Methods, systems, equipment, and storage media for predicting the lifetime of monocrystalline film porous structures.

By acquiring the damage morphology parameters at the hole edge, establishing a geometric model and a finite element model containing the actual damage morphology, and combining the crystal plastic constitutive model for simulation, the problem of accuracy and unified evaluation of life prediction for single-crystal film hole structure components in the prior art is solved, and simultaneous prediction of high-temperature creep life and high-cycle fatigue life is achieved.

CN123116689APending Publication Date: 2026-11-17AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611315030.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing life prediction technologies for single-crystal film-forming hole structures fail to fully consider the differences in hole edge damage morphology caused by different drilling processes, resulting in a large deviation between the life prediction results and the actual life, and also fail to unify the assessment of rupture life and fatigue life.

Method used

By acquiring the damage morphology parameters at the hole edge, a geometric model and a finite element model containing the actual damage morphology are established. Combined with the crystal plastic constitutive model of nickel-based single crystal materials, crystal plastic finite element simulation is performed to obtain the shear stress parameters. The correspondence between high-temperature creep life and maximum shear stress of the slip system, as well as high-cycle fatigue life and shear stress, is established to achieve synchronous prediction.

Benefits of technology

It enables accurate and targeted prediction of the high-temperature creep life and high-cycle fatigue life of single-crystal film hole structures under different drilling processes and hole edge surface conditions, thereby improving the reliability and engineering applicability of the prediction results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123116689A_ABST
    Figure CN123116689A_ABST
Patent Text Reader

Abstract

This application discloses a method, system, device, and storage medium for predicting the lifespan of single-crystal film-forming porous structures. The invention parameterizes and characterizes the damage morphology at the hole edge and establishes a finite element model containing the actual damage morphology. It then combines this with a finite element simulation using a crystal plastic constitutive model of nickel-based single-crystal materials. Based on the shear stress parameters, it predicts both high-temperature creep life and high-cycle fatigue life, achieving a unified assessment of the two failure modes of structural components under different drilling processes, making the prediction results more targeted and reliable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of life prediction technology for monocrystalline film pore structures, specifically to methods, systems, equipment, and storage media for life prediction of monocrystalline film pore structures. Background Technology

[0002] Aero-engine turbine blades operate under complex alternating loads of high temperature, high pressure, and high-frequency vibration for extended periods. To reduce blade operating temperature, film cooling holes are typically installed on the turbine blade surface, allowing cooling airflow to exit through these holes and form a cooling film on the blade surface. While film cooling holes improve blade cooling efficiency, as structural discontinuities, they also cause localized stress concentrations, becoming critical sensitive areas for high-temperature creep damage and high-cycle fatigue damage. Nickel-based single-crystal superalloys possess excellent high-temperature strength, creep resistance, and fatigue resistance, and are widely used in the manufacture of aero-engine turbine blades. Since single-crystal materials lack grain boundaries, their deformation and damage behavior are closely related to crystal orientation, slip system activity, and shear stress. Therefore, when predicting the life of single-crystal film cooling hole structures, the anisotropic mechanical response and slip system shear stress characteristics of the single-crystal material must be fully considered.

[0003] Existing life prediction technologies for single-crystal film-forming hole (FSB) structures typically assess creep life and fatigue life independently, often based on ideal FSB geometry and isotropic material assumptions. Life evaluation models are established using nominal stress, equivalent stress, or macroscopic finite element results. Regarding the surface condition of the FSB hole edges, current methods largely remain at the level of qualitative inspection or process compliance assessment, failing to incorporate the actual damage morphology of the hole edges as input parameters for the life prediction model. Furthermore, different drilling processes (such as EDM and femtosecond laser drilling) introduce drastically different microscopic damage morphologies into the hole walls. EDM easily forms recast layers, microcracks, and heat-affected structures, while femtosecond laser drilling may create prismatic, striped, or ridge-like machining marks. Different processing parameters can also lead to FSB hole roundness errors, diameter deviations, and geometric fluctuations in the hole walls. These damage morphologies caused by different processes have different influence mechanisms and weights on creep stress relaxation and fatigue stress concentration, but existing life prediction methods fail to incorporate them into a unified framework of crystal plasticity finite element analysis.

[0004] Therefore, there is an urgent need to provide a method for predicting the lifespan of single-crystal film pore structures, so as to achieve comprehensive and accurate prediction of the service life and fatigue life of the structures under different film pore surface conditions, making the prediction results more targeted and reliable. Summary of the Invention

[0005] The purpose of this application is to provide a method, system, device and storage medium for predicting the life of single-crystal film pore structures, so as to achieve comprehensive and accurate prediction of the service life and fatigue life of the structures under different film pore surface conditions, and make the prediction results more targeted and reliable.

[0006] To solve the above technical problems: In a first aspect, this application provides a method for predicting the lifetime of a single-crystal film-forming porous structure, including: Obtain the hole edge damage morphology parameters of the single crystal film pore structure to be predicted. The hole edge damage morphology parameters are used to characterize the geometric morphology, surface layer structure or local processing damage of the film pore wall. Based on the hole edge damage morphology parameters, the hole wall of the air film hole is parametrically characterized, and a geometric model of the single crystal air film hole structure containing the hole edge damage morphology is established. A finite element model is established based on the geometric model, and the parameters of the single crystal matrix material and the parameters of the surface layer or local damage area corresponding to the hole edge damage morphology are set in the finite element model. A crystal plastic constitutive model for nickel-based single crystal materials is established. This model is used to describe shear deformation, hardening behavior, and shear stress response in different slip systems. High-temperature sustained load and high-cycle fatigue load conditions were applied to the finite element model respectively to perform crystal plastic finite element simulation and obtain the shear stress parameters of each slip system in the edge region of the air film hole. Based on the results of high-temperature creep test, a correlation was established between high-temperature creep life and maximum shear stress of slip system, and based on the results of high-cycle fatigue test, a correlation was established between high-cycle fatigue life and shear stress parameters in fatigue critical area. By substituting the shear stress parameters into the high-temperature creep life correspondence and the high-cycle fatigue life correspondence, the high-temperature creep life prediction and high-cycle fatigue life prediction of the single-crystal film pore structure are obtained.

[0007] Secondly, this application also provides a life prediction system for single-crystal air-film porous structures, characterized in that it includes: The morphology parameter acquisition module is used to acquire the hole edge damage morphology parameters of the single crystal gas film hole structure to be predicted. The hole edge damage morphology parameters include at least one of the following: gas film hole roundness parameter, recast layer thickness parameter formed by electrical discharge drilling, and prism processing mark depth parameter formed by femtosecond laser drilling. The geometric model building module is used to build a geometric model of a single-crystal gas film hole structure containing the corresponding hole edge damage morphology based on the hole edge damage morphology parameters. The finite element model building module is used to build a finite element model based on the geometric model of the single crystal film pore structure, and to perform finite element characterization on at least one of the single crystal matrix, recast layer, roundness error and prismatic machining marks. The Crystal Plastic Constitutive Model Establishment Module is used to establish a crystal plastic constitutive model for nickel-based single crystal materials. The crystal plastic constitutive model is used to describe the shear stress response of each slip system of the single crystal material under high temperature creep load and high cycle fatigue load. The crystal plasticity finite element calculation module is used to obtain the shear stress parameters of the slip system in the hole edge region of a single crystal film hole structure based on the finite element model and the crystal plasticity constitutive model. The lifespan relationship determination module is used to establish the correspondence between high-temperature creep rupture life and the maximum shear stress of the slip system based on the results of high-temperature creep rupture tests, and to establish the correspondence between high-cycle fatigue life and the maximum shear stress at the critical distance based on the results of high-cycle fatigue tests; and The life prediction module is used to determine the high-temperature creep life and high-cycle fatigue life of the single-crystal film pore structure to be predicted based on the shear stress parameters of the slip system, the correspondence between high-temperature creep life and high-cycle fatigue life.

[0008] Thirdly, this application also provides an electronic device, including: Processor; and Memory that communicates with the processor; The memory stores a program, which, when executed by the processor, causes the electronic device to perform any of the above-mentioned methods for predicting the lifespan of a single-crystal air-film porous structure.

[0009] Fourthly, this application also provides a computer-readable storage medium having a computer program stored thereon, wherein when the computer program is run on a processor, the processor executes the single-crystal film pore structure lifetime prediction method described above.

[0010] As can be seen from the above technical solution, the single-crystal film-tube structure life prediction method provided by the present invention establishes a geometric model and a finite element model containing the actual hole edge damage morphology by using hole edge damage morphology parameters as model input and parametrically characterizing the hole wall. Simultaneously, single-crystal matrix material parameters and surface layer or local damage region parameters corresponding to the hole edge damage morphology are set in the finite element model, enabling the finite element model to reflect the differences in local stress field at the hole edge caused by different drilling processes. By establishing a crystal plastic constitutive model of nickel-based single-crystal material to describe shear deformation, hardening behavior, and shear stress response on different slip systems, the shortcomings of traditional isotropic material assumptions in accurately reflecting single-crystal anisotropy and shear stress concentration in slip systems are overcome. Based on this, crystal plastic finite element simulation is performed by applying high-temperature endurance loading conditions and high-cycle fatigue loading conditions respectively. Based on the correspondence between maximum shear stress and endurance life, and the correspondence between shear stress parameters and fatigue life, the endurance prediction life and fatigue prediction life are obtained simultaneously, achieving a unified evaluation of the structure under both endurance and fatigue failure modes, making the life prediction results more targeted and engineering reliable. Attached Figure Description

[0011] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely some examples or embodiments of this application. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort, and this application can be applied to other similar scenarios based on the provided drawings. Unless obvious from the linguistic context or otherwise specified, the same reference numerals in the drawings represent the same structures or operations.

[0012] Figure 1 This application provides a schematic flowchart of a method for predicting the lifespan of a single-crystal film-forming porous structure. Figure 2 This application provides a schematic diagram for detecting the roundness of air film pores in an embodiment; Figure 3 This application provides a schematic diagram for detecting the thickness of the recast layer. Figure 4 This application provides a schematic diagram for detecting prismatic marks. Figure 5 A cross-sectional view of the air film pores is provided for an embodiment of this application; Figure 6 This application provides a geometric model of a prismatic mark. Figure 7 This application provides a geometric model of a high-temperature endurance test specimen. Figure 8 This application provides a mesh generation method for high-temperature endurance test specimens. Figure 9 This application provides a recast layer mesh partitioning method for its embodiments; Figure 10 This application provides a geometric model for a high-cycle fatigue specimen. Figure 11 This application provides a high-cycle fatigue specimen mesh generation method. Figure 12 This application provides a maximum shear stress gradient direction for a high-temperature creep rupture specimen. Figure 13 This application provides a maximum shear stress gradient direction for a high-cycle fatigue specimen. Figure 14 A flowchart of an iterative algorithm for a single-crystal constitutive model is provided for embodiments of this application; The annotations in the attached figures are explained as follows: 1. Single crystal film pore structure, 11 film pore, 111 inlet section, 112 intermediate section, 113 outlet section. Detailed Implementation

[0013] The inventors discovered that during the service life of aero-engine turbine blades, the film cooling pores, as structural discontinuities, are highly susceptible to becoming damage initiation sites under the combined effects of high-temperature rupture loads and high-cycle fatigue loads. Nickel-based single-crystal superalloys, lacking grain boundary characteristics, exhibit significant anisotropy due to their deformation behavior being controlled by crystal orientation and slip system shear stress. Current life prediction methods typically assess rupture life and fatigue life separately, and are often based on ideal film cooling pore geometry models and isotropic material assumptions. These methods fail to incorporate hole edge damage morphologies caused by different drilling processes (such as recast layers formed by EDM drilling and prismatic machining marks formed by femtosecond laser drilling) into a unified prediction framework, leading to significant discrepancies between predicted and actual life.

[0014] Based on this, this application provides a method for predicting the life of a single-crystal film-forming hole structure. This method obtains the hole edge damage morphology parameters of the structure to be predicted, performs parameterized characterization of the film-forming hole wall, and establishes a geometric model and a finite element model containing the actual damage morphology. Simultaneously, in the finite element model, parameters of the single-crystal matrix material and parameters of the surface layer or local damage region corresponding to the hole edge damage morphology are set. Based on this, combined with a nickel-based single-crystal material crystal plastic constitutive model, high-temperature creep loading and high-cycle fatigue loading conditions are applied to perform crystal plastic finite element simulations, obtaining the shear stress parameters of each slip system in the hole edge region. Then, according to the pre-established correspondence between high-temperature creep life and maximum shear stress, and the correspondence between high-cycle fatigue life and shear stress parameters, the predicted high-temperature creep life and high-cycle fatigue life of the structure are simultaneously obtained. By using the actual damage morphology at the hole edge as model input and employing crystal plastic constitutive modeling to describe the anisotropic deformation behavior of single-crystal materials, the finite element model can realistically reflect the differences in stress field at the hole edge caused by different drilling processes. At the same time, it unifies the lifetime prediction of the two failure modes under the same computational framework, thereby improving the pertinence and accuracy of lifetime prediction.

[0015] See Figures 1 to 13 The method for predicting the lifetime of a single-crystal film-forming porous structure provided in this application includes the following steps: Step S100: Obtain the hole edge damage morphology parameters of the single crystal air film hole structure to be predicted.

[0016] The hole edge damage morphology parameters are used to characterize the geometric morphology, surface layer structure, or local processing damage of the hole wall of the film gas hole 11. Specifically, the geometric morphology may include the roundness error, hole diameter deviation, and geometric undulations of the hole wall of the film gas hole 11; the surface layer structure may include the recast layer and heat-affected layer formed on the hole wall surface by the electrical discharge machining process; local processing damage may include ridge-shaped processing marks, stripe-shaped processing marks, ridge-shaped processing marks, and microcracks formed on the hole wall surface by the femtosecond laser drilling process. In one specific embodiment, the hole wall of the film gas hole 11 can be measured by equipment such as a stereomicroscope, scanning electron microscope, confocal microscope, or three-dimensional optical profilometer to obtain quantitative data of the above-mentioned morphology parameters. This measurement step can be performed on the actual processed structural part or on a sample processed in the same batch as the structural part to be predicted, as long as the morphology parameters characterizing the actual state of the hole wall of the structural part to be predicted can be obtained.

[0017] For example, to measure the roundness parameter of the film-forming orifice 11, an image of the cross-section of the film-forming orifice 11 can be acquired using a stereomicroscope at a magnification of 20x to 50x. Then, image processing software can be used to measure the minimum circumscribed circle diameter and the maximum inscribed circle diameter on this cross-section, and the roundness parameter can be calculated based on the difference between the two. To measure the thickness of the recast layer, a scanning electron microscope can be used at a magnification of 2000x to 5000x to measure multiple detection positions at the inlet section 111, middle section, and outlet section 113 of the film-forming orifice 11. To measure the depth of the prismatic machining marks, a scanning electron microscope can also be used at a magnification of 2000x to 5000x to measure the mark depth at different positions on the wall of the film-forming orifice 11. Of course, depending on different drilling processes and specific morphological types, other suitable measurement methods can also be used, such as using a white light interferometer to measure surface roughness and machining mark depth, or using X-ray tomography to measure the distribution of the internal recast layer. This application does not limit these methods.

[0018] Step S200: Based on the hole edge damage morphology parameters, the hole wall of the gas film hole 11 is parametrically characterized to establish a geometric model of the single crystal gas film hole structure 1 containing the hole edge damage morphology.

[0019] Parametric characterization refers to converting the morphological parameters obtained in step S100 into geometric parameters recognizable by 3D modeling software. For example, the roundness parameter of the film-forming hole 11 is converted into the coordinate offset of the hole wall profile, the recast layer thickness parameter is converted into the radial offset of the hole wall surface, and the depth parameter of the prismatic machining marks is converted into the local undulation along the hole wall surface. In one specific embodiment, a basic 3D model can be first established based on the actual structural dimensions of the single-crystal film-forming hole structure 1 (including the hole diameter, hole depth, inclination angle, hole spacing, and the overall dimensions of the structure). Then, based on the basic model, the hole wall of the film-forming hole 11 is locally corrected according to the measured morphological parameters, and finally, a geometric model of the structure containing the actual hole edge damage morphology is obtained. The 3D modeling software used can be commercial software such as CATIA, SolidWorks, and UG NX, or open-source 3D modeling tools can be used; this application does not limit this.

[0020] In the parametric characterization process, different characterization methods can be used for different types of damage morphologies. For example, for the roundness error of the film pore 11, the actual hole wall profile can be simulated by applying a radial perturbation in the form of a Fourier series to the theoretical circular hole profile; for the recast layer, an additional layer of uniform or non-uniform thickness can be established on the hole wall surface; for prismatic machining marks, periodic or non-periodic groove structures extending along the hole depth direction can be established on the hole wall surface. These characterization methods can be adjusted according to actual measurement data to make the geometric model as close as possible to the hole wall morphology of the actual structural component.

[0021] Step S300: Establish a finite element model based on the geometric model, and set the single crystal substrate material parameters and the surface layer or local damage region parameters corresponding to the hole edge damage morphology in the finite element model.

[0022] Specifically, the geometric model established in step S200 is imported into finite element analysis software, such as commercial finite element software like ABAQUS, ANSYS, and NASTRAN, or an open-source finite element solver is used. The single-crystal matrix portion of the structural component is assigned the mechanical property parameters of nickel-based single-crystal material, including but not limited to elastic modulus, Poisson's ratio, density, coefficient of thermal expansion, and hardening parameters required for subsequent crystal plastic constitutive models. For surface layers or localized damage areas corresponding to hole edge damage morphology, such as recast layers formed by EDM drilling, since the microstructure and mechanical properties of this layer differ significantly from the single-crystal matrix, it is necessary to separately delineate the region and assign independent material parameters in the finite element model. In one specific embodiment, the elastic and hardening parameters of the recast layer can be obtained through nanoindentation experiments and then input into the finite element model. For prismatic machining marks formed by femtosecond laser drilling, since these marks belong to geometric morphology rather than independent material layers, they do not need to be assigned separate material parameters. Instead, their geometric characteristics are reflected in the finite element model through explicit geometric modeling.

[0023] For film-forming porous structures containing a recast layer, during finite element modeling, a shell element mesh or a solid thin-layer mesh can be created on the surface of the porous wall to characterize the recast layer. When using shell elements, the actual thickness of the recast layer is characterized by the thickness definition of the shell elements; when using a solid thin-layer mesh, the thickness of the recast layer is characterized by the geometry of the thin-layer. Regardless of the method used, the material parameters of the recast layer differ from those of the single-crystal matrix and need to be defined separately.

[0024] Step S400: Establish a crystal plastic constitutive model for nickel-based single crystal materials. The crystal plastic constitutive model is used to describe shear deformation, hardening behavior and shear stress response on different slip systems.

[0025] Nickel-based single-crystal superalloys possess a face-centered cubic crystal structure, and their plastic deformation is primarily achieved through the activation of α-slip systems. Within the framework of crystal plasticity theory, the macroscopic deformation of the material is attributed to the cumulative effect of microscopic shear deformation on each slip system. A crystal plasticity constitutive model needs to describe the relationship between the shear strain rate and the resolved shear stress of the slip system, the hardening evolution of the slip system, and the evolution of crystal orientation with deformation. In one specific implementation, this constitutive model is embedded in the finite element method software as a user material subroutine (UMAT or VUMAT). Within each increment step, it calculates the shear strain rate of each slip system based on the current stress state and crystal orientation, and updates the stress, hardening variables, and crystal orientation.

[0026] Specifically, the shear stress in slip system α can be calculated by the double dot product of the Cauchy stress tensor and the orientation factor, which depends on the slip direction vector and the slip surface normal vector. The shear strain rate is described using a power-law flow rule, meaning the ratio of the shear strain rate to the shear stress relative to the reference shear stress is a power function. Hardening behavior is described by the hardening modulus matrix, where the self-hardening modulus and latent hardening modulus control the interaction hardening effects between slip systems and between different slip systems, respectively. Considering the finite deformation case, the decomposition of the plastic velocity gradient is introduced, representing the plastic deformation rate tensor and the plastic rotation rate tensor as the linear superposition of the shear strain rates of each slip system, thus establishing an incremental constitutive relationship between stress rate and strain rate.

[0027] Step S500: Apply high-temperature sustained load and high-cycle fatigue load conditions to the finite element model respectively, perform crystal plastic finite element simulation, and obtain the shear stress parameters of each slip system in the edge region of the air film hole 11.

[0028] In this step, finite element analysis conditions need to be established separately for high-temperature creep load and high-cycle fatigue load. The high-temperature creep load condition simulates the service state of a structural component under constant or approximately constant load in a high-temperature environment. The load conditions can be constant tensile load, constant internal pressure load, or load applied according to the load spectrum corresponding to the high-temperature creep test. The high-cycle fatigue load condition simulates the service state of a structural component under high-frequency alternating load in a high-temperature environment. The load conditions can be periodic loads in the form of sinusoidal waves, or loads applied according to the load spectrum corresponding to the high-cycle fatigue test. When applying boundary conditions, reasonable displacement constraints and load application methods should be set according to the actual clamping method and stress state of the structural component.

[0029] In the finite element simulation of crystal plasticity, due to the highly nonlinear nature of the constitutive model, an incremental iterative solution method is typically employed. Within each incremental step, the stress increment is calculated using the UMAT subroutine based on the strain increment of the current step, and the state variables are updated. Then, equilibrium iterations are performed until convergence. After the simulation is complete, the shear stress parameters on each slip system in the edge region of the air film hole 11 are extracted. These shear stress parameters may include, but are not limited to, the shear stress value, maximum shear stress value, shear stress amplitude, and shear stress ratio of each slip system.

[0030] Step S600: Establish the correspondence between high-temperature creep life and maximum shear stress of slip system based on the results of high-temperature creep test, and establish the correspondence between high-cycle fatigue life and shear stress parameters in fatigue danger area based on the results of high-cycle fatigue test.

[0031] High-temperature creep rupture testing refers to conducting high-temperature creep rupture tests on single-crystal gas film pore 11 specimens under different stress levels, and recording the specimen fracture time as the creep life. The test temperature should simulate the actual service temperature of the structural component, for example, selecting one or more temperature points within the range of 900℃ to 1100℃ for testing. By performing regression analysis on stress level and creep life, a correspondence between creep life and the maximum shear stress of the slip system can be established. In one specific embodiment, this correspondence can be expressed in the form of a critical shear stress model, that is, creep life is inversely proportional to the Nth power of the maximum shear stress of the slip system.

[0032] High-cycle fatigue testing refers to conducting high-cycle fatigue tests on single-crystal gas film pore specimens under different stress levels, recording the fatigue strength or fracture cycle count of the specimens at a specified number of cycles. The test is also conducted at simulated service temperatures. The SN curve (stress-life curve) of the single-crystal material can be obtained from the test data. Under high-cycle fatigue conditions, since fatigue cracks usually initiate from the stress concentration region at the hole edge, the fatigue life is closely related to the shear stress level in the fatigue hazard region. In one specific embodiment, based on the critical distance theory, the shear stress at a certain critical distance from the fatigue fracture hazard point can be used as an equivalent parameter characterizing the stress level in the fatigue hazard region, thereby establishing a correspondence between high-cycle fatigue life and this equivalent shear stress parameter. This correspondence can be established by fitting the shear stress values ​​at the critical distance obtained under different stress levels with the corresponding fatigue lives.

[0033] In step S700, the shear stress parameters are substituted into the high-temperature creep life correspondence and the high-cycle fatigue life correspondence respectively to obtain the high-temperature creep life prediction and high-cycle fatigue life prediction of the single crystal film pore structure 1.

[0034] Specifically, for high-temperature rupture life prediction, the maximum shear stress value of each slip system in the edge region of the film cooling hole 11 is extracted from the finite element simulation results in step S500. This value is then substituted into the correspondence between rupture life and maximum shear stress established in step S600 to calculate the corresponding rupture life prediction value. For high-cycle fatigue life prediction, the fatigue fracture hazard point (usually the maximum shear stress concentration point) at the edge of the film cooling hole 11 is first determined based on the finite element simulation results. Then, the critical distance is determined along the stress gradient direction, and the maximum shear stress value at this critical distance is extracted. This value is then substituted into the SN curve of the single crystal material to obtain the corresponding fatigue life prediction value.

[0035] In this way, the life prediction method provided in this application parameterizes and characterizes the hole edge damage morphology and introduces it into the finite element model. Combined with the shear stress response of the slip system described by the crystal plastic constitutive model, it realizes the simultaneous prediction of the high-temperature creep life and high-cycle fatigue life of the single crystal gas film hole structure 1 under different drilling processes and different hole edge surface states, making the life prediction results more targeted and reliable.

[0036] In some embodiments, the drilling process for the single-crystal film-forming hole structure 1 to be predicted includes at least one of electrical discharge drilling and femtosecond laser drilling. Electrical discharge drilling is a processing method that uses pulsed spark discharge between a tool electrode and the workpiece to generate high temperatures, causing the workpiece material to melt and vaporize, thereby forming a hole. Due to the rapid cooling of the molten metal during the discharge process, electrical discharge drilling typically forms a recast layer on the hole wall surface. This layer has a different microstructure from the substrate and is often accompanied by microcracks. Femtosecond laser drilling is a method of ablation processing of materials using femtosecond-level ultrashort pulse lasers. Due to the extremely short interaction time between the laser and the material, the heat-affected zone is small, but the hole wall surface may form prismatic, striped, or ridge-like micro-geometric morphologies distributed along the hole depth direction. The technical solution of this application is applicable to film-forming hole structures prepared by any of the above drilling processes, and also applicable to structures processed by a combination of two processes (e.g., electrical discharge drilling followed by femtosecond laser finishing).

[0037] In other embodiments, the hole edge damage morphology parameters include at least one of the following: the roundness parameter of the film-forming hole 11, hole diameter deviation, hole wall roughness, recast layer thickness formed by EDM drilling, depth of prismatic machining marks, depth of striped machining marks, depth of ridged machining marks formed by femtosecond laser drilling, microcrack characteristic parameters, and heat-affected zone size parameters. Among these, the roundness parameter of the film-forming hole 11 reflects the degree to which the hole cross-sectional shape deviates from the theoretical circle and is an important indicator for evaluating hole machining quality. Hole diameter deviation reflects the difference between the actual hole diameter and the designed hole diameter. Hole wall roughness reflects the degree of microscopic unevenness on the hole wall surface. Recast layer thickness reflects the thickness of the resolidified molten layer during EDM drilling and is a key parameter for evaluating the degree of thermal damage during EDM drilling. The depth of prismatic, striped, and ridged machining marks reflects the depth of the microscopic geometric marks left by the laser scanning path on the hole wall surface during femtosecond laser drilling. Microcrack characteristic parameters may include crack length, crack depth, and crack density. The heat-affected zone size parameters reflect the extent of the heat-affected zone during machining.

[0038] In practice, depending on the specific drilling process used for the component to be predicted, only the morphological parameters related to that process can be measured. For example, for specimens drilled by electrical discharge machining (EDM), the roundness parameter and the recast layer thickness can be mainly measured; for specimens drilled by femtosecond laser, the roundness parameter and the depth of machining marks can be mainly measured. Of course, if conditions permit, multiple morphological parameters can be measured simultaneously to more comprehensively characterize the hole edge condition.

[0039] In some embodiments, the roundness parameter of the air film orifice 11 is obtained by measuring the minimum circumscribed circle diameter and the maximum inscribed circle diameter of the cross-section of the air film orifice 11, such as... Figure 2 As shown. In specific measurements, a stereomicroscope can be used to observe and acquire images of the cross-section of the air film pore 11 at a magnification of 20x to 50x. Then, image analysis software can be used to determine the diameter of the smallest circumcircle and the diameter of the largest incircle on the cross-section. For a single air film pore 11, the roundness parameter of the i-th air film pore 11 is determined according to the following formula: Among them, the roundness parameter of the i-th air film pore 11 Determined according to the following formula:

[0040] Average roundness parameters of multiple air film pores 11 Determined according to the following formula:

[0041] in, The roundness of the i-th air film pore 11 ( i =1, 2…n), μm; , Here, are the minimum circumcircle and maximum incircle diameters of the i-th film-forming pore 11, respectively, in μm. This average roundness parameter can be used as a statistical measure to characterize the roundness level of the film-forming pores 11 in this batch of structural components or this sample. Of course, when predicting the life of a single structural component, the roundness parameter of a single film-forming pore 11 can also be used directly. Without having to calculate the average.

[0042] In some embodiments, the recast layer thickness is obtained by measuring multiple detection locations at the inlet section 111, middle section, and outlet section 113 of the film gas vent 11, such as... Figure 3 As shown. Specifically, a scanning electron microscope can be used to observe the walls of the air film pores 11 at a magnification of 2000x to 5000x, and the thickness of the recast layer can be measured at each detection location. The average thickness of the recast layer is... ξ Determined according to the following formula:

[0043] in, The thickness measurement value at the i-th recast layer detection location, in μm ( i= 1, 2… n ).

[0044] In one specific implementation, 3 to 5 measurement points can be selected for each segment, totaling 9 to 15 measurement points. Since the thickness of the recast layer may be non-uniform along the hole depth direction and the circumferential direction, taking the average value can better characterize the overall thickness level of the recast layer.

[0045] In some embodiments, the average depth of prismatic, striped, or ridged machining marks η Determined according to the following formula:

[0046] in, Let be the depth measurement value at the i-th machining mark detection location, in μm ( i= 1, 2… n In specific measurements, a scanning electron microscope can be used at a magnification of 2000x to 5000x to observe and measure different locations on the wall of the air film pore 11, such as... Figure 4 As shown. For prismatic machining marks, measurements are typically taken on a cross-section along the hole depth direction on the hole wall; for striped or ridged marks, an appropriate measurement cross-section is selected based on the direction of the mark's extension. Since the depth of machining marks may fluctuate along both the hole depth and circumferential directions, taking the average of multiple measurement locations can better characterize the overall depth level of the machining marks.

[0047] In some implementations, establishing a geometric model includes the following steps: First, a basic three-dimensional model is established based on the actual structural dimensions of the single-crystal film-supported hole structure 1. This basic model includes the external dimensions of the structure, the diameter, depth, axial direction, and location of the film-supported holes 11, as well as the relative positions of multiple film-supported holes 11. The actual structural dimensions can be determined based on design drawings or measurement data of the actual structure.

[0048] Secondly, the contour of the air film orifice 11 is parametrically adjusted based on the roundness parameter of the air film orifice 11, such as... Figure 5 As shown. Specifically, the contour coordinates of the ideal circular hole are corrected according to the roundness measurement data, so that the hole wall contour changes from the theoretical circle to a shape consistent with the actual measurement. In 3D modeling software, this can be achieved by offsetting each point on the theoretical circumference by a certain amount radially. This offset depends on the roundness error distribution corresponding to the angle at which the point is located.

[0049] Then, a recast geometric layer or equivalent surface layer is established on the surface of the gas film hole 11 according to the recast layer thickness. Specifically, for specimens drilled by electrical discharge machining, a layer with a thickness of [missing information] can be added to the surface of the gas film hole 11. ξ A thin layer, the inner surface of which is the actual pore wall profile of the air film pore 11, and the outer surface of which is the interface between the recast layer and the substrate. Since the thickness of the recast layer is typically on the order of micrometers (e.g., 10 μm to 100 μm), it can be regarded as an independent geometric body during geometric modeling.

[0050] Finally, a local geometric undulation structure is established on the surface of the gas film hole 11 according to the depth of the machining marks. Specifically, for the femtosecond laser-drilled specimen, groove-like undulations extending along the hole depth direction can be added to the surface of the gas film hole 11, with a groove depth of [missing information]. The width and spacing are determined based on actual measurement data. These local geometric undulations can be implemented using surface modeling or solid modeling.

[0051] It should be noted that the execution order of the above steps can be adjusted according to the actual situation. For example, if the structural component to be predicted is only drilled using femtosecond laser, the step of establishing the recast layer geometry can be omitted; if only electrical discharge machining is used, the step of establishing the local undulations of the machining marks can be omitted.

[0052] In some implementations, establishing the finite element model includes: meshing the single crystal substrate using solid elements; for film-forming hole structures with a recast layer, establishing a recast layer mesh on the surface of the film-forming hole 11 wall, and characterizing the recast layer by shell element thickness, solid thin layer thickness, or equivalent material layer parameters; for film-forming hole structures with roundness errors or local machining marks, performing explicit geometric modeling of the film-forming hole 11 wall contour and local machining marks.

[0053] Specifically, during the finite element mesh generation process, the single-crystal matrix portion preferentially uses hexahedral reduced integral solid elements (e.g., C3D8R elements) for mesh generation to achieve higher computational accuracy and efficiency. Near the wall of the gas film pore 11, due to the large stress gradient, mesh refinement is necessary to ensure the accuracy of stress calculation. The size of the refined region is typically 1 to 2 times the pore diameter, depending on the magnitude of the stress gradient.

[0054] For the mesh generation of the recast layer, in one specific embodiment, a shell mesh can be established on the surface of the gas film pore 11 using quadrilateral shell elements (e.g., S4R elements), and the actual thickness of the recast layer can be characterized by the thickness definition of the shell elements. This method is suitable when the thickness of the recast layer is much smaller than the pore diameter. In another specific embodiment, a thin mesh can also be established using solid elements, and the thickness of the recast layer can be characterized by the geometric thickness of the thin layer. This method is suitable when the thickness of the recast layer is relatively large, or when a more accurate simulation of the internal stress distribution of the recast layer is required. In yet another specific embodiment, if the recast layer is very thin (e.g., less than 10 μm), a separate recast layer mesh may not be established; instead, the influence of the recast layer can be characterized by applying an equivalent material layer parameter to the surface of the pore wall.

[0055] For film-supported hole structures with roundness errors or local machining marks, since these morphologies are geometric features rather than material features, explicit geometric modeling is used in finite element modeling. This means that these features are already included in the geometric model, and are directly discretized during mesh generation. In other words, the contour of the film-supported hole 11 is modeled according to its actual measured shape, and the prismatic machining marks, as geometric undulations of the hole wall surface, are included in the geometric model. After mesh generation, these geometric features are automatically converted into node and element distributions in the finite element model.

[0056] In some embodiments, the crystal plastic constitutive model includes the slip system shear strain rate equation, the slip system hardening equation, the slip system partial shear stress calculation equation, and the crystal orientation update equation.

[0057] In one specific embodiment, the shear strain rate equation of the slip system is determined according to the following formula:

[0058] in, is the shear strain rate of a single-crystal slip system; is a physical quantity describing the rate of plastic shear deformation in this slip system.

[0059] Let be the reference shear strain rate of the slip system α, which is the shear strain rate of the slip system under the reference stress state.

[0060] This is the reference shear stress for slip system α, reflecting the current strength level of the slip system.

[0061] m is the strain rate exponent, reflecting the material's sensitivity to strain rate. Since m is usually a small positive number (e.g., 0.01 to 0.05), the above equation means that when the shear stress is close to the reference shear stress, the shear strain rate is more sensitive to changes in the shear stress.

[0062] The hardening behavior of a slip system determines the evolution of the reference shear stress with deformation in each slip system. The hardening equation of the slip system is determined by the following formula:

[0063] Where A is the hardening rate coefficient, which is related to material properties and temperature, and is obtained by fitting high-temperature test data; Let α be the reference shear strain rate of the slip system α. It is the shear strain rate of the slip system under the reference stress state (i.e., the derivative of the reference shear strain rate with respect to time), reflecting the rate of evolution of the reference shear strain rate over time.

[0064] The shear stress on the slip system α is calculated by the double dot product of the macroscopic stress tensor and the orientation factor.

[0065] p is the time hardening exponent, which reflects the degree to which the reference shear strain rate decays naturally over time. p is usually a positive value, meaning that the evolution rate of the reference shear strain rate gradually decreases as time goes on.

[0066] t is the creep time, which represents the holding time or creep accumulation time under high temperature sustained load.

[0067] The equation for calculating the component shear stress of a slip system is determined according to the following formula:

[0068] in Let α be the rate of change of the reference shear stress in the slip system α.

[0069] is the hardening modulus, representing the hardening effect of the slip shear of slip system β on slip system α.

[0070] Let be the absolute value of the shear strain rate in slip system β. This equation describes the contribution of shear deformation in all slip systems to the hardening rate of slip system α. The magnitude of α determines the strength of the hardening effect. When α = β, This represents the self-hardening modulus; when α ≠ β, This represents the latent hardening modulus.

[0071] The crystal orientation update equation is determined according to the following formula: Hardening modulus It can be further determined according to the following formula:

[0072] in, The basic part of the hardening matrix represents the hardening caused by the slip shear of slip system β on slip system α; and These are the orientation factors for slip system α and slip system β, respectively. and Let be the corresponding rotation-dependent tensor. The second term in the above expression reflects the additional hardening effect between slip systems due to crystal rotation.

[0073] The basic part of the hardening matrix It can be determined according to the following formula:

[0074] in, Here, is the self-hardening modulus, and q is the potential hardening ratio parameter. The symbol is Kronecker (value 1 when α = β, value 0 when α ≠ β). When α = β, That is, the self-hardening modulus is H; when α≠β, That is, the latent hardening modulus is qH The typical value of q is between 1.0 and 1.4. When q=1, it means that the self-hardening and latent hardening effects are the same.

[0075] The component shear stress on the slip system α is determined by the following formula:

[0076] in, The shear stress is the partial stress on the slip system α. Cauchy stress tensor Let be the orientation factor of the slip system α. This equation is one of the core relations in crystal plasticity theory, relating the macroscopic stress tensor to the decomposed shear stress in the microscopic slip system. Orientation factor It can be calculated using the following formula:

[0077] in, Let α be the direction vector of the sliding system. Let be the unit normal vector of the slip surface where slip system α is located. In fact, it is the symmetric part of the Schmid tensor, and its physical meaning is to project the stress tensor onto the space spanned by the slip direction and the slip surface normal of the slip system.

[0078] Under finite deformation conditions, the effects of geometric nonlinearity need to be considered. The plastic velocity gradient is superimposed according to the shear strain rates of each slip system:

[0079] in, For the plastic velocity gradient tensor; and These represent the slip direction and the slip surface normal under the current configuration. The velocity gradient tensor is decomposed into a symmetric part and an antisymmetric part:

[0080] In the formula: The plastic deformation rate tensor is the symmetrical part of the plastic velocity gradient, reflecting the shape change caused by plastic deformation. The plastic rotation rate tensor is the antisymmetric part of the plastic velocity gradient, reflecting the rotational transformation caused by plastic deformation. The orientation rotation factor can be calculated using the following formula: This is actually the antisymmetric part of the Schmid tensor, reflecting the rigid body rotation effect of the crystal caused by the opening of the slip system. In the finite element method calculation of crystal plasticity, the orientation update of the crystal is achieved through... This is achieved through [the means].

[0081] Within the incremental solution framework, it is necessary to establish the relationship between shear strain rate and stress rate. The relationship between shear strain rate and stress rate on the slip system α is as follows:

[0082] in, Jaumann derivative of Kirchhoff stress tensor under the current configuration is an objective stress rate used to describe the rate of stress evolution with deformation; EMT It is the instantaneous elastic modulus tensor, which reflects the elastic stiffness under the current stress state; D This is the total deformation rate tensor; The rotational contribution term for the slip system α reflects the stress change caused by plastic rotation. The above equation expresses the stress rate as the elastic deformation component (…). EMT : D ) deduct the stress relaxation portion caused by plastic slip in each slip system ( This equation is the core of the incremental stress update in the crystal plastic finite element solver.

[0083] Let EMT be the instantaneous elastic modulus tensor. The instantaneous elastic modulus tensor EMT can be expressed by the following equation:

[0084] In the formula: , and These are three independent elastic constants, which are related to the elastic modulus E, Poisson's ratio ν, and shear modulus G.

[0085] In some implementations, the relationship between high-temperature creep life and the maximum shear stress of the slip system is as follows:

[0086] in, For long lifespan, Let B be the maximum shear stress in the slip system, and B and N be creep parameters. This model is often referred to as the critical shear stress model or the Norton-type creep model. In this model, The larger the size, the shorter the lifespan. B and N The value needs to be determined by fitting data from high-temperature endurance tests. To facilitate parameter fitting, the logarithm of both sides of the above equation can be taken, transforming it into a linear equation between logarithmic lifetime and logarithmic shear stress. The least squares method can then be used to fit and obtain ln... B and N The value.

[0087] In practice, high-temperature creep tests typically need to be conducted at multiple stress levels to obtain sufficient data points for parameter fitting. For example, creep tests can be performed at 3 to 5 different stress levels, recording the fracture time of at least 3 specimens at each stress level, and then averaging the results for fitting. The test temperature should simulate the actual service temperature of the structural component.

[0088] In some implementations, the correspondence between high-cycle fatigue life and the shear stress parameters within the fatigue-critical region is established using the critical distance method. This specifically includes the following steps: First, the fatigue fracture hazard point at the edge of the film cooling hole 11 is determined. Since fatigue cracks typically originate from the location of maximum stress concentration, in one specific embodiment, the point where the maximum shear stress is located in the edge region of the film cooling hole 11 can be identified as the fatigue fracture hazard point. In another specific embodiment, the concept of a critical plane can be used to identify the location with the maximum amplitude of shear stress on each slip surface as the hazard point. When determining the hazard point, the magnitude of the shear stress, the stress gradient, and the crystal orientation of the material need to be comprehensively considered.

[0089] Secondly, the critical distance is determined along the stress gradient direction at the fatigue fracture hazard point. The critical distance refers to the distance from the fatigue fracture hazard point to a point along the stress gradient direction, where the stress value represents the equivalent average stress level within the fatigue hazard region. The magnitude of the critical distance is related to the material's fatigue performance parameters and geometric correction parameters. In one specific embodiment, the critical distance is determined according to the following formula:

[0090] in, r This is the critical distance, in mm. M These are geometric correction parameters, which are related to the specific geometry of the air film orifice 11 and the loading method. The fatigue crack propagation threshold value for the material; This represents the fatigue limit of the material under symmetrical cyclic conditions. The above formula is based on the critical distance theory in linear elastic fracture mechanics. Its physical meaning is that during the fatigue crack initiation stage, the average stress field at the crack tip within the critical distance range controls the accumulation process of fatigue damage. In practical implementation, M and The values ​​can be obtained by inferring from the experimental data or by consulting the material handbook.

[0091] Next, the maximum shear stress at the critical distance is extracted. Specifically, starting from the fatigue fracture hazard point, the critical distance is moved along the stress gradient direction at that point. r The distance is measured to reach a calculation location, and then the maximum shear stress value at that location is extracted. This maximum shear stress value is used as an equivalent parameter characterizing the stress level in the fatigue-prone region.

[0092] Finally, the maximum shear stress at the critical distance is substituted into the SN curve of the single-crystal material to obtain the predicted high-cycle fatigue life. The SN curve is a fundamental characterization of material fatigue performance, describing the relationship between stress level and fatigue life. In one specific implementation, the SN curve can be in the form of a three-parameter power function or the Basquin equation. By substituting the maximum shear stress value at the critical distance into the SN curve equation, the corresponding predicted fatigue life value can be calculated.

[0093] In some implementations, the finite element model is established through a user-defined material subroutine. The user-defined material subroutine updates the stress, slip system shear strain, reference shear stress, hardening variable, material tangential stiffness, and crystal orientation at each time increment, and outputs the simulation results based on the iterative convergence conditions.

[0094] Specifically, this user material subroutine can be implemented using the UMAT or VUMAT interface of ABAQUS software, or the USERMAT interface of ANSYS software. The subroutine's inputs include the strain increment of the current increment step, the stress state at the current moment, and the state variables. Its outputs include the updated stress state, state variables, and the material Jacobian matrix.

[0095] Within each increment step, the subroutine first calculates the shear stress in each slip system based on the strain increment of the current increment step and the stress state at the current moment. Then, it calculates the shear strain rate of each slip system based on the shear stress, and updates the reference shear stress (i.e., hardening variable) and cumulative shear strain of each slip system accordingly. Next, it calculates the stress state at the end of the current increment step based on the updated slip system state, and calculates the material Jacobian matrix (i.e., the derivative of the stress increment with respect to the strain increment) for global equilibrium iteration. Finally, it updates the crystal orientation based on the plastic rotation rate tensor. At the end of each increment step, the subroutine checks whether the convergence condition is met; if not, it continues the iterative calculation.

[0096] In one specific implementation, see Figure 14 The iterative algorithm steps of the subroutine are as follows: Step S910: Read relevant constants, including the material's elastic modulus E, shear modulus G, Poisson's ratio ν; type of active slip system; relationship between cell axis and global coordinate direction; hardening parameter m. Initial hardening modulus h_0; critical shear stress τ_0 of slip system; latent hardening ratio parameter q; iterative correlation parameters.

[0097] Step S920: Initialize relevant variables; the main variables are stress σ, strain ε, and the Jacobi matrix. Reference shear stress Shear strain Decompose shear stress τ and slip surface normal. Sliding direction Cumulative shear strain γ; Step S930: Calculate the increments of relevant variables; the increment calculation method is as follows: Introducing time increment Then, the shear strain on the α-slip system is defined. The increments are as follows:

[0098] exist Introducing linear interpolation: The interpolation parameter is 0; when it equals 0, it represents a simple Euler time integral scheme. The recommended value is 0.5-1.

[0099] Step S940, update the relevant variables, for example:

[0100] Step S950: Determine whether the iteration termination condition is met; In step S960, output the result variable and update it to the initial variable. Repeat step S910 until the total time increment reaches the preset value.

[0101] Step S970: After the total time increment reaches the preset value, the iteration ends and the calculation result is output.

[0102] In some implementations, for air-film porous structures with recast layers, the elastic and hardening parameters of the recast layer are obtained through nanoindentation tests and input into the finite element model.

[0103] Specifically, nanoindentation testing is a method for measuring the mechanical properties of materials at the micrometer scale. Multiple test points are selected in the recast layer region, and cyclic indentation loads are applied to the surface of the recast layer using a nanoindenter, recording the load-displacement curves. By analyzing the load-displacement curves, the elastic modulus and hardness of the recast layer can be calculated. Based on this, combined with microstructural observation of the recast layer (such as SEM / EBSD analysis), the hardening parameters required for the plastic constitutive model of the recast layer's crystals can be further obtained. Since the recast layer is usually a fine-grained or amorphous structure, its hardening behavior may differ significantly from that of a single-crystal matrix. Therefore, directly using matrix parameters for simulation will introduce errors. Nanoindentation testing provides a feasible technical means to obtain the true mechanical properties of the recast layer.

[0104] When the recast layer is thin (e.g., less than 20 μm), nanoindentation tests may be affected by the matrix material. In this case, a lower indentation depth (e.g., no more than 1 / 5 of the recast layer thickness) can be used, or a continuous stiffness measurement technique can be employed to eliminate matrix effects.

[0105] In some implementations, the high-temperature endurance load conditions include constant load or load conditions applied according to the load spectrum corresponding to the high-temperature endurance test. Constant load refers to maintaining a constant load amplitude during the high-temperature endurance test, which is the most common endurance test method. Load conditions applied according to the load spectrum corresponding to the high-temperature endurance test refer to reproducing the loading history of the actual endurance test during the simulation, such as not loading during the heating phase, gradually loading to the target load after reaching the target temperature and maintaining it constant, etc.

[0106] High-cycle fatigue loading conditions include cyclic loading or loading conditions applied according to the load spectrum corresponding to high-cycle fatigue tests. Cyclic loading can be alternating loads in the form of sine waves, triangular waves, or square waves, with loading frequencies typically high (e.g., 10Hz to 1000Hz). Load conditions applied according to the load spectrum corresponding to high-cycle fatigue tests refer to reproducing the loading history of the actual fatigue test during the simulation, such as cyclic loading at a certain stress ratio (minimum stress / maximum stress) and frequency. In finite element simulations of crystal plasticity, one or more typical cycles can usually be selected for simulation, and the amplitude and average value of the shear stress under the cyclic steady state can be extracted as input parameters for fatigue life prediction.

[0107] In some embodiments, a life prediction system for a single-crystal film-forming porous structure 1 is provided for performing any of the prediction methods described above. The system includes: a morphology parameter acquisition module, a geometric model establishment module, a finite element model establishment module, a crystal plastic constitutive model establishment module, a crystal plastic finite element calculation module, a life relationship determination module, and a life prediction module.

[0108] The morphology parameter acquisition module is used to acquire the hole edge damage morphology parameters of the single-crystal film-forming hole structure 1 to be predicted. These parameters include at least one of the following: roundness parameter of the film-forming hole 11, thickness parameter of the recast layer formed by electrical discharge machining, and depth parameter of the prismatic machining marks formed by femtosecond laser drilling. This module can acquire measurement data through a communication interface with the measuring equipment, or receive measurement data input by the user through a human-machine interface.

[0109] The geometric model building module is used to build a geometric model of the single-crystal film-forming hole structure 1 containing the corresponding hole edge damage morphology based on the hole edge damage morphology parameters. This module uses a parametric modeling method to modify the basic film-forming hole 11 model according to the input morphology parameters, generating a three-dimensional geometric model containing the actual damage morphology.

[0110] The finite element model building module is used to build a finite element model based on the geometric model of the single-crystal film-forming porous structure 1, and to perform finite element characterization on at least one of the single-crystal matrix, recast layer, roundness error, and prismatic machining marks. This module is responsible for mesh generation, material property assignment, and boundary condition setting.

[0111] The Crystal Plastic Constitutive Model Establishment Module is used to establish crystal plastic constitutive models for nickel-based single-crystal materials. These models describe the shear stress response of each slip system under high-temperature creep loading and high-cycle fatigue loading. This module can store various types of constitutive models for users to choose from, or import user-defined constitutive models through the user material subroutine interface.

[0112] The Crystal Plasticity Finite Element Calculation Module is used to obtain the shear stress parameters of the slip system in the hole edge region of a single-crystal film-forming hole structure based on the finite element model and the crystal plasticity constitutive model. This module is responsible for calling the finite element solver to perform the calculation and outputting the required stress, strain, and shear stress results.

[0113] The life relationship determination module is used to establish the correspondence between high-temperature creep life and the maximum shear stress of the slip system based on the results of high-temperature creep test, and to establish the correspondence between high-cycle fatigue life and the maximum shear stress at the critical distance based on the results of high-cycle fatigue test. This module can automatically determine the parameters of the correspondence through regression analysis of the test data.

[0114] The life prediction module is used to determine the high-temperature creep life and high-cycle fatigue life of the single-crystal film pore structure 1 to be predicted, based on the shear stress parameters of the slip system, the correspondence between high-temperature creep life and high-cycle fatigue life. This module substitutes the finite element simulation results into the correspondence and outputs the predicted creep life and fatigue life values.

[0115] In some embodiments, an electronic device is provided, including a processor and a memory communicatively connected to the processor. The memory stores a program that, when executed by the processor, causes the electronic device to perform the lifetime prediction method for the single-crystal film porous structure 1 described above. The electronic device can be a desktop computer, laptop computer, workstation, or cloud server, or other device with computing capabilities.

[0116] In some embodiments, a computer-readable storage medium is provided, on which a computer program is stored. When the computer program is run on a processor, it causes the processor to execute any of the above-described methods for predicting the lifetime of a single-crystal film-forming porous structure. The computer-readable storage medium may be a read-only memory (ROM), random access memory (RAM), disk, optical disk, solid-state drive (SSD), or flash memory, as long as it can store a computer program and be read by a computer.

[0117] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.

[0118] In this application, the term "multiple" refers to two or more. The terms "first," "second," etc., are used for descriptive purposes only to distinguish different elements and should not be construed as indicating or implying relative importance, order, or hierarchy. The terms "connect," "install," "fix," etc., should be interpreted broadly. For example, "connect" can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection or an indirect connection through an intermediate medium. The terms "based on," "in response to," and "according to" are used to specify the triggering condition or basis for an action or event, but unless explicitly stated, other triggering conditions or bases are not excluded. The term "and / or" is used to describe the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone.

[0119] In this application, descriptions of positional or numerical relationships such as "substantially the same," "substantially parallel," "substantially perpendicular," and "substantially identical" include, unless otherwise stated, the permissible range of machining, assembly, installation, and measurement errors known in the art. For example, "substantially the same" can mean that the difference between the two is within an acceptable tolerance range relative to a reference value, which depends on the specific technical field and engineering requirements.

[0120] In this application, descriptions and embodiments guided by terms such as "exemplary," "for example," "in one specific embodiment," "optionally," and "in other embodiments" are merely illustrative of the technical solutions of this application and should not be construed as limiting the scope of protection of this application. Unless explicitly stated otherwise, the specific parameters, values, materials, or steps in these embodiments are exemplary, and those skilled in the art can select appropriate implementation methods according to actual needs and specific application scenarios after reading this application.

[0121] In this application, the same or similar parts between the various embodiments can be referred to mutually. Each embodiment focuses on the differences from other embodiments, but the technical features between different embodiments can be combined with each other without contradicting each other to form new implementations. Unless the order of the method steps described in this application is explicitly stated or obviously understood from the context, it should not be construed as having to be performed in the described order. Some steps can be performed in parallel, repeatedly, or in a different order.

[0122] In this application, when referring to numerical ranges, unless otherwise stated, the range includes its endpoints as well as all subranges and specific values ​​within the range. For example, "20 to 50 times" includes 20 times, 50 times, and all integer and non-integer multiples of values ​​between 20 and 50 times.

[0123] The above description of the disclosed embodiments enables those skilled in the art to make or use this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

[0124] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on its differences from other embodiments. Similar or identical parts between embodiments can be referred to interchangeably. All numerical values, parameters, and material types involved in the embodiments of this application are illustrative and can be adjusted according to specific needs in practical applications. The scope of protection of this application is determined by the claims, and the specification and accompanying drawings are used to interpret the content of the claims.

Claims

1. A method for predicting the lifespan of a single-crystal film-forming porous structure, characterized in that, include: Obtain the hole edge damage morphology parameters of the single crystal film pore structure to be predicted. The hole edge damage morphology parameters are used to characterize the geometric morphology, surface layer structure or local processing damage of the film pore wall. Based on the hole edge damage morphology parameters, the hole wall of the air film hole is parametrically characterized, and a geometric model of the single crystal air film hole structure containing the hole edge damage morphology is established. A finite element model is established based on the geometric model, and the single crystal matrix material parameters and the surface layer or local damage region parameters corresponding to the hole edge damage morphology are set in the finite element model. A crystal plastic constitutive model for nickel-based single crystal materials is established. This model is used to describe shear deformation, hardening behavior, and shear stress response in different slip systems. High-temperature sustained load and high-cycle fatigue load conditions were applied to the finite element model respectively to perform crystal plasticity finite element simulation and obtain the shear stress parameters of each slip system in the edge region of the air film hole. Based on the results of high-temperature creep test, a correlation was established between high-temperature creep life and maximum shear stress of slip system, and based on the results of high-cycle fatigue test, a correlation was established between high-cycle fatigue life and shear stress parameters in fatigue critical area. Substituting the shear stress parameters into the high-temperature creep life correspondence and the high-cycle fatigue life correspondence respectively, the high-temperature creep life prediction and high-cycle fatigue life prediction of the single-crystal film pore structure are obtained.

2. The prediction method as described in claim 1, characterized in that, The drilling process for the single-crystal gas film pore structure to be predicted includes at least one of electrical discharge drilling and femtosecond laser drilling.

3. The prediction method as described in claim 1, characterized in that, The hole edge damage morphology parameters include at least one of the following: The parameters of the film pore roundness, pore diameter deviation, pore wall roughness, recast layer thickness formed by electrical discharge drilling, depth of prismatic machining marks formed by femtosecond laser drilling, depth of striped machining marks, depth of ridged machining marks, microcrack characteristic parameters, and heat-affected zone size parameters.

4. The prediction method as described in claim 3, characterized in that, The roundness parameter of the air film orifice is obtained by measuring the minimum circumscribed circle diameter and the maximum inscribed circle diameter of the air film orifice cross section; Wherein, the roundness parameter of the i-th air film pore Determined according to the following formula: Average roundness parameters of multiple air film pores Determined according to the following formula: in, The roundness of the i-th air film pore ( i =1, 2…n), μm; , Let be the minimum circumcircle diameter and the maximum incircle diameter of the i-th air film pore, respectively, in μm.

5. The prediction method as described in claim 3, characterized in that, The thickness of the recast layer is obtained by measuring multiple detection locations at the inlet, middle, and outlet sections of the film gas vent, and the average thickness of the recast layer is... ξ Determined according to the following formula: in, The thickness measurement value at the i-th recast layer detection location, in μm ( i= 1, 2… n ).

6. The prediction method as described in claim 3, characterized in that, The average depth of the prismatic, striped, or ridged machining marks η Determined according to the following formula: in, Let be the depth measurement value at the i-th machining mark detection location, in μm ( i= 1, 2… n ).

7. The prediction method as described in claim 1, characterized in that, Establishing the geometric model includes: A basic three-dimensional model is established based on the actual structural dimensions of the single-crystal film pore structure. The contour of the air film orifice wall is parametrically adjusted based on the roundness parameter of the air film orifice. Based on the thickness of the recast layer, a geometric layer or equivalent surface layer of the recast layer is established on the surface of the air film pore wall. Based on the depth of the machining marks, a local geometric undulation structure is established on the surface of the air film pore wall.

8. The prediction method as described in claim 1, characterized in that, Establishing the finite element model includes: Solid units are used to mesh the single-crystal substrate; For air-film porous structures containing recast layers, a recast layer grid is established on the surface of the air-film porous wall, and the recast layer is characterized by shell unit thickness, solid thin layer thickness or equivalent material layer parameters. For air film hole structures with roundness errors or local machining marks, explicit geometric modeling is performed on the air film hole wall contour and local machining marks.

9. The prediction method as described in claim 1, characterized in that, The crystal plastic constitutive model includes the slip system shear strain rate equation, the slip system hardening equation, the slip system partial shear stress calculation equation, and the crystal orientation update equation; The shear strain rate equation of the slip system is determined according to the following formula: The hardening equation of the slip system is determined according to the following formula: The equation for calculating the shear stress of the slip system is determined according to the following formula: The crystal orientation update equation is determined according to the following formula: in, The shear strain rate of the single-crystal slip system; Reference shear strain rate; Reference shear stress; m is the strain rate exponent; A is the hardening rate coefficient; p is the time hardening exponent; The hardening modulus represents the hardening effect of the slip shear of slip system β on slip system α. H is the self-hardening modulus; q is the potential hardening ratio parameter.

10. The prediction method as described in claim 9, characterized in that, The component shear stress on the slip system α is determined by the following formula: in, The shear stress is the partial stress on the α-slip system. σ is the Cauchy stress tensor; The orientation factor for the slip system α of nickel-based single crystal materials can be calculated by the following formula; in, Let α be the direction vector of the sliding system. Let be the unit normal vector of the slip surface where slip system α is located.

11. The prediction method as described in claim 9, characterized in that, Under finite deformation conditions, the plastic velocity gradient is superimposed according to the shear strain rate of each slip system and decomposed into the plastic deformation rate tensor and the plastic rotation rate tensor. The shear strain rate of the slip system α and the macroscopic deformation rate of the specimen are related as follows: In the formula: For the plastic velocity gradient tensor; Decomposing the velocity gradient tensor yields the following relationship: In the formula: For the plastic deformation rate tensor; For plastic rotation rate tensor; The orientation rotation factor can be calculated using the following formula: The relationship between shear strain rate and stress rate on slip system α is as follows: In the formula: The Jaumann derivative of the Kirchhoff stress tensor for the current configuration; Let EMT be the instantaneous elastic modulus tensor. The instantaneous elastic modulus tensor EMT can be expressed by the following equation: In the formula: , and These are three independent elastic constants, which are related to the elastic modulus E, Poisson's ratio ν, and shear modulus G.

12. The prediction method as described in claim 1, characterized in that, The relationship between high-temperature creep life and maximum shear stress of the slip system is as follows: in, For long lifespan, is the maximum shear stress of the slip system, and B and N are creep parameters.

13. The prediction method as described in claim 1, characterized in that, Establishing the correspondence between high-cycle fatigue life and the shear stress parameters within the fatigue critical region includes: Identify the fatigue fracture risk points at the edges of the air film pores; Determine the critical distance along the stress gradient direction at the fatigue fracture hazard point; Extract the maximum shear stress at the critical distance; Substituting the maximum shear stress at the critical distance into the SN curve of the single crystal material, the high-cycle fatigue prediction life is obtained.

14. The prediction method as described in claim 13, characterized in that, The critical distance Maximum shear stress at The relationship is as follows: In the formula: This represents the threshold value amplitude of the stress intensity factor. R represents the fatigue limit when the stress ratio R = -1; M is the geometric correction parameter. As the critical distance, at the fatigue fracture hazard point, the maximum shear stress value at a distance r from the hazard point is taken along the stress gradient direction as the equivalent average stress level in the hazard area, and this maximum shear stress value is substituted into the SN curve of the single crystal material to obtain the high cycle fatigue life of the film pore structure.

15. The prediction method as described in claim 1, characterized in that, The finite element model is established through a user material subroutine. The user material subroutine updates the stress, slip system shear strain, reference shear stress, hardening variable, material tangential stiffness, and crystal orientation at each time increment, and outputs the simulation results according to the iterative convergence conditions.

16. The prediction method as described in claim 1, characterized in that, For air-film porous structures with recast layers, the elastic and hardening parameters of the recast layers are obtained through nanoindentation tests and input into the finite element model.

17. The prediction method as described in claim 1, characterized in that, The high-temperature endurance load conditions include constant loads or load conditions applied according to the load spectrum corresponding to the high-temperature endurance test; The high-cycle fatigue load conditions include periodic loads or load conditions applied according to the load spectrum corresponding to the high-cycle fatigue test.

18. A life prediction system for a single-crystal film-forming porous structure, characterized in that, include: The morphology parameter acquisition module is used to acquire the hole edge damage morphology parameters of the single crystal gas film hole structure to be predicted. The hole edge damage morphology parameters include at least one of the following: gas film hole roundness parameter, recast layer thickness parameter formed by electrical discharge drilling, and prism processing mark depth parameter formed by femtosecond laser drilling. The geometric model building module is used to build a geometric model of a single-crystal gas film hole structure containing the corresponding hole edge damage morphology based on the hole edge damage morphology parameters. The finite element model building module is used to build a finite element model based on the geometric model of the single crystal film pore structure, and to perform finite element characterization on at least one of the single crystal substrate, recast layer, roundness error and prismatic machining marks. The crystal plastic constitutive model establishment module is used to establish a crystal plastic constitutive model of nickel-based single crystal materials. The crystal plastic constitutive model is used to describe the shear stress response of each slip system of the single crystal material under high temperature endurance load and high cycle fatigue load. The crystal plasticity finite element calculation module is used to obtain the slip system shear stress parameters of the hole edge region of the single crystal gas film hole structure based on the finite element model and the crystal plasticity constitutive model. The life relationship determination module is used to establish the correspondence between high-temperature creep life and maximum shear stress of slip system based on the results of high-temperature creep test, and to establish the correspondence between high-cycle fatigue life and maximum shear stress at critical distance based on the results of high-cycle fatigue test. as well as The life prediction module is used to determine the high-temperature creep life and high-cycle fatigue life of the single crystal film pore structure to be predicted based on the shear stress parameters of the slip system, the correspondence between high-temperature creep life and high-cycle fatigue life.

19. An electronic device, characterized in that, include: processor; as well as The memory is communicatively connected to the processor; The memory stores a program, which, when executed by the processor, causes the electronic device to perform the single-crystal air-film porous structure lifetime prediction method according to any one of claims 1 to 17.

20. A computer-readable storage medium having a computer program stored thereon, characterized in that, When the computer program is run on the processor, it causes the processor to execute the life prediction method for single-crystal air film porous structures according to any one of claims 1 to 17.