Circular belt, intermediate transfer belt, transfer device and image forming device

By controlling the area and dispersion diameter of the Voronoi polygon of the conductive particles, and combining a specific range of carbon black and polyimide resins, the problems of fracture resistance and conductive particle dispersion in annular bands were solved, thereby improving the fracture resistance and conductivity maintenance of the annular bands.

CN123113265APending Publication Date: 2026-11-17FUJIFILM BUSINESS INNOVATION CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610085889.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-01-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

When existing annular belts contain resin and conductive particles, observations along the thickness direction of the belt reveal inappropriate distributions of the area and standard deviation of the Voronoi polygons in the Voronoi mosaic of conductive particles, as well as the average dispersion diameter and closest distance of the conductive particles. This results in poor fracture resistance and poor dispersion of conductive particles along the thickness direction of the belt.

Method used

The dispersibility of conductive particles is improved by controlling the area of ​​the Voronoi polygon of the conductive particles to be above 1400 nm2 and below 2000 nm2, the standard deviation to be below 1200 nm2, the average dispersion diameter of the conductive particles to be below 30 nm, and the closest distance distribution to be above 20 nm and below 40 nm, and by using a specific range of carbon black and polyimide resins, especially imides of polyamic acid with all ends being amino groups.

Benefits of technology

It improves the fracture resistance of the annular belt and the dispersion of conductive particles in the belt thickness direction, enhances the electrical resistance and conductivity retention when high voltage is applied, and is suitable for fracture resistance and transfer retention when used in transfer belts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123113265A_ABST
    Figure CN123113265A_ABST
Patent Text Reader

Abstract

This invention relates to an annular belt, an intermediate transfer belt, a transfer apparatus, and an image forming apparatus. The annular belt contains resin and conductive particles. When a cross-section is observed along the belt's thickness direction, the average area of ​​the Voronoi polygons in the Voronoi tessellation, with the centroid of the conductive particles as the generatrix, is 1400 nm. 2 Above and 2000nm 2 The standard deviation of the area of ​​the Voronoi polygon is 1200 nm. 2 Hereinafter, the average dispersion diameter of the conductive particles is less than 30 nm, and the average value of the closest distance distribution of the conductive particles is more than 20 nm and less than 40 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an annular belt, an intermediate transfer belt, a transfer device, and an image forming apparatus. Background Technology

[0002] In image forming apparatuses (copiers, fax machines, printers, etc.) using electrophotographic methods, a toner image formed on the surface of an image holder is transferred to the surface of a recording medium, and then fixed onto the recording medium to form an image. Furthermore, in this transfer of the toner image to the recording medium, for example, an intermediate transfer belt is used. Not limited to image forming apparatuses, various annular belts such as conveyor belts are also used in other apparatuses.

[0003] For example, Patent Document 1 discloses "an annular strip, wherein the ratio (area B / area A) of the curve area B of the region with a particle size exceeding 35 nm in the volume frequency distribution of particles determined by X-ray small-angle scattering to the curve area A of the region with a particle size below 35 nm in the volume frequency distribution is 0.3 or less."

[0004] Patent document 2 discloses "annular strip, wherein the integral value of the statistic L(r) is 0 or more and 0.1 or less when the interparticle distance r is 0.05 μm or more and 0.30 μm or less in the spatial distribution of the first conductive carbon particles present in the 6.3 μm × 4.2 μm evaluation region on the outer periphery."

[0005] Patent document 3 discloses "an electrophotographic tape, wherein when the arithmetic mean of the areas of the Voronoi polygons formed by performing Voronoi tessellation on a cross section of the electrophotographic tape in a direction orthogonal to the circumference with magnesium hydroxide particles exposed on the cross section as the parent point is set as S, and the standard deviation is set as σ, the variation coefficient (=σ / S) is 1.5 or less."

[0006] Patent Document 1: Japanese Patent Application Publication No. 2023-135214

[0007] Patent Document 2: Japanese Patent Application Publication No. 2021-092598

[0008] Patent Document 3: Japanese Patent Application Publication No. 2023-008686 Summary of the Invention

[0009] The objective of this invention is to provide an annular strip in which, when a cross-section is observed along the thickness direction of the strip containing resin and conductive particles, the average area of ​​the Voronoi polygons in the Voronoi mosaic with the centroid of the conductive particles as the parent point is less than 1400 nm. 2 or more than 2000nm 2The standard deviation of the area of ​​the Voronoi polygon exceeds 1200 nm. 2 Compared to cases where the average dispersion diameter of conductive particles exceeds 30 nm or the average value of the closest distance distribution of conductive particles is less than 20 nm or exceeds 40 nm, the fracture resistance and the dispersion of conductive particles in the thickness direction are both excellent.

[0010] The means to solve the above problems include the following methods.

[0011] <1> A ring-shaped belt containing resin and conductive particles, When observing a cross-section along the thickness direction, The average area of ​​the Voronoi polygons in the Voronoi tessellation with the centroid of the conductive particle as the parent point is 1400 nm. 2 Above and 2000nm 2 The standard deviation of the area of ​​the Voronoi polygon is 1200 nm. 2 the following, The average dispersion diameter of the conductive particles is less than 30 nm. The average of the closest distance distribution of the conductive particles is above 20 nm and below 40 nm.

[0012] <2> According to the annular belt described in <1>, wherein, The average area of ​​the Voronoi polygons when the centroid of the conductive particle is used as the generatrix is ​​1600 nm. 2 Above and 1800nm 2 The standard deviation of the area of ​​the Voronoi polygon is 1000 nm. 2 the following, The average dispersion diameter of the conductive particles is less than 27 nm. The average of the closest distance distribution of the conductive particles is above 30 nm and below 35 nm.

[0013] <3> The annular belt according to <1> or <2>, wherein, The conductive particles are carbon black.

[0014] <4> According to the annular belt described in <3>, wherein, The carbon black is carbon black with a surface functional group content of ≥0.3mmol / g and ≤0.6mmol / g when back titrated with NaHCO3.

[0015] <5> According to the annular belt described in <3> or <4>, wherein, The carbon black content relative to 100 parts by weight of the resin is 16 parts by weight or more and 26 parts by weight or less.

[0016] <6> The annular band according to any one of <1> to <5>, wherein, The resin is a polyimide resin.

[0017] <7> According to the annular belt described in <6>, wherein, Polyimide resins are imides of polyamic acids with amino groups at all ends.

[0018] <8> The annular belt according to any one of <1> to <7> contains at least one silicone oil selected from the group consisting of dimethyl silicone oil and modified silicone oil.

[0019] <9> An intermediate transfer belt having any one of <1> to <8> annular belt.

[0020] <10> A transfer device comprising: The intermediate transfer belt transfers a toner image onto the outer peripheral surface and has an annular band as described in any one of <1> to <8>. A primary transfer apparatus comprising a primary transfer component that transfers a toner image formed on the surface of an image holder to the outer peripheral surface of an intermediate transfer belt in a single transfer; and A secondary transfer apparatus having a secondary transfer component configured to contact the outer peripheral surface of the intermediate transfer belt and to transfer the toner image transferred to the outer peripheral surface of the intermediate transfer belt to the surface of a recording medium.

[0021] <11> An image forming apparatus comprising: A toner image forming apparatus having an image holder, and forming a toner image on the surface of the image holder; and The transfer apparatus described in <10> transfers the toner image formed on the surface of the image holder to the surface of the recording medium.

[0022] Invention Effects

[0023] According to the invention described in <1>, an annular strip is provided, wherein, when observing a cross-section along the thickness direction of the annular strip containing resin and conductive particles, the average area of ​​the Voronoi polygons in the Voronoi mosaic with the centroid of the conductive particles as the parent point is less than 1400 nm. 2 or more than 2000nm 2 The standard deviation of the area of ​​the Voronoi polygon exceeds 1200 nm. 2 Compared to cases where the average dispersion diameter of conductive particles exceeds 30 nm or the average value of the closest distance distribution of conductive particles is less than 20 nm or exceeds 40 nm, the fracture resistance and the dispersion of conductive particles in the thickness direction are both excellent.

[0024] According to the invention described in <2>, an annular strip is provided, the average area of ​​which is less than 1600 nm compared to the area of ​​the Voronoi polygon formed by Voronoi tessellation with the centroid of the conductive particle as the parent point. 2 or more than 1800nm 2 The standard deviation of the area of ​​the Voronoi polygon exceeds 1000 nm. 2 Compared to cases where the average dispersion diameter of conductive particles exceeds 27 nm or the average value of the closest distance distribution of conductive particles is less than 30 nm or exceeds 35 nm, the fracture resistance and the dispersion of conductive particles in the thickness direction are both excellent.

[0025] According to the invention described in <3>, an annular belt is provided, which, compared with the case where the conductive particles are conductive oxide particles, has excellent fracture resistance and dispersion of conductive particles in the belt thickness direction.

[0026] According to the invention described in <4>, an annular belt is provided, which, compared with carbon black in which the amount of surface functional groups used for back titration with NaHCO3 is less than 0.3 mmol / g or more than 0.6 mmol / g, exhibits superior dispersion of fracture-resistant and conductive particles in the belt thickness direction.

[0027] According to the invention described in <5>, an annular belt is provided, which, compared to cases where the carbon black content relative to 100 parts by mass is less than 16 parts by mass or more than 26 parts by mass, exhibits superior dispersion of fracture-resistant and conductive particles in the belt thickness direction.

[0028] According to the invention described in <6>, an annular belt is provided, which, compared with the case where the resin is a polyamide-imide resin, exhibits superior resistance to breakage and excellent dispersion of conductive particles in the belt thickness direction.

[0029] According to the invention described in <7>, an annular belt is provided that, compared to the case where the polyimide resin is an imide of polyamic acid with all ends having carboxyl groups, exhibits superior dispersion of fracture-resistant and conductive particles in the belt thickness direction.

[0030] According to the invention described in <8>, an annular strip is provided, wherein, when observing a cross-section along the thickness direction of the strip containing resin and conductive particles, the average area of ​​the Voronoi polygons in the Voronoi mosaic with the centroid of the conductive particles as the generatrix is ​​less than 1400 nm. 2 or more than 2000nm 2 The standard deviation of the area of ​​the Voronoi polygon exceeds 1200 nm. 2Compared to cases where the average dispersion diameter of conductive particles exceeds 30 nm or the average value of the closest distance distribution of conductive particles is less than 20 nm or exceeds 40 nm, dimethyl silicone oil contains superior fracture resistance and dispersion of conductive particles in the thickness direction.

[0031] According to the inventions described in <9>, <10>, or <11>, an intermediate transfer belt is provided, along with a transfer apparatus and an image forming apparatus having the intermediate transfer belt. This intermediate transfer belt is applicable to annular belts containing resin and conductive particles, where, when observing a cross-section along the belt thickness direction, the average area of ​​the Voronoi polygons in a Voronoi mosaic with the centroid of the conductive particles as the parent point is less than 1400 nm. 2 or more than 2000nm 2 The standard deviation of the area of ​​the Voronoi polygon exceeds 1200 nm. 2 Compared to annular bands where the average dispersion diameter of conductive particles exceeds 30 nm or the average value of the closest distance distribution of conductive particles is less than 20 nm or exceeds 40 nm, it exhibits superior fracture resistance and transfer retention. Attached Figure Description

[0032] The embodiments of the present invention will be described in detail with reference to the following figures.

[0033] Figure 1 This is a schematic structural diagram illustrating an example of the image forming apparatus according to this embodiment; Figure 2 This is a schematic structural diagram showing the periphery of the secondary transfer section in another example of the image forming apparatus according to this embodiment. Detailed Implementation

[0034] Hereinafter, an embodiment of the present invention will be described as an example. These descriptions and examples illustrate the embodiments and do not limit the scope of the embodiments.

[0035] In this embodiment, within the numerical ranges recorded in stages, the upper or lower limit value recorded within one numerical range can be replaced with the upper or lower limit value of other numerical ranges recorded in stages. Furthermore, within the numerical ranges recorded in this embodiment, the upper or lower limit value of that numerical range can be replaced with the values ​​shown in the examples.

[0036] In this embodiment, the term "process" includes not only independent processes, but also processes that achieve their desired purpose even when they cannot be clearly distinguished from other processes.

[0037] In this embodiment, the structure is not limited to the structure shown in the accompanying drawings. Furthermore, the sizes of the components in the drawings are conceptual, and the relative sizes of the components are not limited thereto.

[0038] In this embodiment, each component may contain a plurality of corresponding substances. When referring to the amount of each component in the composition in this embodiment, if a plurality of substances corresponding to each component are present in the composition, it refers to the total amount of such plurality of substances present in the composition, unless otherwise stated.

[0039] [Ringed Belt]

[0040] The annular belt involved in this embodiment contains resin and conductive particles.

[0041] When observing a cross-section along the thickness direction, the average area of ​​the Voronoi polygons in the Voronoi mosaic with the centroid of the conductive particles as the parent point is 1400 nm. 2 Above and 2000nm 2 Below, the standard deviation of the area of ​​the Voronoi polygon is 1200 nm. 2 The average dispersion diameter of the conductive particles is less than 30 nm, and the average value of the closest distance distribution of the conductive particles is more than 20 nm and less than 40 nm.

[0042] In the past, in annular strips, conductive particles had the function of imparting conductivity to the strip, but on the other hand, they also became a reason for reducing fracture resistance.

[0043] Therefore, techniques for improving the dispersion of conductive particles are known (Patent Documents 1-3, etc.).

[0044] However, due to recent demands for improved performance, further improvements are expected.

[0045] Therefore, in the annular belt according to this embodiment, when observing the cross-section along the belt thickness direction, the average area of ​​the Voronoi polygon, the standard deviation of the Voronoi polygon area, the average dispersion diameter of the conductive particles, and the average value of the closest distance distribution of the conductive particles are controlled within the aforementioned ranges. This improves not only the dispersion in the belt surface direction but also the dispersion of conductive particles in the belt thickness direction. Furthermore, it suppresses conductive particles from becoming the starting point of fracture.

[0046] In summary, based on the above structure, the annular belt involved in this embodiment is an annular belt with excellent fracture resistance and dispersion of conductive particles in the belt thickness direction.

[0047] Furthermore, the annular tape according to this embodiment possesses the aforementioned characteristics, thus improving electrical conductivity under high voltage and enhancing conductivity retention. Therefore, if the annular tape according to this embodiment is applied to transfer tapes (especially intermediate transfer tapes), it exhibits excellent fracture resistance and transfer retention.

[0048] The following is a detailed description of the annular belt involved in this embodiment.

[0049] (Area of ​​the Voronoi polygon)

[0050] In the annular band described in this embodiment, the average area of ​​the Voronoi polygons in the Voronoi mosaic with the centroid of the conductive particles as the parent point is 1400 nm. 2 Above and 2000nm 2 The following, for example, is preferably 1500nm 2 Above and 1900nm 2 The preferred option below is 1600nm. 2 Above and 1800nm 2 the following.

[0051] If the average area of ​​the Voronoi polygon is less than 1400 nm 2 This will lead to a decrease in fracture resistance and a deterioration in the dispersion of conductive particles along the thickness direction.

[0052] If the average area of ​​the Voronoi polygon exceeds 2000 nm 2 This leads to non-uniformity in conductivity due to the deterioration of the dispersion of conductive particles in the thickness direction.

[0053] Therefore, by setting the average area of ​​the Voronoi polygon within the aforementioned range, the dispersion of fracture-resistant and conductive particles along the thickness direction is improved.

[0054] The standard deviation of the area of ​​the Voronoi polygon is 1200 nm. 2 The following, for example, is preferably 1000nm 2 Below, 900nm is preferred. 2 the following.

[0055] If the standard deviation of the area of ​​the Voronoi polygon exceeds 1200 nm 2 This will lead to a decrease in fracture resistance and a deterioration in the dispersion of conductive particles along the thickness direction.

[0056] The average area and standard deviation of the area of ​​the Voronoi polygons are determined as follows.

[0057] A specimen is collected from the annular belt that is the object, with the cross-section cut along the belt thickness direction as the observation plane.

[0058] The cross-section of the sample was observed using scanning transmission electron microscopy (STEM), and STEM images were recorded at a magnification of 100,000x, showing the entire cross-section in the thickness direction. The recorded STEM images were analyzed using image analysis software (ImageJ: manufactured by the National Institutes of Health, USA) at a resolution of 0.010 μm / pixel.

[0059] Using the centroids of all conductive particles present in the STEM image as the parent points, perform Voronoi polygon tessellation (drawing perpendicular bisecting lines on the straight lines connecting adjacent parent points and tessell the closest regions of each parent point), and measure the area of ​​all the Voronoi polygons formed.

[0060] Here, regarding the center of gravity of a conductive particle, when the conductive particle exists in the form of a primary particle, it refers to the center of gravity of the primary particle of the conductive particle; when the conductive particle exists in the form of a secondary particle, it refers to the center of gravity of the secondary particle of the conductive particle.

[0061] Furthermore, the centroids of the primary and secondary conductive particles refer to the points where the number of pixels within the region of the primary and secondary particles is set to n, and the xy coordinates of each pixel are set to x. i y i When (i=1, 2, ..., n), the x-coordinate of the centroid = (x i (total of) / n, the y-coordinate of the centroid = (y i (total of) / n.

[0062] The steps for determining the area of ​​the Voronoi polygon using image processing software (ImageJ: manufactured by the National Institutes of Health) are as follows.

[0063] 1. Define the relationship between the number of pixels in the image and the actual distance using Analyze→Set Scale. For example, when 144 pixels are equivalent to 1.5μm, enter Distance in Pixels: 144, Known distance: 1.5, and check the checkboxes, Global.

[0064] 2. Select Image→Type→8-bit.

[0065] 3. Select Image → Adjust → Threshold, check Dark background, and click the Auto button.

[0066] 4. Remove speckled image noise using Process→Noise→Despeckle.

[0067] 5. By using Process→Binary→watershed, the conductive particles observed by overlapping are mosaicked through a process that highlights the outline of the conductive particles.

[0068] 6. Using Process→Binary→Voronoi, create a Voronoi polygon with the "center of gravity" of the conductive particles as the parent point.

[0069] 7. Eliminate line segments originating from the outermost conductive particles that do not form Voronoi polygons.

[0070] 8. Select Image→Type→8-bit.

[0071] 9. Adjust the image using Image→Adjust→Threshold to make the edges of the Voronoi polygon red.

[0072] 10. Use Edit→Invert to reverse the black and white colors, so that the edges of the Voronoi polygons become white.

[0073] 11. Calculate the area of ​​the Voronoi polygon by using Analyze→AnalyzeParticle(size: 0-Infinity, Circularity: 0.00-1.00, Show:Outlines).

[0074] Perform the above operation 5 times, and calculate the arithmetic mean of the area of ​​the obtained Voronoi polygons and the standard deviation of the area of ​​the Voronoi polygons.

[0075] (Average dispersion diameter of conductive particles)

[0076] The average dispersion diameter of the conductive particles is less than 30 nm, and more preferably less than 27 nm.

[0077] If the average dispersion diameter of conductive particles exceeds 30 nm, both the fracture resistance and the dispersion of conductive particles in the thickness direction decrease.

[0078] There is no particular limitation on the lower limit of the average dispersion diameter of the conductive particles, but the average dispersion diameter of the conductive particles is preferably 10 nm or more, and more preferably 13 nm or more.

[0079] The method for determining the average dispersion diameter of conductive particles is as follows.

[0080] A specimen is collected from the annular belt that is the object, with the cross-section cut along the belt thickness direction as the observation plane.

[0081] The cross-section of the sample was observed using scanning transmission electron microscopy (STEM), and STEM images were recorded at a magnification of 100,000x, showing the entire cross-section in the thickness direction. The recorded STEM images were analyzed using image analysis software (ImageJ: manufactured by the National Institutes of Health, USA) at a resolution of 0.010 μm / pixel.

[0082] In the STEM image, the circular equivalent diameter of the observed conductive particles is determined and set as the dispersion diameter of the conductive particles. Here, regarding the dispersion diameter of conductive particles, when the conductive particles exist in the form of primary particles, it represents the dispersion diameter of the primary particles of the conductive particles; when the conductive particles exist in the form of secondary particles, it represents the dispersion diameter of the secondary particles of the conductive particles.

[0083] Perform the above operation 5 times and calculate the arithmetic mean of the obtained dispersion diameters.

[0084] (The average value of the closest distance distribution of conductive particles)

[0085] The average value of the closest distance distribution of conductive particles is 20 nm or more and 40 nm or less, preferably 30 nm or more and 35 nm or less, and more preferably 30 nm or more and 33 nm or less.

[0086] Even if the average value of the closest distance distribution of conductive particles is less than 20 nm or more than 40 nm, the fracture resistance and the dispersion of conductive particles in the thickness direction are both reduced.

[0087] The method for determining the average value of the closest distance distribution of conductive particles is as follows.

[0088] A specimen is collected from the annular belt that is the object, with the cross-section cut along the belt thickness direction as the observation plane.

[0089] The cross-section of the sample was observed using scanning transmission electron microscopy (STEM), and STEM images were recorded at a magnification of 100,000x, showing the entire cross-section in the thickness direction. The recorded STEM images were analyzed using image analysis software (ImageJ: manufactured by the National Institutes of Health, USA) at a resolution of 0.010 μm / pixel.

[0090] Measure the distances between adjacent parent points, using the centroid of all conductive particles present in the STEM image as the parent point. The closest distance is called the nearest distance. This process is applied to all particles in the image, and the distribution of nearest distances is calculated. The arithmetic mean of the obtained nearest distance distributions is taken as the mean of the nearest distance distribution.

[0091] (composition)

[0092] The annular strip according to this embodiment contains resin and conductive particles. Specifically, for example, the annular strip is composed of a monolayer of a resin layer containing conductive particles. Furthermore, if necessary, the annular strip (the resin layer constituting it) may also contain silicone oil or other known components.

[0093] Here, in order to set the average area of ​​the Voronoi polygon, the standard deviation of the area of ​​the Voronoi polygon, the average dispersion diameter of the conductive particles, and the average value of the closest distance distribution of the conductive particles within the above-mentioned range, for example, as the resin, a polyimide resin (especially an imide of polyamic acid with all ends being amino) is suitable, and as the conductive particles, carbon black (especially carbon black with a surface functional group amount within a specific range when back-titrated using NaHCO3) is preferred.

[0094] -Resin-

[0095] Examples of resins include polyimide resin (PI resin), polyamide-imide resin (PAI resin), aromatic polyetherketone resin (e.g., aromatic polyetherketone resin), polyphenylene sulfide resin (PPS resin), polyetherimide resin (PEI resin), polyester resin, polyamide resin, polycarbonate resin, etc.

[0096] From the viewpoint of improving the bending resistance during rotary drive, the resin is preferably, for example, a polyimide resin (i.e., a resin containing structural units having imide bonds), more preferably a polyimide resin, a polyamide-imide resin, and even more preferably a polyimide resin.

[0097] As a polyimide resin, for example, an imide of polyamic acid (a precursor of polyimide resin) can be cited as a polymer of a tetracarboxylic dianhydride and a diamine compound.

[0098] As a polyimide resin, for example, a resin having a structural unit represented by the following general formula (I) can be cited.

[0099] [Chemical Formula 1]

[0100] In general formula (I), R 1 R represents a tetravalent organic group.2 It represents a divalent organic group.

[0101] As a result of R 1 Examples of tetravalent organic groups include aromatic groups, aliphatic groups, cyclic aliphatic groups, groups composed of aromatic and aliphatic groups, or groups in which these groups have been substituted. Specifically, examples of tetravalent organic groups include, for instance, residues of tetracarboxylic dianhydrides, which will be described later.

[0102] As a result of R 2 Examples of divalent organic groups include aromatic groups, aliphatic groups, cyclic aliphatic groups, groups composed of aromatic and aliphatic groups, or groups in which these groups have been substituted. Specifically, examples of divalent organic groups include, for instance, residues of diamine compounds described later.

[0103] Specifically, examples of tetracarboxylic dianhydrides used as raw materials for polyimide resins include pyromellitic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4-biphenyltetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxyphenyl)sulfonic dianhydride, perylene-3,4,9,10-tetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl) ether dianhydride, and ethylenetetracarboxylic dianhydride.

[0104] Specific examples of diamine compounds used as raw materials for polyimide resins include 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,3'-dichlorobenzidine, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 1,5-diaminonaphthalene, m-phenylenediamine, p-phenylenediamine, 3,3'-dimethyl-4,4'-benzidine, benzidine, and 3,3'-dimethylbenzidine. Aniline, 3,3'-dimethoxybenzidine, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenylpropane, 2,4-bis(aminotert-butyl)toluene, bis(p-β-amino-tert-butylphenyl) ether, bis(p-β-methyl-δ-aminophenyl)benzene, bis-p-(1,1-dimethyl-5-amino-pentyl)benzene, 1-isopropyl-2,4-m-phenylenediamine, m-phenylenediamine, p-phenylenediamine, di(p-aminocyclohexyl)methane, Hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, diaminopropyltetradiamine, 3-methylheptanediamine, 4,4-dimethylheptanediamine, 2,11-diaminododecane, 1,2-bis-3-aminopropoxyethane, 2,2-dimethylpropanediamine, 3-methoxyhexanediamine, 2,5-dimethylheptanediamine, 5-methylnonanediamine, 2,17-diaminoeicosane (2,17-diamino) eicosadecane), 1,4-diaminocyclohexane, 1,10-diamino-1,10-dimethyldecane, 12-diaminooctadecane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, piperazine, H2N(CH2)3O(CH2)2O(CH2)NH2, H2N(CH2)3S(CH2)3NH2, H2N(CH2)3N(CH3)2(CH2)3NH2, etc.

[0105] Examples of polyamide-imide resins include resins that have both imide and amide bonds in repeating units.

[0106] More specifically, polyamide-imide resins can be categorized as polymers of trivalent carboxylic acid compounds (also known as tricarboxylic acids) with anhydride groups and diisocyanate or diamine compounds.

[0107] Tricarboxylic acids, for example, are preferably trimellitic anhydride and its derivatives. In addition to tricarboxylic acids, tetracarboxylic dianhydrides, aliphatic dicarboxylic acids, aromatic dicarboxylic acids, etc., can be used in combination.

[0108] Examples of diisocyanate compounds include 3,3'-dimethylbiphenyl-4,4'-diisocyanate, 2,2'-dimethylbiphenyl-4,4'-diisocyanate, biphenyl-4,4'-diisocyanate, biphenyl-3,3'-diisocyanate, biphenyl-3,4'-diisocyanate, 3,3'-diethylbiphenyl-4,4'-diisocyanate, 2,2'-diethylbiphenyl-4,4'-diisocyanate, 3,3'-dimethoxybiphenyl-4,4'-diisocyanate, 2,2'-dimethoxybiphenyl-4,4'-diisocyanate, naphthalene-1,5-diisocyanate, and naphthalene-2,6-diisocyanate.

[0109] As diamine compounds, examples include compounds having the same structure as the aforementioned isocyanates, but with an amino group replacing the isocyanate group.

[0110] As a polyimide resin, an imide of polyamic acid with all its ends being amino groups is particularly preferred (i.e., an imide of polyamic acid with amino groups at both ends of the molecular chain). If an imide of polyamic acid with all its ends being amino groups is used, the dispersibility of conductive particles (especially carbon black with a surface functional group content of 0.3 mmol / g or more and 0.6 mmol / g or less when back-titrated with NaHCO3) can be easily improved. As a result, the average area of ​​the Voronoi polygon, the average dispersion diameter of the conductive particles, and the average value of the closest distance distribution of the conductive particles can be easily controlled within the aforementioned ranges.

[0111] Here, polyamic acid with all terminals being amino groups is a polyamic acid in which the ratio Y / X of the total molar amount of terminal carboxyl groups (Y) to the total molar amount of terminal amino groups (X) is 0 (i.e., Y=0).

[0112] Furthermore, the total molar amount (X) of the terminal amino groups is determined by titrating the polyamic acid composition using an acid (e.g., hydrochloric acid, etc.) after neutralization. On the other hand, the total molar amount (Y) of the terminal carboxyl groups is determined by titrating the polyamic acid composition using an alkali (e.g., sodium hydroxide, etc.) after neutralization.

[0113] In the reaction of tetracarboxylic dianhydrides with diamine compounds, polyamic acids with all terminals being amino groups can be synthesized by using more diamine compounds.

[0114] The resin content relative to the annular band (the resin layer constituting it) is preferably 60% by mass or more and 95% by mass or less, more preferably 70% by mass or more and 95% by mass or less, and even more preferably 75% by mass or more and 90% by mass or less.

[0115] -Conductive particles-

[0116] As conductive particles, examples include electrical conductivity (e.g., volume resistivity less than 10).7 Ω cm (hereinafter the same) or semiconducting (e.g., volume resistivity of 10 cm). 7 Ω cm or more and 10 13 Ω Powder (below cm, the same applies below)

[0117] Specifically, conductive particles include, for example, conductive carbon particles and metal oxide particles.

[0118] Carbon black is an example of a conductive carbon particle.

[0119] Examples of carbon black include Ketjen black, furnace black, channel black, and acetylene black. Surface-treated carbon black (hereinafter also referred to as "surface-treated carbon black") can also be used.

[0120] Surface-treated carbon black is obtained by imparting to its surface groups such as carboxyl groups, quinone groups, lactone groups, and hydroxyl groups. Examples of surface treatment methods include air oxidation, which involves reacting with air in a high-temperature atmosphere; reaction with nitrogen oxides or ozone at room temperature (e.g., 22°C); and oxidation with ozone at a low temperature after air oxidation in a high-temperature atmosphere.

[0121] Examples of metal oxide particles include tin oxide particles, titanium oxide particles, zinc oxide particles, and zirconium oxide particles.

[0122] Examples of conductive particles include metal particles (e.g., aluminum particles, nickel particles, etc.) and ionic conductive particles (e.g., potassium titanate particles, LiCl particles, etc.).

[0123] Among them, the conductive particles are preferably, for example, carbon black.

[0124] Furthermore, carbon black is preferably carbon black with a surface functional group content of 0.3 mmol / g or more and 0.6 mmol / g or less (e.g., preferably 0.4 mmol / g or more and 0.5 mmol / g or less) that can be back titrated with NaHCO3.

[0125] Here, carbon black with a surface functional group content within the above range, when back-titrated using NaHCO3, is equivalent to carbon black with a reduced carboxyl group content.

[0126] If carbon black (especially carbon black with a surface functional group content of 0.3 mmol / g or more and 0.6 mmol / g or less when back titrated with NaHCO3) is used, the dispersibility of carbon black relative to polyimide resins (especially imides of polyamic acids with all ends being amino groups) is improved. As a result, it is easy to control the average area of ​​the Voronoi polygon, the standard deviation of the Voronoi polygon area, the average dispersion diameter of conductive particles, and the average value of the closest distance distribution of conductive particles within the aforementioned ranges.

[0127] Methods for controlling the amount of surface functional groups in carbon black within the above-mentioned range by back titration with NaHCO3 include liquid-phase oxidation treatment using nitric acid (HNO3), sulfuric acid (H2SO4), etc., and using nitric oxide (NO3) x Methods such as gas-phase oxidation treatment with ozone (O3), oxygen plasma treatment, and heating oxidation treatment.

[0128] The method for determining the amount of surface functional groups in carbon black by back titration using NaHCO3 is as follows.

[0129] First, after drying the carbon black at 100°C and removing the moisture, 100 mg of the sample was weighed to obtain the sample.

[0130] Add 3 mL of 0.1 mol / L NaHCO3 aqueous solution and 40 mL of pure water to the obtained sample, perform ultrasonic dispersion for 5 minutes, stir for 1 hour, filter with a 0.45 μm diameter injection filter, and use 20 mL of the supernatant to prepare the titration adjustment solution.

[0131] The conditioning solution was titrated with a 0.1 mol / L hydrochloric acid aqueous solution, and the titration amount was determined from the inflection point. The amount of surface functional groups of carbon black was compared with the amount of alkaline reagent consumed to a blank solution without carbon black (total volume 43 mL), and calculated using the following formula.

[0132] Calculation formula: Amount of surface acidic groups in 1g x = {(0.1×α) - (0.1×β×43÷20)}×1000÷d

[0133] α: Equivalent volume of blank solution added (L). β: Equivalent volume of sample solution added (L). d: Weight of carbon black (mg) The primary average particle size of the conductive particles is preferably 2 nm or more and 40 nm or less, more preferably 8 nm or more and 20 nm or less, and even more preferably 10 nm or more and 15 nm or less.

[0134] Regarding the primary average particle size of conductive particles, in the method for determining the average dispersion diameter of conductive particles, only the circular equivalent diameter of the primary particles of conductive particles is measured, and it is set as the arithmetic mean of the obtained primary particles.

[0135] The content of conductive particles (especially carbon black) relative to 100 parts by mass of resin is preferably 16 parts by mass or more and 26 parts by mass or less, more preferably 18 parts by mass or more and 24 parts by mass or less, and even more preferably 20 parts by mass or more and 23 parts by mass or less.

[0136] If the content of conductive particles (especially carbon black) is 16 parts by mass or more, it is easy to control the average area of ​​the Voronoi polygon, the standard deviation of the area, the average dispersion diameter of the conductive particles, and the average value of the closest distance distribution of the conductive particles within the above range.

[0137] If the content of conductive particles (especially carbon black) is less than 26 parts by mass, it is easy to suppress the reduction of fracture resistance.

[0138] -Silicone oil-

[0139] Silicone oil has the function of improving the cleanliness of the annular belt.

[0140] Examples of silicone oils include linear silicone oils such as dimethyl silicone oil, methylhydrosilicone oil, diphenyl silicone oil, methylphenyl silicone oil, and chlorophenyl silicone oil; and modified silicone oils such as alkyl-modified silicone oil, aralkyl-modified silicone oil, polyether-modified silicone oil, polyester-modified silicone oil, fluoroalkyl-modified silicone oil, amino-modified silicone oil, alkoxy-modified silicone oil, epoxy-modified silicone oil, and carboxyl-modified silicone oil.

[0141] From the viewpoint of improving cleanliness, the silicone oil is preferably at least one selected from the group consisting of dimethyl silicone oil and modified silicone oil.

[0142] The modified silicone oil is a dimethyl silicone oil formed by replacing part of the methyl group of dimethyl silicone oil with an organic functional group. Examples of the modified silicone oils mentioned above are provided. Among these, aralkyl-modified silicone oil and polyether-modified silicone oil are preferred, and aralkyl-modified silicone oil is more preferred.

[0143] -Other ingredients-

[0144] Other components include, for example, fillers for improving mechanical strength, antioxidants for preventing thermal degradation of the belt, surfactants for improving flowability, and heat-resistant anti-aging agents.

[0145] When other components are present, the content of the other components relative to the annular band (the resin layer constituting it) is preferably more than 0% by mass and less than 10% by mass, more preferably more than 0% by mass and less than 5% by mass, and even more preferably more than 0% by mass and less than 1% by mass.

[0146] (Thickness of the annular belt)

[0147] The thickness of the annular strip (resin layer constituting it) involved in this embodiment is preferably 60 μm or more and 120 μm or less, and more preferably 60 μm or more and 110 μm or less.

[0148] In addition, the thickness of the annular belt was measured as follows.

[0149] That is, the thickness of the annular band is observed in the cross section along the thickness direction using an optical microscope or a scanning electron microscope, and the thickness of the annular band of the test object is measured at 10 locations, with the average value set as the thickness.

[0150] (Young's modulus)

[0151] From the viewpoint of improving fracture resistance, the Young's modulus of the annular belt involved in this embodiment is preferably 2900 MPa or more and 5500 or less, and more preferably 3000 MPa or more and 3600 or less.

[0152] The Young's modulus of the annular band can be adjusted, for example, by the type of resin and the weight-average molecular weight of the resin.

[0153] The method for determining the Young's modulus of annular belts is as follows.

[0154] Using a tensile testing machine (MODEL-1605N, manufactured by Aikoh Engineering Co., Ltd.), the annular belt was cut into 80mm × 5mm pieces with the circumference of the belt as the long side. The length of the test piece between the chuck clamps was then set to 40mm, and the test was conducted at a tensile speed of 20mm / min. The Young's modulus was calculated from the slope of the region where the SS curve became a straight line (Strain range: 10N-38N).

[0155] (Manufacturing method of annular belt)

[0156] The manufacturing method of the annular belt involved in this embodiment includes, for example, the following steps: coating a resin solution containing resin or its precursor and conductive particles onto the surface of a mold to form a coating film. The coating is heated and dried, and the precursor is reacted as needed (e.g., imidization in the case of a polyimide resin precursor) to form a resin film; and Remove the resin film from the mold.

[0157] Then, the resin film is removed from the mold and set as a ring.

[0158] The mold is not particularly limited, but a cylindrical mold is preferred. The substrate can be a metal substrate. Furthermore, molds made of other materials such as resin, glass, or ceramic can be used instead of metal molds. Additionally, a glass coating, ceramic coating, or silicone or fluorine-based release agent can be applied to the surface of the mold.

[0159] Furthermore, common methods for coating resin solutions include, for example, blade coating, wire rod coating, spraying, dip coating, bead coating, air knife coating, and curtain coating.

[0160] In the manufacturing method of the annular strip according to this embodiment, the following operations are preferably performed, for example. Through these operations, the average area of ​​the Voronoi polygon, the standard deviation of the area of ​​the Voronoi polygon, the average dispersion diameter of the conductive particles, and the average value of the closest distance distribution of the conductive particles can be easily controlled within the above-mentioned ranges.

[0161] The operation of dispersing conductive particles (especially carbon black) in a resin solution under ultra-high pressure The process of adding dispersants for resin solutions and conductive particles (especially carbon black). The conductive particles (especially carbon black) are pre-micronized using a media disperser. (Uses of ring belts) The annular belt described in this embodiment can be used, for example, as an annular belt for an image forming apparatus in an electrophotographic manner. Examples of annular belts for an image forming apparatus in an electrophotographic manner include intermediate transfer belts, transfer belts (i.e., recording media conveyor belts), fixing belts (heating belts, pressure belts, etc.), and conveyor belts (i.e., recording media conveyor belts).

[0162] In addition to the annular belt for image forming apparatus, the annular belt involved in this embodiment can also be used for conveyor belts, drive belts, laminated belts, electrical insulating materials, piping covering materials, electromagnetic wave insulating materials, heat source insulators, electromagnetic wave absorbing films, and other strip-shaped components.

[0163] The annular strip described in this embodiment may have functional layers provided on its outer peripheral surface and inner peripheral surface, depending on the application. However, the annular strip described in this embodiment may, for example, be used as a resin substrate.

[0164] [Transfer Device]

[0165] The transfer apparatus according to this embodiment includes: an intermediate transfer belt for transferring a toner image on its outer peripheral surface; a primary transfer apparatus having a primary transfer member for transferring a toner image formed on the surface of an image holder to the outer peripheral surface of the intermediate transfer belt in one step; and a secondary transfer apparatus having a secondary transfer member that is disposed in contact with the outer peripheral surface of the intermediate transfer belt and for transferring the toner image transferred to the outer peripheral surface of the intermediate transfer belt to the surface of a recording medium in a secondary step.

[0166] Furthermore, an intermediate transfer belt having the annular belt described in this embodiment is suitable as the intermediate transfer belt.

[0167] The transfer apparatus described in this embodiment may include a cleaning device or other known apparatus such as a cleaning device having a cleaning component for cleaning the outer peripheral surface of the intermediate transfer belt.

[0168] (Intermediate transfer belt)

[0169] The intermediate transfer belt has the annular belt described in this embodiment.

[0170] The intermediate transfer belt can be a single layer of annular belt or a laminate in which the annular belt is a resin substrate layer. As a laminate, for example, it can be a laminate having a resin substrate layer, an elastic layer disposed on the resin substrate layer, and an anti-stick layer disposed on the elastic layer, or a laminate having a resin substrate layer and an anti-stick layer disposed on the resin substrate layer.

[0171] The elastic layer will be explained.

[0172] The elastic layer is composed of heat-resistant elastic material.

[0173] Examples of heat-resistant elastic materials include silicone rubber and fluororubber.

[0174] Examples of silicone rubbers include RTV (Room Temperature Vulcanizing) silicone rubber, HTV (High Temperature Vulcanizing) silicone rubber, and liquid silicone rubber. More specifically, examples include polydimethyl silicone rubber, methyl vinyl silicone rubber, methyl phenyl silicone rubber, and fluorosilicone rubber.

[0175] Examples of fluororubbers include vinylidene fluoride rubbers, tetrafluoroethylene / propylene rubbers, tetrafluoroethylene / perfluoromethyl vinyl ether rubbers, phosphazene rubbers, and fluoropolyethers.

[0176] The elastic layer may contain other components. Examples of other components include fillers, conductive agents, softeners (such as paraffin waxes), processing aids (such as stearic acid), anti-aging agents (such as amines), vulcanizing agents (such as sulfur, metal oxides, and peroxides), and functional fillers (such as alumina).

[0177] The anti-stick layer is explained.

[0178] The non-stick layer may contain heat-resistant non-stick materials, for example.

[0179] Examples of heat-resistant, non-stick materials include fluororubber, fluororesin, silicone resin, and polyimide resin.

[0180] Among these, fluoropolymers are preferred as heat-resistant, non-stick materials. Specifically, examples of fluoropolymers include tetrafluoroethylene / perfluoroalkyl vinyl ether copolymer (PFA), polytetrafluoroethylene (PTFE), tetrafluoroethylene / hexafluoropropylene copolymer (FEP), polyethylene / tetrafluoroethylene copolymer (ETFE), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), and vinyl fluoride (PVF).

[0181] In addition, the intermediate transfer belt adopts a known structure other than the annular belt described in this embodiment.

[0182] -Volume resistivity of the intermediate transfer belt-

[0183] A commonly used logarithmic value for the volume resistivity of the intermediate transfer belt when a voltage of 100V is applied for 10 seconds is, for example, 8.0 (logΩ). cm or more and 13.5 (logΩ) (cm) or less, more preferably 8.5 (logΩ) cm or more and 13.2 (logΩ) (cm) or less.

[0184] The volume resistivity of the intermediate transfer belt when a voltage of 500V was applied for 10 seconds was measured by the following method.

[0185] A microammeter (R8430A manufactured by ADVANTEST CORPORATION) was used as the resistance measuring instrument, and a UR probe (manufactured by Nittoseiko Analytech Co., Ltd.) was used as the probe. Regarding volume resistivity (logΩ)... The intermediate transfer belt was measured at 18 points (cm) under the conditions of 100V voltage, 10-second application time, and 1kgf pressure. Measurements were taken at 6 points at equal intervals along the circumference and 3 points at the center and both ends along the width. The average value was calculated. The measurements were conducted at 22℃ and 55%RH.

[0186] (Surface resistivity of the intermediate transfer belt)

[0187] The commonly used logarithmic value of the surface resistivity of the intermediate transfer belt when a 100V voltage is applied to its outer peripheral surface for 10 seconds is preferably 9.5 (logΩ / suq.) or more and 15.0 (logΩ / suq.) or less, more preferably 10.5 (logΩ / suq.) or more and 14.0 (logΩ / suq.) or less, and especially preferably 11.0 (logΩ / suq.) or more and 13.5 (logΩ / suq.) or less.

[0188] In addition, the unit of surface resistivity, logΩ / suq., is expressed as the logarithm of the resistance value per unit area. It is also expressed as log(Ω / suq.), logΩ / square, logΩ / □, etc.

[0189] The surface resistivity of the outer peripheral surface of the intermediate transfer belt when a voltage of 100V was applied for 10 seconds was measured by the following method.

[0190] As the resistance measuring instrument, a microammeter (R8430A manufactured by ADVANTEST CORPORATION) was used, and a UR probe (manufactured by Nittoseiko Analytech Co., Ltd.) was used as the probe. The surface resistivity (logΩ / suq.) of the outer circumference of the annular strip was measured at 18 points: 6 points at equal intervals along the circumference, and 3 points at the center and two ends along the measurement width. The average value was calculated. The measurements were performed at 22°C and 55%RH.

[0191] (One-time transfer device)

[0192] In a primary transfer apparatus, a primary transfer component is positioned opposite to an image holder across an intermediate transfer belt. In this apparatus, the toner image is transferred onto the outer periphery of the intermediate transfer belt in a single transfer by applying a voltage of opposite polarity to the toner's charge polarity to the intermediate transfer belt using the primary transfer component.

[0193] (Secondary transfer device)

[0194] In a secondary transfer apparatus, a secondary transfer component is disposed on the toner image holding side of an intermediate transfer belt. Furthermore, the secondary transfer apparatus, for example, includes both the secondary transfer component and a back panel disposed on the side of the intermediate transfer belt opposite to the toner image holding side. In this apparatus, a transfer electric field is formed by clamping the intermediate transfer belt and the recording medium using the secondary transfer component and the back panel, thereby transferring the toner image on the intermediate transfer belt onto the recording medium a second time.

[0195] The secondary transfer component can be a secondary transfer roller or a secondary transfer belt. Additionally, a back-side component, for example, can be a back-side roller.

[0196] (Cleaning device)

[0197] In the cleaning apparatus, a cleaning component is disposed on the toner image holding side of the intermediate transfer belt. Furthermore, the cleaning apparatus, for example, includes both the cleaning component and a back panel component disposed on the side of the intermediate transfer belt opposite to the toner image holding side. In the cleaning apparatus, for example, while the intermediate transfer belt is held by the cleaning component and the back panel component, the outer peripheral surface of the intermediate transfer belt is cleaned by the cleaning component.

[0198] In addition, cleaning components include cleaning scrapers and cleaning brushes.

[0199] Furthermore, the transfer apparatus according to this embodiment can be a transfer apparatus that transfers a toner image onto the surface of a recording medium via a plurality of intermediate transfer bodies. That is, the transfer apparatus may be, for example, a transfer apparatus that transfers the toner image from an image holder to a first intermediate transfer body in one step, and then transfers the toner image from the first intermediate transfer body to a second intermediate transfer body in two steps, and then transfers the toner image from the second intermediate transfer body to the recording medium in three steps.

[0200] The transfer apparatus applies an intermediate transfer belt having the annular belt described in this embodiment to at least one of a plurality of intermediate transfer bodies.

[0201] [Image forming apparatus]

[0202] The image forming apparatus according to this embodiment includes: a toner image forming apparatus for forming a toner image on the surface of an image holder; and a transfer apparatus for transferring the toner image formed on the surface of the image holder to the surface of a recording medium. Furthermore, the transfer apparatus described in this embodiment is applicable.

[0203] Examples of toner image forming apparatuses include: an image holder, a charging device for charging the surface of the image holder, an electrostatic latent image forming apparatus for forming an electrostatic latent image on the surface of the charged image holder, and a developing apparatus for forming a toner image by developing the electrostatic latent image formed on the surface of the image holder with a developer containing a toner.

[0204] The image forming apparatus according to this embodiment is applicable to known image forming apparatuses such as a fixing apparatus for fixing a toner image transferred to the surface of a recording medium; a cleaning apparatus for cleaning the surface of an image holder before it is charged after the toner image is transferred; an antistatic apparatus for irradiating the surface of an image holder with antistatic light to eliminate static electricity after the toner image is transferred and before it is charged; and an image holder heating member for raising the temperature of the image holder to lower the relative temperature.

[0205] The image forming apparatus described in this embodiment can be either a dry developing image forming apparatus or a wet developing image forming apparatus (a developing method that utilizes liquid developer).

[0206] Furthermore, in the image forming apparatus according to this embodiment, the portion having the image holder can be a box structure (processing box) that is detachable from the image forming apparatus. As a processing box, for example, a processing box having a toner image forming apparatus and a transfer apparatus is preferably used.

[0207] Hereinafter, an example of the image forming apparatus according to this embodiment will be described with reference to the accompanying drawings. However, the image forming apparatus according to this embodiment is not limited to this. In addition, the main parts shown in the figures will be described, and the description of other parts will be omitted.

[0208] (Image forming apparatus)

[0209] Figure 1 This is a schematic structural diagram showing the structure of the image forming apparatus according to this embodiment.

[0210] like Figure 1 As shown, the image forming apparatus 100 according to this embodiment is, for example, a series-type intermediate transfer image forming apparatus, which includes: a plurality of image forming units 1Y, 1M, 1C, 1K (an example of a tonal image forming apparatus) that form tonal images of each color component by electrophotography; a primary transfer unit 10 that sequentially transfers (primarily transfers) the tonal images of each color component formed by each image forming unit 1Y, 1M, 1C, 1K onto an intermediate transfer belt 15; a secondary transfer unit 20 that transfers (secondarily transfers) the overlapping tonal images transferred to the intermediate transfer belt 15 onto a paper K, which is a recording medium; and a fixing device 60 that fixes the secondary transferred image onto the paper K. Furthermore, the image forming apparatus 100 has a control unit 40 that controls the operation of each device (each unit).

[0211] Each image forming unit 1Y, 1M, 1C, 1K of the image forming apparatus 100 has a photoreceptor 11 (an example of an image holder) that holds a tonal image formed on a surface and rotates in the direction of arrow A.

[0212] Around the photoreceptor 11, as an example of a charged component, an electric charge 12 is provided to charge the photoreceptor 11. As an example of an electrostatic latent image forming apparatus, a laser exposure unit 13 is provided to write an electrostatic latent image onto the photoreceptor 11 (the exposure beam is represented by the symbol Bm in the figure).

[0213] Furthermore, around the photoreceptor 11, as an example of a developing member, a developing unit 14 is provided that contains toners of various color components and visualizes the electrostatic latent image on the photoreceptor 11 through the toners, and a primary transfer roller 16 is provided that transfers the toner images of various color components formed on the photoreceptor 11 to the intermediate transfer belt 15 through the primary transfer section 10.

[0214] Furthermore, a photoreceptor cleaner 17 is provided around the photoreceptor 11 to remove residual toner from the photoreceptor 11, and an electrophotographic device consisting of a belt conveyor 12, a laser exposer 13, a developer 14, a primary transfer roller 16, and the photoreceptor cleaner 17 is arranged sequentially along the rotation direction of the photoreceptor 11. These image forming units 1Y, 1M, 1C, and 1K are arranged in a generally linear order from the upstream side of the intermediate transfer belt 15 in the sequence of yellow (Y), magenta (M), cyan (C), and black (K).

[0215] Intermediate transfer belt 15 passes through various rollers along Figure 1 Arrow B indicates that the roller is driven (rotated) in a cyclical manner at a speed that meets the intended purpose. The rollers include a drive roller 31 that rotates the intermediate transfer belt 15 by a motor (not shown) with excellent constant speed; a support roller 32 that supports the intermediate transfer belt 15, which extends in a substantially linear shape along the arrangement direction of each photoreceptor 11; a tension application roller 33 that functions as a correction roller to apply tension to the intermediate transfer belt 15 and prevent it from serpentinizing; a back roller 25 provided on the secondary transfer section 20; and a cleaning back roller 34 provided on the cleaning section for scraping off residual toner from the intermediate transfer belt 15.

[0216] The primary transfer section 10 is composed of a primary transfer roller 16 disposed opposite to the photoreceptor 11 via an intermediate transfer belt 15. The primary transfer roller 16 is pressed against the photoreceptor 11 via the intermediate transfer belt 15, and a voltage (primary transfer bias) of opposite polarity to the polarity of the toner (designated as negative polarity, hereinafter the same) is applied to the primary transfer roller 16. As a result, the toner images on each photoreceptor 11 are sequentially electrostatically adsorbed onto the intermediate transfer belt 15, forming overlapping toner images on the intermediate transfer belt 15.

[0217] The secondary transfer section 20 is configured to have a back roller 25 and a secondary transfer roller 22 disposed on the toner image holding side of the intermediate transfer belt 15.

[0218] The back roller 25 is formed with a surface resistivity of 1×10⁻⁶. 7 Ω / □ or higher and 1×10 10 For Ω / □ and below, the hardness is set to, for example, 70° (Asker C: manufactured by KOBUNSHI KEIKI CO.,LTD., the same below). The back roller 25 is disposed on the back side of the intermediate transfer belt 15 to form the opposing electrode of the secondary transfer roller 22, and is in contact with a metal power supply roller 26 that stably applies the secondary transfer bias voltage.

[0219] On the other hand, the secondary transfer roller 22 has a volume resistivity of 10. 7.5 Ω cm or more and 10 8.5 Ω A cylindrical roller less than cm in diameter. Furthermore, the secondary transfer roller 22 is press-fitted to the back roller 25 across the intermediate transfer belt 15, and the secondary transfer roller 22 is grounded to form a secondary transfer bias between itself and the back roller 25, so that the toner image is transferred to the paper K conveyed to the secondary transfer section 20.

[0220] Furthermore, on the downstream side of the secondary transfer section 20 of the intermediate transfer belt 15, an intermediate transfer belt cleaning component 35 is provided to remove residual toner or paper dust from the intermediate transfer belt 15 after the secondary transfer and to clean the outer peripheral surface of the intermediate transfer belt 15, which can be freely contacted and separated.

[0221] Furthermore, on the downstream side of the secondary transfer section 20 of the secondary transfer roller 22, a secondary transfer roller cleaning component 22A is provided to remove residual toner or paper dust from the secondary transfer roller 22 after the secondary transfer and to clean the outer peripheral surface of the intermediate transfer belt 15. The secondary transfer roller cleaning component 22A may be a cleaning scraper, but it may also be a cleaning roller.

[0222] In addition, the intermediate transfer belt 15, the primary transfer roller 16, the secondary transfer roller 22, and the intermediate transfer belt cleaning component 35 correspond to an example of the transfer device.

[0223] Here, the image forming apparatus 100 may also be configured to have a secondary transfer belt (an example of a secondary transfer component) instead of the secondary transfer roller 22. Specifically, as Figure 2 As shown, the image forming apparatus 100 includes a secondary transfer device, which includes a secondary transfer belt 23, a drive roller 23A disposed opposite to the back roller 25 via an intermediate transfer belt 15 and the secondary transfer belt 23, and an idler roller 23B that supports the secondary transfer belt 23 together with the drive roller 23A.

[0224] On the other hand, a reference sensor (position sensor) 42 is provided upstream of the yellow image forming unit 1Y. This reference sensor generates a reference signal that serves as a reference for obtaining the image forming time of each of the image forming units 1Y, 1M, 1C, and 1K. Furthermore, an image density sensor 43 for image quality adjustment is provided downstream of the black image forming unit 1K. The reference sensor 42 is configured to identify a mark provided on the back side of the intermediate transfer belt 15 and generate a reference signal. Based on the indication from the control unit 40 based on the identification of this reference signal, each of the image forming units 1Y, 1M, 1C, and 1K begins to form an image.

[0225] Furthermore, in the image forming apparatus according to this embodiment, the conveying member for conveying the paper K includes a paper receiving section 50 for receiving the paper K, a paper feed roller 51 for taking out and conveying the paper K stacked in the paper receiving section 50 at a predetermined time, a conveying roller 52 for conveying the paper K delivered by the paper feed roller 51, a conveying guide 53 for sending the paper K conveyed by the conveying roller 52 into the secondary transfer section 20, a conveyor belt 55 for conveying the paper K after secondary transfer by the secondary transfer roller 22 to the fixing device 60, and a fixing inlet guide 56 for guiding the paper K to the fixing device 60.

[0226] Next, the basic image generation process of the image forming apparatus according to this embodiment will be described.

[0227] In the image forming apparatus of this embodiment, image data output from an image reading device (not shown) or a personal computer (PC) (not shown) is processed by an image processing device (not shown) and then an image generation operation is performed by image forming units 1Y, 1M, 1C, and 1K.

[0228] In the image processing device, various image processing techniques are applied to the input image data, including shadow correction, position offset correction, brightness / color space conversion, gamma correction, border removal, color editing, and motion editing. The processed image data is then converted into grayscale data of four colors: Y, M, C, and K, and output to the laser exposure unit 13.

[0229] In the laser exposure unit 13, based on the input pigment grayscale data, for example, an exposure beam Bm emitted from a semiconductor laser is applied to the photoreceptors 11 of each of the image forming units 1Y, 1M, 1C, and 1K. In each photoreceptor 11 of the image forming units 1Y, 1M, 1C, and 1K, after the surface is charged by the charger 12, the surface is scanned and exposed by the laser exposure unit 13 to form an electrostatic latent image. The formed electrostatic latent image is developed by each of the image forming units 1Y, 1M, 1C, and 1K into tonal images of Y, M, C, and K respectively.

[0230] The toner image formed on the photoreceptors 11 of the image forming units 1Y, 1M, 1C, and 1K is transferred to the intermediate transfer belt 15 in the primary transfer section 10 where each photoreceptor 11 contacts the intermediate transfer belt 15. More specifically, in the primary transfer section 10, the primary transfer roller 16 applies a voltage (primary transfer bias voltage) of opposite polarity to the polarity (negative polarity) of the toner to the substrate of the intermediate transfer belt 15, thereby sequentially overlapping the toner image on the outer peripheral surface of the intermediate transfer belt 15 to perform a primary transfer.

[0231] After the toner image is sequentially transferred onto the outer periphery of the intermediate transfer belt 15, the intermediate transfer belt 15 moves, and the toner image is conveyed to the secondary transfer section 20. When the toner image is conveyed to the secondary transfer section 20, the paper feed roller 51 in the conveying member rotates in sync with the arrival of the toner image at the secondary transfer section 20, supplying paper K of the target size from the paper receiving section 50. The paper K supplied by the paper feed roller 51 is conveyed by the conveyor roller 52 and passes through the conveyor guide 53 to reach the secondary transfer section 20. Before reaching the secondary transfer section 20, the paper K temporarily stops, and the alignment roller (not shown) rotates in sync with the movement of the intermediate transfer belt 15 holding the toner image, thereby aligning the position of the paper K with the position of the toner image.

[0232] In the secondary transfer section 20, the secondary transfer roller 22 is pressed onto the back roller 25 via the intermediate transfer belt 15. At this time, the paper K, which is being conveyed on time, is held between the intermediate transfer belt 15 and the secondary transfer roller 22. At this time, if a voltage (secondary transfer bias voltage) of the same polarity as the polarity (negative polarity) of the toner is applied from the power supply roller 26, a transfer electric field is formed between the secondary transfer roller 22 and the back roller 25. Furthermore, the unfixed toner image held on the intermediate transfer belt 15 is electrostatically transferred onto the paper K in the secondary transfer section 20, which is pressed by the secondary transfer roller 22 and the back roller 25.

[0233] Then, the paper K with the electrostatically transferred toner image is conveyed intact from the intermediate transfer belt 15 by the secondary transfer roller 22 and conveyed to the conveyor belt 55 located downstream of the secondary transfer roller 22 in the paper conveying direction. On the conveyor belt 55, the paper K is conveyed to the fixing device 60 at the optimal conveying speed corresponding to the fixing device 60. The unfixed toner image on the paper K conveyed to the fixing device 60 is fixed onto the paper K by the fixing device 60 through a fixing process using heat and pressure. Furthermore, the paper K with the fixed image is conveyed to the paper discharge receiving section (not shown) provided in the discharge section of the image forming apparatus.

[0234] On the other hand, after the transfer of paper K is completed, the residual toner remaining on the intermediate transfer belt 15 is transferred to the cleaning section as the intermediate transfer belt 15 rotates, and is removed from the intermediate transfer belt 15 by the cleaning back roller 34 and the intermediate transfer belt cleaning component 35.

[0235] The above describes the implementation method, but it is not intended to be limited to the above implementation method. Various modifications, alterations, and improvements are possible.

[0236] Example

[0237] The following describes embodiments of the present invention, but the present invention is not limited to these embodiments. Furthermore, in the following description, unless otherwise stated, "parts" and "%" refer to mass.

[0238] <Synthesis of Polyamic Acid>

[0239] (Preparation of polyamic acid solution DA-A1)

[0240] As a polyamic acid with all its ends being amino groups (i.e., a polyamic acid with amino groups at both ends of its molecular chain), polyamic acid DA-A1 and a polyamic acid solution DA-A1 containing it are synthesized by the following method.

[0241] 83.48 g (416.9 mmol) of 4,4'-diaminodiphenyl ether (hereinafter referred to as "ODA"), a diamine compound, was added to 800 g of N-methyl-2-pyrrolidone (hereinafter referred to as "NMP") and dissolved while stirring at room temperature (25°C).

[0242] Next, 116.52 g (396.0 mmol) of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride (hereinafter referred to as "BPDA") was slowly added as a tetracarboxylic acid dianhydride. After the tetracarboxylic acid dianhydride was added and dissolved, the temperature of the reaction solution was heated to 60°C, and then the polymerization reaction was carried out for 20 hours while maintaining the temperature of the reaction solution to obtain a reaction solution containing polyamic acid DA-A1 and NMP.

[0243] The reaction solution was filtered through a #800 stainless steel mesh and cooled to room temperature (25°C) to obtain a polyamic acid solution DA-A1.

[0244] (Preparation of polyamic acid solution DC-A1)

[0245] As a polyamic acid with carboxyl groups at all ends (i.e., a polyamic acid with carboxyl groups at both ends of the molecular chain), polyamic acid DC-A1 and a polyamic acid solution DC-A1 containing it were synthesized by the following method.

[0246] The ODA was set to 79.57 g (397.4 mmol), and the BPDA was set to 120.43 g (409.3 mmol). Otherwise, the reaction solution containing polyamic acid DC-A1 and NMP was obtained in the same manner as polyamic acid DA-A1.

[0247] The reaction solution was then filtered through a #800 stainless steel mesh and cooled to room temperature (25°C) to obtain a polyamic acid solution DC-A1.

[0248] <Preparation of Conductive Particles>

[0249] (COLOUR BLACK FW1)

[0250] Prepare “COLOUR BLACK FW1” manufactured by Orion Engineered Carbons SA (average particle size = 13 nm, surface functional group content = 0.20 mmol / g when back titrated with NaHCO3).

[0251] (Acid-treated product 1 of COLOUR BLACK FW1)

[0252] Orion Engineered Carbons SA’s “COLOUR BLACK FW1” was subjected to nitric acid-based liquid-phase treatment to obtain acid-treated product 1 of COLOUR BLACK FW1 (average particle size in one step = 13 nm, surface functional group content determined by back titration with NaHCO3 = 0.60 mmol / g).

[0253] However, the amount of surface functional groups can be adjusted by changing the concentration of nitric acid during acid treatment.

[0254] (Acid-treated product 2 of COLOUR BLACK FW1)

[0255] Orion Engineered Carbons SA’s “COLOUR BLACK FW1” was subjected to nitric acid-based liquid-phase treatment to obtain acid-treated product 2 of COLOUR BLACK FW1 (average particle size in one step = 13 nm, surface functional group content determined by back titration with NaHCO3 = 0.40 mmol / g).

[0256] However, the amount of surface functional groups can be adjusted by changing the concentration of nitric acid during acid treatment.

[0257] (COLOUR BLACK FW1 acid-treated product 3)

[0258] Orion Engineered Carbons SA’s “COLOUR BLACK FW1” was subjected to nitric acid-based liquid-phase treatment to obtain acid-treated product 3 of COLOUR BLACK FW1 (average particle size in one step = 13 nm, surface functional group content determined by back titration using NaHCO3 = 0.65 mmol / g).

[0259] However, the amount of surface functional groups can be adjusted by changing the concentration of nitric acid during acid treatment.

[0260] (COLOUR BLACK FW1 acid-treated product 4)

[0261] Orion Engineered Carbons SA’s “COLOUR BLACK FW1” was subjected to nitric acid-based liquid-phase treatment to obtain acid-treated product 4 of COLOUR BLACK FW1 (average particle size in one step = 13 nm, surface functional group content determined by back titration with NaHCO3 = 0.32 mmol / g).

[0262] However, the amount of surface functional groups can be adjusted by changing the concentration of nitric acid during acid treatment.

[0263] (COLOUR BLACK FW1 acid-treated product 5)

[0264] Orion Engineered Carbons SA’s “COLOUR BLACK FW1” was subjected to nitric acid-based liquid-phase treatment to obtain acid-treated product 5 of COLOUR BLACK FW1 (average particle size in one step = 13 nm, surface functional group content determined by back titration with NaHCO3 = 0.28 mmol / g).

[0265] However, the amount of surface functional groups can be adjusted by changing the concentration of nitric acid during acid treatment.

[0266] (COLOUR BLACK FW2)

[0267] Prepare “COLOUR BLACK FW2” (average particle size = 13 nm, surface functional group content = 0.45 mmol / g by back titration using NaHCO3) manufactured by Orion Engineered Carbons SA.

[0268] (COLOUR BLACK FW200)

[0269] Prepare Orion Engineered Carbons SA's "COLOUR BLACK FW200 (single average particle size = 13 nm, surface functional group content determined by back titration using NaHCO3 = 0.90 mmol / g)".

[0270] (COLOUR BLACK FW310)

[0271] Prepare “COLOUR BLACK FW310” manufactured by Orion Engineered Carbons SA (average particle size = 9 nm, surface functional group content = 0.30 mmol / g when back titrated with NaHCO3).

[0272] <Example 1>

[0273] -Manufacturing of coating liquid-

[0274] A dispersion was obtained by adding COLOURBLACK FW2 as conductive particles and aralkyl-modified silicone oil (Shin-Etsu Chemical Co., Ltd., KF-410) as silicone oil to a polyamic acid solution DA-A1 (solid content 18% by mass).

[0275] Here, the amount of conductive particles and the amount of silicone oil are set as shown in Table 1 (parts by mass relative to 100 parts by mass of polyimide resin after imidization of polyamic acid).

[0276] Next, the dispersion was passed through a 0.1 mm diameter orifice at a pressure of 220 MPa using a high-pressure impact disperser (JOKOH Co., Ltd.), and dispersed by 10 collisions of the slurry divided into two parts, thus obtaining the coating liquid.

[0277] -Manufacturing of the Ring Belt-

[0278] An aluminum cylinder with an outer diameter of 430 mm and a length of 600 mm was prepared. The coating liquid was dispensed onto the outer circumference of the cylinder through a distributor with a width of 500 mm, resulting in a thickness of 80 μm.

[0279] The coated cylinder was kept horizontal and heated at 140°C for 30 minutes to dry the coating.

[0280] A polyimide resin film was formed by heating the dried coating to a maximum temperature of 320°C for 120 minutes.

[0281] The polyimide resin film was peeled off the mold by hand. The axial center of the polyimide resin film was cut into a 363 mm wide section to obtain an annular strip with a thickness of 80 μm.

[0282] <Example 2>

[0283] The amount of conductive particles and silicone oil was adjusted to the amounts shown in Table 1 (parts relative to 100 parts by mass of polyimide resin after imidization of polyamic acid), and otherwise annular belts were obtained in the same manner as in Example 1.

[0284] <Example 3>

[0285] As conductive particles, acid-treated product 1 of COLOUR BLACK FW1 was used, and the amount of conductive particles and silicone oil was adjusted to the amounts shown in Table 1 (parts relative to 100 parts by mass of polyimide resin after imidization of polyamic acid). Otherwise, an annular belt was obtained in the same manner as in Example 1.

[0286] <Example 4>

[0287] As conductive particles, acid-treated product 2 of COLOUR BLACK FW1 was used, and the amount of conductive particles and silicone oil was adjusted to the amounts shown in Table 1 (parts relative to 100 parts by mass of polyimide resin after imidization of polyamic acid). Otherwise, an annular belt was obtained in the same manner as in Example 1.

[0288] <Example 5>

[0289] As conductive particles, acid-treated product 3 of COLOUR BLACK FW1 was used, and the amount of conductive particles and silicone oil was adjusted to the amounts shown in Table 1 (parts relative to 100 parts by mass of polyimide resin after imidization of polyamic acid). Otherwise, an annular belt was obtained in the same manner as in Example 1.

[0290] <Example 6>

[0291] As conductive particles, acid-treated product 4 of COLOUR BLACK FW1 was used, and the amount of conductive particles and silicone oil was adjusted to the amounts shown in Table 1 (parts by weight relative to 100 parts by weight of polyimide resin after imidization of polyamic acid). Otherwise, an annular belt was obtained in the same manner as in Example 1.

[0292] <Example 7>

[0293] The amount of conductive particles and silicone oil was adjusted to the amounts shown in Table 1, and otherwise an annular strip was obtained in the same manner as in Example 1.

[0294] <Example 8>

[0295] An annular band was obtained in the same manner as in Example 1, except that the amount of conductive particles was adjusted to the amounts shown in Table 1 without the use of silicone oil.

[0296] <Example 9>

[0297] As conductive particles, acid-treated product 5 of COLOUR BLACK FW1 was used, and the amount of conductive particles and silicone oil was adjusted to the amounts shown in Table 1 (parts by weight relative to 100 parts by weight of polyimide resin after imidization of polyamic acid). Otherwise, an annular belt was obtained in the same manner as in Example 1.

[0298] <Example 10>

[0299] As a polyamic acid solution, DC-A1 (18% by mass of solids) was used to adjust the amount of conductive particles and silicone oil to the amounts shown in Table 1 (parts relative to 100 parts by mass of polyimide resin after imidization of polyamic acid). Otherwise, an annular band was obtained in the same manner as in Example 1.

[0300] <Example 11>

[0301] The amount of conductive particles and silicone oil was adjusted to the amounts shown in Table 1, and otherwise an annular strip was obtained in the same manner as in Example 1.

[0302] <Example 12>

[0303] The amount of conductive particles and silicone oil was adjusted to the amounts shown in Table 1, and otherwise an annular strip was obtained in the same manner as in Example 1.

[0304] <Example 13>

[0305] The amount of conductive particles and silicone oil was adjusted to the amounts shown in Table 1, and otherwise an annular strip was obtained in the same manner as in Example 1.

[0306] <Example 14>

[0307] A dispersion was obtained by adding COLOUR BLACKFW2 as conductive particles and aralkyl-modified silicone oil (Shin-Etsu Chemical Co., Ltd., KF-410) as silicone oil to a polyamide-imide resin (trade name HPC-9000F-8L, manufactured by Resonac Holdings Corporation, marked "PAI" in the table) (18% by mass of solids). The amounts of conductive particles and silicone oil were adjusted to the amounts shown in Table 1 (parts by mass relative to 100 parts by mass of the polyimide resin after imidization of polyamic acid). Otherwise, annular belts were obtained in the same manner as in Example 1.

[0308] <Comparative Example 1>

[0309] A dispersion was obtained by adding COLOUR BLACK FW200 as conductive particles and aralkyl-modified silicone oil (Shin-Etsu Chemical Co., Ltd., KF-410) as silicone oil to a polyimide resin (trade name JIV300R, manufactured by JFE Chemical Corporation, marked "A" in the table). The amounts of conductive particles and silicone oil were adjusted to the amounts shown in Table 1 (parts by weight relative to 100 parts by weight of the polyimide resin after imidization of polyamic acid). Otherwise, annular belts were obtained in the same manner as in Example 1.

[0310] <Comparative Example 2>

[0311] A dispersion was obtained by adding COLOUR BLACK FW1 as conductive particles and aralkyl-modified silicone oil (Shin-Etsu Chemical Co., Ltd., KF-410) as silicone oil to a polyimide resin (trade name JIV300R, manufactured by JFE Chemical Corporation, marked "A" in the table). The amounts of conductive particles and silicone oil were adjusted to the amounts shown in Table 1 (parts by weight relative to 100 parts by weight of the polyimide resin after imidization of polyamic acid). Otherwise, annular belts were obtained in the same manner as in Example 1.

[0312] <Comparative Example 3>

[0313] A dispersion was obtained by adding COLOURBLACK FW200 as conductive particles to a polyamic acid solution DA-A1 (18% by mass of solids). The amount of conductive particles was adjusted to the amounts shown in Table 1 (parts by mass relative to 100 parts by mass of the polyimide resin after imidization of the polyamic acid). Otherwise, annular bands were obtained in the same manner as in Example 1.

[0314] <Comparative Example 4>

[0315] A dispersion was obtained by adding COLOUR BLACK FW200 as conductive particles to a polyimide resin (trade name JIV300R, manufactured by JFE Chemical Corporation) (A). The amount of conductive particles was adjusted to the amounts shown in Table 1 (parts by weight relative to 100 parts by weight of the polyimide resin after imidization of polyamic acid). Otherwise, an annular band was obtained in the same manner as in Example 1.

[0316] <Comparative Example 5>

[0317] A dispersion was obtained by adding COLOUR BLACK FW310 as conductive particles to a polyimide resin (trade name JIV300R, manufactured by JFE Chemical Corporation, marked "A" in the table). The amount of conductive particles was adjusted to the amounts shown in Table 1 (parts by weight relative to 100 parts by weight of the polyimide resin after imidization of polyamic acid). Otherwise, an annular band was obtained in the same manner as in Example 1.

[0318] <Comparative Example 6>

[0319] A dispersion was obtained by adding COLOUR BLACK FW1 as conductive particles to a polyimide resin (trade name JIV300R, manufactured by JFE Chemical Corporation, marked "A" in the table). The amount of conductive particles was adjusted to the amounts shown in Table 1 (parts by weight relative to 100 parts by weight of the polyimide resin after imidization of polyamic acid). Otherwise, an annular band was obtained in the same manner as in Example 1.

[0320] <Evaluation 1>

[0321] (Characteristic Evaluation)

[0322] The following characteristics of the annular belts of Examples 1, 2, 7, 8, 16 and Comparative Examples 1 to 2 were measured according to the methods described.

[0323] The average area of ​​the Voronoi polygons in a Voronoi tessellation with the centroid of the conductive particle as the parent point. Average dispersion diameter of conductive particles The average value of the closest distance distribution of conductive particles (Implementation Evaluation) As intermediate transfer belts, the annular belts of Examples 1, 2, 7, 8, 16 and Comparative Examples 1 to 2 were mounted on an evaluation image forming apparatus ("Revoria Press SC285" manufactured by FUJIFILM Business Innovation Corporation).

[0324] Then, the following evaluation was performed using an image forming apparatus.

[0325] -Transferability-

[0326] The image forming apparatus was evaluated by continuously printing 10,000 halftone images (50% magenta) on DYNIC CORPORATION OZK (188μm thick) sheets in a low-temperature, low-humidity environment (10°C, 15% humidity). The image quality before and after printing was evaluated below. Using an X-Rite 938 image density meter (manufactured by X-Rite Corporation), the image density was randomly measured at 10 points on the last image, and the difference between the maximum and minimum measured image density values ​​was calculated as the image density difference.

[0327] The evaluation criteria are as follows.

[0328] A+: Image density difference is below 0.1, making it visually unrecognizable.

[0329] A: The image density difference is less than 0.2, making it visually unrecognizable.

[0330] B: Image density difference exceeding 0.2 and below 0.25 is difficult to visually identify.

[0331] B-: Image density difference exceeding 0.25 and below 0.3, visually identifiable but within acceptable limits.

[0332] C: The image density difference exceeds 0.3, which is easily visually identifiable and is outside the allowable range.

[0333] -Fragment resistance-

[0334] The image forming apparatus was evaluated by performing continuous travel without paper feed. The number of rotations until the intermediate transfer belt broke during continuous travel was evaluated.

[0335] The evaluation criteria are as follows.

[0336] A+: No breakage after more than 2.4 million cycles.

[0337] A: Fracture occurs at a cycle count exceeding 1.6 million but less than 2.4 million.

[0338] B: Fracture occurs at a rate of 800,000 cycles or more but less than 1,600,000 cycles.

[0339] B-: Fracture occurs at a rate of 480,000 to 800,000 cycles.

[0340] C: Fracture occurs at a cycle count exceeding 200,000 cycles but less than 480,000 cycles.

[0341] D: Fracture occurs when the number of cycles is less than 200,000.

[0342] -Cleanliness-

[0343] By evaluating the image forming apparatus, after outputting 10,000 full-page grid images (converted to 1% density) on A4-sized plain paper in a high-temperature and high-humidity environment (28°C, 85%RH), we observed the striped cleaning defects after the solid part of the transfer tape and the squeegee protruded 100% into the contact area without transfer.

[0344] The evaluation criteria are as follows.

[0345] A: No cleaning issues were observed.

[0346] B: Poor cleaning is defined as a level of inability to be visually identifiable.

[0347] C: Poor cleaning is clearly visually identifiable.

[0348] <Rating 2>

[0349] The annular bands of Examples 3-6, 9-14 and Comparative Examples 3-6 were evaluated in the same manner as Evaluation 1.

[0350] [Table 1]

[0351] As can be seen from the above results, in the embodiments, the fracture resistance and transfer retention are both superior compared with the comparative examples.

[0352] Therefore, it can also be seen that, compared with the annular belt of the comparative example, the annular belt of the embodiment has excellent dispersion of fracture-resistant and conductive particles in the belt thickness direction.

[0353] This implementation includes the following methods.

[0354] (1) A ring-shaped belt containing resin and conductive particles, When observing a cross-section along the thickness direction, The average area of ​​the Voronoi polygons in the Voronoi tessellation with the centroid of the conductive particle as the parent point is 1400 nm. 2 Above and 2000nm 2 The standard deviation of the area of ​​the Voronoi polygon is 1200 nm. 2 the following, The average dispersion diameter of the conductive particles is less than 30 nm. The average of the closest distance distribution of the conductive particles is above 20 nm and below 40 nm.

[0355] (2) According to the annular belt described in (1), wherein, The average area of ​​the Voronoi polygons when the centroid of the conductive particle is used as the generatrix is ​​1600 nm.2 Above and 1800nm 2 The standard deviation of the area of ​​the Voronoi polygon is 1000 nm. 2 the following, The average dispersion diameter of the conductive particles is less than 27 nm. The average of the closest distance distribution of the conductive particles is above 30 nm and below 35 nm.

[0356] (3)) According to (1) or (2) the annular belt, wherein, The conductive particles are carbon black.

[0357] (4)) According to the annular belt described in (3), The carbon black is carbon black with a surface functional group content of ≥0.3mmol / g and ≤0.6mmol / g when back titrated with NaHCO3.

[0358] (5)) According to (3) or (4)) the annular belt, wherein, The carbon black content relative to 100 parts by weight of the resin is 16 parts by weight or more and 26 parts by weight or less.

[0359] (6)) An annular band according to any one of (1) to (5), wherein, The resin is a polyimide resin.

[0360] (7)) According to the annular belt described in (6), Polyimide resins are imides of polyamic acids with amino groups at all ends.

[0361] (8)) The annular strip according to any one of (1) to (7) contains at least one silicone oil selected from the group consisting of dimethyl silicone oil and modified silicone oil.

[0362] (9) An intermediate transfer belt having an annular belt as described in any one of (1) to (8).

[0363] (10) A transfer device comprising: The intermediate transfer belt transfers a toner image onto the outer peripheral surface and has an annular belt as described in any one of ((1)) to ((8)); A primary transfer apparatus comprising a primary transfer component that transfers a toner image formed on the surface of an image holder to the outer peripheral surface of an intermediate transfer belt in a single transfer; and A secondary transfer apparatus having a secondary transfer component configured to contact the outer peripheral surface of the intermediate transfer belt and to transfer the toner image transferred to the outer peripheral surface of the intermediate transfer belt to the surface of a recording medium.

[0364] (11) An image forming apparatus comprising: A toner image forming apparatus having an image holder, and forming a toner image on the surface of the image holder; and The transfer apparatus described in (10) transfers the toner image formed on the surface of the image holder to the surface of the recording medium.

[0365] The effects of the above methods are as follows.

[0366] According to the invention described in (1), an annular strip is provided, wherein, when observing a cross-section along the thickness direction of the strip containing resin and conductive particles, the average area of ​​the Voronoi polygons in the Voronoi mosaic with the centroid of the conductive particles as the parent point is less than 1400 nm. 2 or more than 2000nm 2 The standard deviation of the area of ​​the Voronoi polygon exceeds 1200 nm. 2 Compared to cases where the average dispersion diameter of conductive particles exceeds 30 nm or the average value of the closest distance distribution of conductive particles is less than 20 nm or exceeds 40 nm, the fracture resistance and the dispersion of conductive particles in the thickness direction are both excellent.

[0367] According to the invention involved in ((2)), an annular strip is provided, the average area of ​​which is less than 1600 nm compared with the area of ​​the Voronoi polygon when the centroid of the conductive particle is used as the parent point for Voronoi tessellation. 2 or more than 1800nm 2 The standard deviation of the area of ​​the Voronoi polygon exceeds 1000 nm. 2 Compared to cases where the average dispersion diameter of conductive particles exceeds 27 nm or the average value of the closest distance distribution of conductive particles is less than 30 nm or exceeds 35 nm, the fracture resistance and the dispersion of conductive particles in the thickness direction are both excellent.

[0368] According to the invention involved in ((3)), an annular belt is provided, which has excellent fracture resistance and dispersion of conductive particles in the belt thickness direction compared with the case where the conductive particles are conductive oxide particles.

[0369] According to the invention involved in (4), an annular belt is provided, which, compared with carbon black in which the amount of surface functional groups for back titration using NaHCO3 is less than 0.3 mmol / g or more than 0.6 mmol / g, exhibits superior dispersion of fracture-resistant and conductive particles in the belt thickness direction.

[0370] According to the invention involved in ((5)), an annular belt is provided, which has excellent dispersion of fracture-resistant and conductive particles in the belt thickness direction compared with the case where the content of carbon black relative to 100 parts by mass is less than 16 parts by mass or more than 26 parts by mass.

[0371] According to the invention involved in (6), an annular belt is provided, which has excellent fracture resistance and dispersion of conductive particles in the belt thickness direction compared with the case where the resin is polyamide-imide resin.

[0372] According to the invention involved in ((7)), an annular belt is provided, which has excellent fracture resistance and dispersion of conductive particles in the belt thickness direction compared to the case where the polyimide resin is an imide of polyamic acid with all ends being carboxyl groups.

[0373] According to the invention described in (8), an annular strip is provided, wherein, when observing a cross-section along the thickness direction of the strip containing resin and conductive particles, the average area of ​​the Voronoi polygons in the Voronoi mosaic with the centroid of the conductive particles as the parent point is less than 1400 nm. 2 or more than 2000nm 2 The standard deviation of the area of ​​the Voronoi polygon exceeds 1200 nm. 2 Compared to cases where the average dispersion diameter of conductive particles exceeds 30 nm or the average value of the closest distance distribution of conductive particles is less than 20 nm or exceeds 40 nm, dimethyl silicone oil contains superior fracture resistance and dispersion of conductive particles in the thickness direction.

[0374] According to the inventions described in (9), (10), or (11), an intermediate transfer belt is provided, as well as a transfer apparatus and an image forming apparatus having the intermediate transfer belt. The intermediate transfer belt is applicable to annular belts containing resin and conductive particles, where, when observing a cross-section along the belt thickness direction, the average area of ​​the Voronoi polygons in a Voronoi mosaic with the centroid of the conductive particles as the parent point is less than 1400 nm. 2 or more than 2000nm 2 The standard deviation of the area of ​​the Voronoi polygon exceeds 1200 nm. 2Compared to annular bands where the average dispersion diameter of conductive particles exceeds 30 nm or the average value of the closest distance distribution of conductive particles is less than 20 nm or exceeds 40 nm, it exhibits superior fracture resistance and transfer retention.

[0375] The embodiments of the present invention described above are provided for illustrative purposes. Furthermore, these embodiments do not encompass the entirety of the invention, nor do they limit the invention to the disclosed methods. It will be apparent to those skilled in the art that various modifications and variations will be readily understood. These embodiments were chosen and described to most readily explain the principles and applications of the invention. Thus, those skilled in the art can understand the invention through various modifications that are assumed to be optimized for specific uses of various embodiments. The scope of the invention is defined by the foregoing claims and their equivalents.

[0376] Symbol Explanation

[0377] 1Y, 1M, 1C, 1K - Image forming unit; 10 - Primary transfer unit; 11 - Photoreceptor; 12 - Belt charger; 13 - Laser exposure unit; 14 - Developer; 15 - Intermediate transfer belt; 16 - Primary transfer roller; 17 - Photoreceptor cleaner; 20 - Secondary transfer unit; 22 - Secondary transfer roller; 22A - Secondary transfer roller cleaning component; 25 - Back roller; 26 - Power supply roller; 31 - Drive roller; 32 - Support roller; 33 - Tension application roller; 34 - Clean back roller; 35 - Intermediate transfer belt cleaning component; 40 - Control unit; 42 - Reference sensor; 43 - Image density sensor; 50 - Paper receiving unit; 51 - Paper feed roller; 52 - Conveyor roller; 53 - Conveyor guide; 55 - Conveyor belt; 56 - Fixing entrance guide; 60 - Fixing device; 100 - Image forming apparatus.

Claims

1. A ring-shaped belt containing resin and conductive particles, When observing a cross-section along the thickness direction, The average area of ​​the Voronoi polygons in the Voronoi tessellation with the centroid of the conductive particle as the parent point is 1400 nm. 2 Above and 2000nm 2 The standard deviation of the area of ​​the Voronoi polygon is 1200 nm. 2 the following, The average dispersion diameter of the conductive particles is less than 30 nm. The average of the closest distance distribution of the conductive particles is above 20 nm and below 40 nm.

2. The annular belt according to claim 1, wherein, The average area of ​​the Voronoi polygons when the centroid of the conductive particle is used as the generatrix is ​​1600 nm. 2 Above and 1800nm 2 The standard deviation of the area of ​​the Voronoi polygon is 1000 nm. 2 the following, The average dispersion diameter of the conductive particles is less than 27 nm. The average of the closest distance distribution of the conductive particles is above 30 nm and below 35 nm.

3. The annular belt according to claim 1 or 2, wherein, The conductive particles are carbon black.

4. The annular belt according to claim 3, wherein, The carbon black is carbon black with a surface functional group content of ≥0.3mmol / g and ≤0.6mmol / g when back titrated with NaHCO3.

5. The annular belt according to claim 3 or 4, wherein, The carbon black content relative to 100 parts by weight of the resin is 16 parts by weight or more and 26 parts by weight or less.

6. The annular belt according to any one of claims 1 to 5, wherein, The resin is a polyimide resin.

7. The annular belt according to claim 6, wherein, Polyimide resins are imides of polyamic acids with amino groups at all ends.

8. The annular belt according to any one of claims 1 to 7, comprising at least one silicone oil selected from the group consisting of dimethyl silicone oil and modified silicone oil.

9. An intermediate transfer belt having an annular belt as described in any one of claims 1 to 8.

10. A transfer device comprising: The intermediate transfer belt transfers a toner image onto its outer peripheral surface and has an annular belt as described in any one of claims 1 to 8; A primary transfer apparatus comprising a primary transfer component that transfers a toner image formed on the surface of an image holder to the outer peripheral surface of an intermediate transfer belt in a single transfer; and A secondary transfer apparatus having a secondary transfer component configured to contact the outer peripheral surface of the intermediate transfer belt and to transfer the toner image transferred to the outer peripheral surface of the intermediate transfer belt to the surface of a recording medium.

11. An image forming apparatus comprising: A toner image forming apparatus having an image holder, and forming a toner image on the surface of the image holder; and The transfer apparatus of claim 10 transfers the toner image formed on the surface of the image holder to the surface of the recording medium.

Citation Information

Patent Citations

  • Endless belt, method for manufacturing endless belt, transfer device, and image forming apparatus

    JP2021092598A

  • Belt for electrophotography and electronic photograph image formation device using the same

    JP2023008686A

  • Endless belt, transfer device, and image forming device

    JP2023135214A