Positive electrode sheet and its preparation method and battery
By setting a double-layer reinforcing coating at the base of the electrode, the problem of balancing mechanical reinforcement of the electrode and purity of the welding area is solved, achieving high toughness and reliable welding of the electrode, and improving the safety and life of the battery.
Patent Information
- Application Number
- CN202611039515.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to improve the mechanical strength of the electrode tab while ensuring that the welded area of the electrode tab region retains its uncoated metallic nature, leading to problems such as weak welds, increased contact resistance, and weld failure.
A double-layered reinforcing coating is applied to the base of the electrode tab. The lower layer consists of carboxylated metallic carbon nanotubes or graphene nanosheets, while the upper layer consists of transition metal borides, carbides, or carbon-based superhard materials. This forms a synergistic protective system that combines toughness and hardness, ensuring mechanical reinforcement at the base of the electrode tab and the purity of the welding area.
It effectively suppresses the generation and propagation of cracks, ensures the mechanical strength of the tabs and the reliability of welding, avoids poor welding, and improves the safety and cycle life of the battery.
Smart Images

Figure CN123120634A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and more specifically, to a positive electrode sheet, its preparation method, and a battery. Background Technology
[0002] In the field of high-energy-density lithium-ion battery manufacturing using ultra-thin current collectors (such as aluminum foil with a thickness of less than 15μm), current collectors are becoming thinner and lighter to improve battery energy density and power performance. Under this trend, the tabs, as a key structure connecting the internal and external circuits of the battery, face severe challenges to their mechanical reliability. During subsequent processes such as cutting, folding, and ultrasonic welding, the tabs are repeatedly subjected to mechanical stress, making them highly susceptible to fatigue microcracks at their root (i.e., the transition region adjacent to the coating area). These microcracks not only lead to an abnormal increase in the battery's internal resistance and localized temperature rise, but in severe cases, they can even cause tab breakage, directly threatening the battery's safety performance and cycle life. Therefore, effectively enhancing the mechanical strength of the tabs, especially at their root, has become an important technical requirement in this field.
[0003] To address these needs, related technologies often employ a method of integrally coating the current collector with reinforcing materials such as polymers or ceramics to improve the overall hardness of the current collector. However, this approach has inherent limitations. First, introducing an additional inactive coating onto the entire surface of the current collector often significantly deteriorates the interfacial adhesion between the active coating (such as the cathode material coating) and the current collector substrate, potentially causing the active layer to peel off during battery cycling. More critically, this integral coating strategy cannot avoid the welding area of the electrode tabs. In processes such as ultrasonic welding, the principle relies on direct metallurgical bonding between metal current collectors. Any non-metallic coating present in the welding area will become an insulating barrier, severely hindering effective metal-metal contact, leading to weak welds (false welds), a surge in contact resistance, or even weld failure.
[0004] Therefore, existing technologies, when attempting to solve the problem of mechanical strengthening of the electrode tab, struggle to simultaneously ensure effective reinforcement of the tab area and the purity and weldability of the welding area. Specifically, how to precisely strengthen vulnerable areas such as the root of the electrode tab to suppress microcrack formation while ensuring that the welding area at the end of the electrode tab used for connection retains its uncoated metallic nature, thus not affecting subsequent reliable welding processes, has become a pressing technical problem to be solved. Summary of the Invention
[0005] In view of this, the present invention aims to at least partially solve one of the technical problems in the related art. To this end, the present invention provides a positive electrode sheet, a method for preparing the same, and a battery, which can effectively solve the problem of mechanical strengthening of the tab, while simultaneously ensuring effective reinforcement of the tab area and the purity and solderability of the welding area.
[0006] To solve the above-mentioned technical problems, this application is implemented as follows: According to one aspect of this application, an embodiment of this application provides a positive electrode sheet, the positive electrode sheet comprising: Current collector and tabs formed by extending from said current collector; An active coating is disposed on at least one surface of the current collector; A first reinforcing coating is disposed on at least one side surface of the root of the electrode ear; The reinforcing coating includes a lower first conductive layer and an upper second conductive layer; The first conductive layer includes a first conductive material, and the second conductive layer includes a second conductive material; The first conductive material includes at least one of carboxylated metallic carbon nanotubes and carboxylated graphene nanosheets; the second conductive material includes at least one of transition metal borides, transition metal carbides / nitrides, and carbon-based superhard materials. The term "base of the electrode" refers to the end of the electrode closest to the current collector.
[0007] In some embodiments, the length of the first reinforcing coating is 30% to 70% of the tab length, and the width of the first reinforcing coating is the same as the tab width.
[0008] In some embodiments, the positive electrode further includes a second reinforcing coating disposed on at least one side of the edge at the junction of the current collector and the tab.
[0009] In some embodiments, the length of the second reinforcing coating is 1~2μm, and the width of the second reinforcing coating is the same as the width of the current collector.
[0010] In some embodiments, the first conductive layer further includes a first adhesive and an additive, wherein the mass ratio of the first conductive material, the first adhesive, and the additive is (70~82):(20~30):(1~3).
[0011] In some of these embodiments, the additive includes at least one of 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, and N-butyl-N-methylpyrrolidine bis(trifluoromethanesulfonyl)imide.
[0012] In some embodiments, the carboxyl content in the carboxylated metallic carbon nanotubes is 1 at% to 2 at%.
[0013] In some embodiments, the carboxyl content in the carboxylated graphene nanosheets is 1 at% to 2 at%.
[0014] In some of these embodiments, the thickness of the first conductive layer is 3 μm to 20 μm.
[0015] In some embodiments, the second conductive layer further includes a conductive reinforcing agent, a second binder, and an additive, wherein the mass ratio of the second conductive material, the conductive reinforcing agent, the second binder, and the additive is (70~85):(6~10):(10~18):(2~5).
[0016] In some embodiments, the conductive enhancer includes at least one of graphene and graphite nanosheets.
[0017] In some embodiments, the additive includes at least one of polyamide-imide, polyether-imide, and polysulfone.
[0018] In some of these embodiments, the particle size Dv50 of the second conductive material is 200 nm to 500 nm.
[0019] In some of these embodiments, the thickness of the second conductive layer is 3 μm to 20 μm.
[0020] In some of these embodiments, the active coating includes a third binder.
[0021] In some embodiments, the first adhesive, the second adhesive, and the third adhesive are selected from the same adhesive.
[0022] In some of these embodiments, the first adhesive, the second adhesive, and the third adhesive each independently include at least one of polyvinylidene chloride and polyvinylidene fluoride-hexafluoropropylene.
[0023] According to another aspect of this application, embodiments of this application provide a method for preparing a positive electrode sheet, comprising the following steps: An active slurry is coated on a first region of at least one side surface of the current collector, and after drying, a current collector containing an active coating is obtained. A first conductive paste is coated on a second region of the current collector surface containing an active coating, and after drying, a first conductive layer is obtained. A second conductive paste is coated onto the surface of the first conductive layer and dried to obtain the second conductive layer, forming a reinforced coating. The positive electrode sheet is obtained after die cutting; The first region is a current collector region for setting an active coating, and the second region is a current collector region and a tab region for setting a reinforcing coating. The reinforcing coating includes a first reinforcing coating.
[0024] In some embodiments, the preparation of the first conductive paste includes the following steps: The first conductive material, binder, and additives are mixed in the first solvent to obtain the first conductive paste.
[0025] In some embodiments, the viscosity of the first conductive paste is 7000 mPa·s to 9000 mPa·s.
[0026] In some embodiments, the solid content of the first conductive paste is 10% to 12%.
[0027] In some of these embodiments, the first solvent includes at least one of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0028] In some embodiments, the preparation of the second conductive paste includes the following steps: The second conductive material, conductive reinforcing agent, second binder, and additives are mixed in a second solvent to obtain a second conductive slurry.
[0029] In some embodiments, the viscosity of the second conductive paste is 8000 mPa·s to 12000 mPa·s.
[0030] In some embodiments, the solid content of the second conductive paste is 15% to 25%.
[0031] In some of these embodiments, the second solvent includes at least one of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0032] According to another aspect of this application, an embodiment of this application provides a battery including a positive electrode sheet, the positive electrode sheet including the aforementioned positive electrode sheet, or including a positive electrode sheet prepared according to the aforementioned preparation method.
[0033] Implementing the technical solution of the present invention has at least the following beneficial effects: In this embodiment, a positive electrode is provided, which constitutes a synergistic protective system combining toughness and hardness by forming a reinforced coating with a double-layer structure on at least one side surface of the electrode root. The reinforced coating comprises a lower first conductive layer and an upper second conductive layer. The first conductive layer directly contacts the current collector surface and its composition includes carboxylated metallic carbon nanotubes or carboxylated graphene nanosheets. Carbon nanotubes or graphene nanosheets are chosen because they possess excellent flexibility and one-dimensional / two-dimensional structural characteristics, enabling them to absorb and dissipate external stress through their deformation and slippage. Carboxylation treatment, for example, by introducing a certain stoichiometric ratio of carboxyl functional groups onto their surface, can significantly improve their dispersibility in solvents, reduce agglomeration, and simultaneously allow the carboxyl groups to form hydrogen bonds or other intermolecular forces with polar groups in the binder, enhancing the cohesive strength within the layer and the bonding force between layers. This provides the entire reinforced coating with a highly tough and stable electron transport channel. The second conductive layer comprises at least one of transition metal borides, transition metal carbides or nitrides, and carbon-based superhard materials. The high hardness of these materials is utilized to construct a robust protective shell on the surface. The lower layer absorbs and buffers stress, while the upper layer resists surface damage. Together, they suppress the generation and propagation of cracks in the ultrathin current collector.
[0034] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0035] Figure 1 The diagram shown is a schematic diagram of a positive electrode structure provided in an embodiment of the present invention.
[0036] Figure 2 The diagram shown is a schematic diagram of a positive electrode structure provided in an embodiment of the present invention.
[0037] 1-Active coating, 2-First reinforcing coating, 3-End welding area, 4-Second reinforcing coating. Detailed Implementation
[0038] The present application will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the present application.
[0039] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges or individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0040] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0041] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0042] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0043] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0044] In lithium-ion batteries, the tabs, as an extension of the current collector, undergo multiple machining processes, including slitting, folding, and subsequent ultrasonic welding. As the thickness of the current collector decreases, especially when using ultra-thin aluminum foil at the 8μm to 15μm level, fatigue microcracks are easily generated at the junction of the tab root and the current collector body under repeated processing and subsequent usage stresses. Once these microcracks form and propagate, they increase the DC internal resistance in the tab area, causing abnormal temperature rises during charging and discharging, and in severe cases, even leading to complete tab breakage and failure, threatening the battery's safety and lifespan.
[0045] In related technologies, some solutions attempt to improve mechanical strength by coating the entire surface of the current collector with polymer or ceramic materials. However, this approach interferes with the interface between the active coating and the current collector, deteriorating their adhesion. More critically, the welding area at the end of the electrode requires direct metallurgical bonding between metals. Any residual non-metallic coating will hinder energy transfer and atomic diffusion during ultrasonic welding, resulting in incomplete welds or insufficient weld strength. Other solutions that only reinforce a single material in a localized area often struggle to simultaneously achieve the high toughness required to resist crack initiation in the electrode root region and the high surface hardness required to resist external mechanical scratches.
[0046] In view of this, embodiments of this application provide a positive electrode sheet, the positive electrode sheet comprising: Current collector and tabs formed by extending from said current collector; Active coating 1 is disposed on at least one side surface of the current collector; A first reinforcing coating 2 is disposed on at least one side surface of the root of the electrode ear; The reinforcing coating includes a lower first conductive layer and an upper second conductive layer; The first conductive layer includes a first conductive material, and the second conductive layer includes a second conductive material; The first conductive material includes at least one of carboxylated metallic carbon nanotubes and carboxylated graphene nanosheets; the second conductive material includes at least one of transition metal borides, transition metal carbides / nitrides, and carbon-based superhard materials. The term "base of the electrode" refers to the end of the electrode closest to the current collector.
[0047] In a specific example of this application, refer to the appendix to the specification. Figure 1 The structure shown illustrates a lithium-ion battery electrode comprising a current collector serving as a substrate. The current collector can be made of a metal foil commonly used in the field for positive electrodes, such as aluminum foil. One function of the current collector is to carry the active coating 1 and conduct electrons. The active coating 1 is coated on the main surface of the current collector; this area is called the active region. The current collector extends outward at specific edges to form one or more protrusions, which are called tabs. Depending on their function, the tabs can be divided along their length into a root reinforcement region and an end welding region 3. The root reinforcement region is adjacent to the current collector body and is the starting point extending from the current collector and bearing bending stress. The end welding region 3 is located at the outermost end of the tab furthest from the current collector body and is used for subsequent connection to the battery cover or busbar via ultrasonic welding.
[0048] In this application, "the root of the electrode tab" generally refers to the section of the electrode tab that is close to the current collector and directly bears the mechanical processing stresses such as cutting, folding, and ultrasonic welding, as well as the bending stresses during use.
[0049] This application provides a positive electrode sheet, which forms a synergistic protective system combining toughness and hardness by providing a reinforcing coating comprising a bilayer structure on at least one side surface at the root of the electrode tab. The reinforcing coating comprises a lower first conductive layer and an upper second conductive layer. The first conductive layer directly contacts the current collector surface and its composition includes carboxylated metallic carbon nanotubes or carboxylated graphene nanosheets. Carbon nanotubes or graphene nanosheets are chosen because they possess excellent flexibility and one-dimensional / two-dimensional structural characteristics, enabling them to absorb and dissipate external stress through their deformation and slippage. Carboxylation treatment, for example, by introducing a certain stoichiometric ratio of carboxyl functional groups onto their surface, can significantly improve their dispersibility in solvents, reduce agglomeration, and simultaneously allow the carboxyl groups to form hydrogen bonds or other intermolecular forces with polar groups in the binder, enhancing the cohesive strength within the layer and the bonding force between layers. This, in turn, provides the entire reinforcing coating with a highly tough and stable electron transport channel. The second conductive layer comprises at least one of transition metal borides, transition metal carbides or nitrides, and carbon-based superhard materials, utilizing the high hardness of these materials to construct a robust protective shell on the surface. The lower layer absorbs and buffers stress, while the upper layer resists surface damage; their combined action suppresses the generation and propagation of cracks on the ultrathin current collector. Furthermore, the current collector surface of the welding area 3 at the end of the electrode retains the original exposed state of the metal foil, without any form of composite reinforcement layer. This ensures that during ultrasonic welding, the high-frequency mechanical vibration applied by the welding head allows the metal atoms of the electrode to directly contact and diffuse with the metal atoms of the component to be joined, thereby achieving a reliable metallurgical connection. This simultaneously ensures the metal purity of the welding area, achieving a balance between the mechanical strength and weldability of the electrode.
[0050] In some embodiments, the carboxylated metallic carbon nanotubes include at least one of single-walled carbon nanotubes, double-armed carbon nanotubes, and multi-walled carbon nanotubes.
[0051] In some embodiments, the thicknesses of the first reinforcing coating 2 and the second reinforcing coating 4 are preferably kept consistent.
[0052] In some embodiments, the length of the first reinforcing coating 2 is 30% to 70% of the tab length, for example, it can be 30%, 50%, 70%, or other values within the above range; the width of the first reinforcing coating 2 is consistent with the tab width. This allows the first reinforcing coating 2 to precisely cover the root region of the tab, where stress is most concentrated, extending from the edge of the current collector. This effectively resists bending and tearing stress in this region while avoiding the welding area at the end, ensuring no coating interference in the weld area during ultrasonic welding, achieving metallurgical bonding, and stabilizing the connection quality.
[0053] In some embodiments, the positive electrode further includes a second reinforcing coating 4, which is disposed on at least one side of the edge at the junction of the current collector and the tab. See the appendix to this specification for details. Figure 2 The second reinforcing coating has the same composition as the first reinforcing coating.
[0054] In some embodiments, the length of the second reinforcing coating 4 is 1~2μm, for example, it can be 1μm, 1.5μm, 2μm, or other values within the above range; the width of the second reinforcing coating 4 is consistent with the width of the current collector.
[0055] In this application, a mechanical buffer barrier is constructed by adding a micron-sized strip-shaped second reinforcing coating 4 at the edge where the current collector and the tab meet. This effectively disperses the concentrated stress generated at the interface when the tab is folded, preventing stress from being transmitted to the current collector body and causing tearing. At the same time, it avoids introducing additional thickness in the area coated with the active coating 1, ensuring the flatness and consistency of the active area.
[0056] In some embodiments, the first conductive layer further includes a first binder and an additive, wherein the mass ratio of the first conductive material, the first binder, and the additive is (70~82):(20~30):(1~3). For example, it can be 70:30:3, 76:25:2, 82:20:1, or other values within the above range. By controlling this ratio within the above range, the conductivity, flexibility, and processability of the coating can be balanced: when the content of conductive carbon material is 70~82 parts, the cured coating has a sufficiently low volume resistivity to undertake the task of tab current transmission, while avoiding the coating from becoming brittle and losing its toughness due to excessive carbon material.
[0057] In some embodiments, the additive includes at least one selected from 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, and N-butyl-N-methylpyrrolidine bis(trifluoromethanesulfonyl)imide. For example, it can be 1-ethyl-3-methylimidazolium tetrafluoroborate or 1-butyl-3-methylimidazolium tetrafluoroborate. The cations of the additive adsorb onto the surface of the first conductive agent through π-π and cation-π interactions. Utilizing steric hindrance and electrostatic repulsion, the agglomeration of the first conductive agent in the high-solids-content slurry is effectively suppressed, ensuring the formation of a uniform and stable conductive network.
[0058] In some embodiments, the carboxyl content in the carboxylated metallic carbon nanotubes is 1 at% to 2 at%. For example, it is 1 at%, 1.5 at%, 2 at%, or other values within the above range.
[0059] In some embodiments, the carboxyl content in the carboxylated graphene nanosheets is 1 at% to 2 at%. For example, it is 1 at%, 1.5 at%, 2 at%, or other values within the above range.
[0060] In some embodiments, the thickness of the first conductive layer is 3 μm to 20 μm. For example, it can be 3 μm, 6 μm, 12 μm, 18 μm, 20 μm, or other values within the above range.
[0061] In some embodiments, the second conductive layer further includes a conductive reinforcing agent, a second binder, and an additive, wherein the mass ratio of the second conductive material, the conductive reinforcing agent, the second binder, and the additive is (70~85):(6~10):(10~18):(2~5). For example, it is 70:10:18:5, 80:8:12:5, 85:6:10:2, or other ratios within the above range.
[0062] In some embodiments, the conductive enhancer includes at least one of graphene and graphite nanosheets. For example, it may be graphene.
[0063] In some embodiments, the additive includes at least one of polyamide-imide, polyether-imide, and polysulfone. For example, it can be polyamide-imide or polyether-imide. Preferably, it is polyamide-imide, whose molecular chain contains both polar amide groups (-NH-CO-) and imide groups. These strongly polar groups can generate strong van der Waals forces and hydrogen bonds with the oxide layer on the surface of the second conductive material and the defects or oxygen-containing functional groups on the surface of the conductive reinforcing agent, providing excellent adsorption capacity. When added as an additive, it establishes a robust molecular bridging network between the second conductive material, the conductive reinforcing agent, and the second binder, significantly improving the cohesive strength of the second conductive layer and its interlayer bonding force with the first conductive layer.
[0064] In some embodiments, the particle size Dv50 of the second conductive material is 200nm to 500nm. For example, it can be 200nm, 300nm, 400nm, 500nm, etc., or other values within the above range.
[0065] In some embodiments, the thickness of the second conductive layer is 3 μm to 20 μm. For example, it can be 3 μm, 6 μm, 12 μm, 18 μm, 20 μm, or other values within the above range.
[0066] In some embodiments, the active coating 1 includes a third binder. Further, the active coating 1 also includes a positive electrode active material and a positive electrode conductive agent, wherein the types of the positive electrode active material and the positive electrode conductive agent are not particularly limited, and materials commonly used in the art can be selected.
[0067] In some embodiments, the first, second, and third adhesives are selected from the same adhesive. Using the same adhesive in the first reinforcing coating 2, the second reinforcing coating 4, and the active coating 1 achieves a gradient transition interface with chemical compatibility and thermomechanical matching, effectively eliminating interfacial barriers between different coating layers. This significantly enhances the adhesion between the reinforcing coating and the active coating 1, reduces interfacial contact resistance, and ensures consistent electrochemical stability and swelling behavior of each layer in the electrolyte.
[0068] In some embodiments, the first adhesive, the second adhesive, and the third adhesive each independently include at least one of polyvinylidene chloride and polyvinylidene fluoride-hexafluoropropylene, for example, polyvinylidene chloride.
[0069] Based on the same inventive concept, this application provides a method for preparing a positive electrode sheet, including the following steps: An active slurry is coated on a first region of at least one side surface of the current collector, and after drying, a current collector containing the active coating 1 is obtained. A first conductive paste is coated on the second region of the current collector surface containing the active coating 1, and the first conductive layer is obtained after drying. A second conductive paste is coated onto the surface of the first conductive layer and dried to obtain the second conductive layer, forming a reinforced coating. The positive electrode sheet is obtained after die cutting; The first region is a current collector region for setting the active coating 1, and the second region is a current collector region and a tab region for setting the reinforcing coating. The reinforcing coating includes a first reinforcing coating 2.
[0070] In some embodiments, the preparation of the first conductive paste includes the following steps: The first conductive material, binder, and additives are mixed in the first solvent to obtain the first conductive paste.
[0071] In some embodiments, the viscosity of the first conductive paste is 7000 mPa·s to 9000 mPa·s. For example, it can be 7000 mPa·s, 8000 mPa·s, 9000 mPa·s, or other values within the above range.
[0072] In some embodiments, the solid content of the first conductive paste is 10% to 12%. For example, it can be 10%, 11%, 12%, or other values within the above range.
[0073] In some embodiments, the first solvent includes at least one of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. For example, it may be N-methylpyrrolidone or N,N-dimethylformamide.
[0074] In some embodiments, the preparation of the second conductive paste includes the following steps: The second conductive material, conductive reinforcing agent, second binder, and additives are mixed in a second solvent to obtain a second conductive slurry.
[0075] In some embodiments, the viscosity of the second conductive paste is 8000 mPa·s to 12000 mPa·s. For example, it can be 8000 mPa·s, 10000 mPa·s, 12000 mPa·s, or other values within the above range.
[0076] In some embodiments, the solid content of the second conductive paste is 15% to 25%. For example, it can be 15%, 20%, 25%, or other values within the above range.
[0077] In some embodiments, the second solvent includes at least one of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. For example, it may be N-methylpyrrolidone or N,N-dimethylformamide.
[0078] In some embodiments, the coating of the first and second conductive pastes is preferably performed using a dual-channel slit extrusion coating machine with a die spacing of 15 mm; coating speed: 10~12 m / min; oven pre-drying section: temperature: 85~88℃, air velocity: 6~8 m / s, time: 1~3 min, to quickly remove solvent and initially establish interlayer bonding; cross-linking curing section: temperature: 105~110℃, air velocity: 4~6 m / s, time: 2~5 min, to promote cross-linking reaction, allowing the molecular chains of the first and second binders to acquire sufficient mobility, enabling further diffusion and entanglement within and between layers of the coating, forming a denser and more stable polymer network structure. Simultaneously, the high temperature also promotes the full cross-linking reaction between the carboxyl groups and other functional groups in the first conductive layer and the binder, further improving the mechanical properties and interfacial bonding strength of the coating.
[0079] In some embodiments, a rolling step is included after the drying process to reinforce the coating with a compaction density of 2.2~2.8 g / cm³. 3 .
[0080] Based on the same inventive concept, embodiments of this application provide a battery including a positive electrode sheet, wherein the positive electrode sheet includes the aforementioned positive electrode sheet, or includes a positive electrode sheet prepared according to the aforementioned preparation method.
[0081] Because this battery contains the positive electrode provided in the embodiments of this application, it has superior safety and cycle life.
[0082] In some embodiments, the battery may be a lithium-ion battery. The battery stacking type may be, for example, a wound or stacked battery, and the structural type may be, for example, a prismatic (aluminum, steel, etc.) battery, a pouch battery, or a cylindrical battery, etc., and there is no specific limitation.
[0083] In some embodiments, the battery further includes a negative electrode, an electrolyte, and a separator. That is, the battery includes a positive electrode, a negative electrode, an electrolyte, and a separator.
[0084] In this embodiment, the materials and structures of the negative electrode current collector, the conductive agent and the binder in the negative electrode active coating are not limited, and the positive electrode structure and composition known in the art that can be used in secondary batteries can be selected.
[0085] In this embodiment, the specific material or type of the separator is not limited, and any separator known in the art that can be used in secondary batteries can be selected.
[0086] It should also be noted that the battery in this application does not limit the specific material or type of electrolyte. Any components and types known in the art that can be used in secondary batteries can be selected, as long as the purpose of this application can be achieved.
[0087] Since the battery provided in this embodiment of the invention adopts all the technical solutions of the above embodiments, it has at least all the beneficial effects brought about by the technical solutions of the above embodiments, and will not be described in detail here.
[0088] The following describes the implementation methods of this application. The implementation methods described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the implementation methods, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents, materials, or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0089] Example 1 Preparation of the first conductive paste Weigh metallic single-walled carbon nanotube (SWCNT) powder and vacuum dry at 200℃ for 2 hours to remove adsorbed moisture and gas. Place the dried SWCNT in a three-necked flask, and slowly pour in a mixed acid (H2SO4:HNO3 mass ratio 9:3), with a SWCNT to mixed acid mass ratio of 1:80, ensuring the SWCNT is completely submerged. Place the flask on a magnetic stirrer, install a reflux condenser, and turn on stirring and heating, continuously refluxing at 60℃ for 4 hours. After the reaction is complete, allow it to cool naturally to room temperature. Slowly pour the reaction mixture into a large amount of 4℃ ice-water mixture for dilution and to terminate the reaction. Wash repeatedly using a centrifuge until the pH of the supernatant is close to 7. Transfer the washed carboxylated SWCNT filter cake to a vacuum oven and vacuum dry at 60℃ for 24 hours. After drying, gently grind the lumpy product to obtain a fluffy carboxylated SWCNT powder with a carboxyl group content of 1.5 at.
[0090] Polyvinylidene fluoride (PVDF) powder was dissolved in a solvent comprising 65% of the total N-methylpyrrolidone (NMP) to form a homogeneous slurry. Under continuous stirring, 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIMBF4) ionic liquid was added to the slurry and stirred until homogeneous. The carboxylated SWCNTs were slowly added at 3000 rpm using a high-speed shear disperser. The remaining 35% of the NMP solvent was added, and the slurry was transferred to a planetary ball mill and ball-milled at 600 rpm for 8 hours to obtain a homogeneous and stable first conductive slurry with a viscosity of 7000 mPa·s and a solid content of 10%. The mass ratio of carboxylated SWCNTs, PVDF, and EMIMBF4 was 78:20:1.
[0091] Preparation of the second conductive paste PVDF was dissolved in NMP. Sheet graphene was added to the PVDF solution under low-speed stirring, first stirred at 1000 rpm, then dispersed at 5000 rpm for 50 minutes. Titanium diboride (TiB2) submicron particles with a D50 of 200 nm and polyamide-imide (PAI) were added, and the mixture was transferred to a planetary ball mill and ball-milled for 8 hours to obtain a uniformly dispersed second conductive slurry with a viscosity of 8000 mPa·s and a solid content of 15%. The mass ratio of TiB2, sheet graphene, PVDF, and PAI was 70:6:10:2.
[0092] Preparation of active substance slurry The positive electrode active material lithium iron phosphate, conductive agent conductive carbon black and binder PVDF are mixed in a mass ratio of 95:3:2 to obtain the upper mixed material; the positive electrode active material lithium iron phosphate, conductive agent conductive carbon black and binder PVDF are mixed in a mass ratio of 96:2:2 to obtain the bottom mixed material; the mixed materials are thoroughly stirred in NMP to obtain the positive electrode slurry.
[0093] Current collector pretreatment The current collector is made of 15μm thick aluminum foil, which is ultrasonically cleaned with 1% dilute acid to remove surface oil and oxides; then dried in an oven at 80℃ for 10 minutes. Functional areas are defined: the reinforced area is located at the base of the tab, with a width consistent with the tab width and a length L1 equal to 35% of the total tab length L; the active area is coated with active material and is tightly connected to the reinforced area boundary; and the welding area is located at the end of the tab, with a length of 4mm.
[0094] Slurry coating A dual-channel slot extrusion coating machine was used, with a die spacing of 15mm and a coating speed of 10m / min. The slurry for both the reinforced and active regions was coated simultaneously. After coating, the slurry entered an oven. The pre-drying section was at 85℃ with an air velocity of 6m / s for 3 minutes; the cross-linking curing section was at 105℃ with an air velocity of 6m / s for 5 minutes. After drying, a reinforced coating and an active coating were obtained. These were then rolled (the compaction density of the reinforced coating and the active coating were both 2.4g / cm³). 3 2.5g / cm 3 The positive electrode sheet is obtained by ( ). The total thickness of the reinforcing coating is 26 μm, of which the thickness of the bottom layer (first conductive layer) is 13 μm, the thickness of the top layer (second conductive layer) is 13 μm, and the thickness of the activation material layer is 80 μm.
[0095] Example 2 The difference between Example 2 and Example 1 is that in Example 2, the mass ratio of carboxylated SWCNT, PVDF and EMIMBF4 is 70:25:1 when preparing the first conductive paste.
[0096] Example 3 The difference between Example 3 and Example 1 is that in Example 3, the mass ratio of carboxylated SWCNT, PVDF and EMIMBF4 is 82:30:3 when preparing the first conductive paste.
[0097] Example 4 The difference between Example 4 and Example 1 is that in Example 4, the mass ratio of TiB2:sheet graphene:PVDF:PAI in the preparation of the second conductive paste is 70:6:10:2.
[0098] Example 5 The difference between Example 5 and Example 1 is that in Example 5, the mass ratio of TiB2:sheet graphene:PVDF:PAI is 85:10:10:2 when preparing the second conductive paste.
[0099] Example 6 The difference between Example 6 and Example 1 is that the thickness of the first conductive layer in Example 6 is 3 μm and the thickness of the second conductive layer is 3 μm.
[0100] Example 7 The difference between Example 7 and Example 1 is that the thickness of the first conductive layer in Example 7 is 20 μm and the thickness of the second conductive layer is 20 μm.
[0101] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 uses uncarboxylated SWCNTs.
[0102] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 does not contain a first conductive layer, and the thickness of the second conductive layer is 26 μm.
[0103] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that Comparative Example 3 does not contain a second conductive layer, and the thickness of the first conductive layer is 26 μm.
[0104] Performance testing 1. Test of bending resistance of tab coating Test principle: By simulating the repeated bending stress that the tabs may experience during battery assembly and use, the mechanical integrity (crack resistance, peeling resistance) and the stability (resistance change) of the conductive path of the functional coating are evaluated.
[0105] Cut sample strips containing the tab regions coated with the functional coating from the prepared positive electrode sheet. The sample strips are typically 20 mm wide and long enough to be clamped and bent. Ensure good electrical connections at both ends of the sample strip (for clamping and connecting the resistance meter). Secure the sample strip flat on the test fixture, ensuring the bending axis is aligned with the mandrel center. Use a four-wire resistance meter to measure and record the initial resistance value R0 of the tab coating area on the sample strip. The measurement location should cover the entire functional coating area. Observe and record the coating surface condition under an optical microscope, ensuring there are no initial cracks or damage. Start the bending test machine and set the parameters: Bending angle: 180° (i.e., bending from a straight position at 0° to a position parallel to the starting face). Bending rate: 30 times / minute. Total number of cycles: 100 cycles (one cycle includes bending from 0° to 180° and returning to 0°). During the test, monitor and record the resistance value R0 every 10 cycles. n (n is the current cycle number). After 100 bends, carefully remove the sample and place it flat on the observation table. Visually inspect the coating for visible cracks, peeling, powdering, or flaking. Final resistance measurement: Measure the resistance R again at the same location as in the initial state using the four-wire method. 100 Calculation of resistance change rate: Resistance change rate = [(R)] 100 – R0) / R0] × 100%.
[0106] 2. Battery manufacturing Preparation of negative electrode sheet: The negative electrode active material (graphite), conductive agent (conductive carbon black) and binder (CMC) are mixed in a mass ratio of 96:2:2 to obtain a mixed material. The mixed material is thoroughly stirred in deionized water to obtain a negative electrode slurry. The obtained slurry is coated on conventional copper foil (copper foil thickness 4.5μm), and after drying and rolling, a negative electrode sheet is obtained.
[0107] The separator is made of 7μm PE base film, and a 3μm PVDF adhesive layer is coated on both sides of the PE base film and a 3μm ceramic layer is coated on one side (the ceramic layer faces the positive electrode to prevent the risk of high voltage breakdown).
[0108] Electrolyte: Ethylene carbonate (EC) and dimethyl carbonate (DMC) are mixed in a volume ratio of 1:1. Then, fully dried lithium salt LiPF6 is dissolved in the mixed organic solvent at a ratio of 1 mol / L to prepare the electrolyte.
[0109] Battery assembly: After weighing, the electrode sheets are directly used as the negative electrodes of the lithium-ion batteries. The 2032 coin cell is assembled in an Ar-filled glove box. The assembly sequence from top to bottom is: negative electrode shell, gasket, spacer, lithium sheet, separator, self-supporting electrode sheet, and positive electrode shell, resulting in a coin cell. (1) Internal resistance test The internal resistance of different groups of batteries was obtained using a battery internal resistance meter.
[0110] (2) Energy density test First, weigh the battery and record the weight as m. Then, at 25°C, charge the battery at a constant current of 0.33C to 3.65V, and then charge it at a constant voltage of 3.65V until the current is ≤0.05C. After standing for 5 minutes, discharge it at a constant current of 0.33C to 2.0V to obtain the discharge energy Q. The battery energy density is calculated as Q / m.
[0111] (3) 200-cycle capacity retention test At 25℃, with initial and cutoff voltages of 2.2V and 3.65V respectively, the battery is first charged at 1C to 3.65V, then charged at a constant voltage of 3.65V until the current decreases to 0.05C. Next, it is discharged at 0.5C to 2.2V, then charged at 1C to 3.65V again, then charged at a constant voltage of 3.65V until the current decreases to 0.05C, and finally discharged at 0.5C to 2.2V. This charging and discharging cycle is repeated, and the discharge capacity of each cycle is recorded. For example, the capacity retention rate of the Nth cycle = discharge capacity of the Nth cycle / discharge capacity of the first cycle × 100%. Calculate the capacity retention rate after the 200th cycle.
[0112] The test results of each embodiment and comparative example are shown in Table 1.
[0113] Table 1 Based on the test results of the examples and comparative examples, the electrochemical performance of the batteries prepared in Examples 1-7 is significantly better than that of Comparative Examples 1-3, indicating that the positive electrode prepared in this application can effectively solve the problem of electrode tab mechanical reinforcement. Among them, the battery prepared in Example 1 achieved a capacity retention rate of 97% after 200 cycles at room temperature. The improved conductivity at the edge of the positive electrode effectively reduced the internal resistance of the battery, thereby improving the battery capacity retention rate.
[0114] The test results from Comparative Example 1 show that the removal of SWCNT carboxylation weakens the inter-material bonding, resulting in decreased bending resistance and conductivity. Removing the top layer of graphene hinders the formation of a three-dimensional conductive network, leading to weak conductivity.
[0115] The test results of Comparative Examples 2 and 3 show that the dual-layer composite structure of the present invention, with its highly conductive bottom layer and highly hard top layer, has irreplaceable synergistic advantages. A single functional layer cannot simultaneously meet the dual requirements of conductivity and anti-bending performance for the tab area. The lack of a conductive network in the bottom layer prevents effective current collection. When the hard TiB2 layer is directly coated onto the aluminum foil surface, the lack of a flexible CNT bottom layer for transition leads to stress concentration between layers after hot pressing and cooling, making it prone to brittle cracking or even large-area peeling during bending or vibration. The absence of a hard layer makes the tabs susceptible to scratches from tooling during cutting, winding, and ultrasonic welding processes, increasing the risk of internal short circuits.
[0116] The parts of this invention not described in detail are techniques known to those skilled in the art.
[0117] The basic principles of the present invention have been described above with reference to specific embodiments. However, it should be noted that the advantages, benefits, and effects mentioned in the present invention are merely examples and not limitations, and should not be considered as essential features of each embodiment of the present invention. Furthermore, the specific details disclosed above are for illustrative and facilitative purposes only, and are not limitations. These details do not limit the present invention to the necessity of employing the aforementioned specific details.
[0118] It should be noted that the terms "and / or" or " / " used herein are merely descriptions of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. The singular forms "a," "described," and "the" used in the embodiments of the invention and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise.
[0119] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, then the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single element or multiple elements. Item B may contain a single element or multiple elements. Item C may contain a single element or multiple elements.
[0120] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A positive electrode plate, characterized in that, The positive electrode includes: Current collector and tabs formed by extending from said current collector; An active coating is disposed on at least one surface of the current collector; A first reinforcing coating is disposed on at least one side surface of the root of the electrode ear; The reinforcing coating includes a lower first conductive layer and an upper second conductive layer; The first conductive layer includes a first conductive material, and the second conductive layer includes a second conductive material; The first conductive material includes at least one of carboxylated metallic carbon nanotubes and carboxylated graphene nanosheets; the second conductive material includes at least one of transition metal borides, transition metal carbides / nitrides, and carbon-based superhard materials. The term "base of the electrode" refers to the end of the electrode closest to the current collector.
2. The positive electrode sheet according to claim 1, characterized in that, The length of the first reinforcing coating is 30% to 70% of the length of the tab, and the width of the first reinforcing coating is the same as the width of the tab.
3. The positive electrode sheet according to claim 1, characterized in that, The positive electrode further includes a second reinforcing coating, which is disposed on at least one side of the edge at the junction of the current collector and the electrode tab. The length of the second reinforcing coating is 1~2μm, and the width of the second reinforcing coating is the same as the width of the current collector.
4. The positive electrode sheet according to claim 1, characterized in that, The first conductive layer satisfies at least one of the following features (1) to (4): (1) The first conductive layer further includes a first adhesive and an additive, wherein the mass ratio of the first conductive material, the first adhesive, and the additive is (70~82):(20~30):(1~3); The additive includes at least one of 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, and N-butyl-N-methylpyrrolidine bis(trifluoromethanesulfonyl)imide. (2) The content of carboxyl groups in the carboxylated metallic carbon nanotubes is 1 at%~2 at%; (3) The content of carboxyl groups in the carboxylated graphene nanosheets is 1 at%~2 at%; (4) The thickness of the first conductive layer is 3μm~20μm.
5. The positive electrode sheet according to claim 1, characterized in that, The second conductive layer satisfies at least one of the following features (1) to (3): (1) The second conductive layer further includes a conductive reinforcing agent, a second binder, and an additive, wherein the mass ratio of the second conductive material, the conductive reinforcing agent, the second binder, and the additive is (70~85):(6~10):(10~18):(2~5); The conductive enhancer includes at least one of graphene and graphite nanosheets; The additives include at least one of polyamide imide, polyether imide, and polysulfone; (2) The particle size Dv50 of the second conductive material is 200nm~500nm; (3) The thickness of the second conductive layer is 3μm~20μm.
6. The positive electrode sheet according to claim 1, characterized in that, The active coating includes a third binder; The first adhesive, the second adhesive, and the third adhesive are selected from the same type of adhesive; The first adhesive, the second adhesive, and the third adhesive each independently include at least one of polyvinylidene chloride and polyvinylidene fluoride-hexafluoropropylene.
7. A method for preparing a positive electrode sheet, characterized in that, Includes the following steps: An active slurry is coated on a first region of at least one side surface of the current collector, and after drying, a current collector containing an active coating is obtained. A first conductive paste is coated on a second region of the current collector surface containing an active coating, and after drying, a first conductive layer is obtained. A second conductive paste is coated onto the surface of the first conductive layer and dried to obtain the second conductive layer, forming a reinforced coating. The positive electrode sheet is obtained after die cutting; The first region is a current collector region for setting an active coating, and the second region is a current collector region and a tab region for setting a reinforcing coating. The reinforcing coating includes a first reinforcing coating.
8. The preparation method according to claim 7, characterized in that, The preparation of the first conductive paste includes the following steps: The first conductive material, binder, and additives are mixed in a first solvent to obtain a first conductive paste. The viscosity of the first conductive paste is 7000 mPa·s to 9000 mPa·s; The solid content of the first conductive paste is 10%~12%; The first solvent includes at least one of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
9. The preparation method according to claim 7, characterized in that, The preparation of the second conductive paste includes the following steps: The second conductive material, the conductive reinforcing agent, the second binder, and the additives are mixed in the second solvent to obtain the second conductive slurry; The viscosity of the second conductive paste is 8000 mPa·s to 12000 mPa·s; The solid content of the second conductive paste is 15%~25%; The second solvent includes at least one of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
10. A battery, comprising a positive electrode, characterized in that, The positive electrode sheet includes the positive electrode sheet according to any one of claims 1 to 6, or the positive electrode sheet prepared by the preparation method according to any one of claims 7 to 9.