Composite cathode materials, composite cathodes and batteries
By using composite materials of graphene and conductive graphite, and the improved hydrothermal reaction of graphene oxide with p-phenylenediamine, a stable conductive network is formed, which solves the conductivity and strength problems of carbon-based conductive agents in batteries, and improves the energy density and cycle stability of batteries.
Patent Information
- Application Number
- CN202510618352.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing carbon-based conductive agents have limited specific surface area and insufficient interfacial bonding when constructing conductive networks, which makes electron/ion transport channels prone to breakage, affecting the rate performance and cycle stability of batteries.
Graphene oxide was prepared by modifying the Hummers method using graphene and conductive graphite composite materials, and p-phenylenediamine was used as a structural modifier to form a stable conductive network through hydrothermal reduction reaction. Polyimide was then used as a binder to enhance the electrode strength.
It improves the conductivity and mechanical strength of the electrodes, enhances the energy density and cycle stability of the battery, effectively inhibits electrolyte decomposition, and extends battery life.
Smart Images

Figure CN123120729A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of chemical electrode material manufacturing, and more specifically, to a composite cathode material, a cathode using the cathode material, and a battery. Background Technology
[0002] With the increasing demands of new energy vehicles for higher energy density, faster charging performance, and longer cycle life of power batteries, performance optimization of cathode materials for ion batteries has become a core focus of technological breakthroughs in the industry. While current mainstream carbon-based conductive agents (such as acetylene black and carbon nanotubes) can construct conductive networks, their limited specific surface area and insufficient interfacial bonding with active materials make electron / ion transport channels prone to breakage during high-rate charge and discharge, severely restricting the battery's rate performance and cycle stability.
[0003] Graphene, as a novel two-dimensional carbon material, offers an ideal carrier for constructing three-dimensional conductive networks due to its ultra-high specific surface area (2630 m² / g) and electron mobility (15000 cm² / V·s). However, its practical application still faces three major technical bottlenecks: First, the van der Waals forces between graphene sheets easily lead to stacking and aggregation, reducing the effective specific surface area and hindering ion diffusion; second, pure graphene has insufficient mechanical strength, and cracks easily occur during electrode coating, leading to structural collapse; third, traditional mechanical mixing methods are difficult to achieve stable composites of graphene with other conductive agents (such as carbon nanotubes), and weak interfacial bonding forces lead to dynamic instability of the conductive network during charging and discharging.
[0004] Therefore, it is indeed necessary to provide an improved composite cathode material to achieve a dual breakthrough in the construction of the conductive network of carbon materials and the stability of the electrode structure. Summary of the Invention
[0005] The purpose of this invention is to provide a composite cathode material, cathode sheet, and battery to solve the problems of low capacity, low strength, and rapid capacity decay of carbon materials.
[0006] A composite cathode material is prepared by the following method: carbon material powder is dispersed in a first solvent and ultrasonically dispersed to obtain a carbon material dispersion; a structural modifier is mixed with the carbon material dispersion and subjected to a hydrothermal reduction reaction to obtain a composite cathode material dispersion; the composite cathode material dispersion is centrifuged, precipitated, washed, and dried to obtain the composite cathode material.
[0007] Furthermore, the carbon material includes a first carbon material and a second carbon material, wherein the first and second carbon materials are selected from graphene, conductive graphite, conductive carbon black, carbon nanotubes, activated carbon, and chopped carbon fibers.
[0008] Graphene possesses a two-dimensional honeycomb lattice structure of tightly packed carbon atoms, with large multi-atom π bonds running through the entire layer, thus exhibiting excellent electrical conductivity. Graphene's layered structure can supplement the internal conductive network of electrodes, enhancing electrode conductivity; however, its small particle size and poor dispersibility make it prone to agglomeration. Conductive graphite exhibits highly unequal-axis flake-like structures with an average thickness of 57 nm, containing a large number of free electrons, which is beneficial for creating thin electrode coatings to improve battery capacity. Simultaneously, graphite's layered structure helps improve the peeling force of coatings on the electrode surface, thereby enhancing electrode strength. Conductive carbon black particles aggregate into chain-like or grape-like structures, exhibiting high structural integrity, a large specific surface area, and tight packing, which facilitates close particle contact and the formation of a conductive network. Carbon nanotubes mainly consist of several to dozens of layers of coaxial cylindrical tubes composed of hexagonally arranged carbon atoms, with a layer-to-layer distance of approximately 0.34 nm. The carbon material of this invention can also be carbon nanotubes, whose structure is the same as the layered structure of graphite, exhibiting good electrical conductivity when used as electrode materials. Short-cut carbon fiber is made by processing carbon fibers into bundles with a slugging agent and then cutting them to a specified length. It has high strength, high modulus, and low electrical resistance, and can effectively enhance the strength and toughness of the cathode surface.
[0009] Furthermore, the first carbon material is graphene, and the second carbon material is conductive graphite.
[0010] Graphene is a two-dimensional structure formed by a single layer of tightly packed carbon atoms, while conductive graphite is essentially composed of multiple stacked graphene layers. This similar layered structure allows graphene and graphite to maintain good compatibility and interfacial bonding when composited. The difference in the number of continuous layers between graphene and graphite provides the composite material with a rich conductive network and spatial structure. Graphene's single-layer structure enables extremely fast electron transport and excellent conductivity; while graphite's multilayer structure provides more charge storage space and more stable structural support. When the two are composited, the conductive network of graphene can run throughout the entire composite material, forming a highly efficient charge transport channel. Simultaneously, graphite's multilayer structure provides the composite material with more pores and channels, facilitating electrolyte penetration and ion diffusion.
[0011] Furthermore, the first carbon material is graphene oxide prepared by the improved Hummers method.
[0012] The improved Hummers method offers several advantages over other graphene oxide preparation methods, such as the Brodie and Staudenmaier methods, including simpler operation, lower cost, shorter reaction time, higher efficiency, and higher safety. Graphene oxide possesses abundant carboxyl, hydroxyl, and epoxy functional groups, which enhance its solubility in polar solvents, facilitating the preparation of uniform electrode materials. Simultaneously, the steric hindrance effect increases the interlayer spacing of graphene, reducing interlayer aggregation and promoting ion diffusion and transport in the electrode material. Furthermore, it facilitates covalent functionalization of graphene, making it an optimal raw material for further functionalization.
[0013] The high specific surface area and abundant functional groups of graphene oxide enable electrode materials to store more charge, thereby increasing the energy density of the battery. The conductive network and ion diffusion channels of graphene oxide facilitate rapid charge transport and ion diffusion, allowing the electrode materials to maintain excellent performance under high-rate charge-discharge conditions. Simultaneously, the structural stability of graphene oxide ensures that the electrode materials maintain structural integrity during charge-discharge processes, thus improving cycle stability.
[0014] Furthermore, the structural modifier is one or a mixture of at least two of p-phenylenediamine, o-phenylenediamine, and m-phenylenediamine.
[0015] The structural modifier phenylenediamine undergoes thermal polymerization on the surface and between the layers of carbon material powder, significantly strengthening the network structure between the carbon material layers and improving the strength and stability of the composite electrode material. Phenylenediamine also possesses reducing properties, reducing graphene oxide during hydrothermal processes, further increasing the electronic conductivity of the composite material.
[0016] The two amino groups in the phenylenediamine molecule have lone pairs of electrons, which can react with the dissociation products of AlCl3 in the electrolyte (such as Al2Cl7). - AlCl4 -Coordination bonds are formed. During hydrothermal treatment, the amino group is partially oxidized to nitrogen-containing functional groups (such as pyridine nitrogen and pyrrole nitrogen). These nitrogen-doped sites further fix Cl· through electrostatic adsorption or hydrogen bonding, inhibiting the migration of Cl· and electrolyte decomposition. Simultaneously, the pore structure and surface functional groups of nitrogen-doped carbon can physically confine Cl·, reducing its loss during cycling and lowering the corrosion rate of the aluminum anode by the electrolyte. Further, the structural modifier is preferably p-phenylenediamine. During positive electrode charging, aluminum tetrachloride anions convert electrons into chlorine radicals and aluminum heptachloride anions. After accumulation, chlorine radicals undergo a coupling reaction to produce chlorine gas. This chlorine gas travels to the negative electrode and reacts with the aluminum, corroding it and causing capacity loss. The p-phenylenediamine structural modifier in this invention can effectively fix chlorine radicals on the positive electrode, allowing chlorine gas to come into contact with electrons during discharge, reducing chlorine radicals or chlorine gas to aluminum tetrachloride anions and preventing capacity loss.
[0017] p-Phenylenediamine has a symmetrical structure, and the degree of polymerization can be effectively controlled by adjusting hydrothermal conditions during the polymerization process. During hydrothermal polymerization, most of the oxygen-containing groups in graphene oxide are consumed by p-phenylenediamine. The remaining p-phenylenediamine molecules partially adhere to the graphene and graphite surfaces, while some react with themselves to form p-phenylenediamine oligomers that aggregate between layers, increasing interlayer spacing and reducing graphite agglomeration. Loading p-phenylenediamine effectively disrupts the integrity of the graphene network structure, thereby increasing the porosity and specific surface area of the composite electrode material.
[0018] Furthermore, the first solvent is at least one of methanol, ethanol, acetone, and water.
[0019] Furthermore, the hydrothermal reaction temperature is 70-150℃, and the reaction time is 2-24h.
[0020] The present invention also provides a method for preparing the composite positive electrode, comprising the following steps: The composite cathode material and binder are added to a second solvent, heated and stirred thoroughly to obtain a cathode slurry; the composite cathode material slurry is uniformly coated onto a current collector and dried until the solvent is completely evaporated and a solid film is formed to obtain a uniform, crack-free battery cathode sheet.
[0021] Further, the second solvent is one or more of N-methylpyrrolidone, dichloromethane, toluene, xylene, n-hexane, and cyclohexanone; the adhesive is one or more of pyromellitic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, polyvinylidene fluoride, styrene-butadiene rubber, and polyacrylic acid; and the current collector is one of carbon cloth, carbon sheet, nickel foam, and aluminum foil.
[0022] When polyimide is used as an electrode binder, there is a problem in its processing and molding, because polyimide has a high melting point and is difficult to directly form into thin films. Therefore, a two-step method is usually adopted. First, polyamic acid is generated by the low-temperature polycondensation reaction of dianhydride and diamine. The polyamic acid solution is then formed into a thin film using an appropriate film-forming method (such as impregnation or casting). Then, an intramolecular dehydration cyclization reaction is carried out at high temperature to convert the polyamic acid into polyimide. In this invention, amino organic compounds are added during the synthesis of composite cathode materials, and oligomers are formed on carbon materials through a sufficient hydrothermal reaction. When preparing the cathode slurry, the dianhydride in the added binder can fully crosslink and polycondense with the diamine, a structural modifier in the cathode material, under heating conditions to form polyamic acid. After the cathode slurry is coated onto the current collector to form a film, it is dried at high temperature to produce polyimide. The synthesis of polyimide can not only serve as a supplementary binder to fully bond the cathode material powder and current collector, enhancing the strength of the cathode sheet, but it can also polymerize with p-phenylenediamine between carbon material layers to further increase the interlayer spacing of the graphite sheet, enhance the electronic conductivity network between carbon materials, and thus improve the conductivity of the electrode sheet.
[0023] Furthermore, the heating temperature is 40–70°C, the drying temperature is 60–200°C, and the drying time is 1–4 hours.
[0024] The present invention also provides a battery comprising a positive electrode, an electrolyte, a negative electrode, and a separator as described in the present invention, wherein the separator is a glass fiber membrane and the electrolyte is an aluminum chloride-based room temperature molten salt.
[0025] Furthermore, the aluminum chloride-based room temperature molten salt is one of aluminum chloride-1-ethyl-3-methylimidazolium chloride, aluminum chloride-1-butyl-3-methylimidazolium chloride, aluminum chloride-triethylamine hydrochloride, aluminum chloride-urea, aluminum chloride-acetamide, aluminum chloride-propionamide, and aluminum chloride-butyramide.
[0026] The beneficial effects of this invention are: The composite cathode material provided by this invention can effectively improve the porosity and conductive structure of carbon cathodes, increase current density, and achieve higher energy density and discharge rate. The composite cathode material prepared by this invention can effectively improve the strength and stability of electrode sheets, and improve the first-efficiency and cycle efficiency of secondary batteries.
[0027] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and are not intended to limit the invention. Attached Figure Description
[0028] Figure 1 Example 1 shows the 0.1C, 0.5C, and 2C charge-discharge curves of the battery.
[0029] Figure 2Examples 1, 2, and 3 show the capacity retention rate of batteries after 1000 cycles. Detailed Implementation
[0030] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0031] It should be noted that in this application, the graphene oxide is prepared by a modified Hummers method. The surface of the graphene oxide contains abundant oxygen-containing functional groups, and the abundance of oxygen-containing functional groups is beneficial for the next step of functionalization modification of the graphene oxide.
[0032] In some embodiments, the method for preparing the graphene oxide may specifically include: 20g of graphite powder was placed in a 500mL beaker, and 200mL of concentrated H₂SO₄ was added and stirred for 5min. Then, 20g of KMnO₄ was added under an ice-water bath and stirred continuously for 15min to obtain a dark green solution. The beaker was then placed in a 60℃ constant temperature water bath for 2h to obtain a brown solution. 50mL of distilled water was added to the mixed solution, and it was transferred to a 95℃ constant temperature water bath for stirring. After 15min, another 50mL of distilled water was added. After cooling to room temperature, hydrogen peroxide was added while stirring until the mixed liquid turned a bright yellow. The mixed solution was washed with distilled water until neutral and sonicated for 1h. The mixed solution was centrifuged, and the precipitate was dried at 90℃ for 24h to obtain dry graphene oxide powder. Example 1
[0033] Step 1: Preparation of the positive electrode: 2g of graphene oxide (the first carbon material) and 8g of conductive graphite powder (the second carbon material) were ultrasonically dispersed in 100ml of ethanol for 10min to obtain a carbon composite material dispersion. 1g of p-phenylenediamine (a structural modifier) was added to the above carbon composite material dispersion, stirred evenly, and then transferred to a high-pressure reactor lined with polytetrafluoroethylene. After hydrothermal reduction reaction at 100℃ for 12h, a carbon composite material dispersion was obtained. The composite cathode material dispersion was centrifuged to precipitate, washed, vacuum dried at 60℃ for 8h, and ground to obtain composite cathode material powder.
[0034] Weigh 10g of the composite cathode material prepared above and 1g of pyromellitic dianhydride, add them to 100ml of N-methylpyrrolidone solvent, stir evenly, and heat to 60℃ for 2h to obtain a composite cathode slurry. Coat the composite cathode slurry evenly onto carbon cloth and dry at 150℃ for 2h to prepare a composite cathode sheet.
[0035] Step 2: Preparation of the negative electrode: The negative electrode is metallic aluminum, which is prepared into 0.1 mm aluminum foil electrodes by rolling, cutting and cleaning.
[0036] Step 3: Preparation of electrolytes: At room temperature, 160g of 1-ethyl-3-methylimidazolium chloride and 220g of anhydrous aluminum chloride were weighed and dried in an oven at 105℃ for 12h to completely remove moisture from the sample; 200g of anhydrous aluminum chloride and 146.6g of 1-ethyl-3-methylimidazolium chloride were weighed in a glove box, mixed and stirred thoroughly for 8h to obtain liquid molten salt electrolyte.
[0037] Step 3: Battery fabrication: Using glass filter paper as a separator, the positive electrode, separator, and negative electrode are sequentially placed in the battery packaging. Liquid electrolyte is injected between the positive and negative electrodes. The battery is then sealed, left to stand, and shaped to produce a secondary battery with dimensions of 40×100×100mm. 3 . Example 2
[0038] The preparation method and proportions of Example 2 are the same as those of Example 1, except that the first carbon material, graphene oxide, is changed to 1g in step one. Example 3
[0039] The preparation method and proportions of Example 3 are the same as those of Example 1, except that the first carbon material, graphene oxide, is changed to 3g in step one. Example 4
[0040] Example 4 is prepared in the same way and in the same proportion as Example 1, except that the binder in step one is replaced with 1,4,5,8-naphthalenetetracarboxylic dianhydride. Example 5
[0041] Example 5 is prepared in the same way and with the same proportions as Example 1, except that the binder in step one is replaced with polyvinylidene fluoride. Example 6
[0042] Example 6 is prepared in the same way and in the same proportion as Example 1, except that the adhesive in step one is replaced with polyacrylic acid. Example 7
[0043] The preparation method and proportions of Example 7 are the same as those of Example 1, except that the first carbon material in step one is replaced with graphene. Example 8
[0044] The preparation method and proportions of Example 8 are the same as those of Example 1, except that the second carbon material in step one is replaced with conductive carbon black. Example 9
[0045] The preparation method and proportions of Example 9 are the same as those of Example 1, except that the second carbon material in step one is replaced with activated carbon. Example 10
[0046] The preparation method and proportions of Example 10 are the same as those of Example 1, except that the second carbon material in step one is replaced with short-cut carbon fiber. Example 11
[0047] The preparation method and proportions of Example 11 are the same as those of Example 1, except that the structural modifier in step one is replaced with m-phenylenediamine. Example 12
[0048] Example 12 is prepared in the same way and in the same proportion as Example 1, except that the structural modifier in step one is replaced with o-phenylenediamine.
[0049] Comparative Example 1 The preparation method and proportions of Comparative Example 1 and Example 1 are the same, except that no structural modifier is added in step one.
[0050] A series of tests were performed on the various embodiments of the present invention using the following methods: Resistivity test: The overall resistance of the electrode is directly measured using an ACCFilm film resistance meter. The resistance measured includes the resistance of the probe itself, the contact resistance between the probe and the coating, the coating resistance, the contact resistance between the coating and the current collector, and the resistance of the current collector itself.
[0051] Battery capacity and first-efficiency test: At 25°C, the secondary batteries prepared in each example and comparative example were charged at a constant current rate of 0.1C to the charging cutoff voltage of 4.25V, and then charged at a constant voltage rate until the current ≤0.05C. After standing for 5 minutes, they were discharged at a constant current rate of 0.1C to the discharge cutoff voltage of 2V. This charge-discharge cycle was repeated 5 times to activate the batteries. The batteries activated at a 0.1C rate were then charged and discharged at rates of 0.1C, 0.5C, and 2C, and the battery capacity at different rates was measured.
[0052] Capacity retention test: At 25°C, the secondary batteries prepared in each example and comparative example were charged at a constant current rate of 0.33C to the charging cutoff voltage of 4.25V, then charged at a constant voltage until the current ≤0.05C, allowed to stand for 5 minutes, and then discharged at a constant current rate of 0.33C to the discharge cutoff voltage of 2V, allowed to stand for 5 minutes. This constitutes one charge-discharge cycle. The batteries were subjected to cyclic charge-discharge tests using this method, and the capacity retention rate of the secondary batteries after 1000 cycles was calculated.
[0053] The test results of each embodiment of the present invention are shown in Table 1.
[0054] Table 1
[0055] The phenylenediamine structural modifier provided by this invention polymerizes on the surface and between layers of carbon material powder under hydrothermal conditions, strengthening the network structure between the carbon material layers and providing abundant nitrogen functional groups, which is beneficial for improving the strength, conductivity, and chlorine fixation capability of the composite electrode material. The only difference in the operation steps between Example 1 and Comparative Example 1 is that no structural modifier was added in Comparative Example 1, while different isomers of phenylenediamine were used as structural modifiers in Examples 11 and 12. Among them, the resistance of the composite cathode prepared in Comparative Example 1 was 153 mΩ, which was much higher than that in Example 1, while the energy density and cycle retention rate were lower than those in Example 1, indicating that the phenylenediamine structural modifier provided by this invention has excellent modifying effect on composite carbon cathode materials.
[0056] The structural modifier phenylenediamine in this invention has three isomers: p-phenylenediamine, m-phenylenediamine, and o-phenylenediamine. Their different molecular structures determine their different properties. Among them, the symmetrical distribution of the para-amino group in p-phenylenediamine makes it easier to form a uniform carbon layer structure during carbonization. Therefore, in Examples 1, 11, and 12, the composite cathode using p-phenylenediamine as the structural modifier exhibits the best performance.
[0057] Due to their identical layered structure and different particle sizes, graphite and graphene, after hydrothermal composite with phenylenediamine, form a highly conductive network, which facilitates electron conduction. Therefore, when the first conductive agent in the composite cathode is conductive graphite and the second conductive agent is graphene nanoparticles, the composite cathode exhibits the best conductivity and the best battery performance. Thus, in Examples 1, 8, 9, and 10, when the first carbon material in the cathode slurry is graphene oxide, the different choices of the second carbon material significantly affect the performance of the composite cathode. When the second carbon material is conductive graphite, the composite cathode has the lowest resistance (39 mΩ) and the highest energy density (521 mAh / g) of the resulting battery. When the second carbon material is chopped carbon fiber, the composite cathode has the highest resistance (128 mΩ) and the lowest energy density (139 mAh / g) of the resulting battery.
[0058] Compared to untreated graphene, oxidized graphene has a higher specific surface area and more functional groups, providing more reaction sites and enhancing binding strength in hydrothermal composite reactions. This helps the electrode sheet store more charge, thereby improving the battery's energy density and high-rate performance. A comparison of the data from Examples 1 and 7 shows that when the second carbon material in the cathode slurry is entirely graphite, oxidizing the graphene of the first carbon material reduces the resistivity of the composite cathode from 109 mΩ to 39 mΩ, increases the 0.1C capacity density from 165 mAh / g to 521 mAh / g, and increases the 0.5C capacity density from 138 mAh / g to 499 mAh / g.
[0059] When the first and second carbon materials in the cathode slurry are of equal composition, the ratio between them will affect the internal conductive structure of the cathode, thus affecting the performance of the cathode and the battery. Graphene oxide has a small particle size; when added in excess, it tends to agglomerate, failing to form effective cross-links with the graphite sheet structure, resulting in excessively high local resistance. Conversely, when too little graphene oxide is added, its conductivity is not significant. In Examples 1 to 3, the first and second carbon materials are a combination of high-performance graphene oxide and graphite, with a mass ratio of 1 to 3:8. When the mass ratio of the first carbon material to the second carbon material is 2:8, the composite cathode has the lowest resistance of 39 mΩ, and the resulting battery has the highest energy density of 521 mAh / g.
[0060] Different binders have a certain impact on the resistance and mechanical properties of the composite cathode. Since the structural modifier in the cathode material provided by this invention is p-phenylenediamine, and dianhydride binders can form polymers with diamine, effectively bonding the carbon cathode slurry and current collector, this is beneficial for improving the uniformity and mechanical strength of the composite cathode. Different binders were used in Examples 1, 7-10. The composite cathode using a dianhydride binder had a lower resistance, the lowest being 39 mΩ, while the composite cathode prepared in Example 6, using polyacrylic acid, a commonly used binder for cathode materials, had a resistance of 63 mΩ.
[0061] The composite cathode material prepared by this invention can effectively improve the conductive structure of carbon cathode, increase current density, and achieve higher energy density and discharge rate. The composite cathode sheet prepared by this invention can effectively improve the strength and stability of the electrode sheet and adsorb chlorine free radicals and chlorine gas generated during charging and discharging, thereby improving the cycle efficiency of the secondary battery.
[0062] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions conceived without inventive effort should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. A composite cathode material, characterized in that, The composite cathode material is prepared by the following method: carbon material powder is dispersed in a first solvent and ultrasonically dispersed to obtain a carbon material dispersion; a structural modifier is mixed with the carbon material dispersion and subjected to a hydrothermal reduction reaction to obtain a composite cathode material dispersion; the composite cathode material dispersion is centrifuged, precipitated, washed, and dried to obtain the composite cathode material.
2. The composite cathode material according to claim 1, characterized in that, The carbon material includes a first carbon material and a second carbon material, which are selected from graphene, conductive graphite, conductive carbon black, carbon nanotubes, activated carbon, and chopped carbon fibers, respectively.
3. The composite cathode material according to claim 2, characterized in that, The first carbon material is graphene, the second carbon material is conductive graphite, and the first carbon material is graphene oxide prepared by the modified Hummers method.
4. The composite cathode material according to claim 1, characterized in that, The structural modifier is one or a mixture of at least two of p-phenylenediamine, o-phenylenediamine, and m-phenylenediamine.
5. The composite cathode material according to claim 1, characterized in that, The first solvent is at least one of methanol, ethanol, acetone, and water.
6. The composite cathode material according to claim 1, characterized in that, The hydrothermal reaction is carried out at a temperature of 70-150℃ for 2-24 hours.
7. A composite positive electrode, characterized in that, The preparation method includes the following steps: adding the composite cathode material and binder according to any one of claims 1 to 6 into a second solvent, heating and stirring thoroughly to obtain a cathode slurry; uniformly coating the composite cathode slurry onto a current collector, drying until the solvent is completely evaporated and a solid film is formed to obtain a composite cathode.
8. The composite positive electrode according to claim 7, characterized in that, The second solvent is one or more of N-methylpyrrolidone, dichloromethane, toluene, xylene, n-hexane, and cyclohexanone; the adhesive is one or more of pyromellitic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, polyvinylidene fluoride, styrene-butadiene rubber, and polyacrylic acid; and the current collector is one of carbon cloth, carbon sheet, nickel foam, and aluminum foil.
9. A battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte, characterized in that, The positive electrode is the composite positive electrode as described in claim 8, the negative electrode is aluminum foil, the separator is a glass fiber membrane, and the electrolyte is an aluminum chloride-based room temperature molten salt.
10. The battery according to claim 9, characterized in that, The aluminum chloride-based room temperature molten salt is one of aluminum chloride-1-ethyl-3-methylimidazolium chloride, aluminum chloride-1-butyl-3-methylimidazolium chloride, aluminum chloride-triethylamine hydrochloride, aluminum chloride-urea, aluminum chloride-acetamide, aluminum chloride-propionamide, and aluminum chloride-butyramide.