A plasma processing device and its cavity stabilization method
By performing hydration sealing and vacuum baking on the surface of the inner liner of the semiconductor plasma processing equipment, a dense gamma alumina layer is formed, and an alumina cap layer and a silicon oxide layer are deposited on it. This solves the stability problem of the inner wall of the cavity in a highly active plasma environment, and achieves stability of the hydrogen production process and extension of the inner wall life.
Patent Information
- Application Number
- CN202611467364.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-17
AI Technical Summary
Even after the anodic aluminum oxide coating seals the inner wall of the semiconductor plasma processing equipment, pores still exist. This leads to the loss of the inner wall surface layer under the highly active H-containing plasma and free radical environment, resulting in particle shedding and affecting the stability of the hydrogen production process.
A hydrated alumina layer is formed by hydrating and sealing the anodic alumina layer on the surface of the liner, and a dense gamma alumina layer is formed by vacuum baking. An alumina cap layer and a non-stoichiometric silicon oxide layer are then formed on its surface by atomic layer deposition, thus constructing a multi-layer dense stacked structure to improve stability.
It effectively avoids the source of particle generation, improves the stability of the cavity wall in a hydrogen-containing plasma environment, maintains the stability of hydrogen free radical concentration, and extends the service life of the cavity inner wall.
Smart Images

Figure CN123120594A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor processing technology, and in particular to a plasma processing device and a cavity stabilization method thereof. Background Technology
[0002] If the inner wall material (lining) of the reaction chamber in a semiconductor plasma processing device is made of aluminum, a hard oxide coating (anodized aluminum oxide layer) is typically added to its surface. Compared to the bare aluminum surface, the addition of a hard oxide coating can, to some extent, reduce the bombardment and erosion damage of plasma (hydrogen process) on the inner wall surface (the hard oxide coating thickness can reach tens of micrometers, approximately 15,000 times the thickness of the natural oxide layer, and its density is approximately 5 times that of the natural oxide layer, theoretically enhancing the protection of the underlying aluminum by nearly 5 orders of magnitude). When the inner wall surface of the chamber is eroded by H free radicals, it releases aluminum oxide rather than metallic Al, thus providing a certain degree of protection. However, the anodized aluminum oxide coating has nanopores, which can significantly adsorb water vapor, reaction gases, and byproduct residues, affecting the stability of the H free radical concentration. Therefore, the anodized aluminum oxide coating is also subjected to surface sealing treatment to reduce the vertical capillary / honeycomb porosity in the anodized aluminum oxide coating. However, even after sealing, some porosity usually remains. In a highly active H-containing plasma and free radical environment, this can still cause some loss of the inner wall surface of the cavity, leading to particle shedding and instability in the H free radical concentration, which in turn affects the instability of the hydrogen production process results. Therefore, it is necessary to study a process method that can significantly improve the above problems. Summary of the Invention
[0003] The purpose of this application is to overcome the aforementioned problems in the prior art and provide a plasma processing device and its cavity stabilization method for use in hydrogen production processes to improve the stability of H radical concentration and improve particulate defects.
[0004] To achieve the above objectives, the technical solution of this application is as follows: According to a first aspect of this application, embodiments of this application provide a cavity stabilization method for a plasma processing apparatus, comprising: A liner for a plasma processing equipment cavity is provided. The liner is made of aluminum alloy and has an anodized aluminum layer on its working side surface. Using water vapor, the surface of the anodic aluminum oxide layer is hydrated and sealed to form a hydrated aluminum oxide layer on the surface of the anodic aluminum oxide layer. Vacuum baking is performed to cause the hydrated alumina layer to undergo dehydration condensation and phase transformation reaction, forming a dense gamma alumina layer. An alumina cap layer is formed on the surface of the gamma alumina layer using an atomic layer deposition process. The liner is installed on the inner wall of the cavity; Hexamethyldisiloxane carried by a carrier gas bubble and excess oxygen are introduced into the cavity, and plasma mode is activated to react on the surface of the alumina cap layer to form a first silicon oxide layer with a non-stoichiometric ratio. A first mixture of hydrogen and nitrogen gas is introduced into the cavity, and plasma mode is activated to perform the hydrogen process.
[0005] In some embodiments, the method further includes: after performing the hydration sealing treatment, using a nitric acid solution to de-ash the surface of the liner.
[0006] In some embodiments, the method further includes: before forming the first silicon oxide layer, introducing oxygen into the cavity and activating the plasma mode to activate the surface of the aluminum oxide cap layer.
[0007] In some embodiments, the method further includes: after forming the first silicon oxide layer, introducing a second mixed gas of hydrogen and nitrogen into the cavity and activating plasma mode to stabilize the first silicon oxide layer.
[0008] In some embodiments, the water vapor is prepared using deionized water, and triethanolamine is added to the water vapor. The water vapor has a conductivity of less than 2 μS / cm and a chloride ion content of less than 1 ppm. The amount of triethanolamine added is 0.5 g / L to 2 g / L. When performing the hydration sealing treatment, the temperature is 100℃ to 115℃, the pressure is 0.02 MPa to 0.05 MPa, and the time is 2 min / μm to 3 min / μm.
[0009] In some embodiments, an ultrasonic-assisted descaling treatment is performed on the surface of the liner using a nitric acid solution with a volume concentration of 15% to 20%, at a temperature of 20°C to 25°C, an ultrasonic frequency of 35kHz to 45kHz, and a time of 30s to 60s.
[0010] In some embodiments, the vacuum baking process is performed when the vacuum degree is less than 1×10⁻⁶. -3 Torr, with a heating rate of 2℃ / min to 5℃ / min, a first plateau temperature of 200℃ to 350℃, a first plateau holding time of 50min to 70min, a second plateau temperature of 450℃ to 550℃, a second plateau holding time of 2 hours to 4 hours, a cooling rate of less than 5℃ / min, and a furnace exit temperature of less than 100℃.
[0011] In some embodiments, when forming the alumina cap layer, the first precursor includes trimethylaluminum, the second precursor includes H2O, the temperature is 200℃~250℃, the number of cycles is 300 to 500, the introduction time of the first precursor is 0.05s~0.1s in each cycle, the introduction time of the second precursor is 0.05s~0.1s, and the single purging time is 10s~20s.
[0012] In some embodiments, the thickness of the alumina cap layer is 30 nm to 50 nm.
[0013] In some embodiments, the method further includes: after forming the alumina cap layer, performing in-situ vacuum annealing at a temperature of 280°C to 320°C for 1 to 2 hours.
[0014] In some embodiments, when performing the hydrogen process, the hydrogen flow rate in the first mixed gas is greater than 4% to 40%, and the nitrogen flow rate is less than 96% to 60%.
[0015] In some embodiments, during the hydrogen production process, the concentration of hydrogen free radicals and the number of particles are monitored. If either exceeds the limit, the hydrogen production process is paused, and hexamethyldisiloxane carried by a carrier gas bubble and excess oxygen are introduced into the cavity again. The plasma mode is then activated to react on the surface of the first silicon oxide layer to form a second silicon oxide layer with a non-stoichiometric ratio. A second mixed gas of hydrogen and nitrogen is introduced into the cavity, and the plasma mode is activated to stabilize the second silicon oxide layer. Then, the hydrogen production process is resumed, and when a threshold is triggered, the machine is stopped and the liner is replaced.
[0016] In some embodiments, the threshold includes the cumulative number of times the second silicon oxide layer is formed reaching 3 to 5 times, or the cumulative duration of the hydrogen process reaching 500 to 1000 hours.
[0017] In some embodiments, when forming the first silicon oxide layer and the second silicon oxide layer, the flow ratio of the introduced oxygen to the hexamethyldisiloxane carried by the carrier gas bubble is 8 or more.
[0018] In some embodiments, the carbon content in the first silicon oxide layer and the second silicon oxide layer is less than 5 at.
[0019] In some embodiments, when forming the first silicon oxide layer and the second silicon oxide layer, the flow rate of hexamethyldisiloxane carried by the carrier gas bubbling is 20 SCCM to 100 SCCM, the flow rate of oxygen is 200 SCCM to 1000 SCCM, the pressure is 200 mTorr to 500 mTorr, the source power is 300 W to 800 W, the bias power is 0 W, and the temperature is 150 °C to 300 °C.
[0020] In some embodiments, the reaction time for forming the first silicon oxide layer is 10 min to 40 min, or the thickness of the first silicon oxide layer is 50 nm to 150 nm.
[0021] In some embodiments, the reaction time for forming the second silicon oxide layer is 10 min to 15 min, or the thickness of the second silicon oxide layer is 30 nm to 50 nm.
[0022] In some embodiments, during the activation process, the oxygen flow rate is 300 SCCM to 800 SCCM, the pressure is 200 mTorr to 500 mTorr, the source power is 300 W to 1000 W, the bias power is 0 W, the temperature is 150 °C to 250 °C, and the time is 5 min to 15 min.
[0023] In some embodiments, during the stabilization treatment, the hydrogen flow rate in the second mixed gas is less than 4%, the nitrogen flow rate is more than 96%, the nitrogen flow rate is 480 SCCM to 520 SCCM, the pressure is 200 mTorr to 400 mTorr, the source power is 200 W to 500 W, the bias power is 0 W, the temperature is 150 °C to 250 °C, and the time is 5 min to 15 min.
[0024] According to a second aspect of this application, embodiments of this application also provide a plasma processing apparatus, including a cavity, wherein an inner liner is provided on the inner wall of the cavity, and the inner liner is obtained using a cavity stabilization method for a plasma processing apparatus as provided in any of the embodiments of the first aspect above.
[0025] The embodiments of this application may have, or at least have, the following advantages: (1) By performing hydration sealing treatment on the anodic aluminum oxide layer on the surface of the liner to form a hydrated alumina (boehmite) layer, and then causing the hydrated alumina layer to undergo dehydration condensation and phase transformation reaction to form a dense gamma alumina (γ-Al2O3) layer, the harmful phase transformation that will inevitably occur during the service of the liner in the cavity (hydrated alumina will inevitably undergo dehydration shrinkage-stress drift-microcracks-particle generation at the working temperature of 150℃~500℃ in the cavity) can be completed and cured in advance by a vacuum baking treatment. This allows the cavity wall after the liner is installed to enter a thermodynamically stable state before the plasma treatment process (from "passively enduring wall aging" to "actively eliminating aging sources"). This effectively avoids the source of particle generation and improves the stability of the cavity wall in a hydrogen-containing plasma environment. Furthermore, a high-density alumina cap layer and a first silicon oxide layer (SiO2-like inorganic film) with an etching rate far lower than that of carbon films under hydrogen radical etching during hydrogen processing are further formed on the surface of the densified anodic alumina layer using atomic layer deposition. x This allows the chemical properties of the protective film on the wall to be compatible with the hydrogen process, and the hydroxylation state of the surface of the first silicon oxide layer can be stably maintained by the water vapor / hydrogen plasma environment, so that the recombination consumption of hydrogen free radicals on the wall becomes an approximately constant value.
[0026] (2) By introducing excess oxygen during the formation of the first / second silicon oxide layer, the carbon content in the first / second silicon oxide layer is ensured to be less than 5 at%, significantly reducing the etching damage to the wall surface caused by hydrogen free radicals during the hydrogen process, greatly reducing particle shedding, and effectively maintaining the constant wall surface state, thereby stabilizing the amount of hydrogen free radicals reaching the wafer during the hydrogen process. After the formation of the first / second silicon oxide layer, a second mixed gas of hydrogen and nitrogen with low hydrogen content is introduced into the cavity to stabilize the first / second silicon oxide layer. The nitrogen-hydrogen plasma with low hydrogen content can be used to eliminate the Si-H / Si-OH dangling bonds inside the first / second silicon oxide layer film and remove weakly adsorbed fragments. Therefore, by forming a silicon oxide layer online as a passivation protective film on the wall surface, the density of the protective layer on the inner wall surface is improved, effectively reducing the probability of hydrogen plasma / free radicals invading the inner wall surface layer. This reduces the residue and reaction inside the porous structure of the anodic aluminum oxide layer, improves the concentration stability of hydrogen free radicals in the cavity, and achieves the stabilization of the cavity under hydrogen processing.
[0027] (3) By repeatedly forming a second silicon oxide layer on the surface of the first silicon oxide layer whenever the monitored value exceeds the limit during the hydrogen production process, the wall film layer is regenerated, and the cavity is renewed and protected, thus avoiding the long-term effects of hydrogen and significantly extending the service life of the cavity inner wall. When the threshold is triggered, the liner is replaced by stopping the machine and a brand-new silicon oxide layer is rebuilt on the cavity wall, maintaining the long-term stability of the cavity operation.
[0028] Other advantages of this application will be described in the following detailed description. Attached Figure Description
[0029] Figure 1 This is a flowchart of a cavity stabilization method for a plasma processing device provided in a preferred embodiment of this application.
[0030] Figure 2 This is a schematic diagram of the structure of a plasma processing device provided in a preferred embodiment of this application.
[0031] In the diagram: 10. Cavity; 11. Inner wall; 12. Air inlet; 13. Heating platform; 14. Exhaust port. Detailed Implementation
[0032] To address the issue that even after sealing, the surface of the anodic aluminum oxide layer on the aluminum liner of a plasma processing device cavity still retains some porosity, which, under highly active H-containing plasma and free radical environments, still causes some loss of the cavity inner wall surface, leading to particle shedding and unstable H free radical concentration, thus affecting the instability of hydrogen production process results, this application provides a cavity stabilization method for a plasma processing device, comprising the following steps: A liner for a plasma processing equipment cavity is provided. The liner is made of aluminum alloy and has an anodized aluminum layer on its working side surface. Using water vapor, the surface of the anodic aluminum oxide layer is hydrated and sealed to form a hydrated aluminum oxide layer on the surface of the anodic aluminum oxide layer. Vacuum baking is performed to cause the hydrated alumina layer to undergo dehydration condensation and phase transformation reaction, forming a dense gamma alumina layer. An alumina cap layer is formed on the surface of the gamma alumina layer using an atomic layer deposition process. The liner is installed on the inner wall of the cavity; Hexamethyldisiloxane carried by a carrier gas bubble and excess oxygen are introduced into the cavity, and plasma mode is activated to react on the surface of the alumina cap layer to form a first silicon oxide layer with a non-stoichiometric ratio. A first mixture of hydrogen and nitrogen gas is introduced into the cavity, and plasma mode is activated to perform the hydrogen process.
[0033] This application embodiment involves steam hydration sealing of the anodic aluminum oxide layer on the surface of the liner to form a hydrated alumina (boehmite) layer. Vacuum baking then causes dehydration condensation and phase transformation reactions in the hydrated alumina layer, forming a dense gamma-alumina (γ-Al2O3) layer. This process pre-completes and solidifies the harmful phase transformation that inevitably occurs during the liner's service life in the cavity, ensuring the cavity wall is thermodynamically stable before plasma treatment, effectively mitigating particle generation at its source. Furthermore, atomic layer deposition (ALD) is used to form an alumina cap layer and a first silicon oxide layer (SiO2-like inorganic film) on the dense gamma-alumina layer. This first silicon oxide layer has a much lower etching rate under hydrogen radicals during hydrogen processing compared to carbon films. x This allows the chemical properties of the wall protection film to be compatible with hydrogen processes, and forms a nearly carbon-free, all-inorganic wall protection system with a multi-layered, dense, stacked structure. This improves the concentration stability of H free radicals in the cavity and achieves the stabilization of the cavity under hydrogen-containing plasma processes.
[0034] This application also provides a plasma processing device, including a cavity, the inner wall of which is provided with an inner liner, the inner liner being obtained using the cavity stabilization method of the plasma processing device described above.
[0035] The specific embodiments of this application will now be described in detail with reference to the accompanying drawings.
[0036] refer to Figure 1 In a first aspect, embodiments of this application provide a cavity stabilization method for a plasma processing apparatus, which may sequentially include the following steps: Step S11: Provide a liner for the plasma processing equipment cavity, wherein the working side surface of the liner has an anodic aluminum oxide layer.
[0037] refer to Figure 2 In some embodiments, a cavity stabilization method for a plasma processing apparatus according to this application can be used to improve the cavity wall stability of a plasma processing apparatus (e.g., a plasma debinding apparatus or a plasma surface treatment apparatus) and enhance the process stability of the plasma processing apparatus cavity. The plasma processing apparatus includes a cavity 10, which can be used to perform a plasma processing process (hydrogen process) using a hydrogen-containing gas (e.g., H2) as the base process gas.
[0038] In some embodiments, the cavity 10 has an inner wall 11, on which a liner (not shown) is applied. The working side surface of the liner facing the cavity constitutes the inner wall surface of the cavity 10. The liner is made of aluminum alloy, and at least the working side of the aluminum alloy surface has an anodized aluminum layer (hard oxide coating). A hot stage 13 is provided in the cavity 10 for placing production wafers (product wafers) to be processed in the plasma processing process, and for maintaining the process temperature during processing by heating and temperature control. An air inlet 12 is provided on the top of the cavity 10 for introducing an excitation gas (a rare gas, such as one or more inert gases like He, Ne, Ar, Kr, etc.) and a process gas used in the plasma processing process (hydrogen process) (including a first mixed gas of H2 and N2, etc.). The process gas entering the cavity 10 can be excited by the excitation gas in the cavity to form plasma, which is used to process the production wafers placed on the hot stage 13. The air inlet 12 is also used to introduce oxygen, hexamethyldisiloxane carried by the carrier gas bubble, and a second mixed gas of H2 and N2 used in the embodiments of this application. These gases are excited by the excitation gas to form plasma, which is used to treat the working side surface of the liner laid on the inner wall of the cavity. An exhaust port 14 is provided at the bottom of the cavity 10 for discharging waste gas and controlling the cavity pressure.
[0039] Step S12: Use water vapor to perform a hydration sealing treatment on the surface of the anodic aluminum oxide layer, forming a hydrated aluminum oxide layer on the surface of the anodic aluminum oxide layer.
[0040] Before installing the liner with an anodized aluminum layer on its working side surface onto the inner wall 11 of the cavity 10, the surface of the liner in its component state is treated as follows to form a highly dense protective film layer on its surface. Then, the liner is installed onto the inner wall 11 of the cavity 10 to improve the stability of hydrogen free radical concentration and reduce particulate defects during the hydrogen production process in the cavity.
[0041] In some embodiments, water vapor is used to perform a hydration sealing treatment (pressurized steam sealing treatment) on the surface of the anodic aluminum oxide layer on the offline liner. The water vapor reacts with the porous alumina (Al₂O₃) on the surface of the anodic aluminum oxide layer to form a hydrated alumina (boehmite, AlOOH) layer. The reaction formula is as follows: Al₂O₃ + H₂O → 2AlOOH Hydrated alumina (boehmite) is a hydroxyl oxide containing structural water and exhibiting a hydrogen-bonded layered structure with low density. Boehmite has an orthorhombic crystal system and a layered structure (AlO6 octahedrons form double-layered structures with shared edges, connected by hydrogen bonds between layers). These interlayer hydrogen bonds are the root cause of its "soft, loose, and scalable" structure. During hydration sealing, it relies on its crystallization and growth within the pores to fill the voids.
[0042] When the porous amorphous anodic aluminum oxide film comes into contact with water vapor, a dissolution-precipitation crystallization process will occur: "surface hydroxylation → weak dissolution of aluminum species → supersaturation in the pores and reprecipitation and crystallization into AlOOH → volume expansion of 30% to 50%, thus wedging the pores".
[0043] Anodized aluminum layers typically have a porous structure with vertical capillary / honeycomb-like nanopores (channels) on their surface. By using water vapor for hydration sealing treatment, the pores on the surface of the anodized aluminum layer can be thoroughly sealed, and the formation of surface flocculent matter can be reduced.
[0044] In some embodiments, prior to hydration sealing, an alkaline cleaning agent (pH=9-10) can be used to ultrasonically degrease the surface of the liner (pretreatment) at a temperature of 45°C-55°C (e.g., 50°C) for 8-12 minutes (e.g., 10 minutes). Afterward, three ultrasonic rinses can be performed using deionized water. Following rinsing, the liner is dried with nitrogen and then baked at 75°C-85°C (e.g., 80°C) for 25-35 minutes (e.g., 30 minutes).
[0045] In some embodiments, pressurized steam sealing (hydration sealing) is performed on the surface of the anodized aluminum layer on the liner using water vapor mixed with an anti-fouling agent. Here, the conventional boiling water immersion method is avoided to reduce the formation of surface flocculent material.
[0046] In some embodiments, the water vapor is prepared using deionized water, and the water vapor has an electrical conductivity of less than 2 μS / cm and a chloride ion content of less than 1 ppm.
[0047] In some embodiments, the anti-fouling agent includes triethanolamine. The amount of triethanolamine added to the water vapor is 0.5 g / L to 2 g / L. By adding the anti-fouling agent to the water vapor, the formation of surface flocculent matter can be effectively reduced.
[0048] In some embodiments, during the hydration sealing treatment, the temperature is 100℃~115℃, the pressure is 0.02MPa~0.05MPa (gauge pressure), and the time is 2min / μm~3min / μm based on the thickness of the anodized aluminum layer. During the hydration sealing treatment, it is important to avoid incomplete sealing due to insufficient sealing time, or excessive sealing time leading to an increase in surface flocculent matter.
[0049] In some embodiments, after hydration sealing, the surface of the liner (anodized aluminum layer with hydrated aluminum oxide layer) can be quickly rinsed with deionized water for 25-35 seconds (e.g., 30 seconds) and dried with nitrogen. Then, immediately (to avoid prolonged moisture absorption), the surface of the liner is subjected to ultrasonic-assisted descaling at a 15%-20% nitric acid solution at 20°C-25°C (room temperature) (to avoid excessive temperature damaging the sealed layer). The ultrasonic frequency is 35kHz-45kHz (low power to assist in peeling off residues at the orifice) for 30-60 seconds (only dissolving surface flocculent formations without damaging the filler) to remove residual ash and discoloration after sealing (no flaky / petal-like morphology on the surface), restoring the surface to a smooth finish (no ash residue when wiped with a white cloth), improving surface quality, and preventing ash stains from affecting subsequent processes. Afterwards, the surface of the liner can be ultrasonically rinsed with deionized water for, for example, three passes, and dried with nitrogen. The rinsing process can only be completed when the resistivity of the deionized water reaches 15 MΩ·cm or higher after the final ultrasonic rinsing.
[0050] Step S13: Perform vacuum baking treatment to cause the hydrated alumina layer to undergo dehydration condensation and phase transformation reaction to form a gamma alumina layer.
[0051] In some embodiments, after deashing, the liner is subjected to vacuum baking, causing the hydrated alumina in the hydrated alumina layer on the surface of the liner (anodic alumina layer) to lose structural water upon heating and undergo a gamma phase transition, transforming into a transition phase alumina (gamma alumina, γ-Al2O3), thus forming a gamma alumina layer on the surface of the anodic alumina layer (hydrated alumina layer). The reaction formula is as follows: 2AlOOH → γ-Al₂O₃ + H₂O↑ Gamma alumina has a cubic crystal system with a defective spinel structure. Oxygen ions form a cubic close-packed framework, while Al ions randomly occupy octahedral and tetrahedral voids (cation vacancy structure). Gamma alumina is a three-dimensional rigid network without interlayer hydrogen bonds, and its hardness and density are much higher than boehmite.
[0052] In some embodiments, vacuum baking processes can be performed using baking equipment such as vacuum ovens or vacuum furnaces.
[0053] In some embodiments, when performing vacuum baking, the vacuum degree is less than 1×10⁻⁶. -3 Torr, preferably with a vacuum degree less than 1×10 -4 Torr allows for faster dehydration and prevents moisture regain.
[0054] In some embodiments, when performing vacuum baking, the heating rate is 2°C / min to 5°C / min to prevent excessively rapid heating from causing stress concentration during phase transformation, which could lead to the formation of microcracks.
[0055] In some embodiments, during the vacuum baking process, two holding platforms, a first platform and a second platform, are set up during the heating phase. The temperature of the first platform (dehydration temperature) is 200℃ to 350℃, for example, 300℃; the holding time of the first platform is 50min to 70min, for example, 60min; the temperature of the second platform (phase change temperature) is 450℃ to 550℃, for example, 500℃; the holding time of the second platform is 2 hours to 4 hours, for example, 3 hours. The first platform temperature and the specific holding time allow for the thorough removal of physically adsorbed water from the hydrated alumina layer, facilitating a more complete and thorough phase change reaction at the second platform temperature. This promotes the rearrangement of the dehydrated framework into a high-density phase and the shrinkage to form a gamma-alumina layer with a continuous, dense, rigid three-dimensional network.
[0056] In some embodiments, during vacuum baking, after the second platform's heat preservation period ends, a cooling phase begins. The cooling rate is 5°C / min or less. For example, the cooling rate may be 5°C / min or less, or 4°C / min or less, or 3°C / min or less, or 2°C / min or less, or 1°C / min or less, but is not limited to these. By performing slow cooling at the aforementioned lower cooling rate, thermal stress cracking of the film layer can be prevented. The oven exit temperature is less than 100°C. For example, the oven exit temperature may be less than 100°C, or less than 90°C, or less than 80°C, or less than 70°C, or less than 50°C, or less than 30°C, or less than 10°C, but is not limited to these.
[0057] The microscopic processes (topological transformations) of boehmite phase transitions may include: (1) At a temperature of about 200℃~350℃, boehmite first removes the interlayer physically adsorbed water and some weakly bound hydroxyl groups, and the interlayer hydrogen bonds begin to break. (2) At a temperature of about 450℃~550℃, the main dehydroxylation stage is the condensation and dehydration of adjacent hydroxyl groups (2-OH →-O- + H2O↑), and the layered structure collapses; (3) The oxygen skeleton basically remains in situ rearranged (topological relationship is preserved), and Al ions are redistributed into spinel lattice sites to form γ-Al2O3.
[0058] In this embodiment, further heating (e.g., above 800°C) should be avoided to prevent the γ phase from eventually transforming into α-Al₂O₃ (corundum) via the δ / θ phase. This is because the γ phase already possesses sufficient density and chemical stability, and the α phase transformation is accompanied by a greater risk of shrinkage and cracking.
[0059] Boehmite has a density of approximately 3.0 g / cm³. 3 The density of γ-Al₂O₃ is approximately 3.5 g / cm³. 3 ~3.7g / cm 3 After dehydration, boehmite loses material (theoretically about 15% weight loss), causing the framework to shrink. The remaining framework rearranges into a high-density phase, and the flocculent / plate-like morphology collapses and shrinks into a continuous, dense body. The loose, layered structure of boehmite, supported by hydrogen bonds, transforms into a rigid three-dimensional Al-O network after the phase transition—its mechanical strength, hardness, and resistance to plasma erosion all increase significantly. This application utilizes the above-described principle. A hydrated alumina layer (boehmite layer) is formed by hydrating and sealing the surface of the anodic alumina layer of the liner. This hydrated alumina layer is then vacuum-baked to induce dehydration, condensation, and phase transformation, resulting in a denser gamma-alumina layer. This pre-application vacuum baking process pre-completes and solidifies the harmful phase transformation that inevitably occurs during the liner's service life in the cavity (hydrated alumina inevitably undergoes dehydration and shrinkage → stress drift → microcracks → particle generation at the cavity's operating temperature of 150℃~500℃). This ensures that the cavity wall after liner installation is thermodynamically stable before plasma treatment (shifting from "passively enduring wall aging" to "actively eliminating aging sources"). This effectively avoids particle generation at its source, improving the stability of the cavity wall in a hydrogen-containing plasma environment.
[0060] In some embodiments, the vacuum baking process can be performed under a full vacuum or a dry nitrogen atmosphere.
[0061] Step S14: Using atomic layer deposition (ALD) technology, form an aluminum oxide cap layer on the surface of the gamma alumina layer.
[0062] In some embodiments, after a dense gamma-alumina layer is formed on the surface of the anodic aluminum oxide layer on the liner by performing sealing and baking processes, an atomic layer deposition process can be used to form an aluminum oxide cap layer (made of Al2O3) on the surface of the gamma-alumina layer to further improve the surface quality and protective capability of the liner.
[0063] By using atomic layer deposition (ALD) technology, a smooth and dense alumina cap layer can be formed on the surface of the gamma alumina layer, which can provide good anti-etching and blocking effect against hydrogen free radicals in hydrogen-containing processes.
[0064] In some embodiments, atomic layer deposition (ALD) equipment, such as batch thermal ALD equipment suitable for processing large parts or single-piece thermal ALD equipment, can be used to perform the ALD process. The volume of the reaction chamber of the ALD equipment must be able to accommodate the liner.
[0065] In some embodiments, a plasma-enhanced atomic layer deposition (PEALD) process can be used to form the alumina cap layer, which can make the alumina cap layer more dense.
[0066] In some embodiments, when forming an alumina cap layer using atomic layer deposition (ALD), the first precursor may include trimethylaluminum (TMA), and the second precursor may include H₂O. The deposition temperature is 200°C to 250°C, for example, 220°C. The number of cycles is 300 to 500 (growth rate approximately 0.1 nm / cycle), for example, 400 cycles. During each cycle, the cycle dosage is: the first precursor (TMA) is introduced for 0.05 s to 0.1 s, for example, 0.08 s; the second precursor (H₂O) is introduced for 0.05 s to 0.1 s, for example, 0.08 s; and the single nitrogen purging time is 10 s to 20 s, for example, 15 s. For the inner lining, CVD mode can be avoided within the aforementioned purging time range.
[0067] In some embodiments, the thickness (target thickness) of the alumina cap layer is 30 nm to 50 nm. For example, the thickness of the alumina cap layer can be 30 nm, 31 nm, 33 nm, 35 nm, 37 nm, 40 nm, 42 nm, 45 nm, 48 nm, or 50 nm, or any value between any two of the aforementioned thickness values. Within the aforementioned thickness range, the deposited alumina cap layer is sufficient to cover the surface of the liner and seal microcracks without generating significant film stress.
[0068] In some embodiments, after the alumina cap layer is formed, an annealing process is performed to further densify the alumina cap layer and remove any residual film. The annealing process may include vacuum annealing. When performing vacuum annealing, the annealing temperature is 280°C to 320°C, for example, 300°C. The annealing time is 1 hour to 2 hours, for example, 1 hour.
[0069] Step S15: Install the liner onto the inner wall of the cavity.
[0070] In some embodiments, after forming an alumina cap layer on the surface of the liner, the offline treatment of the liner surface is completed. The liner can then be installed as follows: Figure 2On the inner wall 11 of the cavity 10 shown (by splicing and installing multiple inner lining parts), the working side surface of the inner lining parts facing the cavity forms the inner wall surface of the cavity 10, thereby giving the inner wall of the cavity an alumina (alumina cap layer) surface.
[0071] Next, the inner wall surface of cavity 10 needs to undergo the following online treatment to further improve the protective ability of the inner wall surface and the concentration stability of hydrogen free radicals.
[0072] Step S16: Introduce hexamethyldisiloxane carried by a carrier gas bubble and excess oxygen into the cavity, and turn on the plasma mode to react and form a first silicon oxide layer on the surface of the alumina cap layer.
[0073] refer to Figure 2 In some embodiments, before forming the first silicon oxide layer, oxygen is introduced into the cavity 10 to perform plasma activation treatment on the surface of the alumina cap layer on the inner wall surface. Then, the first silicon oxide layer is formed on the alumina cap layer with the activated surface.
[0074] Oxygen can be introduced into the cavity 10 through the air inlet 12, and the continuous plasma mode (radio frequency is continuously on) is turned on. The excited gas in the cavity 10 generates oxygen plasma. The oxygen free radicals in the oxygen plasma are used to clean the surface of the alumina cap layer (the inner wall surface of the cavity) on the installed liner, remove organic contaminants, and activate the surface of the alumina cap layer. The slight etching effect of oxygen free radicals on the surface of the alumina cap layer hydroxylates / activates the surface of the alumina cap layer, thereby improving the adhesion of the subsequently deposited first silicon oxide layer.
[0075] In some embodiments, during the activation process, the oxygen (O2) flow rate is 300 SCCM to 800 SCCM, for example, the oxygen (O2) flow rate may be 500 SCCM. The pressure is 200 mTorr to 500 mTorr, for example, the pressure may be 300 mTorr. The source power is 300 W to 1000 W, for example, the source power may be 600 W. The bias power is 0 W. The temperature is 150°C to 250°C, for example, the temperature may be 200°C. The time is 5 min to 15 min, for example, the time may be 10 min.
[0076] In some embodiments, after activation, oxygen supply is stopped, radio frequency is turned off, and purge gas is introduced to purge the cavity. The purge gas can be a non-reactive gas such as N2, with a flow rate of 500 SCCM to 1000 SCCM, a pressure of 250 mTorr to 350 mTorr, and a purge time of 5 min to 10 min.
[0077] In some embodiments, during the activation process, a co-wafer (not a product wafer) may be placed on the hot stage 13 to protect the surface of the hot stage 13.
[0078] In some embodiments, after activation, hexamethyldisiloxane (HMDSO) carried by a carrier gas bubble and excess oxygen are introduced into the cavity 10 as reactants. A continuous plasma mode is activated using the cavity's own radio frequency source, exciting the reactants to form plasma within the cavity. This plasma then reacts on the alumina cap layer surface of the inner wall 11 to form a first silicon oxide layer. The deposited first silicon oxide layer (SiO2) x This is a SiO2-like inorganic film with a non-stoichiometric ratio. Due to the excess oxygen, the deposited first silicon oxide layer is almost carbon-free, thus making it compatible with hydrogen processes using hydrogen radicals.
[0079] The mainstream existing cavity conditioning technology uses a carbon-containing polymer film for protection on the inner wall of the cavity. Its inherent drawback is that the film itself becomes a carbon source, making it susceptible to continuous etching by hydrogen free radicals during the process, leading to wall surface drift. Therefore, this application takes a different approach, utilizing excess oxygen to perform plasma polymerization with the HMDSO precursor to form plasma, which is then deposited on the inner wall surface. This allows for the online formation of a SiO2-like inorganic film (first silicon oxide layer) with extremely low carbon content (less than 5 at%), serving as a wall protection film. This transforms the chemical properties of the online-formed first silicon oxide layer from a carbon film conflicting with the process objectives to an oxide film compatible with the decarbonization process (hydrogenation process). Furthermore, the first silicon oxide layer (SiO2... x The etching rate of this SiO2-like inorganic film under hydrogen free radicals is much lower than that of carbon film, and its surface hydroxylation state can be stably maintained by water vapor / hydrogen plasma environment, so that the recombination consumption of hydrogen free radicals on the wall surface becomes an approximately constant value, thereby improving the stability of the cavity wall.
[0080] In some embodiments, when forming the first silicon oxide layer, the flow rate ratio of the introduced oxygen to the hexamethyldisiloxane carried by the carrier gas bubble is 8 or more (oxygen flow rate: hexamethyldisiloxane carried by the carrier gas bubble ≥ 8: 1) to ensure that the introduced oxygen is in an excess state and to minimize the carbon content of the deposited first silicon oxide layer.
[0081] In some embodiments, the carbon content in the first silicon oxide layer is less than 5 at%, in order to maximize the film's resistance to hydrogen free radical attacks.
[0082] In some embodiments, during the formation of the first silicon oxide layer, the flow rate (equivalent flow rate) of hexamethyldisiloxane carried by the carrier gas bubbling is 20 SCCM to 100 SCCM, for example, the flow rate of hexamethyldisiloxane carried by the carrier gas bubbling can be 50 SCCM, and the temperature of the source bottle (bubbler / vaporizer) is 30°C to 50°C. The oxygen flow rate is 200 SCCM to 1000 SCCM, for example, the oxygen flow rate can be 400 SCCM. The chamber pressure is 200 mTorr to 500 mTorr, for example, the chamber pressure can be 300 mTorr. The source power is 300 W to 800 W (to avoid excessive power causing excessive dissociation of HMDSO, leading to an increase in the carbon content of the membrane), for example, the source power can be 500 W. The bias power is 0 W. The temperature is 150°C to 300°C (consistent with the hydrogen process), for example, the temperature can be 200°C.
[0083] In some embodiments, the deposition time (reaction time) for forming the first silicon oxide layer is 10 min to 40 min, for example, 20 min.
[0084] In some embodiments, the thickness of the first silicon oxide layer is 50 nm to 150 nm. For example, the thickness of the first silicon oxide layer may be 100 nm (the deposition rate is about 3 nm / min to 8 nm / min).
[0085] In some embodiments, nitrogen gas can be introduced as a dilution gas to stabilize the plasma during the formation of the first silicon oxide layer. The flow rate of the nitrogen gas introduced as a dilution gas is 300 SCCM or less, based on the flow rates of the oxygen gas and the hexamethyldisiloxane carried by the carrier gas bubble, for example, 100 SCCM.
[0086] By introducing excess oxygen during the formation of the first silicon oxide layer, the carbon content in the first silicon oxide layer is ensured to be less than 5 at%, which significantly reduces the etching damage to the wall surface caused by hydrogen free radicals in the hydrogen process and effectively maintains the constant wall surface state, thereby stabilizing the amount of hydrogen free radicals reaching the wafer in the hydrogen process.
[0087] In some embodiments, after the first silicon oxide layer is formed, a second mixed gas of hydrogen and nitrogen is introduced into the cavity 10, and the plasma mode is turned on to perform online post-treatment (stabilization treatment) on the first silicon oxide layer after film formation, so as to stabilize the surface of the first silicon oxide layer.
[0088] In some embodiments, when stabilizing the first silicon oxide layer, the hydrogen flow rate in the second mixed gas is less than 4%, and the nitrogen flow rate is more than 96%, for example, the hydrogen flow rate is 4% and the nitrogen flow rate is 96%; the nitrogen flow rate is 480 SCCM to 520 SCCM, for example, the nitrogen flow rate can be 500 SCCM; the pressure is 200 mTorr to 400 mTorr, for example, the pressure can be 300 mTorr; the source power is 200 W to 500 W, for example, the source power can be 300 W; the bias power is 0 W; the temperature is 150°C to 250°C, for example, the temperature can be 200°C; and the time is 5 min to 15 min, for example, the time can be 10 min.
[0089] After the first silicon oxide layer is formed, a second mixed gas of hydrogen and nitrogen with a low hydrogen content is introduced into the cavity to stabilize the first silicon oxide layer. The nitrogen-hydrogen plasma with a low hydrogen content can be used to eliminate the Si-H / Si-OH dangling bonds inside the first silicon oxide layer film and remove weakly adsorbed fragments to prevent wall degassing problems during the first wafer of the hydrogen process.
[0090] In some embodiments, during the activation process, deposition of the first silicon oxide layer, and stabilization process, a protective substrate may be placed on the hot stage 13, and the substrate may be removed from the cavity 10 after the above processes are completed.
[0091] Step S17: Introduce a first mixture of hydrogen and nitrogen into the cavity and activate plasma mode to perform the hydrogen process.
[0092] In some embodiments, after the above process is completed, the hydrogen process can be started, and the surface of the production wafer (not shown) placed on the hot stage 13 is subjected to plasma treatment (e.g., adhesive removal or surface treatment).
[0093] In some embodiments, during the hydrogen process, a production wafer is introduced into the cavity 10, placed on the heated stage 13, and a first mixture of hydrogen and nitrogen as process gases is introduced into the cavity 10. A continuous plasma mode is activated, and the surface of the production wafer is treated using the hydrogen- and nitrogen-containing plasma generated by exciting the first mixture of hydrogen and nitrogen. After treatment, the production wafer is removed from the cavity 10. When processing multiple production wafers, the currently processed production wafer is removed from the cavity 10 before the next production wafer is introduced for further processing.
[0094] In some embodiments, during the hydrogen process, the hydrogen flow rate in the first mixture of hydrogen and nitrogen is greater than 4% to 40%, and the nitrogen flow rate is less than 96% to 60%. For example, in a hydrogen process with high hydrogen content (generally a high-hydrogen process), the hydrogen flow rate in the first mixture of hydrogen and nitrogen may be 20%, and the nitrogen flow rate may be 80%; while in a hydrogen process with even higher hydrogen content (higher-hydrogen process), the hydrogen flow rate in the first mixture of hydrogen and nitrogen may reach 40%, and the nitrogen flow rate may be 60%. The hydrogen process (high-hydrogen process) can be understood with reference to existing technologies.
[0095] Through the above treatment, a protective system is formed on the inner wall surface (working side surface of the liner) with a multi-layer protective system consisting of an anodic aluminum oxide layer, a hydrated aluminum oxide layer, a gamma aluminum oxide layer, an aluminum oxide cap layer, and a first silicon oxide layer. This improves the protective capability of the inner wall surface, significantly reduces the etching damage to the wall surface caused by hydrogen free radicals in the hydrogen process, greatly reduces particle shedding, and reduces the probability of H plasma / free radicals invading the inner wall surface. This, in turn, reduces the residue and reaction inside the porous structure of the anodic aluminum oxide layer, and improves the concentration stability of H free radicals in the cavity.
[0096] In some embodiments, during the hydrogen process, the concentration of hydrogen free radicals (hydrogen spectral signal) and the number of particles can be monitored through optical emission spectrometry (OES) tracking and particle sampling. When the hydrogen spectral signal becomes abnormal or the number of particles exceeds the limit, the hydrogen process will be paused, and the regeneration of the silicon oxide layer on the inner wall will be triggered. At this time, the plasma processing equipment will control the reintroduction of hexamethyldisiloxane carried by the carrier gas bubble and excess oxygen into the cavity 10, and activate the plasma mode to react and form a second silicon oxide layer with a non-stoichiometric SiO2-like inorganic film on the surface of the first silicon oxide layer on the inner wall 11. After the formation of the second silicon oxide layer, a second mixed gas of hydrogen and nitrogen with low hydrogen content will be introduced into the cavity 10, and the plasma mode will be activated to stabilize the surface of the second silicon oxide layer, thereby repairing the surface of the first silicon oxide layer damaged during the hydrogen process. This effectively reduces particle generation, enables online maintenance, avoids fluctuations in the etching rate of the cavity, prevents fluctuations in the plasma processing process, and improves the continuous stability of the cavity under the hydrogen process. Afterwards, the hydrogen production process can be resumed. In this way, by repeatedly forming a second silicon oxide layer on the surface of the first silicon oxide layer and performing a stabilization treatment whenever the monitored value exceeds the limit during the hydrogen production process, the wall film layer is regenerated, the cavity is renewed and protected, the long-term effects of hydrogen are avoided, and the service life of the inner wall of the cavity is significantly extended.
[0097] In some embodiments, when forming the second silicon oxide layer, the flow ratio of the introduced oxygen to the hexamethyldisiloxane carried by the carrier gas bubble is 8 or more to ensure that the introduced oxygen is in an excess state and to minimize the carbon content of the deposited second silicon oxide layer.
[0098] In some embodiments, the carbon content in the second silicon oxide layer is less than 5 at%, in order to maximize the resistance of the regenerated film layer to hydrogen free radical attacks.
[0099] In some embodiments, when forming the second silicon oxide layer, the flow rate (equivalent flow rate) of hexamethyldisiloxane carried by the carrier gas bubbling is 20 SCCM to 100 SCCM, for example, the flow rate of hexamethyldisiloxane carried by the carrier gas bubbling can be 50 SCCM, and the temperature of the source bottle (bubbler / vaporizer) is 30°C to 50°C. The oxygen flow rate is 200 SCCM to 1000 SCCM, for example, the oxygen flow rate can be 400 SCCM. The chamber pressure is 200 mTorr to 500 mTorr, for example, the chamber pressure can be 300 mTorr. The source power is 300 W to 800 W (to avoid excessive power causing excessive dissociation of HMDSO, leading to an increase in the carbon content of the membrane), for example, the source power can be 500 W. The bias power is 0 W. The temperature is 150°C to 300°C (consistent with the hydrogen process), for example, the temperature can be 200°C.
[0100] In some embodiments, the deposition time (reaction time) for forming the second silicon oxide layer is 10 min to 15 min, for example, 12 min.
[0101] In some embodiments, the thickness of the formed second silicon oxide layer is 30 nm to 50 nm, for example, the thickness of the second silicon oxide layer may be 40 nm.
[0102] In some embodiments, nitrogen gas can be introduced as a dilution gas to stabilize the plasma during the formation of the second silicon oxide layer. Specifically, based on the flow rates of the introduced oxygen and the hexamethyldisiloxane carried by the carrier gas bubble, the flow rate of the nitrogen gas as a dilution gas is 300 SCCM or less; for example, the nitrogen flow rate can be 100 SCCM.
[0103] In some embodiments, after the second silicon oxide layer is formed, a second mixed gas of hydrogen and nitrogen with a hydrogen flow rate of less than 4% is introduced into the cavity, and the plasma mode is turned on to stabilize the second silicon oxide layer. The nitrogen-hydrogen plasma with low hydrogen content can be used to eliminate the Si-H / Si-OH dangling bonds inside the second silicon oxide layer film and remove weakly adsorbed fragments.
[0104] In some embodiments, when stabilizing the second silicon oxide layer, the nitrogen flow rate is 480 SCCM to 520 SCCM, for example, the nitrogen flow rate can be 500 SCCM. The pressure is 200 mTorr to 400 mTorr, for example, the pressure can be 300 mTorr. The source power is 200 W to 500 W, for example, the source power can be 300 W. The bias power is 0 W. The temperature is 150°C to 250°C, for example, the temperature can be 200°C. The time is 5 min to 15 min, for example, the time can be 10 min.
[0105] In some embodiments, during the hydrogen production process, when a threshold is triggered, a shutdown is initiated, and the cavity 10 is opened to replace the liner on the cavity wall for maintenance. The newly replaced liner, using the cavity stabilization method of the plasma processing equipment provided in any of the above embodiments, has an anodic aluminum oxide layer, a hydrated aluminum oxide layer, a gamma aluminum oxide layer, and an aluminum oxide cap layer formed offline on its working surface. Before the hydrogen production process, a first silicon oxide layer is formed online on the aluminum oxide cap layer. The replaced liner can be refurbished and reused in the hydrogen production process after film removal and surface anodizing treatment using the cavity stabilization method of the plasma processing equipment provided in any of the above embodiments.
[0106] In some embodiments, the threshold includes the cumulative number of times the second silicon oxide layer is formed reaching 3 to 5 times. For example, during the hydrogen production process, whenever the monitored value exceeds the limit, the process of forming a second silicon oxide layer and performing a stabilization treatment on the surface of the first silicon oxide layer is repeated once, and the number of repetitions can be 3, 4, or 5. This avoids the continuous thickening and peeling of the film, which can generate particles.
[0107] In some embodiments, the threshold includes a cumulative hydrogen process duration of 500 to 1000 hours, regardless of whether a second silicon oxide layer has been formed on the surface of the first silicon oxide layer and a stabilization treatment has been performed within this time range, in order to avoid stress accumulation, aging, and peeling off of the film layer to generate particles after long-term operation.
[0108] In a second aspect, an embodiment of the present application provides a plasma processing apparatus, which includes a cavity and an inner liner on the inner wall of the cavity. The inner liner is obtained using the cavity stabilization method of the plasma processing apparatus provided in any of the embodiments of the first aspect described above.
[0109] refer to Figure 2 In some embodiments, the plasma processing equipment may include a plasma adhesive removal device or a plasma surface treatment device. The cavity 10 provided in the plasma processing equipment is a plasma processing cavity and can be used to perform a plasma processing process (hydrogen process) using a first mixed gas of hydrogen and nitrogen as the base process gas.
[0110] In some embodiments, the cavity 10 has an inner wall 11, on which a liner (not shown) is applied. The working side surface of the liner facing the cavity constitutes the inner wall surface of the cavity 10. The liner is made of aluminum alloy, and at least the working side of the aluminum alloy surface is sequentially provided with an anodic aluminum oxide layer (hard oxide coating), a hydrated aluminum oxide layer, a gamma aluminum oxide layer, an aluminum oxide cap layer, and a first silicon oxide layer. A hot stage 13 is provided at the bottom of the cavity 10 for placing the production wafer (production wafer) to be processed in the plasma processing process, and the temperature can be controlled by a heating and temperature control device provided on the hot stage 13 to maintain the process temperature during processing. An air inlet 12 is provided at the top of the cavity 10 for introducing an excitation gas (a rare gas, such as one or more inert gases such as He, Ne, Ar, Kr, etc.) and a process gas (including a first mixed gas, etc.) used in the plasma processing process. The process gas entering the cavity 10 is excited by the excitation gas in the cavity to form plasma, which is used to perform the plasma processing process on the production wafer placed on the hot stage 13. The air inlet 12 is also used to introduce oxygen, hexamethyldisiloxane carried by the carrier gas bubble, and the first mixed gas used in the embodiments of this application, etc. These gases are excited by the excitation gas to form plasma, which is used to treat the working side surface of the inner liner laid on the inner wall of the cavity. An exhaust port 14 is provided at the bottom of the cavity 10 for discharging waste gas and controlling the cavity pressure.
[0111] Before the liner is installed on the inner wall of the cavity, the cavity stabilization method of the plasma processing equipment provided in the above-mentioned embodiment of the present application is used to form a hydrated alumina layer, a gamma alumina layer, and an alumina cap layer on the surface of the anodic alumina layer. After installation on the inner wall of the cavity, the cavity stabilization method of the plasma processing equipment provided in the embodiment of the present application is executed to activate the surface of the alumina cap layer exposed on the inner wall of the cavity to improve the film-substrate adhesion. A first silicon oxide layer with a non-stoichiometric ratio is deposited on the surface of the alumina cap layer to form a multi-layered dense stacked structure resistant to hydrogen free radical etching on the inner wall of the cavity, constituting a near-carbon-free all-inorganic wall protection system as a consumable functional layer, thereby improving the stability of H free radical concentration and improving particulate defects.
[0112] In summary, this embodiment of the application forms a hydrated alumina (boehmite) layer by performing a water vapor hydration sealing treatment on the anodic alumina layer on the surface of the liner. Then, through vacuum baking, the hydrated alumina layer undergoes dehydration condensation and phase transformation reactions to form a dense gamma-alumina (γ-Al2O3) layer. This allows the harmful phase transformation that inevitably occurs during the liner's service life in the cavity to be completed and solidified in advance in one step. This ensures that the cavity wall surface after the liner is installed is thermodynamically stable before plasma treatment, effectively avoiding particle generation at its source. Furthermore, by forming an alumina cap layer and a first silicon oxide layer (SiO2-like inorganic film with an etching rate far lower than that of carbon films under hydrogen radical etching in hydrogen processes) on the dense gamma-alumina layer, the application achieves this effect. x This allows the chemical properties of the wall protection film to be compatible with hydrogen processes, and forms a nearly carbon-free, all-inorganic wall protection system with a multi-layered, dense, stacked structure. This improves the concentration stability of H free radicals in the cavity, reduces particle shedding, and stabilizes the cavity under hydrogen-containing plasma processes.
[0113] The above are merely preferred embodiments of this application. These embodiments are not intended to limit the scope of protection of this application. Therefore, any equivalent changes made based on the description and drawings of this application should also be included within the scope of protection of this application.
Claims
1. A method of stabilizing a chamber of a plasma processing apparatus, characterized by, In order, they include: A liner for a plasma processing equipment cavity is provided. The liner is made of aluminum alloy and has an anodized aluminum layer on its working side surface. Using water vapor, the surface of the anodic aluminum oxide layer is hydrated and sealed to form a hydrated aluminum oxide layer on the surface of the anodic aluminum oxide layer. Vacuum baking is performed to cause the hydrated alumina layer to undergo dehydration condensation and phase transformation reaction, forming a dense gamma alumina layer. An alumina cap layer is formed on the surface of the gamma alumina layer using an atomic layer deposition process. The liner is installed on the inner wall of the cavity; Hexamethyldisiloxane carried by a carrier gas bubble and excess oxygen are introduced into the cavity, and plasma mode is activated to react on the surface of the alumina cap layer to form a first silicon oxide layer with a non-stoichiometric ratio. A first mixture of hydrogen and nitrogen gas is introduced into the cavity, and plasma mode is activated to perform the hydrogen process.
2. The cavity stabilization method for the plasma processing equipment according to claim 1, characterized in that, Also includes: After the hydration sealing treatment, the surface of the inner liner is de-dusted using a nitric acid solution. And / or, it also includes: before forming the first silicon oxide layer, introducing oxygen into the cavity and turning on the plasma mode to activate the surface of the aluminum oxide cap layer; After the first silicon oxide layer is formed, a second mixed gas of hydrogen and nitrogen is introduced into the cavity, and plasma mode is activated to stabilize the first silicon oxide layer.
3. The method of chamber stabilization of a plasma processing apparatus of claim 2, wherein, The water vapor is prepared using deionized water, and triethanolamine is added to the water vapor. The water vapor has a conductivity of less than 2 μS / cm and a chloride ion content of less than 1 ppm. The amount of triethanolamine added is 0.5 g / L to 2 g / L. During the hydration sealing treatment, the temperature is 100℃ to 115℃, the pressure is 0.02 MPa to 0.05 MPa, and the time is 2 min / μm to 3 min / μm. And / or, an ultrasonic-assisted descaling treatment is performed on the surface of the liner using a 15% to 20% nitric acid solution at a temperature of 20℃ to 25℃, an ultrasonic frequency of 35 kHz to 45 kHz, and a time of 30 s to 60 s. And / or, during the vacuum baking treatment, the vacuum degree is less than 1 × 10⁻⁶. -3 Torr, with a heating rate of 2℃ / min to 5℃ / min, a first plateau temperature of 200℃ to 350℃, a first plateau holding time of 50min to 70min, a second plateau temperature of 450℃ to 550℃, a second plateau holding time of 2 hours to 4 hours, a cooling rate of less than 5℃ / min, and a furnace exit temperature of less than 100℃.
4. The method of chamber stabilization of a plasma processing apparatus of claim 1, wherein, When forming the alumina cap layer, the first precursor includes trimethylaluminum, the second precursor includes H2O, the temperature is 200℃~250℃, the number of cycles is 300 to 500, the introduction time of the first precursor in each cycle is 0.05s~0.1s, the introduction time of the second precursor is 0.05s~0.1s, and the single purging time is 10s~20s; And / or, the thickness of the alumina cap layer is 30nm to 50nm; and / or, it further includes: after forming the alumina cap layer, performing in-situ vacuum annealing treatment at a temperature of 280℃ to 320℃ for 1 hour to 2 hours; and / or, when performing the hydrogen process, the hydrogen flow rate in the first mixed gas accounts for more than 4% to 40%, and the nitrogen flow rate accounts for less than 96% to 60%.
5. The cavity stabilization method for the plasma processing equipment according to claim 2, characterized in that, During the hydrogen production process, the concentration and particle count of hydrogen free radicals are monitored. If either exceeds the limit, the hydrogen production process is paused, and hexamethyldisiloxane carried by a carrier gas bubble and excess oxygen are introduced into the cavity again. The plasma mode is then activated to react on the surface of the first silicon oxide layer to form a second silicon oxide layer with a non-stoichiometric ratio. A second mixed gas of hydrogen and nitrogen is introduced into the cavity, and the plasma mode is activated to stabilize the second silicon oxide layer. Then, the hydrogen production process is resumed, and when a threshold is triggered, the machine is stopped and the liner is replaced.
6. The cavity stabilization method for the plasma processing equipment according to claim 5, characterized in that, The threshold includes the cumulative number of times the second silicon oxide layer is formed reaching 3 to 5 times, or the cumulative duration of the hydrogen process reaching 500 to 1000 hours.
7. The cavity stabilization method for the plasma processing equipment according to claim 5, characterized in that, When the first silicon oxide layer and the second silicon oxide layer are formed, the flow rate ratio of the introduced oxygen to the hexamethyldisiloxane carried by the carrier gas bubble is 8 or more; and / or, the carbon content in the first silicon oxide layer and the second silicon oxide layer is less than 5 at.
8. The cavity stabilization method for the plasma processing equipment according to claim 5, characterized in that, When forming the first silicon oxide layer and the second silicon oxide layer, the flow rate of hexamethyldisiloxane carried by the carrier gas bubbling is 20 SCCM to 100 SCCM, the flow rate of oxygen is 200 SCCM to 1000 SCCM, the pressure is 200 mTorr to 500 mTorr, the source power is 300 W to 800 W, the bias power is 0 W, and the temperature is 150 °C to 300 °C; and / or, when forming the first silicon oxide layer, the reaction time is 10 min to 40 min, or, the thickness of the first silicon oxide layer is 50 nm to 150 nm; and / or, when forming the second silicon oxide layer, the reaction time is 10 min to 15 min, or, the thickness of the second silicon oxide layer is 30 nm to 50 nm.
9. The cavity stabilization method for the plasma processing equipment according to claim 2, characterized in that, During the activation treatment, the oxygen flow rate is 300 SCCM to 800 SCCM, the pressure is 200 mTorr to 500 mTorr, the source power is 300 W to 1000 W, the bias power is 0 W, the temperature is 150 °C to 250 °C, and the time is 5 min to 15 min; and / or, during the stabilization treatment, the hydrogen flow rate in the second mixed gas accounts for less than 4%, the nitrogen flow rate accounts for more than 96%, the nitrogen flow rate is 480 SCCM to 520 SCCM, the pressure is 200 mTorr to 400 mTorr, the source power is 200 W to 500 W, the bias power is 0 W, the temperature is 150 °C to 250 °C, and the time is 5 min to 15 min.
10. A plasma processing device, characterized in that, The device includes a cavity, the inner wall of which is provided with an inner liner, the inner liner being obtained using the cavity stabilization method of the plasma processing device as described in any one of claims 1-9.