Methods for manufacturing electrode mixtures and electrode active material sheets

By melting ethylene carbonate during the mixing process of the electrode compound, and using it as a lubricant to reduce friction, the problem of damage to active material particles under high solid content was solved, thus achieving efficient preparation of the electrode compound.

CN123120731APending Publication Date: 2026-11-17TOYOTA JIDOSHA KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511999385.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2025-12-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

When mixing electrode compounds at high solid content, the surface of active material particles is easily damaged, and a high-power mixing device is required.

Method used

By at least partially melting ethylene carbonate during the mixing process, it acts as a lubricant to reduce the frictional load during mixing and allows for dry film formation at room temperature.

Benefits of technology

This method suppresses surface damage to active material particles and reduces reliance on high-power mixing equipment, thus achieving efficient electrode preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120731A_ABST
    Figure CN123120731A_ABST
Patent Text Reader

Abstract

This invention discloses a method for manufacturing an electrode mixture and a method for manufacturing electrode active material sheets. The object of this invention is to suppress the possibility of surface damage to active material particles during the mixing of electrode mixtures with high solids concentrations and / or the necessity of using high-power mixing equipment. The method of this invention for manufacturing an electrode mixture comprises: (a) providing an electrode mixture precursor comprising active material particles, a binder, and ethylene carbonate; and (b) mixing the electrode mixture precursor, wherein in step (b), the ethylene carbonate is at least partially melted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing an electrode mixture and a method for manufacturing electrode active material sheets. Background Technology

[0002] Electrode mixtures are mixtures containing at least active material particles and binders, used to form an active material layer.

[0003] For example, Patent Document 1 discloses an electrode for an energy storage device, comprising: a self-supporting dry electrode film containing dry carbon particles and dry microfiberized binder particles; and a current collector. The electrode described in Patent Document 1 has a low binder material content, low equivalent series resistance, and achieves the desired mechanical properties.

[0004] Furthermore, Patent Document 2 discloses an electrode for a secondary battery, comprising: a dry electrode membrane containing an active material with an average particle size of 0.05 μm to 3 μm, a conductive agent, and a fibrous binder; and a current collector on which the electrode membrane is stacked. The electrode described in Patent Document 2 comprises a dry electrode membrane, which, although containing active material with small particle size, exhibits excellent flexibility and minimizes breakage.

[0005] Patent Document 1: Japanese Patent Application Publication No. 2022-003694

[0006] Patent Document 2: Japanese Patent Publication No. 2024-505952 Summary of the Invention

[0007] In dry film formation using rolling, electrode binders need to be mixed at high solids concentrations. During this mixing process, especially during the fiberization of the binder, the surfaces of the active material particles may be damaged due to high friction between the particles constituting the electrode binder, and / or a high-power mixing device may be required.

[0008] Therefore, the object of the present invention is to suppress the above-mentioned problems when mixing electrode mixtures with high solid content.

[0009] The present invention achieves the above objectives through the following means.

[0010] (Method 1)

[0011] A method for manufacturing an electrode mixture, comprising:

[0012] (a) Providing an electrode mixture precursor comprising active material particles, a binder, and ethylene carbonate; and

[0013] (b) Mix the above electrode preparation precursor, and

[0014] In step (b), the ethylene carbonate is at least partially melted.

[0015] (Method 2)

[0016] According to the method for manufacturing the electrode mixture described in Method 1, wherein,

[0017] In step (b), the electrode mixture precursor is heated with a heater to at least partially melt the ethylene carbonate.

[0018] (Method 3)

[0019] According to the method for manufacturing the electrode mixture as described in method 1 or 2, wherein,

[0020] In step (b), the electrode additive precursor is heated by friction generated during mixing, causing the ethylene carbonate to melt at least partially.

[0021] (Method 4)

[0022] The method for manufacturing the electrode mixture according to any one of methods 1 to 3, wherein,

[0023] The adhesive mentioned above is polytetrafluoroethylene.

[0024] (Method 5)

[0025] A method for manufacturing an electrode active material sheet, comprising:

[0026] Provide the electrode mixture described above, manufactured by the manufacturing method of any one of methods 1 to 4; and

[0027] The electrode mixture is pressed using a pressing component.

[0028] Invention Effects

[0029] According to the method of the present invention, it is possible to suppress the possibility of surface damage to active material particles when mixing electrode mixtures in a state of high solid component concentration and / or the necessity of using high-power mixing equipment. Attached Figure Description

[0030] Figure 1 This is a graph representing the results of an embodiment. Detailed Implementation

[0031] The embodiments of the present invention will now be described in detail. However, the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the spirit of the invention.

[0032] <<Methods for Manufacturing Electrode Compounds>>

[0033] The method for manufacturing the electrode mixture of the present invention includes:

[0034] (a) Providing an electrode mixture precursor comprising active material particles, a binder, and ethylene carbonate; and

[0035] (b) Mix the above electrode preparation precursor, and

[0036] In step (b), the ethylene carbonate is at least partially melted.

[0037] According to the above method, it is possible to suppress the possibility of surface damage to active material particles when mixing electrode mixtures in a state of high solid component concentration and / or the necessity of using high-power mixing equipment.

[0038] In previous methods, when mixing electrode compounds at high solids concentrations, especially during the fiberization of the binder, the friction between the particles constituting the electrode compounds was high, which may have damaged the surface of the active material particles.

[0039] In contrast, in the method of the present invention, an electrode compound precursor containing ethylene carbonate is used, and the electrode compound precursor is mixed at a temperature above the melting point of ethylene carbonate. This allows the ethylene carbonate in the electrode compound precursor to melt and be used as a lubricant, thereby reducing the load during mixing and thus solving the above-mentioned problems.

[0040] Furthermore, since ethylene carbonate is a solid at room temperature (25°C) and is an electrolyte component, it is not necessary to dry and remove ethylene carbonate after film formation. Therefore, the entire film formation process can be implemented as a dry film formation process.

[0041] (Electrode mixture)

[0042] In this invention, the electrode compound is a material made by mixing active material particles, binder and ethylene carbonate.

[0043] (Active substance particles)

[0044] In this invention, active material particles are contained in the electrode mixture. The active material particles of this invention can be either positive electrode active material particles or negative electrode active material particles.

[0045] In this invention, the material of the positive electrode active material particles is not particularly limited. Examples of positive electrode active material particles include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), and lithium nickel-cobalt-manganese oxide (NCM:LiCoO2). 1 / 3 Ni 1 / 3 Mn 1 / 3 O2), Lithium nickel cobalt aluminate (LiNi) 0.8 (CoAl) 0.2O2), lithium iron phosphate (LFP), lithium manganese iron phosphate (LMFP), Li 1+x Mn 2-x-y M y O4 (where M is one or more metallic elements selected from Al, Mg, Co, Fe, Ni and Zn) represents heteroelemental substitutions for Li-Mn spinel, etc., but is not limited to these.

[0046] In this invention, the material of the negative electrode active material particles is not particularly limited. For example, the negative electrode active material particles can be metallic lithium, or materials capable of absorbing and releasing metal ions such as lithium ions. Examples of materials capable of absorbing and releasing metal ions such as lithium ions include alloy-based negative electrode active materials, carbon materials, and lithium titanate (Li4Ti5O). 12 It includes silicon carbide (SiC), silicon particles, etc., but is not limited to these.

[0047] There are no particular limitations on alloy-based anode active materials; for example, Si alloy-based anode active materials or Sn alloy-based anode active materials can be cited. Si alloy-based anode active materials include silicon, silicon oxide, silicon carbide, silicon nitride, etc., or their solid solutions. Furthermore, Si alloy-based anode active materials can contain metallic elements other than silicon, such as iron (Fe), cobalt (Co), antimony (Sb), bismuth (Bi), lead (Pb), nickel (Ni), copper (Cu), zinc (Zn), germanium (Ge), indium (In), tin (Sn), and titanium (Ti). Sn alloy-based anode active materials include tin, tin oxide, tin nitride, etc., or their solid solutions. Furthermore, Sn alloy-based anode active materials can contain metallic elements other than tin, such as iron (Fe), cobalt (Co), antimony (Sb), bismuth (Bi), lead (Pb), nickel (Ni), copper (Cu), zinc (Zn), germanium (Ge), indium (In), tin (Sn), and titanium (Ti).

[0048] As a carbon material, there are no particular limitations; examples include hard carbon, soft carbon, and graphite (also known as black lead).

[0049] In this invention, the shape of the active material particles is not particularly limited; for example, they can be particle-shaped. When the active material particles are particle-shaped, the particle size D of the active material particles... 50 For example, the particle size can be 1.0 nm or larger, 5.0 nm or larger, or 10.0 nm or larger, and can be 500.0 μm or smaller, 100.0 μm or smaller, 50.0 μm or smaller, or 30.0 μm or smaller. Furthermore, in this invention, the particle size D... 50 The median particle size is the particle size at which the cumulative value of the particle size distribution of the volume reference obtained by laser diffraction and scattering is 50%.

[0050] The content of active substance particles in the electrode mixture of the present invention is not particularly limited, and can be 1.0% or more by mass, 5.0% or more by mass, 10.0% or more by mass, 15.0% or more by mass, or 20.0% or more by mass, and can be less than 50.0% by mass, less than 45.0% by mass, less than 40.0% by mass, less than 35.0% by mass, or less than 30.0% by mass.

[0051] In this invention, at least one of the dispersant, conductive agent and solid electrolyte may be included in the electrode mixture.

[0052] In this invention, the conductive additive included in the electrode mixture can be a conductive additive known as a conductive additive for secondary batteries. Specifically, examples of conductive additives include carbon materials, such as Ketjen Black (KB), fumed carbon fiber (VGCF), acetylene black (AB), carbon nanotubes (CNT), carbon nanofibers (CNF), carbon black, coke, and graphite. Conductive additives can also be metallic materials that can withstand the environment during battery use. One type of conductive additive can be used alone, or two or more can be used in combination. The conductive additive can be in various forms, such as powder or fiber.

[0053] The content of conductive additive in the electrode mixture of the present invention is not particularly limited, and can be 0.1% or more by mass, 0.5% or more by mass, 1.0% or more by mass, 3.0% or more by mass, or 5.0% or more by mass, and can be less than 20.0% by mass, less than 15.0% by mass, less than 10.0% by mass, less than 8.0% by mass, or less than 5.0% by mass.

[0054] In this invention, the solid electrolyte arbitrarily included in the electrode mixture can be any solid electrolyte known as a solid electrolyte for secondary batteries. Examples of solid electrolytes include inorganic solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, and halide solid electrolytes, as well as organic polymer electrolytes such as polymer electrolytes. From the viewpoint of heat resistance, sulfide solid electrolytes and oxide solid electrolytes are particularly preferred. The solid electrolyte can be, for example, in particulate form. A single solid electrolyte can be used alone, or two or more can be used in combination.

[0055] Examples of sulfide solid electrolytes include, for example, solid electrolytes containing Li, X (where X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S. Furthermore, sulfide solid electrolytes may further contain at least one of O and a halogen element. Examples of halogen elements include F, Cl, Br, and I. The sulfide solid electrolyte can be glass (amorphous) or glass-ceramic. Examples of sulfide solid electrolytes include, but are not limited to, Li₂S-P₂S₅, LiI-Li₂S-P₂S₅, LiI-LiBr-Li₂S-P₂S₅, Li₂S-SiS₂, Li₂S-GeS₂, and Li₂S-P₂S₅-GeS₂.

[0056] Examples of oxide solid electrolytes include Li7La3Zr2O. 12 Li 7-x La3Zr 1-x Nb x O 12 Li 7- 3x La3Zr2Al x O 12 Li 3x La 2 / 3-x TiO3, Li 1+x Al x Ti 2-x (PO4)3, Li 1+x Al x Ge 2-x (PO4)3, Li3PO4 or Li 3+x PO 4-x N x (LiPON), etc., but not limited to these. Oxide solid electrolytes can be amorphous or crystalline.

[0057] Examples of halide solid electrolytes include NaBH4 and NaB. 10 H 10 NaCB9H 10 NaCB 11 H 12 NaB 12 Cl 12 And so on, but not limited to these.

[0058] Examples of polymer electrolytes include polyethylene oxide (PEO), polypropylene oxide (PPO), and their copolymers, but are not limited to these.

[0059] The content of solid electrolyte in the electrode mixture of the present invention is not particularly limited, and can be 1.0% or more by mass, 5.0% or more by mass, 10.0% or more by mass, 13.0% or more by mass, or 15.0% or more by mass, and can be less than 30.0% by mass, less than 20.0% by mass, less than 15.0% by mass, or less than 10.0% by mass.

[0060] (Adhesive)

[0061] In this invention, the binder is included in the electrode compound.

[0062] In this invention, the binder included in the electrode mixture can be a binder known as a binder used in secondary batteries. Examples of binders include styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), acrylonitrile-butadiene rubber (ABR), butadiene rubber (BR), polyvinylidene fluoride (PVDF), and polytetrafluoroethylene (PTFE). A single binder can be used alone, or two or more can be used in combination.

[0063] In particular, when the binder is polytetrafluoroethylene (PTFE) or other materials that require fiberization through shearing, the method of the present invention can suppress the damage to the active material particles during fiberization, and therefore the method of the present invention is preferred.

[0064] The content of binder in the electrode adhesive of the present invention is not particularly limited, and can be 0.1% or more by mass, 0.5% or more by mass, 1.0% or more by mass, 3.0% or more by mass, or 5.0% or more by mass, and can be less than 20.0% by mass, less than 15.0% by mass, less than 10.0% by mass, less than 8.0% by mass, or less than 5.0% by mass.

[0065] (Ethylene carbonate)

[0066] In this invention, active material particles, binder and ethylene carbonate are included in the electrode mixture.

[0067] In this invention, the content of ethylene carbonate in the electrode mixture is not particularly limited, and can be 0.1% or more by mass, 0.5% or more by mass, 1.0% or more by mass, 3.0% or more by mass, 5.0% or more by mass, or 10.0% or more by mass, and can be less than 30.0% by mass, less than 25.0% by mass, less than 20.0% by mass, less than 15.0% by mass, less than 13.0% by mass, less than 10.0% by mass, less than 9.0% by mass, less than 8.0% by mass, or less than 6.0% by mass.

[0068] <Process (a)>

[0069] In the method of the present invention for manufacturing electrode mixtures, firstly, an electrode mixture precursor comprising active material particles, a binder, and ethylene carbonate is provided.

[0070] (Electrode preparation precursor)

[0071] In this invention, the electrode preparation precursor comprises active material particles, a binder, and ethylene carbonate.

[0072] For details regarding the electrode mixture precursor of the present invention, please refer to the above description relating to the electrode mixture of the present invention.

[0073] <Process (b)>

[0074] In the method of the present invention for manufacturing electrode mixtures, the electrode mixture precursor is then compounded. In the present invention, in step (b), ethylene carbonate is at least partially melted.

[0075] In step (b) of the present invention, the method of at least partially melting ethylene carbonate is not particularly limited. For example, the electrode preparation precursor can be heated by a heater to at least partially melt ethylene carbonate, or the electrode preparation precursor can be heated by friction generated during mixing to at least partially melt ethylene carbonate.

[0076] In the method of this invention, shear stress is applied to the binder contained in the electrode binder precursor by mixing, thereby causing the binder to become fiberized. In this invention, the shear stress is not particularly limited and can be 10 N·m or more, 20 N·m or more, 40 N·m or more, or 60 N·m or more, and can be 200 N·m or less, 180 N·m or less, 160 N·m or less, or 120 N·m or less.

[0077] <<Manufacturing Method of Electrode Active Material Sheets>>

[0078] The method for manufacturing electrode active material sheets according to the present invention includes:

[0079] Provide the above-described electrode mixture manufactured by the method described in this invention; and

[0080] The electrode mixture is pressed using a pressing component.

[0081] (Electrode active material sheet)

[0082] In this invention, the electrode active material sheet is obtained by pressing the electrode mixture using a pressing component.

[0083] The electrode active material sheet of the present invention can be manufactured directly on a current collector, or it can be coated on other substrates to serve as a self-supporting film-like electrode active material sheet.

[0084] In this invention, the thickness of the electrode active material sheet is not particularly limited. For example, it can be 0.1 μm or more, 0.5 μm or more, 1.0 μm or more, 3.0 μm or more, 5.0 μm or more, or 10.0 μm or more, and it can be less than 1000.0 μm, less than 700.0 μm, less than 500.0 μm, less than 300.0 μm, or less than 100.0 μm.

[0085] In this invention, the density of the electrode active material sheet is not particularly limited and can be 0.5 g / cm³. 3 Above, 0.7g / cm 3 Above, 1.0g / cm 3 Above, 1.5g / cm 3 Above or 2.0 g / cm 3 The above, and can be 15.0 g / cm³ 3 Below, 10.0g / cm 3 Below, 8.0g / cm 3 Below, 6.0g / cm 3 Below, 4.0g / cm 3 Below or 3.0g / cm 3 the following.

[0086] <Providence of Electrode Mixture>

[0087] In the method of the present invention for manufacturing electrode active material sheets, firstly, an electrode mixture manufactured by the method described in the present invention is provided.

[0088] For details regarding the electrode mixture in the method of manufacturing electrode active material sheets of the present invention, please refer to the above description relating to the method of manufacturing the electrode mixture of the present invention.

[0089] <Suppression of Electrode Mixture>

[0090] In the method of the present invention for manufacturing electrode active material sheets, the electrode mixture is then pressed using a pressing component.

[0091] In this invention, the pressing component is not particularly limited. Furthermore, the pressing pressure is not particularly limited; it can be 5 kN / cm or more, 10 kN / cm or more, 50 kN / cm or more, 80 kN / cm or more, or 100 kN / cm or less, or 500 kN / cm or less, 300 kN / cm or less, 200 kN / cm or less, or 100 kN / cm or less.

[0092] The invention will be further described in detail with reference to the embodiments shown below, but the scope of the invention is not limited to these embodiments.

[0093] Example

[0094] <<Example 1>>

[0095]

[0096] Lithium iron phosphate (LFP) particles with carbon coating were prepared as the positive electrode active material particles. At this time, the mass ratio of LFP to carbon coating was 98.5% by mass: 1.5% by mass, and the thickness of the carbon coating was 2 nm. The positive electrode active material and ethylene carbonate were mixed at 1000 rpm for 30 seconds using a mixer to obtain the active material mixture.

[0097] <Mixing with adhesive>

[0098] As a binder, polytetrafluoroethylene (PTFE) was prepared. Using a mixer, the binder and the above-mentioned active material mixture were mixed at 10,000 rpm for 60 seconds to obtain the electrode additive precursor. At this point, the mass ratio of the positive electrode active material particles, ethylene carbonate, and PTFE was 82.7% by mass: 12.3% by mass: 5.0% by mass.

[0099] <Shearing of Adhesive>

[0100] The mixture was heated to 70°C and mixed at 60 rpm for 20 seconds using an intermittent kneader. Shear stress was applied to the electrode mixture precursor to fibrousize the PTFE, thereby obtaining the electrode mixture described in Example 1.

[0101] The shear stress at this point is 85 N·m.

[0102] <Evaluation>

[0103] The electrode mixture precursor and electrode mixture were pressurized to achieve a density of 2.0 g / cm³. 3 The resistance was measured.

[0104] <<Comparative Example 1>>

[0105] Except that it does not contain ethylene carbonate and the mass ratio of positive electrode active material particles to PTFE is 95.0% by mass: 5.0% by mass, the electrode mixture involved in Comparative Example 1 was obtained in the same manner as in Example 1.

[0106] <<Evaluation>>

[0107] The resistances of the electrode mixture precursors and electrode mixtures of Comparative Example 1 and Example 1 are shown in the figure. Figure 1 middle.

[0108] like Figure 1As shown, in Example 1 and Comparative Example 1, the resistance increased when the electrode mixture precursor was subjected to shear stress to form the electrode mixture. This indicates that when the electrode mixture precursor is subjected to shear stress to form the electrode mixture, the surface of the active material particles is damaged by the shear force.

[0109] like Figure 1 As shown, when comparing Example 1 with Comparative Example 1, the resistance of the electrode mixture of Example 1, which contains ethylene carbonate, is less than that of the electrode mixture of Comparative Example 1, which does not contain ethylene carbonate. This indicates that the ethylene carbonate suppresses damage to the surface of the active material particles contained in the electrode mixture. Therefore, it can be confirmed that by including ethylene carbonate in the electrode mixture precursor, damage to the surface of the active material particles contained in the electrode mixture is suppressed.

Claims

1. A method for manufacturing an electrode mixture, characterized in that, include: (a) Providing an electrode preparation precursor comprising active material particles, a binder and ethylene carbonate; as well as (b) Compounding the electrode preparation precursor, and In step (b), the ethylene carbonate is at least partially melted.

2. The method for manufacturing the electrode mixture according to claim 1, characterized in that, In step (b), the electrode mixture precursor is heated with a heater to at least partially melt the ethylene carbonate.

3. The method for manufacturing the electrode mixture according to claim 1, characterized in that, In step (b), the electrode mixture precursor is heated by friction generated during mixing, causing the ethylene carbonate to melt at least partially.

4. The method for manufacturing the electrode mixture according to claim 1, characterized in that, The adhesive is polytetrafluoroethylene.

5. A method for manufacturing an electrode active material sheet, characterized in that, include: Provided an electrode mixture manufactured by the method for manufacturing an electrode mixture according to claim 1; and The electrode mixture is pressed using a pressing component.

Citation Information

Patent Citations

  • Electrode film for energy storage device, electrode and energy storage device

    JP2022003694A

  • Electrode for secondary battery, method for producing same, and secondary battery including said electrode

    JP2024505952A