneck in the manufacturing of advanced node OMOG masks.

[0007] Therefore, there is an urgent need for a critical dimension control method for OMOG blank masks that can predict the final critical dimension after Cr etching and compensate in a timely manner, so as to overcome the limitations of existing technologies such as unidirectional compensation, quality degradation, insufficient accuracy, and applicability only to nodes above 55nm, and significantly reduce the scrap rate of advanced node OMOG blank masks caused by dimensional mean deviation and OOS. Summary of the Invention

[0008] The technical problem to be solved by the present invention is to provide a method for manufacturing an opaque MoSi mask, which can predict the final critical dimensions after Cr etching and compensate in a timely manner, thus significantly improving the process yield.

[0009] To address the aforementioned problems, this invention provides a method for manufacturing an opaque MoSi mask, comprising: providing a blank mask, the blank mask comprising a light-transmitting substrate, a MoSi light-shielding material layer covering the light-transmitting substrate, and a chromium material layer covering the MoSi light-shielding material layer; etching the chromium material layer to form a chromium pattern layer; measuring the critical dimension of the opening of the chromium pattern layer; obtaining a predicted value of the critical dimension of the opening of the MoSi light-shielding layer based on the measured value of the critical dimension and a preset MoSi etching deviation relationship; comparing the predicted value with a target value of the critical dimension of the opening of the MoSi light-shielding layer; if the predicted value is greater than the target value, reducing the basic MoSi etching time; if the predicted value is less than the target value, increasing the basic MoSi etching time; using the chromium pattern layer as a shielding layer, etching the MoSi light-shielding material layer according to the adjusted basic MoSi etching time to form the MoSi light-shielding layer; and removing the chromium pattern layer to form an opaque MoSi mask comprising the light-transmitting substrate and the MoSi light-shielding layer.

[0010] In one embodiment, the step of etching the chromium material layer further includes: forming a photoresist pattern layer on the chromium material layer; using the photoresist pattern layer as a masking layer, etching the chromium material layer to form the chromium pattern layer.

[0011] In one embodiment, the step of etching the MoSi light-shielding material layer further includes: using the photoresist pattern layer and the chromium pattern layer together as a shielding layer; the step of removing the chromium pattern layer further includes: first removing the photoresist pattern layer, then removing the chromium pattern layer, or simultaneously removing the photoresist pattern layer and the chromium pattern layer.

[0012] In one embodiment, the step of etching the MoSi light-shielding material layer further includes removing the photoresist pattern layer.

[0013] In one embodiment, the preset MoSi etching deviation relationship includes a preset difference between the critical size of the opening of the chromium patterned layer and the critical size of the opening of the MoSi light-shielding layer.

[0014] In one embodiment, if the deviation between the predicted value and the target value is within a preset tolerance range, the basic MoSi etching time is not adjusted.

[0015] In one embodiment, the basic MoSi etching time consists of the endpoint detection time and the over-etching time, wherein the over-etching time includes a basic over-etching time and a compensation margin; if the predicted value is greater than the target value, the compensation margin is reduced, and if the predicted value is less than the target value, the compensation margin is increased.

[0016] In one embodiment, the increase or decrease in the compensation margin is linearly related to the change in the value of the critical dimension.

[0017] In one embodiment, the manufacturing method further includes pre-calibrating the critical dimensions of the openings of the MoSi light-shielding layer corresponding to different MoSi etching times through experiments, so as to obtain the correspondence between the MoSi etching time and the changes in critical dimensions.

[0018] The above technical solution measures the critical dimensions of the opening in the chromium patterned layer after etching the chromium material layer and predicts the critical dimensions of the opening in the final MoSi light-shielding layer based on a preset MoSi etching deviation relationship. Then, utilizing the characteristic of opaque MoSi (OMOG) masks as non-phase-shifting masks that do not require control of phase shift angle and transmittance, bidirectional and precise compensation of the critical dimensions of the opening in the final MoSi light-shielding layer is achieved by adjusting the MoSi etching time. This manufacturing method overcomes the fundamental defects of existing Cr etching plus etching compensation methods, such as unidirectional compensation, quality degradation, insufficient precision, and applicability only to nodes above 55nm. It significantly reduces the scrap rate caused by CDMTT exceeding specifications for opaque MoSi (OMOG) masks at advanced nodes of 28nm, 14nm, 7nm and below, while requiring no additional equipment or process steps, offering significant advantages of low cost, ease of implementation, and high efficiency.

[0019] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and are not intended to limit the invention. Techniques, methods, and apparatus known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and apparatus should be considered part of the specification. Attached Figure Description

[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 This is a schematic diagram of the steps in a method for manufacturing an opaque MoSi mask according to an embodiment of the present invention; Figure 2 This is a cross-sectional schematic diagram of a blank mask provided in the manufacturing method of an opaque MoSi mask according to an embodiment of the present invention. Figure 3 This is a cross-sectional schematic diagram of the formation of a chromium pattern layer in a method for manufacturing an opaque MoSi mask according to an embodiment of the present invention; Figure 4This is a cross-sectional schematic diagram of the etching of the MoSi light-shielding material layer in the manufacturing method of the opaque MoSi mask provided in an embodiment of the present invention; Figure 5 This is a schematic cross-sectional view of an opaque MoSi mask formed in a manufacturing method of an opaque MoSi mask according to an embodiment of the present invention. Figure 6 This is the compensation strategy verification data for the manufacturing method provided in the embodiments of this application; Figure 7 This is a comparative verification data between the manufacturing method provided in the embodiments of this application and the existing Cr etching plus etching compensation method.

[0022] Explanation of reference numerals in the attached figures: 100, transparent substrate; 110, MoSi light-shielding material layer; 120, chromium material layer; 200, chromium pattern layer; 201, first opening; 210, photoresist pattern layer; 300, MoSi light-shielding layer; 301, second opening. Detailed Implementation

[0023] The technical solutions in the embodiments of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0024] Figure 1 This is a schematic diagram illustrating the steps of a method for manufacturing an opaque MoSi mask according to an embodiment of the present invention, as shown below. Figure 1 As shown, the manufacturing method includes: step S10, providing a blank mask, the blank mask including a light-transmitting substrate, a MoSi light-shielding material layer covering the light-transmitting substrate, and a chromium material layer covering the MoSi light-shielding material layer; step S11, etching the chromium material layer to form a chromium pattern layer; step S12, measuring the critical dimension of the opening of the chromium pattern layer; step S13, obtaining a predicted value of the critical dimension of the opening of the MoSi light-shielding layer based on the measured value of the critical dimension and a preset MoSi etching deviation relationship; step S14, converting the predicted value... Compared with the target value of the critical dimension of the opening of the MoSi light-shielding layer, if the predicted value is greater than the target value, the basic MoSi etching time is reduced; if the predicted value is less than the target value, the basic MoSi etching time is increased; in step S15, using the chromium pattern layer as a shielding layer, the MoSi light-shielding material layer is etched according to the adjusted basic MoSi etching time to form the MoSi light-shielding layer; in step S16, the chromium pattern layer is removed to form an opaque MoSi mask including the light-transmitting substrate and the MoSi light-shielding layer.

[0025] The method for manufacturing an opaque MoSi mask provided in this invention measures the critical dimensions of the openings in the chromium patterned layer after etching the chromium material layer and predicts the critical dimensions of the openings in the final MoSi light-shielding layer based on a preset MoSi etching deviation relationship. Utilizing the characteristic of the opaque MoSi (OMOG) mask as a non-phase-shifting mask that eliminates the need to control the phase shift angle and transmittance, bidirectional and precise compensation of the critical dimensions of the openings in the final MoSi light-shielding layer is achieved by adjusting the MoSi etching time. This method overcomes the fundamental defects of existing Cr etching plus etching compensation methods, such as unidirectional compensation, quality degradation, insufficient accuracy, and applicability only to nodes above 55nm. It significantly reduces the scrap rate caused by CD MTT exceeding specifications for opaque MoSi (OMOG) masks at advanced nodes of 28nm, 14nm, 7nm, and below. Furthermore, it requires no additional equipment or process steps, offering significant advantages such as low cost, ease of implementation, and high efficiency.

[0026] Figures 2-5 This is a process flow diagram of a method for manufacturing an opaque MoSi mask according to an embodiment of the present invention. The following is in conjunction with... Figures 1-5 A method for manufacturing an opaque MoSi mask according to an embodiment of the present invention will be described in detail.

[0027] refer to Figure 1 as well as Figure 2 As in step S10, a blank mask is provided, the blank mask including a light-transmitting substrate 100, a MoSi light-shielding material layer 110 covering the light-transmitting substrate 100, and a chromium material layer 120 covering the MoSi light-shielding material layer 110.

[0028] The light-transmitting substrate 100 is typically made of quartz, which has high light transmittance, low coefficient of thermal expansion, and excellent chemical stability, providing mechanical support and optical pathways for the photomask. In this embodiment, the light-transmitting substrate 100 is a glass substrate.

[0029] The MoSi light-shielding material layer 110 covers the surface of the transparent substrate 100 and has light-shielding properties. It replaces the traditional chromium material layer as the light-shielding layer for the final manufactured MoSi mask, effectively absorbing ultraviolet light in the exposure band and achieving high-precision pattern masking. In this embodiment, the MoSi light-shielding material layer 110 is an opaque MoSiON (molybdenum silicon oxynitride) thin film. MoSiON is a composite thin film material whose optical constants (refractive index n and extinction coefficient k) can be precisely controlled by adjusting the ratio of oxygen and nitrogen, making it completely opaque in the deep ultraviolet lithography band, thus meeting the light-shielding requirements of advanced nodes at 28nm and below.

[0030] The chromium material layer 120 covers the surface of the MoSi light-shielding material layer 110. The chromium material layer 120 and the MoSi light-shielding material layer 110 have good adhesion and can withstand the thermal and mechanical stresses in subsequent photoresist coating, baking and multiple etching cycles, ensuring the integrity of the film interface throughout the manufacturing process.

[0031] refer to Figure 1 as well as Figure 3 As in step S11, the chromium material layer 120 is etched to form a chromium pattern layer 200. The purpose of this step is to precisely transfer a predefined pattern onto the chromium material layer 120, thereby forming the chromium pattern layer 200, which provides a reliable hard mask for the etching of the MoSi light-shielding material layer 110. A portion of the MoSi light-shielding material layer 110 is exposed through an opening in the chromium pattern layer 200 (hereinafter referred to as the first opening 201). These exposed areas will be removed in subsequent etching steps, while the chromium-covered areas are protected and retained, thus enabling the precise transfer of the pattern on the chromium pattern layer 200 to the MoSi light-shielding material layer 110.

[0032] As an example, the step of etching the chromium material layer 120 further includes: A photoresist pattern layer 210 is formed on the chromium material layer 120, the pattern of which corresponds to the pattern designed on the photomask. A portion of the chromium material layer 120 is exposed through windows in the photoresist pattern layer 210. These exposed areas will be removed in a subsequent chromium etching step, while the areas covered by the photoresist are protected and retained, thereby precisely transferring the pattern on the photoresist pattern layer 210 to the chromium material layer 120. Specifically, this step further includes: forming a photoresist material layer on the chromium material layer 120 using a spin-coating process, the photoresist material layer covering the upper surface of the chromium material layer 120; and patterning the photoresist material layer using standard photolithography processes such as exposure and development, thereby forming the photoresist pattern layer 210.

[0033] Using the photoresist pattern layer 210 as a masking layer, the chromium material layer 120 is etched to form the chromium pattern layer 200. Specifically, in this step, using the photoresist pattern layer 210 as a masking layer, the chromium material layer 120 is etched using a dry etching or wet etching process to transfer the pattern on the photoresist pattern layer 210 to the chromium material layer 120, thereby forming the chromium pattern layer 200.

[0034] refer to Figure 1 as well as Figure 3As in step S12, the critical dimensions of the first opening 201 of the chromium pattern layer 200 are measured, that is, the width or spacing (AEI CD) of each first opening 201 in the chromium pattern layer 200 formed after the chromium material layer 120 is etched is precisely measured.

[0035] In some embodiments, an optical critical dimension measuring device may be used to measure the critical dimension of the first opening 201 of the chromium pattern layer 200. In another embodiment, a scanning electron microscope may be used to measure the critical dimension of the first opening 201 of the chromium pattern layer 200.

[0036] Furthermore, in one embodiment, the timing of the step of measuring the critical dimensions of the first opening 201 of the chromium pattern layer 200 depends on the subsequent etching step of the MoSi light-shielding material layer 110.

[0037] Specifically, if the subsequent step is to first remove the photoresist pattern layer 210, and then etch the MoSi light-shielding material layer 110 using the chromium pattern layer 200 as a single shielding layer, then the step of measuring the critical dimension of the first opening 201 of the chromium pattern layer 200 can be performed after the step of removing the photoresist pattern layer 210. This is because after the photoresist removal step, the surface of the chromium pattern layer 200 is completely exposed, and the measuring equipment can directly detect the first opening 201 of the chromium pattern layer 200. There is no interference or obstruction of the measurement signal by the photoresist pattern layer 210, and the measurement results are intuitive and reliable. Although the photoresist removal process may produce a weak chemical or physical effect on the edge of the chromium pattern layer 200, since the subsequent etching of the MoSi light-shielding material layer 110 is also performed after the removal of the photoresist pattern layer 210, the effect of this effect has been incorporated into the preset MoSi etching deviation relationship, and therefore will not reduce the prediction accuracy.

[0038] If the subsequent step involves etching the MoSi light-shielding material layer 110 using both the photoresist pattern layer 210 and the chromium pattern layer 200 as shielding layers, then the step of measuring the critical dimension of the first opening 201 of the chromium pattern layer 200 can be performed directly after the chromium pattern layer 200 is formed and before the photoresist pattern layer 210 is removed. The photoresist pattern layer 210 plays a protective role during the etching process of the chromium material layer 120, and its edge closely matches the edge of the chromium pattern layer 200. However, under the coverage of the photoresist pattern layer 210, the sidewall of the first opening 201 of the chromium pattern layer 200 has not yet been exposed to the subsequent resist stripping solution or plasma. Therefore, the measured CD value completely excludes any dimensional changes that may be introduced by the resist stripping process. Furthermore, since the subsequent MoSi etching will use the composite structure of the photoresist pattern layer 210 and the chromium pattern layer 200 as a shielding layer, the presence of the photoresist pattern layer 210 will not change the geometry of the first opening 201 of the chromium pattern layer 200. Measuring before removing the photoresist pattern layer 210 allows the true state of the chromium etching to be locked as a fixed benchmark, avoiding random errors that may occur due to fluctuations in the photoresist removal conditions after removing the photoresist pattern layer 210. In addition, the photoresist pattern layer 210 has a certain degree of light transmittance or can be penetrated under deep ultraviolet or electron beam measurement conditions. Modern optical CD measurement equipment can distinguish the signal contributions of the photoresist and the chromium pattern layer 200 through modeling, thereby accurately extracting the size of the first opening 201 of the chromium pattern layer 200 without sacrificing measurement accuracy due to the presence of the photoresist. Therefore, completing the measurement before the photoresist patterning layer 210 can obtain CD data that is closer to the actual process state, providing a higher confidence input for subsequent prediction based on the preset MoSi etching deviation relationship, thereby improving the control accuracy of the entire critical dimension compensation method.

[0039] refer to Figure 1 As in step S13, based on the measured values ​​of the key dimensions and the preset MoSi etching deviation relationship, the opening of the MoSi light-shielding layer 300 (marked in) is obtained. Figure 4 The following description refers to the predicted value of the critical dimension of the second opening 301. The MoSi light-shielding layer 300 is the MoSi light-shielding layer 300 in the finally formed opaque MoSi mask.

[0040] The preset MoSi etching deviation relationship describes the intrinsic connection between the critical dimension (AEICD) of the first opening 201 of the chromium patterned layer 200 and the critical dimension of the second opening 301 of the finally formed MoSi light-shielding layer 300. Specifically, in one embodiment, the preset MoSi etching deviation relationship includes a preset difference between the critical dimension of the first opening 201 of the chromium patterned layer 200 and the critical dimension of the second opening 301 of the light-shielding layer. This difference represents the dimensional change caused by factors such as undercut during the MoSi etching process. By calculating this preset difference with the measured value of AEICD, the predicted value of the critical dimension of the second opening 301 of the MoSi light-shielding layer 300 after MoSi etching can be calculated, thereby realizing the prediction of the critical dimension of the second opening 301 of the finally formed MoSi light-shielding layer 300 before MoSi etching.

[0041] As an example, in some embodiments, the preset difference can be obtained through experimental calibration, that is, under the same process conditions, the critical dimension (AEI CD) of the first opening 201 of the chromium pattern layer 200 of a batch of test samples and the critical dimension of the second opening 301 of the finally formed MoSi light-shielding layer 300 are measured respectively, and the average difference between the two is calculated as the preset difference.

[0042] refer to Figure 1 As in step S14, the predicted value is compared with the target value of the critical dimension of the second opening 301 of the MoSi light-shielding layer 300. If the predicted value is greater than the target value, the basic MoSi etching time is reduced. If the predicted value is less than the target value, the basic MoSi etching time is increased. If the predicted value is equal to the target value, the basic MoSi etching time is not changed.

[0043] Specifically, if the predicted value is greater than the target value, it indicates that the critical dimension of the second opening 301 of the final MoSi light-shielding layer 300 may be too large. In this case, the basic MoSi etching time needs to be reduced to decrease the lateral drilling amount, so that the critical dimension of the second opening 301 of the final MoSi light-shielding layer 300 returns to the target value. If the predicted value is less than the target value, it indicates that the critical dimension of the second opening 301 of the final MoSi light-shielding layer 300 may be too small. In this case, the basic MoSi etching time needs to be increased to increase the lateral drilling amount, so that the critical dimension of the second opening 301 of the final MoSi light-shielding layer 300 increases to the target value. The manufacturing method described in this invention can perform bidirectional adaptive compensation for critical dimensions based on actual measurements, rather than traditional methods that are limited to unidirectional compensation.

[0044] In some embodiments, if the deviation between the predicted value and the target value is within a preset tolerance range, the basic MoSi etching time is not adjusted. Specifically, if the predicted value is greater than the sum of the target value and the preset tolerance, the basic MoSi etching time is reduced; if the predicted value is less than the difference between the target value and the preset tolerance, the basic MoSi etching time is increased; if the predicted value is equal to the sum of the target value and the preset tolerance, or if the predicted value is equal to the difference between the target value and the preset tolerance, the basic MoSi etching time remains unchanged. This preset tolerance range can be flexibly set according to the CD specifications of different technology nodes. For example, for the 28nm node, the tolerance range can be set to ±4nm (i.e., the preset tolerance is 4nm), and for the 7nm node, it can be set to ±1.4nm (i.e., the preset tolerance is 1.4nm). When the predicted value falls within this range, it indicates that the current process status is good, and no intervention is required. Subsequent steps can be executed directly according to the standard process, thus ensuring both accuracy and production efficiency.

[0045] The composition of the basic MoSi etching time is another important aspect of achieving accurate CD compensation. In some embodiments, the basic MoSi etching time consists of the endpoint detection time (EPD Time) and the over-etch time. The endpoint detection time is the moment when the etching equipment detects, via optical or mass spectrometry signals, that the MoSi light-shielding material layer 110 has just been etched through, while the over-etch time is the additional time added to ensure that any residual MoSi material at the bottom of the MoSi light-shielding material layer 110 is completely removed. Further, the over-etch time includes a basic over-etch time and a compensation margin. The basic over-etch time ensures the thoroughness of the etching, while the compensation margin is an adjustable space specifically reserved for CD compensation. When compensation is required, if the predicted value is greater than the target value, the compensation margin is decreased; if the predicted value is less than the target value, the compensation margin is increased. This design, which separates the compensation margin from the over-etch time, allows adjustments to be made directly to the compensation margin without affecting the basic etching process window, thereby ensuring process stability and controllability.

[0046] As an example, in one embodiment, the compensation margin is 5 seconds, that is, 5 seconds are added to the normal over-etching time as the base MoSi etching time, i.e., T_base = T_EPD + OE_base + 5s, where T_base is the base MoSi etching time, T_EPD is the endpoint detection time, OE_base is the over-etching time, and the adjustment range of the adjustment amount ΔT_adj is -5s to +5s. Then, the adjusted base MoSi etching time (i.e. the actual MoSi etching time) T_final = T_base + ΔT_adj.

[0047] Furthermore, in one embodiment, the increase or decrease in the compensation margin is linearly related to the change in the critical dimension. As an example, experimental calibration shows that under specific MoSi etching parameters, for every 1 second increase or decrease in MoSi etching time, the critical dimension of the second opening 301 of the ultimately formed MoSi light-shielding layer 300 changes by approximately 1 nanometer. This linear relationship makes the calculation of the compensation amount very simple and intuitive; the difference between the predicted and target values ​​(in nanometers) can be directly converted into the corresponding number of seconds to determine the etching time that needs adjustment, thus achieving high-precision quantitative compensation.

[0048] Furthermore, in some embodiments, the manufacturing method provided by the present invention further includes pre-calibrating the critical dimensions of the opening of the light-shielding layer corresponding to different MoSi etching times through experiments, so as to obtain the correspondence between MoSi etching time and critical dimension changes. Specifically, a set of blank mask samples are prepared, and a consistent chromium pattern layer 200 is formed under the same Cr etching conditions. Then, different MoSi etching times are used for etching, and the critical dimensions of the second opening 301 of the final MoSi light-shielding layer 300 formed for each set of samples are measured. By fitting and analyzing the data, a linear function relationship between etching time and CD change can be obtained. These calibration data will be stored in the process formulation for subsequent production use. Based on the difference between the predicted value and the target value of the critical dimension of the second opening 301 of the MoSi light-shielding layer 300, combined with the correspondence between MoSi etching time and critical dimension changes, the adjustment amount of the basic MoSi etching time can be determined.

[0049] refer to Figure 1 as well as Figure 4 As in step S15, the MoSi light-shielding material layer 110 is etched according to the adjusted base MoSi etching time, using the chromium pattern layer 200 as a shielding layer, to form the MoSi light-shielding layer 300.

[0050] Since the opaque MoSi (OMOG) mask manufactured by the method provided in this embodiment of the invention is not a phase-shifting mask (PSM), its MoSi light-shielding layer is only used as a light-shielding layer, and there is no need to control the phase shift angle and transmittance. Therefore, adjusting the MoSi etching time within a certain range will not have any impact on the optical quality of the opaque MoSi (OMOG) mask, but will only change the critical dimension value of the second opening 301 of the finally formed MoSi light-shielding layer 300. This characteristic makes it feasible and safe to compensate for CD deviation by adjusting the MoSi etching time, which is also the fundamental reason why this invention can achieve high-quality compensation.

[0051] In some embodiments, the step of etching the MoSi light-shielding material layer 110 further includes using the photoresist pattern layer 210 and the chromium pattern layer 200 together as a shielding layer. That is, when etching the MoSi light-shielding material layer 110, the photoresist pattern layer 210 has not yet been removed, and together with the chromium pattern layer 200, they form a double-layer shielding structure, enhancing the protection of the underlying MoSi light-shielding material layer 110 and ensuring the sharpness of the pattern edges. Accordingly, in the subsequent step of removing the chromium pattern layer 200, it is possible to remove the photoresist pattern layer 210 first and then remove the chromium pattern layer 200, or to remove the photoresist pattern layer 210 and the chromium pattern layer 200 simultaneously. Both methods can achieve the final cleaning of the mask.

[0052] In some embodiments, the step of etching the MoSi light-shielding material layer 110 further includes removing the photoresist pattern layer 210. That is, before etching the MoSi light-shielding material layer 110, the photoresist pattern layer 210 is completely stripped away, leaving only the chromium pattern layer 200 as the sole hard mask layer. This method can prevent the photoresist pattern layer 210 from carbonizing or deforming due to high temperature or plasma bombardment during the etching process of the MoSi light-shielding material layer 110, thereby ensuring the purity of the etching environment and the stability of the etching results.

[0053] refer to Figure 1 as well as Figure 5 As in step S16, the chromium pattern layer 200 is removed, thereby forming an opaque MoSi mask including the light-transmitting substrate 100 and the MoSi light-shielding layer 300. The second opening 301 of the MoSi light-shielding layer 300 exposes the light-transmitting substrate 100.

[0054] In some embodiments, the removal of the chromium pattern layer 200 can be achieved using either wet etching or dry etching processes, the specific choice depending on process compatibility and environmental requirements. At this point, an opaque MoSi (OMOG) mask with precise CD compensation is manufactured. Its CD MTT has been precisely controlled within the target specification range through bidirectional adjustment of the MoSi etching time, significantly reducing the scrap rate caused by CD exceeding specifications.

[0055] Furthermore, in one embodiment, the bidirectional compensation method for MoSi etching time described above enables precise control of critical dimensions at different process nodes.

[0056] Figure 6 This is the compensation strategy verification data for the manufacturing method provided in the embodiments of this application. For example... Figure 6As shown, the manufacturing method provided in this application has a bidirectional compensation capability of ±5nm for advanced nodes such as 28nm, 14nm, and 7nm, enabling complete coverage of critical dimension control. Verification data shows that before adopting the dual compensation method of this application, the out-of-specification (OOS) rates for critical dimension target values ​​at 28nm, 14nm, and 7nm nodes were as high as 5-10%, 15-25%, and 30-50%, respectively. However, after using critical dimension prediction after chromium layer etching combined with molybdenum silicon oxynitride etching time compensation, the OOS rates for each node decreased to below 1%, below 2%, and below 5%, respectively. The above verification data confirms that the method of this application can be widely applied to the critical dimension control of opaque molybdenum silicon oxynitride blank masks at all advanced nodes of 28nm, 14nm, 7nm, and below, reducing the scrap rate caused by critical dimension target values ​​exceeding specifications by more than 90%, significantly improving process yield.

[0057] Figure 7 This is a comparison and verification data between the manufacturing method provided in the embodiments of this application and the existing Cr etching plus etching compensation method. For example... Figure 7 As shown, existing chromium etching plus etching methods are limited in the compensation direction, only able to compensate when the critical aperture size is small, and they alter the sidewall profile of the chromium layer, causing degradation of critical aperture linearity and large fluctuations in control accuracy. This method is only applicable to technology nodes of 55nm and above. The manufacturing method provided in this application completely overcomes these technical bottlenecks, achieving bidirectional adaptive compensation for both large and small critical aperture sizes. Since the opaque MoSi mask is a non-phase-shifting mask, adjusting the MoSi etching time does not affect the phase shift angle or transmittance, nor does it affect the sidewall profile of the chromium layer, thus avoiding degradation of indicators such as critical aperture linearity. Simultaneously, the adjustment of the MoSi etching time directly affects the etching amount of the MoSi material layer, with a clear linear relationship and small fluctuations, resulting in superior control accuracy compared to existing indirect control methods. Furthermore, the manufacturing method of this application does not require additional equipment costs and can be widely applied to critical aperture control of opaque MoSi blank masks at all advanced nodes of 28nm, 14nm, 7nm and below, significantly improving process yield.

[0058] It should be noted that references to "an embodiment," "an embodiment," "an exemplary embodiment," "some embodiments," etc., in the specification indicate that the described embodiments may include specific features, structures, or characteristics, but each embodiment may not necessarily include that specific feature, structure, or characteristic. Furthermore, such phrases do not necessarily refer to the same embodiment. In addition, when a specific feature, structure, or characteristic is described in connection with an embodiment, whether explicitly described or not, implementing such a feature, structure, or characteristic in conjunction with other embodiments is within the knowledge of those skilled in the art.

[0059] It should be noted that the terms "comprising" and "having," and their variations, used in this invention document are intended to cover non-exclusive inclusion. The terms "first," "second," etc., are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence, unless explicitly indicated by the context. It should be understood that such data used interchangeably where appropriate. Furthermore, embodiments and features within embodiments of this invention can be combined with each other unless otherwise specified. In addition, descriptions of well-known components and technologies have been omitted in the above description to avoid unnecessarily obscuring the concepts of this invention. In the various embodiments described above, each embodiment focuses on its differences from other embodiments; similar or identical parts between embodiments can be referred to interchangeably.

[0060] The above description is only a preferred embodiment of the present invention. It should be noted that those skilled in the art can make several improvements and modifications without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for manufacturing an opaque MoSi photomask, characterized in that, include: A blank mask is provided, the blank mask comprising a light-transmitting substrate, a MoSi light-shielding material layer covering the light-transmitting substrate, and a chromium material layer covering the MoSi light-shielding material layer; The chromium material layer is etched to form a chromium pattern layer; Measure the critical dimensions of the openings in the chromium patterned layer; Based on the measured values ​​of the critical dimensions and the preset MoSi etching deviation relationship, the predicted values ​​of the critical dimensions of the opening of the MoSi light-shielding layer are obtained. The predicted value is compared with the target value of the critical dimension of the opening of the MoSi light-shielding layer. If the predicted value is greater than the target value, the basic MoSi etching time is reduced; if the predicted value is less than the target value, the basic MoSi etching time is increased. Using the chromium patterned layer as a shielding layer, the MoSi light-shielding material layer is etched according to the adjusted base MoSi etching time to form the MoSi light-shielding layer; The chromium pattern layer is removed to form an opaque MoSi mask that includes the light-transmitting substrate and the MoSi light-shielding layer.

2. The manufacturing method according to claim 1, characterized in that, The step of etching the chromium material layer further includes: A photoresist pattern layer is formed on the chromium material layer; Using the photoresist pattern layer as a masking layer, the chromium material layer is etched to form the chromium pattern layer.

3. The manufacturing method according to claim 2, characterized in that, The step of etching the MoSi light-shielding material layer further includes: using the photoresist pattern layer and the chromium pattern layer together as a shielding layer; the step of removing the chromium pattern layer further includes: first removing the photoresist pattern layer, then removing the chromium pattern layer, or simultaneously removing the photoresist pattern layer and the chromium pattern layer.

4. The manufacturing method according to claim 2, characterized in that, The step of etching the MoSi light-shielding material layer includes removing the photoresist pattern layer.

5. The manufacturing method according to claim 1, characterized in that, The preset MoSi etching deviation relationship includes the preset difference between the critical dimension of the opening of the chromium pattern layer and the critical dimension of the opening of the MoSi light-shielding layer.

6. The manufacturing method according to claim 1, characterized in that, If the deviation between the predicted value and the target value is within the preset tolerance range, the basic MoSi etching time will not be adjusted.

7. The manufacturing method according to claim 1, characterized in that, The basic MoSi etching time consists of the endpoint detection time and the over-etching time. The over-etching time includes the basic over-etching time and the compensation margin. If the predicted value is greater than the target value, the compensation margin is reduced. If the predicted value is less than the target value, the compensation margin is increased.

8. The manufacturing method according to claim 7, characterized in that, The increase or decrease in the compensation margin is linearly related to the change in the value of the critical dimension.

9. The manufacturing method according to claim 1, characterized in that, The manufacturing method further includes pre-calibrating the critical dimensions of the opening of the MoSi light-shielding layer at different MoSi etching times through experiments, so as to obtain the correspondence between the MoSi etching time and the change of critical dimensions.