A silicon-based anode material and its preparation method, and a lithium-ion battery.

By preparing silicon-based anode materials with nano-silicon dispersed in a three-dimensional carbon framework and combining them with MXene conductive bridging structures, the volume expansion and conductive network problems of silicon-based anode materials were solved, thereby improving the cycle stability and capacity of lithium-ion batteries.

CN123120736APending Publication Date: 2026-11-17TIANFU JIANGXI LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611355078.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Silicon-based anode materials in lithium-ion batteries suffer from problems such as large volume expansion, easy aggregation and shedding of nano-silicon, heavy stacking of MXene sheets, and easy breakage of conductive networks, resulting in uneven structure and poor conductivity.

Method used

A functional preemulsion was formed by mixing carbon source monomers, nitrogen-containing functional monomers, multifunctional crosslinking monomers and silane coupling monomers. A silicon-based anode material with nano-silicon dispersed in a three-dimensional carbon framework was prepared by using microchannel continuous flow mixing dispersion and strong shear gelation technology. Combined with MXene conductive bridging structure, a stable conductive network was formed.

Benefits of technology

This study achieved structural uniformity and stable conductivity of silicon-based anode materials, improved the cycle performance and safety of lithium-ion batteries, and increased battery capacity and initial coulombic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120736A_ABST
    Figure CN123120736A_ABST
Patent Text Reader

Abstract

This invention relates to the field of lithium-ion battery technology, and particularly to a silicon-based anode material, its preparation method, and a lithium-ion battery. A polymerizable component is obtained by mixing a carbon source monomer, a nitrogen-containing functional monomer, a multifunctional crosslinking monomer, and a silane coupling monomer. This polymerizable component is then formulated into a functional pre-emulsion, ensuring uniform pre-mixing and providing a homogeneous, polymerizable, and crosslinkable continuous medium for nano-silicon and MXene nanosheets. A highly uniform reaction system at the microscale is formed through continuous flow mixing and dispersion in microchannels, followed by strong shear gelation and Joule heat treatment to obtain the silicon-based anode material. This integrated preparation path of "functional pre-emulsion – continuous flow mixing and dispersion in microchannels – strong shear gelation – Joule heat carbonization" yields a silicon-based anode material with a uniform and stable structure, good conductivity, and stable cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium battery technology, specifically to a silicon-based anode material and its preparation method, and a lithium battery. Background Technology

[0002] With the rapid development of new energy vehicles, energy storage systems, and high-power electronic devices, lithium-ion batteries are facing higher demands for energy density, high rate performance, and long cycle life. Silicon-based anode materials are considered important candidate materials for improving the energy density of lithium-ion batteries due to their theoretical specific capacity being far higher than that of graphite anodes.

[0003] However, silicon-based anodes still face significant technical bottlenecks in practical applications. First, silicon undergoes substantial volume expansion and contraction during lithium insertion / extraction, easily leading to pulverization of the active material, damage to the electrode structure, and breakage of the conductive network. Second, while nano-silicon can mitigate the volume effect to some extent, its large specific surface area makes it prone to aggregation, inducing continuous electrolyte decomposition and causing irreversible capacity loss. Furthermore, silicon itself has poor electronic conductivity, necessitating an external conductive network to maintain stable electrochemical reactions.

[0004] MXene, as a two-dimensional conductive material, possesses high electronic conductivity, a layered structure, and abundant surface functional groups, making it suitable as an external conductive network to improve the conductivity of silicon-based anodes. However, MXene is prone to layer recombination during the composite process, leading to a decrease in effective conductive area and increased susceptibility to breakage. Furthermore, if silicon and MXene are simply mixed physically to form a composite structure, phase separation and structural instability can easily occur during subsequent drying, heat treatment, and electrochemical cycling, making it difficult to achieve continuous, uniform, and stable dispersion of silicon and MXene. Additionally, MXene layers are prone to recombination, hindering the formation of a long-term stable conductive network. Nanoscale silicon is also susceptible to migration, aggregation, or detachment during heat treatment and cycling. Summary of the Invention

[0005] To address the problems of large volume expansion of silicon, easy agglomeration and shedding of particles, heavy stacking of MXene sheets, easy breakage of conductive networks, and insufficient structural uniformity of silicon-based anode materials, this invention provides a silicon-based anode material, its preparation method, and a lithium-ion battery.

[0006] This invention provides a method for preparing a silicon-based anode material, specifically comprising the following steps: mixing a carbon source monomer, a nitrogen-containing functional monomer, a multifunctional crosslinking monomer, and a silane coupling monomer to obtain a polymerizable component; dissolving the polymerizable component in an emulsion medium to obtain a functional pre-emulsion; mixing nano-silicon with a solvent to obtain a nano-silicon dispersion; mixing MXene nanosheets with a solvent to obtain an MXene nanosheet dispersion; continuously mixing and dispersing the functional pre-emulsion, nano-silicon dispersion, MXene nanosheet dispersion, and an initiator in a microchannel to obtain a reaction mixture; gelling the reaction mixture under shear to obtain a gelled precursor; and subjecting the gelled precursor to Joule heat treatment in an inert atmosphere to obtain the silicon-based anode material.

[0007] Furthermore, the mass ratio of carbon source monomer, nitrogen-containing functional monomer, multifunctional crosslinking monomer, and silane coupling monomer is (20-70):(5-40):(1-30):(0.5-15).

[0008] Further, the carbon source monomer includes any one or more combinations of furan-based carbon source monomers, polyphenol-based carbon source monomers, benzoxazine-based carbon source monomers, phenolic resin carbon source monomers, and polyimide carbon source monomers; the nitrogen-containing functional monomer includes any one or more combinations of 1-vinylimidazolium, 4-vinylpyridine, 2-vinylpyridine, N-vinylpyrrolidone, acrylamide, methacrylamide, N-hydroxymethylacrylamide, melamine, cyanuric acid, and triazine monomers; and / or, the multifunctional crosslinking monomer includes any one or more combinations of triallyl isocyanurate, triallyl cyanurate, bismaleimide, ethylene glycol dimethacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, and phosphazene multifunctional crosslinking agents; and the silane coupling monomer includes any one or more combinations of γ-methacryloyloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, vinyltriethoxysilane, and vinyltrimethoxysilane. Furthermore, the particle size of the silicon nanoparticles is 80nm-120nm, and the diameter of the MXene nanosheets is 2μm-4μm; and / or, the MXene nanosheets comprise Ti3C2T. x MXene nanosheets, Ti2CT x MXene nanosheets, Nb2CT x MXene nanosheets, V2CT x Any one or more combinations of MXene nanosheets, wherein T x represents surface functional groups, and x represents the average number of surface functional groups.

[0009] Further, the mass ratio of nano-silicon, MXene nanosheets, and polymerizable components is (96-105):(17-28):100; and / or, the initiator includes any one or more combinations of azobisisobutyronitrile, benzoyl peroxide, ammonium persulfate, and potassium persulfate.

[0010] Furthermore, in the microchannel continuous flow mixing and dispersion, the diameter of the microchannel is 50μm-1000μm, and the mixing and dispersion time is 5s-1800s; and / or, the microchannel includes any one or more combinations of T-shaped microchannels, Y-shaped microchannels, serpentine microchannels, spiral microchannels, staggered microchannels, diversion-convergence microchannels, or impinging flow microchannels.

[0011] Furthermore, the shear rate of the shearing action is 1000 s. -1 -20000s -1 The gelation temperature is 40℃-90℃ and the time is 5min-120min; and / or the Joule heat treatment temperature is 500℃-1200℃ and the time is 1s-1800s.

[0012] The present invention also provides a silicon-based anode material, which is prepared by the silicon-based anode material preparation method described above. The silicon-based anode material includes nano-silicon, MXene conductive bridging structures, and a three-dimensional carbon skeleton. The nano-silicon is dispersed in the three-dimensional carbon skeleton, and the MXene conductive bridging structures are interspersed in the interior or surface of the three-dimensional carbon skeleton. The MXene conductive bridging structures form a conductive bridge between the three-dimensional carbon skeleton and the nano-silicon. An interface anchoring structure is present between the nano-silicon and the three-dimensional carbon skeleton.

[0013] Furthermore, the three-dimensional carbon framework has a framework body, a nitrogen-doped structure, and a porous structure. The nitrogen-doped structure is distributed in the framework body, and the parts of the three-dimensional carbon framework that do not contain the framework body form the porous structure.

[0014] The present invention also provides a lithium-ion battery, the lithium-ion battery comprising a positive electrode, an electrolyte, and a negative electrode, wherein the negative electrode comprises the silicon-based negative electrode material as described above.

[0015] Compared with the prior art, the silicon-based anode material, its preparation method, and the lithium-ion battery provided by this invention have the following beneficial effects: 1. This invention provides a method for preparing silicon-based anode materials, which involves mixing carbon source monomers, nitrogen-containing functional monomers, multifunctional crosslinking monomers, and silane coupling monomers to form a functional pre-emulsion, thereby ensuring that the polymerizable components are uniformly mixed beforehand, resulting in nano-silicon and MXene. Nanosheets provide a homogeneous, polymerizable, and crosslinkable continuous medium. Microchannel continuous flow mixing and dispersion utilizes rapid mixing and local shearing within a confined microscale space to reduce nano-silicon agglomeration and MXene nanosheet stacking, resulting in a highly homogeneous reaction mixture of functional preemulsion, nano-silicon dispersion, MXene nanosheet dispersion, and initiator. The reaction mixture gels under strong shear force, which preserves the uniform dispersion of nano-silicon and MXene nanosheets, preventing migration, agglomeration, or stacking during gelation and subsequent Joule heat treatment. Finally, Joule heat treatment achieves rapid and uniform carbonization. Through this integrated preparation pathway of "functional preemulsion - microchannel continuous flow mixing and dispersion - strong shear gelation - Joule heat carbonization," a silicon-based anode material with a uniform and stable structure, good conductivity, and stable cycle performance is obtained.

[0016] 2. This invention further specifies the mass ratio of carbon source monomer, nitrogen-containing functional monomer, multifunctional crosslinking monomer, and silane coupling monomer as (20-70):(5-40):(1-30):(0.5-15). Under this mass ratio design, the carbon source monomer participates in forming the main body of the three-dimensional carbon skeleton, providing sufficient carbon source to form a continuous, dense, and moderately thick three-dimensional carbon skeleton, enabling the carbon skeleton to uniformly cover each nano-silicon particle and form a continuous and efficient conductive network. The content of nitrogen-containing functional monomer is maintained within a good range, providing sufficient active sites, reducing the resistivity of silicon-based anode materials, and improving rate performance. By designing the mass ratio of polymerizable components, a structurally stable and strongly supporting three-dimensional carbon skeleton can be obtained, forming a stable interface anchoring structure between nano-silicon and the three-dimensional carbon skeleton.

[0017] 3. In the technical solution of this invention, the specific selection of carbon source monomer, nitrogen-containing functional monomer, multifunctional crosslinking monomer, and silane coupling monomer is further specified. The carbon source monomer undergoes pyrolysis during subsequent Joule heat treatment, resulting in carbon element rearrangement and forming the main framework of a three-dimensional carbon skeleton. The carbon source monomer can undergo free radical copolymerization with the nitrogen-containing functional monomer, uniformly introducing nitrogen elements into the three-dimensional carbon skeleton, achieving nitrogen doping of the three-dimensional carbon skeleton. By introducing nitrogen doping into the three-dimensional carbon skeleton, more active sites can be introduced, thereby improving the specific capacity of the silicon-based anode material. The functional group crosslinking monomer is used to form the rigid part that provides support in the three-dimensional carbon skeleton. The resulting three-dimensional crosslinked gel network has high mechanical strength and rigidity, effectively suppressing the volume expansion of nano-silicon and preventing the three-dimensional carbon skeleton from cracking due to excessive stress. Simultaneously, the microporous structure formed after carbonization of the three-dimensional crosslinked gel network also provides buffer space for the expansion of nano-silicon. The silane coupling monomer forms an interface anchoring structure between the nano-silicon and the three-dimensional carbon skeleton, preventing the nano-silicon from detaching during cycling and improving the structural stability of the silicon-based anode material during cycling.

[0018] 4. In the technical solution of the present invention, the particle size of the nano-silicon is 80nm-120nm. Within this particle size range, the nano-silicon has a higher specific surface area, which can better adapt to the volume expansion during the charging and discharging process and is less prone to brittleness. The sheet diameter of the MXene nanosheet is 2μm-4μm. This sheet diameter range is conducive to the formation of MXene conductive bridging structures in the three-dimensional carbon framework. The micron-sized sheet diameter can provide a longer and continuous electron transport channel. If the sheet diameter of the MXene nanosheet is too small, it may lead to insufficient transport capacity of the MXene conductive bridging structure and easy loose stacking with the nano-silicon. If the sheet diameter of the MXene nanosheet is too large, it will lead to difficulty in dispersing the MXene nanosheet and local stacking.

[0019] 5. In the technical solution of the present invention, the mass ratio of nano-silicon, MXene nanosheets, and polymerizable components is further defined as (96-105):(17-28):100. The content of nano-silicon is relatively high. As a high-capacity lithium storage active material, nano-silicon can ensure that the prepared silicon-based anode material has a high capacity. As a highly conductive two-dimensional material, MXene nanosheets can form an MXene conductive bridging structure, further improving electron transport efficiency and alleviating the volume expansion of nano-silicon. The content of polymerizable components is close to that of nano-silicon. Polymerizable components are used to form a three-dimensional carbon skeleton, which can form a sufficiently dense and complete three-dimensional carbon skeleton to encapsulate nano-silicon. The formed three-dimensional carbon skeleton can provide sufficient buffer space for the volume expansion of nano-silicon and can also construct a basic conductive network to make up for the poor conductivity of nano-silicon.

[0020] 6. In the technical solution of this invention, the diameter of the microchannel is 50μm-1000μm, and the mixing and dispersion time is 5s-1800s. This size range can handle reactants containing nano-silicon and MXene nanosheets, preventing clogging, and can also achieve high throughput. The micron-sized reaction channel can divide the reactants into extremely thin microlayers, and the distance of the reactants diffusing from the center of the channel to the wall is shortened to the micron level, which can prevent the agglomeration of nano-silicon and the stacking of MXene nanosheets, and can make them uniformly dispersed before re-aggregation.

[0021] 7. In the technical solution of the present invention, the shear rate of the shearing action is 1000s. -1 -20000s -1 At this shear rate, strong shear force can be generated, which can prevent the migration, sedimentation, and local aggregation and overlap of nano-silicon and MXene nanosheets during the gelation process of the reaction mixture system. The gelation temperature is 40℃-90℃ and the time is 5min-120min. At 40℃-90℃, the initiator in the reaction mixture generates highly active free radicals when heated. These free radicals attack the chemical bonds of polymerizable components in the functional preemulsion, causing them to open and thus initiating the reaction and causing the reaction mixture to gel. The Joule heat treatment temperature is 500℃-1200℃ and the time is 1s-1800s, which achieves rapid and uniform bulk phase heating, reduces the problems of nano-silicon migration, particle growth, or local aggregation caused by long-term high-temperature heat treatment, and helps to maintain the integrity of the three-dimensional carbon framework structure and the continuity of the conductive network.

[0022] 8. This invention also provides a silicon-based anode material, which is prepared by the above-described method. The silicon-based anode material comprises nano-silicon, an MXene conductive bridging structure, and a three-dimensional carbon framework. The MXene conductive bridging structure and the three-dimensional carbon framework work synergistically to form a highly efficient and stable conductive network for the silicon-based anode material, uniformly encapsulating the nano-silicon within the conductive network. The nano-silicon, as a high-capacity lithium storage active material, provides high capacity for the silicon-based anode material. The three-dimensional carbon framework forms a globally continuous conductive system; the silicon-based anode material has a uniform and stable structure, low impedance, good conductivity, and strong cycle stability.

[0023] 9. In the silicon-based anode material of the present invention, the three-dimensional carbon framework has a porous structure and a nitrogen-doped structure. The porous structure of the three-dimensional carbon framework can provide sufficient buffer space for the volume expansion of nano-silicon, and the nitrogen-doped structure is beneficial to improving electron transport capability and interfacial polarity. There is an interfacial anchoring structure between the nano-silicon and the three-dimensional carbon framework. The interfacial anchoring structure can anchor the nano-silicon in the three-dimensional carbon framework and prevent the nano-silicon from falling off during charging and discharging.

[0024] 10. The present invention further provides a lithium-ion battery, wherein the negative electrode sheet of the lithium-ion battery includes the silicon-based negative electrode material as described above. The high content of nano-silicon in the silicon-based negative electrode material improves the capacity of the lithium-ion battery. The dual effect of the three-dimensional carbon skeleton and the MXene conductive bridging structure effectively buffers the volume expansion of nano-silicon during charging and discharging, solving the problems of easy pulverization and rapid capacity decay of nano-silicon, and improving the cycle life of the lithium-ion battery. The dense three-dimensional carbon skeleton can effectively isolate the electrolyte, suppress side reactions, and guide the formation of a more stable SEI film, thereby improving the first coulombic efficiency of the lithium-ion battery. The porous structure of the three-dimensional carbon skeleton and the MXene conductive bridging structure, which has both mechanical strength and flexibility, can withstand the compressive stress caused by the expansion of nano-silicon, protecting the internal structure. The MXene conductive bridging structure can effectively suppress the agglomeration of nano-silicon particles, enhancing the structural stability of the electrode and the safety of the lithium-ion battery. Attached Figure Description

[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0026] Figure 1 The flowchart illustrates the specific steps of a method for preparing a silicon-based anode material according to the first embodiment of the present invention.

[0027] Figure 2 This is a schematic diagram of the microstructure of a silicon-based anode material provided in the second embodiment of the present invention.

[0028] Figure 3 for Figure 2 A magnified view of a portion at point A shown in the diagram.

[0029] Figure 4 This is a schematic diagram of the structure of a lithium-ion battery provided in the third embodiment of the present invention.

[0030] Figure 5 This is a flowchart illustrating the preparation steps of a lithium-ion battery according to the third embodiment of the present invention.

[0031] Explanation of reference numerals in the attached diagram: 10. Silicon-based anode material; 11. Nano-silicon; 12. MXene conductive bridging structure; 13. Three-dimensional carbon skeleton; 131. Skeleton body; 132. Nitrogen-doped structure; 133. Porous structure; 14. Interface anchoring structure; 9. Lithium-ion battery; 1. Anode plate; 2. Electrolyte; 3. Positive electrode plate. Detailed Implementation

[0032] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and experimental examples. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0033] In the embodiments provided by this invention, it should be understood that "B corresponding to A" means that B is associated with A, and B can be determined based on A. However, it should also be understood that determining B based on A does not mean determining B solely based on A; B can also be determined based on A and / or other information.

[0034] It should be understood that the phrase "one embodiment" or "an embodiment" throughout the specification means that a specific feature, structure, or characteristic related to the embodiment is included in at least one embodiment of the invention. Therefore, "in one embodiment" or "in an embodiment" appearing throughout the specification does not necessarily refer to the same embodiment. Furthermore, these specific features, structures, or characteristics can be combined in any suitable manner in one or more embodiments. Those skilled in the art should also recognize that the embodiments described in the specification are optional embodiments, and the actions and modules involved are not necessarily essential to the invention.

[0035] In various embodiments of the present invention, it should be understood that the sequence number of each process does not necessarily imply the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process defined by the present invention.

[0036] The flowcharts and block diagrams in the accompanying drawings illustrate methods and possible architectures, functions, and operations according to various embodiments of this application. In this regard, each block in the flowchart or block diagram may represent part of a step. It should also be noted that in some alternative implementations, the functions indicated in the blocks may occur in a different order than those indicated in the drawings. For example, two consecutively indicated blocks may actually be executed substantially in parallel, or they may sometimes be executed in reverse order, depending on the functions involved.

[0037] Please see Figure 1 The first embodiment of the present invention provides a method for preparing a silicon-based anode material, specifically including the following steps: Step S11: Mix carbon source monomer, nitrogen-containing functional monomer, multifunctional crosslinking monomer and silane coupling monomer to obtain polymerizable component, dissolve polymerizable component in emulsion medium to obtain functional pre-emulsion; Step S12: Mix nano-silicon with solvent to obtain nano-silicon dispersion, and mix MXene nanosheets with solvent to obtain MXene nanosheet dispersion; Step S13: The functional preemulsion, nano-silica dispersion, MXene nanosheet dispersion, and initiator are mixed and dispersed in a microchannel continuous flow to obtain a reaction mixture; Step S14: The reaction mixture undergoes gelation under shear to obtain a gelled precursor; and Step S15: The gelled precursor is subjected to Joule heat treatment in an inert atmosphere to obtain silicon-based anode material.

[0038] Specifically, in step S11, the carbon source monomer includes any one or a combination of furan-based carbon source monomers, polyphenol-based carbon source monomers, benzoxazine-based carbon source monomers, phenolic resin carbon source monomers, and polyimide carbon source monomers. The carbon source monomer is used to form the main framework of the three-dimensional carbon skeleton of the silicon-based anode material. During subsequent Joule heat treatment, the carbon source monomer undergoes pyrolysis, and the carbon elements rearrange to participate in the formation of the main framework of the three-dimensional carbon skeleton. The carbon source monomer can undergo free radical copolymerization with nitrogen-containing functional monomers, uniformly introducing nitrogen elements into the three-dimensional carbon skeleton, thus achieving nitrogen doping of the three-dimensional carbon skeleton. In some specific embodiments of the present invention, the carbon source monomer may be furfuryl alcohol.

[0039] Specifically, in step S11, the nitrogen-containing functional monomer includes any one or more combinations of 1-vinylimidazolium, 4-vinylpyridine, 2-vinylpyridine, N-vinylpyrrolidone, acrylamide, methacrylamide, N-hydroxymethylacrylamide, melamine, cyanuric acid, and triazine monomers. The nitrogen-containing functional monomer is used to form a nitrogen-doped structure in a three-dimensional carbon framework. After Joule heat treatment, the nitrogen atoms in the nitrogen-containing functional monomer are embedded in the carbon lattice of the three-dimensional carbon framework. Since a nitrogen atom has one more electron than a carbon atom, nitrogen doping alters the electronic band structure of the three-dimensional carbon framework, increasing the carrier concentration and thus reducing resistivity. The nitrogen-containing functional monomer achieves nitrogen doping of the three-dimensional carbon framework, introducing nitrogen elements into the three-dimensional carbon framework. The nitrogen elements are retained in the three-dimensional carbon framework in the form of pyridine nitrogen, pyrrole nitrogen, graphitic nitrogen, etc., forming a nitrogen-doped structure, which can introduce more active sites and improve the specific capacity of silicon-based anode materials.

[0040] Specifically, in step S11, the multifunctional crosslinking monomer includes any one or a combination of triallyl isocyanurate (TAIC), triallyl cyanurate, bismaleimide, ethylene glycol dimethacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, and phosphazene multifunctional crosslinking agents. During gelation, the multifunctional crosslinking monomer can connect multiple polymer chains, gradually transforming the reaction system from a linear or branched polymer into a three-dimensional crosslinked gel network with spatial network characteristics. The multifunctional crosslinking monomer serves as a rigid supporting component in the framework of the three-dimensional carbon skeleton, effectively suppressing the volume expansion of nano-silicon and preventing the three-dimensional carbon skeleton from cracking due to excessive stress.

[0041] Specifically, in step S11, the silane coupling monomer includes one or more combinations of γ-methacryloxypropyltrimethoxysilane (KH-570), γ-aminopropyltriethoxysilane, vinyltriethoxysilane, and vinyltrimethoxysilane. The silane coupling monomer is used to form an interfacial anchoring structure connecting the nano-silicon and the three-dimensional carbon framework, creating a stable interfacial bond between the nano-silicon and the three-dimensional carbon framework. One end of the silane coupling monomer, having a silane group, undergoes a condensation or coupling reaction with the silanol groups (Si-OH) on the surface of the nano-silicon to generate Si-O-Si bonds; the other end copolymerizes with the carbon source monomer, connecting to the three-dimensional carbon framework, forming an interfacial anchoring structure between the nano-silicon and the three-dimensional carbon framework. This prevents the nano-silicon from detaching during cycling, ensuring that the nano-silicon remains anchored within the three-dimensional carbon framework, reducing the risk of detachment of the nano-silicon in the silicon-based anode material during cycling, and improving the structural stability of the silicon-based anode material during cycling.

[0042] Specifically, in step S11, the carbon source monomer, nitrogen-containing functional monomer, multifunctional crosslinking monomer, and silane coupling monomer are mixed. The mixture can be stirred at room temperature at a speed of 200 r / min-500 r / min for 20 min-30 min.

[0043] Specifically, in step S11, the carbon source monomer, nitrogen-containing functional monomer, multifunctional crosslinking monomer, and silane coupling monomer are polymerizable components, and the mass ratio of the carbon source monomer, nitrogen-containing functional monomer, multifunctional crosslinking monomer, and silane coupling monomer is (20-70):(5-40):(1-30):(0.5-15). It can be understood that, taking the total mass of polymerizable components in the functional preemulsion as 100%, the mass percentage of the carbon source monomer is 20%-70%, the mass percentage of the nitrogen-containing functional monomer is 5%-40%, the mass percentage of the multifunctional crosslinking monomer is 1%-30%, and the mass percentage of the silane coupling monomer is 0.5%-15%.

[0044] Under this mass ratio design, the carbon source monomer and multifunctional cross-linked monomer can form the main body of the three-dimensional carbon skeleton, providing sufficient carbon source to form a continuous, dense, and moderately thick three-dimensional carbon skeleton, enabling the three-dimensional carbon skeleton to uniformly cover each nano-silicon particle and form a continuous and efficient conductive network. The content of nitrogen-containing functional monomers is maintained within a good range, providing sufficient active sites, reducing the resistivity of silicon-based anode materials, and improving rate performance, while avoiding excessive nitrogen doping that would lead to too many defects in the three-dimensional carbon skeleton and reduce mechanical strength. 1%-30% of multifunctional cross-linked monomers ensures that the three-dimensional carbon skeleton has good mechanical strength and rigidity, while avoiding excessive cross-linking that would cause the three-dimensional carbon skeleton to become brittle. The three-dimensional carbon skeleton formed under this ratio can effectively constrain the expansion of nano-silicon and also has a certain degree of flexibility. 0.5%-15% of silane coupling monomers ensures that the silane coupling monomers form sufficient Si-O-Si bonds with nano-silicon, so that a stable interface bond is formed between nano-silicon and the carbon skeleton. By designing the mass ratio of polymerizable components, a three-dimensional carbon skeleton with stable structure and strong support can be obtained, forming a stable interface anchoring structure between nano-silicon and the three-dimensional carbon skeleton, thereby improving the specific capacity, initial coulombic efficiency, cycle stability and expansion suppression capability of silicon-based anode materials.

[0045] Specifically, in step S11, the preparation process of the emulsion medium involves adding a surfactant to a mixed solvent of ethanol / deionized water and stirring until completely dissolved to obtain the emulsion medium. The surfactant includes any one or more combinations of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polyvinylpyrrolidone, polyvinyl alcohol, Tween surfactants, Span surfactants, and hexadecyltrimethylammonium bromide. The amount of surfactant used is 1%-1.5% of the total mass of the polymerizable components. In some embodiments of the present invention, the amount of surfactant used is 1%-1.25%, 1.2%-1.3%, 1.35%-1.4%, 1.45%-1.5% of the total mass of the polymerizable components, etc.; in some specific embodiments of the present invention, the amount of surfactant used is 1.1%, 1.15%, 1.3%, 1.46% of the total mass of the polymerizable components, etc.

[0046] Specifically, in step S11, the premixed liquid is dissolved in an emulsifying medium to obtain a functional preemulsion. Emulsification occurs during this process at a high rotational speed of 8000 rpm-10000 rpm for 20-30 minutes. In some embodiments of the present invention, the rotational speed during emulsification is 8000-8200 rpm, 8500-8800 rpm, 9000-9500 rpm, 9600-10000 rpm, etc.; in some specific embodiments of the present invention, the rotational speed during emulsification is 8100 rpm, 8600 rpm, 9100 rpm, 9700 rpm, etc.

[0047] Specifically, in step S11, carbon source monomers, nitrogen-containing functional monomers, multifunctional crosslinking monomers, and silane coupling monomers are first mixed to obtain a polymerizable component. Premixing the polymerizable component allows the monomers to achieve molecular-level homogeneous mixing through intermolecular diffusion. Adding the polymerizable component to the emulsion medium forms a functional preemulsion with fine and uniform particle size distribution. Without premixing, adding each monomer separately to the emulsion medium would cause the polymerization reaction to occur in different regions, resulting in a loose internal structure or stratification of the functional preemulsion. Premixing ensures that each monomer is uniformly distributed in each emulsion droplet in the subsequently formed functional preemulsion, forming a micro-reaction system that allows the reaction to proceed efficiently.

[0048] Specifically, in step S11, by forming a functional pre-emulsion, the carbon source monomer, nitrogen-containing functional monomer, multifunctional crosslinking monomer, and silane coupling monomer are dispersed in a more uniform state in the emulsion medium, reducing local concentration differences and phase separation caused by differences in the polarity, solubility, and reactivity of each component. The uniformity of dispersion of each monomer in the functional pre-emulsion directly affects the spatial distribution of crosslinking nodes and carbon sources in the subsequent gel network structure, and thus affects the continuity and uniformity of the final three-dimensional carbon skeleton formed after Joule thermal carbonization. Preparing a uniform functional pre-emulsion first provides a homogeneous, polymerizable, and crosslinkable continuous medium for nano-silicon and MXene nanosheets. When nano-silicon and MXene nanosheets are subsequently introduced, the monomers in the functional pre-emulsion can be more uniformly distributed around the nano-silicon and MXene nanosheets, which is beneficial for the subsequent formation of a uniformly composed three-dimensional carbon skeleton.

[0049] In step S12, a nano-silicon dispersion and an MXene nanosheet dispersion are prepared. Specifically, nano-silicon is dispersed in a mixed solvent of ethanol / deionized water, stirred until homogeneous, and then ultrasonically dispersed at room temperature to obtain a uniform and stable nano-silicon dispersion. MXene nanosheets are separately dispersed in a mixed solvent of ethanol / deionized water, stirred until homogeneous, and then ultrasonically dispersed at 0℃-4℃ to obtain a uniform and stable MXene dispersion. The ultrasonic dispersion time is 20-30 minutes.

[0050] It is understandable that both nano-silicon and MXene nanosheets possess extremely high surface energy and small particle size, making them prone to aggregation due to van der Waals forces. A mixture of ethanol and deionized water can provide a solvent with low surface tension. Preparing nano-silicon and MXene nanosheets into corresponding dispersions allows the solvent to penetrate and wet the surfaces of the nano-silicon and MXene nanosheets, as well as the gaps within the aggregates, thus preventing the formation of agglomerates.

[0051] Specifically, in step S12, the particle size of the nano-silicon is 80nm-120nm. Nano-silicon serves as a high-capacity lithium storage active material in silicon-based anode materials, and is the fundamental source of the high energy density of silicon-based anode materials. Within this particle size range, nano-silicon has a higher specific surface area, which can better adapt to volume expansion during charging and discharging, and is less prone to brittleness. The diameter of the MXene nanosheets is 2μm-4μm. This diameter range is beneficial for MXene nanosheets to form MXene conductive bridging structures within a three-dimensional carbon framework. Micrometer-scale diameters provide longer and continuous electron transport channels. Flexible MXene nanosheets can also buffer the volume expansion of nano-silicon. If the diameter of the MXene nanosheets is too small, the transport capacity of the MXene conductive bridging structure may be insufficient, and it may easily form loose stacking with nano-silicon. If the diameter of the MXene nanosheets is too large, it will be difficult to disperse the MXene nanosheets, resulting in localized stacking.

[0052] It is understood that in some embodiments of the present invention, the particle size of the silicon nanoparticles is 80nm-95nm, 88nm-96nm, 102nm-108nm, 114nm-118nm, 115nm-120nm, etc.; in some specific embodiments of the present invention, the particle size of the silicon nanoparticles is 82nm, 97nm, 100nm, 102nm, 105nm, 110nm, 115nm, etc. In some embodiments of the present invention, the sheet diameter of the MXene nanosheets is 2μm-2.2μm, 2.4μm-2.6μm, 2.8μm-3.4μm, 3.8μm-4μm, etc.; in some specific embodiments of the present invention, the sheet diameter of the MXene nanosheets is 2.3μm, 2.5μm, 3.2μm, 3.5μm, etc.

[0053] Specifically, the MXene nanosheets include Ti3C2T x MXene nanosheets, Ti2CT x MXene nanosheets, Nb2CT x MXene nanosheets, V2CT x Any one or more combinations of MXene nanosheets. Wherein, T x represents surface functional groups, and x represents the average number of surface functional groups.

[0054] Specifically, in step S13 above, the functional preemulsion, nano-silicon dispersion, MXene nanosheet dispersion, and initiator are mixed and dispersed using a microchannel continuous flow method to obtain a reaction mixture. Through microchannel continuous flow mixing and dispersion, the nano-silicon dispersion, MXene nanosheet dispersion, and functional preemulsion are rapidly dispersed in a microscale confined space. Compared to ordinary mechanical stirring or static mixing and dispersion, microchannel continuous flow mixing and dispersion can shorten the diffusion path, enhance local shearing and dispersion during the mixing and dispersion process, improve the mixing uniformity of nano-silicon, MXene nanosheets, and functional preemulsion, and reduce nano-silicon migration and agglomeration and MXene nanosheet layer stacking. Microchannel continuous flow mixing and dispersion plays a crucial role in achieving uniform dispersion of nano-silicon and MXene nanosheets, constructing a uniform and stable three-dimensional carbon framework, and improving the cycle stability of silicon-based anode materials. Nano-silicon agglomeration can lead to the formation of aggregates, resulting in significant volume expansion during the charging and discharging of silicon-based anode materials. This rapid accumulation of internal stress can cause internal cracking of the three-dimensional carbon framework of the silicon-based anode material. Microchannel continuous flow mixing and dispersion can ensure uniform dispersion of nano-silicon, preventing this from occurring. Stacking of MXene nanosheets can block the diffusion channels of lithium ions, leading to a deterioration in the rate performance of silicon-based anode materials. Many reactive sites are buried inside, weakening the conductivity of the MXene conductive bridging structure. The MXene conductive bridging structure loses its flexible buffering function, which in turn makes it brittle and prone to breakage under the stress generated by the expansion of nano-silicon. Using microchannel continuous flow mixing and dispersion can effectively avoid the stacking of MXene nanosheets.

[0055] Microchannel continuous flow mixing and dispersion refers to a technique that combines microreactor technology with continuous flow processes to achieve efficient mixing and uniform dispersion of multiphase materials. Within micrometer-scale microchannels, continuous feeding allows materials to form special flow patterns such as laminar flow and vortex flow within a confined space, achieving rapid, controllable, and highly uniform mixing and dispersion of different components. During the mixing and dispersion process, functional preemulsions, nano-silica dispersions, MXene nanosheet dispersions, and initiators are continuously pumped in through their respective inlet channels. The materials converge and flow within the microchannels while simultaneously completing mixing and dispersion, while the mixed products are continuously collected at the output end. Microchannel continuous flow mixing and dispersion provides extremely strong shear forces and ultra-high mixing efficiency, capable of separating reactants into extremely thin microlayers. Within the microchannels, the reaction velocity gradient is extremely high, generating shear forces far exceeding those of conventional stirring. This powerful shear force effectively breaks up the agglomeration of nano-silica and the loose stacking of MXene nanosheets, enabling them to achieve uniform dispersion before re-aggregation. Efficient mixing provides a highly uniform reaction mixture for subsequent gelation and Joule heat treatment, ensuring that the final silicon-based anode material possesses a uniform three-dimensional carbon framework, nano-silicon, and MXene conductive bridging structure. Utilizing microchannel continuous flow technology, efficient mixing and precise process control are achieved. All components undergo nearly identical mixing and dispersion times, allowing for precise control of the reaction process and yielding products with highly consistent structure and properties. This ensures high batch-to-batch consistency and enables high-quality, large-scale production.

[0056] Specifically, in step S13 above, during the continuous flow mixing and dispersion process in the microchannels, the diameter of the microchannels is 50 μm-1000 μm. This size range can handle reactants containing nano-silicon (particle size 80 nm-120 nm) and MXene nanosheets (sheet size 2 μm-4 μm) while preventing clogging, thereby achieving high throughput. In some embodiments of the present invention, the diameter of the microchannels is 60 μm-100 μm, 200 μm-300 μm, 400 μm-500 μm, 600 μm-700 μm, 800 μm-900 μm, etc.; in some specific embodiments of the present invention, the diameter of the microchannels can specifically be 70 μm, 180 μm, 250 μm, 550 μm, 680 μm, 880 μm, etc.

[0057] Specifically, in step S13, the microchannel continuous flow mixing and dispersion time is 5s-1800s. Precisely controlling the microchannel continuous flow dispersion time can effectively avoid droplet aggregation during dispersion and ensure that the obtained reaction mixture is uniform and stable. The microchannel continuous flow mixing and dispersion is carried out at room temperature. In some embodiments of the present invention, the microchannel continuous flow mixing and dispersion time is 10s-100s, 200s-500s, 600s-800s, 1000s-1200s, 1400s-1600s, 1000s-1800s, etc.; in some specific embodiments of the present invention, the microchannel continuous flow mixing and dispersion time is 15s, 50s, 120s, 400s, 800s, 1100s, 1500s, etc.

[0058] Specifically, in step S13, the microchannels used for continuous flow mixing and dispersion include any one or more combinations of T-shaped microchannels, Y-shaped microchannels, serpentine microchannels, spiral microchannels, staggered microchannels, diversion-convergence microchannels, or impact flow microchannels. It can be understood that the microchannels in continuous flow mixing refer to the channels where reactants converge. Through the design of the microchannel shape, utilizing the specific shape and structure of the microchannel, different reactants collide or intersect when they converge in microchannels with specific shapes, repeatedly shearing and re-fusing the reactants. Impact energy is used to disperse the reactants, achieving efficient mixing. For example, serpentine microchannels have a curved structure; when reactants converge in serpentine microchannels, they collide with the curved channel walls, effectively disturbing the laminar flow state of the reactants and promoting efficient and uniform mixing. Specifically, the continuous flow mixing and dispersion can be carried out in a continuous flow microchannel reactor.

[0059] Specifically, carbon source monomers, nitrogen-containing functional monomers, multifunctional crosslinking monomers, and silane coupling monomers are mixed in the functional preemulsion to obtain a polymerizable component. Further, the mass ratio of nano-silicon, MXene nanosheets, and the polymerizable component is (96-105):(17-28):100. At this mass ratio, the content of nano-silicon is relatively high. Nano-silicon, as a high-capacity lithium storage active material, can ensure that the prepared silicon-based anode material has a high capacity. MXene nanosheets, as highly conductive two-dimensional materials, can form MXene conductive bridging structures, further improving electron transport efficiency and alleviating the volume expansion of nano-silicon. The content of the polymerizable component is close to that of nano-silicon. The polymerizable component is used to form a three-dimensional carbon skeleton, which can form a sufficiently dense and complete three-dimensional carbon skeleton to encapsulate the nano-silicon. The formed three-dimensional carbon skeleton can provide sufficient buffer space for the volume expansion of nano-silicon and can also construct a basic conductive network, compensating for the poor conductivity of nano-silicon.

[0060] In some embodiments of the present invention, the mass ratio of nano-silicon, MXene nanosheets, and polymerizable components is (96-100):(20-22):100, (97-100):(18-25):100, (102-105):(25-28):100, etc.; in some specific embodiments of the present invention, the mass ratio of nano-silicon, MXene nanosheets, and polymerizable components is 96:17:100, 98:18:100, 105:28:100, etc.

[0061] Specifically, in step S13, the initiator, functional preemulsion, nano-silica dispersion, and MXene nanosheet dispersion are further mixed and dispersed in a microchannel continuous flow. The weak chemical bonds of the initiator break under heat or redox reactions, generating highly reactive free radicals. These free radicals attack the chemical bonds of the polymerizable components in the functional preemulsion, causing them to open and form new free radicals, thereby initiating a chain polymerization reaction and causing the reaction mixture to gel, thus obtaining a gelled precursor. During the microchannel continuous flow mixing and dispersion, the temperature is at room temperature, and the initiator has not yet begun to react. The microchannel continuous flow mixing and dispersion ensures that the initiator is uniformly dispersed in the reaction mixture, allowing the subsequent gelation reaction to proceed uniformly and rapidly.

[0062] Specifically, the initiator includes any one or a combination of azobisisobutyronitrile (AIBN), benzoyl peroxide, ammonium persulfate, and potassium persulfate. The amount of initiator used is 1%-1.5% of the total mass of the polymerizable components. In some embodiments of the present invention, the amount of initiator used is 1.2%-1.35%, 1.25%-1.3%, 1.36%-1.42%, 1.42%-1.48%, etc., of the total mass of the polymerizable components; in some specific embodiments of the present invention, the amount of initiator used is 1.15%, 1.26%, 1.38%, 1.44%, 1.46%, etc., of the total mass of the polymerizable components.

[0063] Specifically, in step S14 above, the highly homogeneous reaction mixture obtained after continuous flow mixing and dispersion in microchannels is gelled under shearing to obtain a gelled precursor. The shearing rate of the shearing action is 1000 s⁻¹. -1 -20000s -1 At this shear rate, strong shear force can be generated. During the gelation process of the reaction mixture, nano-silicon and MXene nanosheets may still migrate, settle, and locally aggregate and overlap. Under the action of strong shear force, these situations can be avoided. In some embodiments of the present invention, the shear rate is 2500 s⁻¹. -1 -16000s -1 5000s -1 -18000s -1 10000s-1 -12000s -1 16000s -1 -18000s -1 Etc.; In some specific embodiments of the present invention, the shear rate is 3800 s. -1 4500s -1 5800s -1 11500s -1 13600s -1 15000s -1 etc.

[0064] Specifically, in step S14, the gelation temperature is 40℃-90℃ and the time is 5min-120min. At 40℃-90℃, the initiator in the reaction mixture generates highly active free radicals upon heating. These free radicals attack the chemical bonds of the polymerizable components in the functional preemulsion, causing them to open and thus initiating the reaction, resulting in gelation of the reaction mixture. The carbon source monomer can undergo free radical copolymerization with the nitrogen-containing functional monomer, introducing nitrogen into the carbon source monomer backbone. During gelation, the multifunctional crosslinking monomer can connect multiple polymer chains to form crosslinking points, gradually transforming the reaction system from a linear or branched polymer into a dense and stable three-dimensional crosslinked gel network with spatial network characteristics. The silane coupling monomer has a silane group at one end that condenses or couples with the silanol groups (Si-OH) on the surface of the nano-silicon to form Si-O-Si bonds, and the other end connects to the three-dimensional crosslinked gel network through organic unsaturated groups, establishing an interfacial connection between the nano-silicon and the three-dimensional crosslinked gel network through the silane coupling monomer.

[0065] In some embodiments of the present invention, the gelation temperature is 45℃-60℃, 65℃-88℃, 55℃-74℃, 70℃-88℃, 86℃-90℃, etc.; in some specific embodiments of the present invention, the gelation temperature is 48℃, 58℃, 67℃, 76℃, 88℃, etc. In some embodiments of the present invention, the gelation time is 15min-20min, 35min-110min, 45min-100min, 55min-90min, 60min-80min, etc.; in some specific embodiments of the present invention, the gelation time is 18min, 45min, 65min, 110min, 118min, etc.

[0066] Specifically, in step S14, MXene nanosheets are embedded between polymerizable components under strong shear force, thereby entering the three-dimensional cross-linked gel network; the nano-silicon generates Si-O-Si bonds through condensation or coupling reactions between its surface silanol groups (Si-OH) and silane coupling monomers, which chemically anchors the nano-silicon to the three-dimensional cross-linked gel network, and the well-dispersed nano-silicon is quickly fixed in the pores, nodes or gaps of the three-dimensional cross-linked gel network.

[0067] Specifically, in step S15, the gelled precursor obtained in step S14 is freeze-dried or vacuum-dried to remove the solvent, and then subjected to Joule heat treatment in an inert atmosphere to obtain a silicon-based anode material. The Joule heat treatment temperature is 500℃-1200℃, and the time is 1s-1800s. The gelled precursor is placed in an inert atmosphere, a voltage is applied, Joule heat is generated and the temperature rises rapidly, thereby causing the three-dimensional cross-linked gel network to carbonize and form a silicon-based anode material. Joule heat treatment can reduce the problems of nano-silicon migration, particle growth or local agglomeration caused by long-term high-temperature heat treatment by achieving rapid and uniform bulk phase heating, which helps to maintain the integrity of the three-dimensional carbon skeleton structure and the continuity of the conductive network.

[0068] In some embodiments of the present invention, the Joule heat treatment temperature is 550℃-800℃, 680℃-800℃, 700℃-960℃, 850℃-1100℃, 1080℃-1200℃, etc.; in some specific embodiments of the present invention, the Joule heat treatment temperature is 560℃, 780℃, 870℃, 950℃, 1000℃-1005℃, etc. In some embodiments of the present invention, the Joule heat treatment time is 10s-100s, 20s-200s, 100s-400s, 350s-650s, 800s-1200s, 1100s-1500s, etc.; in some specific embodiments of the present invention, the Joule heat treatment time is 15s, 25s, 120s, 600s, 800s, 955s, 1150s, etc.

[0069] Specifically, the voltage for Joule heat treatment is 1V-100V, and the current is 0.1A-100A. In some embodiments of the present invention, the voltage for Joule heat treatment is 10V-20V, 16V-48V, 30V-70V, 55V-80V, etc.; in some specific embodiments of the present invention, the voltage for Joule heat treatment is 4V, 26V, 48V, 50V, 66V, 78V, 95V, etc. In some embodiments of the present invention, the current for Joule heat treatment is 0.6A-10A, 4A-30A, 8A-48A, 20A-68A, 70A-90A, etc.; in some specific embodiments of the present invention, the current for Joule heat treatment is 0.6A, 25A, 36A, 48A, 66A, 85A, etc.

[0070] Specifically, after the Joule heat treatment in step S15, the carbon source monomers, multifunctional crosslinked monomers, and nitrogen-containing functional monomers in the three-dimensional crosslinked gel network are transformed into a three-dimensional carbon skeleton of the silicon-based anode material. The carbon source monomers, as the main carbon source of the three-dimensional carbon skeleton, undergo dehydration, condensation, cracking, and further carbonization at high temperatures to form amorphous carbon or hard carbon structures, constituting the main skeleton of the three-dimensional carbon skeleton. During the Joule heat treatment, the nitrogen-containing functional monomers undergo structural rearrangement and carbonization. Some nitrogen is lost as volatile small molecules, while the remaining nitrogen is retained at the edges, defect sites, or in the graphitized carbon network, forming the nitrogen-doped structure of the three-dimensional carbon skeleton. The multifunctional crosslinked monomers undergo pyrolysis, rearrangement, and carbonization during the heat treatment. Because they have already formed a spatial network with a high crosslinking density during the gelation stage, carbonization can form a carbon structure with a certain rigidity and supporting function, forming the rigid part of the three-dimensional carbon skeleton that provides support. During Joule heat treatment, the polymer components of the three-dimensional cross-linked gel network undergo pyrolysis to generate a large amount of volatile small molecule gas. The small molecule gas is rapidly released into the three-dimensional carbon skeleton to form a large number of porous structures. The porous structure of the three-dimensional carbon skeleton can restrict the migration and aggregation of nano-silicon, providing a buffer space for the volume expansion of nano-silicon during charging and discharging.

[0071] Specifically, during the Joule heat treatment process, the organic groups in the silane coupling monomer undergo thermal decomposition or partial carbonization at high temperatures, and the silane coupling monomer forms an interface anchoring structure between the nano-silicon and the three-dimensional carbon framework; MXene nanosheets form the MXene conductive bridging structure of the silicon-based anode material in the three-dimensional carbon framework, and the nano-silicon, as the conductive phase and electrothermal conversion unit of the silicon-based anode material, is confined within the three-dimensional carbon framework and the MXene conductive bridging structure.

[0072] It is understood that the method for preparing a silicon-based anode material provided in this application involves mixing a carbon source monomer, a nitrogen-containing functional monomer, a multifunctional crosslinking monomer, and a silane coupling monomer to form a functional pre-emulsion, thereby uniformly mixing the polymerizable components in advance to provide a homogeneous, polymerizable, and crosslinkable continuous medium for nano-silicon and MXene nanosheets. The functional pre-emulsion, nano-silicon dispersion, MXene nanosheet dispersion, and initiator are then subjected to microchannel continuous flow mixing and dispersion to obtain a reaction mixture. The microchannel continuous flow mixing and dispersion utilizes rapid mixing and local shearing in a microscale confined space to reduce nano-silicon agglomeration and MXene nanosheet stacking, thereby forming a highly homogeneous reaction system of the functional pre-emulsion, nano-silicon dispersion, MXene nanosheet dispersion, and initiator. The reaction mixture gels under strong shear force, causing polymerization and cross-linking to form a three-dimensional cross-linked gel network before the homogeneous reaction system constructed by continuous microchannel mixing and dispersion is destroyed. The strong shear force preserves the uniform dispersion of nano-silicon and MXene nanosheets, preventing migration, aggregation, or stacking during the gelation reaction and subsequent Joule heat treatment. Finally, Joule heat treatment carbonizes the three-dimensional cross-linked gel network to form a three-dimensional carbon framework, yielding a silicon-based anode material with a three-dimensional carbon framework, nano-silicon, MXene conductive bridging structure, and interface anchoring structure. In the preparation process of this invention, the previous step determines the initial state of the next step; the uniformity of the functional pre-emulsion determines whether each functional component can uniformly contact the nano-silicon and MXene nanosheets during continuous microchannel mixing and dispersion; the effect of continuous microchannel mixing and dispersion determines the spatial distribution of nano-silicon and MXene nanosheets before gelation; and strong shear gelation determines whether this uniform distribution can be maintained during carbonization. By adopting an integrated preparation path of "functional preemulsion-microchannel continuous flow mixing and dispersion-strong shear gelation-Joule thermal carbonization", a silicon-based anode material with uniform and stable structure, good conductivity and stable cycle performance was obtained.

[0073] Please see Figure 2 and Figure 3 The second embodiment of the present invention provides a silicon-based anode material 10, which is prepared by the method for preparing a silicon-based anode material described in the first embodiment.

[0074] Specifically, the silicon-based anode material 10 includes nano-silicon 11, an MXene conductive bridging structure 12, a three-dimensional carbon skeleton 13, and an interface anchoring structure 14; the three-dimensional carbon skeleton 13 has a skeleton body 131, a nitrogen-doped structure 132, and a porous structure 133, the nitrogen-doped structure 132 is distributed in the skeleton body 131, and the porous structure 133 is formed in the parts of the three-dimensional carbon skeleton 13 that do not contain the skeleton body 131.

[0075] Specifically, nano-silicon 11 is dispersed within the three-dimensional carbon framework 13, between framework nodes, or in the porous structure 133, and forms a stable interface anchoring structure 14 with the surrounding three-dimensional carbon framework 13 through silane coupling monomers. MXene conductive bridging structures 12 are interspersed within or on the surface of the three-dimensional carbon framework 13, forming a conductive bridge between the three-dimensional carbon framework 13 and the nano-silicon 11; the nano-silicon 11 and the MXene conductive bridging structures 12 are uniformly distributed within the three-dimensional carbon framework 13; the nano-silicon 11 is confined within the three-dimensional carbon framework 13 and the MXene conductive bridging structures 12.

[0076] Specifically, the three-dimensional carbon skeleton 13 is formed by carbonizing a three-dimensional cross-linked gel network composed of carbon source monomers, nitrogen-containing functional monomers, and multifunctional cross-linked monomers through Joule heat treatment; the carbon source monomers and multifunctional cross-linked monomers form the skeleton body 131 of the three-dimensional carbon skeleton 13, and the nitrogen-containing functional monomers form the nitrogen-containing doped structure 132 of the three-dimensional carbon skeleton 13.

[0077] Specifically, the MXene conductive bridging structure 12 and the three-dimensional carbon framework 13 work together to form a highly efficient and stable conductive network in the silicon-based anode material 10, uniformly distributing nano-silicon 11 within the conductive network. Nano-silicon 11, as a high-capacity lithium storage active material, provides high capacity for the silicon-based anode material 10. The three-dimensional carbon framework 13 forms a globally continuous conductive system. The porous structure 133 of the three-dimensional carbon framework 13 provides ample buffer space for the volume expansion of nano-silicon 11, and the nitrogen-doped structure 132 is beneficial for improving electron transport capability and interfacial polarity. The MXene conductive bridging structure 12 is the backbone of the conductive network, possessing extremely high conductivity and providing a highly efficient electron transport channel. The MXene conductive bridging structure 12 is flexible and can effectively buffer the volume expansion of nano-silicon 11. An interface anchoring structure 14 exists between the nano-silicon 11 and the three-dimensional carbon framework 13, anchoring the nano-silicon 11 within the three-dimensional carbon framework 13 and preventing the nano-silicon 11 from detaching during charging and discharging. The silicon-based anode material 10 has a uniform and stable structure, low impedance, good conductivity, and strong cycle stability.

[0078] Other limitations regarding the silicon-based anode material 10 are the same as in the first embodiment and will not be repeated here.

[0079] See Figure 4 As shown, the third embodiment of the present invention provides a lithium-ion battery 9, which includes a positive electrode 3, an electrolyte 2, and a negative electrode 1. The negative electrode 1 of the lithium-ion battery 9 includes a silicon-based negative electrode material 10 as described in the second embodiment.

[0080] See Figure 5 As shown, the specific preparation process of the lithium-ion battery 9 is as follows: Step S21: Mix the negative electrode material with the conductive agent and binder in a solvent to prepare the negative electrode slurry; Step S22: The negative electrode slurry is coated onto the surface of the current collector, and after pre-drying, vacuum drying, rolling and die-cutting, a negative electrode sheet is obtained; and Step S23: Provide a positive electrode, a separator, and an electrolyte. Assemble the negative electrode obtained in step S22 with the positive electrode and the separator into a soft-pack battery cell. After injecting the electrolyte, allow it to stand, form, degas, seal, and perform capacity testing to obtain a lithium-ion battery.

[0081] Specifically, in step S21, the negative electrode material can be the silicon-based negative electrode material 10 described in the first embodiment of the present invention. Alternatively, the negative electrode material can be a mixture of the aforementioned silicon-based negative electrode material 10 and negative electrode materials such as graphite, artificial graphite, natural graphite, hard carbon, soft carbon, and silicon-oxygen materials; the present invention does not limit this. The conductive agent includes one or more combinations of conductive carbon black, carbon nanotubes, graphene, and vapor-grown carbon fibers; the binder includes one or more combinations of sodium carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, sodium alginate, and polyvinylidene fluoride; and the solvent can be deionized water.

[0082] Specifically, in step S21, the mass ratio of the negative electrode material, conductive agent, and binder is (90-95):(2-5):(1-5). In some embodiments of the present invention, the mass ratio of the negative electrode material, conductive agent, and binder is (92-95):(2-5):(1-5), (93-94):(3-5):(1-3), (92-95):(2-5):(2-3), etc. In some specific embodiments of the present invention, the mass ratio of the negative electrode material, conductive agent, and binder is 92:5:3, 95:3:2, 95:2:3, etc.

[0083] Specifically, in step S22, the pre-drying temperature is 80℃-90℃, and the vacuum drying temperature is 100℃-120℃. In some embodiments of the present invention, the pre-drying temperature is 80℃-84℃, 82℃-86℃, 85℃-88℃, 87℃-90℃, etc.; in some specific embodiments of the present invention, the pre-drying temperature is 81℃, 83℃, 84.5℃, 89℃, 90℃, etc. In some embodiments of the present invention, the vacuum drying temperature is 102℃-108℃, 104℃-106℃, 105℃-115℃, 112℃-118℃, etc.; in some specific embodiments of the present invention, the vacuum drying temperature is specifically 103℃, 107℃, 110℃, 116℃, 120℃, etc.

[0084] Specifically, in step S23, the positive electrode 3 is prepared using a high-nickel ternary positive electrode material (NCM811). NCM811, conductive agent, and binder are mixed in a mass ratio of (94-97):(2-4):(1-2), and N-methylpyrrolidone is added to prepare a positive electrode slurry, which is then coated onto the surface of an aluminum foil. After drying, rolling, and die-cutting, the positive electrode 3 is obtained.

[0085] Specifically, in step S23, the electrolyte 2 is a mixed solution of lithium hexafluorophosphate (LiPF6) electrolyte and ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC), wherein the concentration of lithium hexafluorophosphate (LiPF6) is 0.8 mol / L-1.2 mol / L, and the volume ratio of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate is 1:1:1. Fluorinated ethylene carbonate is also added to the electrolyte 2 as a film-forming additive, and the volume ratio of fluorinated ethylene carbonate to the total volume of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate is 0.05:0.95.

[0086] When the silicon-based anode material 10 of the present invention is applied to a lithium-ion battery 9, the high content of nano-silicon 11 improves the capacity of the lithium-ion battery 9. Through the dual action of the three-dimensional carbon skeleton 13 and the MXene conductive bridging structure 12, the volume expansion of nano-silicon 11 during charging and discharging is effectively buffered, solving the problems of easy pulverization and rapid capacity decay of nano-silicon 11, and improving the cycle life of the lithium-ion battery 9. The dense three-dimensional carbon skeleton 13 can effectively isolate the electrolyte 2, suppress side reactions, and guide the formation of a more stable SEI film, improving the first coulombic efficiency of the lithium-ion battery 9. The porous structure 133 of the three-dimensional carbon skeleton 13 and the MXene conductive bridging structure 12, which combines mechanical strength and flexibility, can withstand the compressive stress caused by the expansion of nano-silicon 11, protecting the internal structure. The MXene conductive bridging structure 12 can effectively suppress the agglomeration of nano-silicon 11 particles, enhancing the structural stability of the electrode and the safety of the lithium-ion battery 9. When the silicon-based anode material 10 of the present invention is applied to a lithium-ion battery 9, the energy density, cycle life, and safety of the resulting lithium-ion battery 9 are significantly improved.

[0087] To better illustrate the excellent performance of the silicon-based anode material prepared by the technical solution protected by this invention, this invention further provides the following specific experimental examples and comparative examples as specific examples of the silicon-based anode material and its preparation method claimed by this invention.

[0088] Experimental Example 1: 1. Preparation of functional preemulsions Furfuryl alcohol (carbon source monomer), 1-vinylimidazole (nitrogen-containing functional monomer), TAIC (multifunctional crosslinking monomer), and KH-570 (silane coupling monomer) were added to a reaction vessel in a mass ratio of 55:20:15:10. The mixture was stirred at room temperature for 30 min to ensure thorough mixing and obtain a polymerizable component.

[0089] Sodium dodecyl sulfate was added to a mixed solvent of ethanol / deionized water and stirred until completely dissolved to obtain an emulsion medium. Subsequently, under high-speed emulsification conditions, the polymerizable component was slowly added to the emulsion medium, with the emulsification speed controlled at 8000 rpm and the emulsification time at 20 min, to obtain a homogeneous and stable functional pre-emulsion; wherein the amount of sodium dodecyl sulfate added was 1.5% of the total mass of the polymerizable component.

[0090] 2. Preparation of nano-silicon dispersions and MXene nanosheet dispersions Nano-silicon with a particle size of 80-120 nm was added to a mixed solvent of ethanol / deionized water and ultrasonically dispersed for 30 min to obtain a nano-silicon dispersion. Ti3C2T with a flake diameter of 2-3 μm x MXene (in its chemical formula, T) x (x represents the average number of surface functional groups) Nanosheets were added to a mixed solvent of deionized water and ethanol and ultrasonically dispersed for 20 min under 0°C ice bath conditions to obtain MXene dispersion.

[0091] The mass ratio of nano-silicon to MXene nanosheets is 96:17.

[0092] 3. Microchannel continuous flow mixing and dispersion The nano-silicon dispersion, MXene nanosheet dispersion, functional preemulsion, and AIBN initiator were continuously mixed in a microchannel continuous flow reactor using metering pumps. The microchannel continuous flow reactor was a serpentine microchannel reactor with a channel characteristic size of 300 μm. The mass ratio of polymerizable components in the nano-silicon, MXene nanosheets, and functional preemulsion was 96:17:100, and the amount of AIBN initiator added was 1% of the total mass of polymerizable components in the functional preemulsion.

[0093] The feed flow rates of the nano-silicon dispersion, MXene nanosheet dispersion, functional preemulsion, and initiator were controlled so that the polymerizable components in the nano-silicon, MXene nanosheets, and functional preemulsion entered the microchannel reactor at a mass ratio of 96:17:100. The residence time of the reaction system in the microchannel was controlled to be 300 s, and the mixture was mixed and dispersed at room temperature to obtain the reaction mixture.

[0094] 4. Strong shear gelation The reaction mixture obtained in the previous step was subjected to high-speed shearing to induce gelation of the reaction system. The temperature was raised to 65°C, and the shear rate was controlled at 8000 s⁻¹. - ¹, the gelation time was 30 min, and the gelled precursor was obtained.

[0095] 5. Joule heat treatment The gelled precursor is freeze-dried or vacuum-dried to remove the solvent, and then placed in an argon atmosphere to undergo Joule heating. The Joule heating temperature is controlled at 800℃ and the treatment time is 180s. After the treatment is completed, it is naturally cooled to room temperature under argon protection to obtain the silicon-based anode material.

[0096] 6. Preparation of negative electrode sheet The above-mentioned silicon-based anode material, conductive carbon black, carbon nanotubes, sodium carboxymethyl cellulose, styrene-butadiene rubber and polyacrylic acid were mixed in a mass ratio of 92:2:1:1.5:1.5:2, and deionized water was added as a solvent. The mixture was stirred and dispersed to obtain anode slurry. The anode slurry was uniformly coated on the surface of copper foil current collector, and after pre-drying at 80°C, vacuum drying at 110°C, rolling and die-cutting, anode sheet was obtained.

[0097] 7. Lithium-ion battery manufacturing The positive electrode sheet is prepared using NCM811 ternary positive electrode material. Specifically, NCM811, conductive carbon black, carbon nanotubes, and polyvinylidene fluoride are mixed in a mass ratio of 97:1:0.8:1.2, and N-methylpyrrolidone is added to prepare a positive electrode slurry, which is then coated onto the surface of aluminum foil. After drying, rolling, and die-cutting, the positive electrode sheet is obtained. The electrolyte is a mixed solution of lithium hexafluorophosphate (LiPF6) electrolyte and ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC), wherein the concentration of lithium hexafluorophosphate (LiPF6) is 1 mol / L, and the volume ratio of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate is 1:1:1. Fluorinated ethylene carbonate is also added to the electrolyte as a film-forming additive, and the volume ratio of fluorinated ethylene carbonate to the total volume of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate is 0.05:0.95.

[0098] The positive electrode, negative electrode, and separator are assembled into a soft-pack battery cell. After injecting electrolyte, the cell is allowed to stand, form, degas, be finally sealed, and undergo capacity testing to obtain a lithium-ion battery.

[0099] Experimental Example 2: The difference from Experimental Example 1 is that in the preparation of the functional preemulsion, the mass ratio of furfuryl alcohol, 1-vinylimidazole, TAIC, and KH-570 is 50:20:20:10, and the TAIC content is higher than in Experimental Example 1. The remaining processing steps and reaction conditions are the same as in Experimental Example 1.

[0100] Experimental Example 3: The difference from Experimental Example 1 is that in the preparation of the functional preemulsion, the mass ratio of furfuryl alcohol, 1-vinylimidazole, TAIC, and KH-570 is 50:20:15:15, and the KH-570 content is higher than in Experimental Example 1. The remaining processing steps and reaction conditions are the same as in Experimental Example 1.

[0101] Experimental Example 4: The difference from Experimental Example 1 is that, during the microchannel continuous flow mixing and dispersion process, the polymerizable components in the nano-silicon, MXene nanosheets, and functional preemulsion are in a mass ratio of 105:28:100, increasing the proportion of MXene nanosheets. The mass ratio of each monomer in the polymerizable components remains the same as in Experimental Example 1. The remaining processing steps and reaction conditions are the same as in Experimental Example 1.

[0102] Experimental Example 5: The difference from Experimental Example 1 is that the Joule heat treatment temperature is 900℃ and the Joule heat treatment time is 120s. The remaining treatment steps and reaction conditions are the same as in Experimental Example 1.

[0103] Comparative Example 1: The difference from Experimental Example 1 is that, instead of using a microchannel continuous flow reaction mixing and dispersion method, conventional mechanical stirring was used to mix the functional preemulsion, nano-silica dispersion, MXene nanosheet dispersion, and initiator. The functional preemulsion, nano-silica dispersion, MXene nanosheet dispersion, and AIBN initiator described in Example 1 were sequentially added to a reaction vessel and mechanically stirred at 1000 rpm for 60 min at room temperature to obtain the reaction mixture. The remaining processing steps and reaction conditions were the same as in Experimental Example 1.

[0104] Comparative Example 2: The difference from Experimental Example 1 is that, instead of undergoing gelation under strong shear, the resulting reaction mixture was directly subjected to static polymerization or direct drying. Specifically, the reaction mixture obtained by continuous flow mixing and dispersion in microchannels was allowed to stand at 65°C for 60 min to allow the system to undergo a normal gelation reaction. The remaining processing steps and reaction conditions were the same as in Experimental Example 1.

[0105] Comparative Example 3: The difference from Experimental Example 1 is that the KH-570 silane coupling monomer was not added to the functional preemulsion, and the corresponding mass part of KH-570 was made up with furfuryl alcohol. Specifically, in the preparation of the functional preemulsion, the mass ratio of furfuryl alcohol, 1-vinylimidazole, and TAIC was 65:20:15. The remaining processing steps and reaction conditions were the same as in Experimental Example 1.

[0106] Comparative Example 4: The difference from Experimental Example 1 is that MXene nanosheets were not added, and the polymerizable component in the functional preemulsion was used to make up the corresponding mass. Specifically, during the microchannel continuous flow mixing and dispersion process, the mass ratio of nano-silicon to the polymerizable component in the functional preemulsion was 96:117. The remaining processing steps and reaction conditions were the same as in Experimental Example 1.

[0107] Comparative Example 5: The difference from Experimental Example 1 is that Joule heat treatment was not used; instead, conventional tube furnace carbonization was employed. Specifically, the gelled precursor, after strong shear gelation and drying, was placed in a tube furnace and heated to 800°C at a rate of 5°C / min under an argon atmosphere, held at that temperature for 2 h, and then allowed to cool naturally to room temperature. The remaining processing steps and reaction conditions were the same as in Experimental Example 1.

[0108] Comparative Example 6: The difference from Experimental Example 1 is that the functional preemulsion composed of furfuryl alcohol, 1-vinylimidazole, TAIC, and KH-570 in Experimental Example 1 was replaced with a preemulsion composed of styrene, acrylonitrile, and divinylbenzene, wherein the mass ratio of styrene, acrylonitrile, and divinylbenzene was 55:35:10. The remaining treatment steps and reaction conditions were the same as in Experimental Example 1.

[0109] The initial coulombic efficiency, reversible specific capacity, cycle capacity retention, rate performance, impedance change, and cycle thickness expansion rate of the lithium-ion batteries obtained in Experimental Examples 1-5 and Comparative Examples 1-6 were tested.

[0110] First reversible specific capacity test: At 25℃, formation is performed with a small current, and the first discharge capacity is recorded. This capacity is then divided by the mass of the active material in the negative electrode. The resulting specific capacity is the first reversible specific capacity (mAh / g) of the negative electrode material.

[0111] First Coulomb efficiency test: At 25°C, formation was performed with a small current, and the first charge capacity and the first discharge capacity were recorded. First Coulomb efficiency = (first discharge capacity / first charge capacity) × 100%.

[0112] Cyclic performance test: At 25°C, a 0.5C charge and 1C discharge regime was used for cyclic testing, and the capacity retention rate was recorded after 100, 300 and 500 cycles.

[0113] Thickness expansion test: Test the initial thickness of the battery cell and the thickness after cycling under full charge, and calculate the thickness expansion rate after 300 cycles and 500 cycles.

[0114] Rate performance testing: Discharge tests were conducted at 0.2C, 0.5C, 1C and 2C rates, and the capacity retention rate under 1C and 2C conditions was recorded.

[0115] Impedance testing: Electrochemical impedance spectroscopy was used to test the initial impedance of the cell and the impedance change after 300 cycles to evaluate the interface stability and the retention of the conductive network.

[0116] Evaluation of electrode condition after cycling: The lithium-ion battery is subjected to 300 cycles of charge and discharge. After cycling, the negative electrode is observed to see whether phenomena such as pulverization, expansion, cracking, and local detachment occur. This is used to evaluate the overall structural stability of silicon-based negative electrode materials.

[0117] Table 1. Performance test results of lithium-ion batteries in experimental examples and comparative examples.

[0118] Table 2. Rate performance and impedance test results of lithium-ion batteries in experimental examples and comparative examples.

[0119] As shown in Tables 1 and 2, when the silicon-based anode materials obtained in Examples 1-5 are applied to lithium-ion batteries, the lithium-ion batteries all exhibit high initial reversible specific capacity, high initial coulombic efficiency, superior cycle capacity retention, and low cycle thickness expansion. In Examples 1-5, the initial reversible specific capacity of the lithium-ion batteries is greater than or equal to 1996 mAh·g. 1 The initial coulomb efficiency is greater than or equal to 89.8%, the 500-cycle capacity retention is greater than or equal to 89.1%, the 500-cycle thickness expansion rate is less than or equal to 22.2%, the 3C capacity retention is greater than or equal to 82.5%, and the initial impedance is less than or equal to 42Ω. The negative electrode sheet maintained good condition after 300 cycles, with a diameter of cm². In Experiment 1, a functional pre-emulsion system composed of furfuryl alcohol, 1-vinylimidazole, TAIC, and KH-570 was used, combined with microchannel continuous flow dispersion, strong shear gelation, and Joule heat treatment under argon atmosphere. The resulting lithium-ion battery exhibited the best overall performance, achieving an initial reversible specific capacity of 2018 mAh / g, an initial coulombic efficiency of 90.6%, a 300-cycle capacity retention of 94.8%, a 500-cycle capacity retention of 90.5%, and a 300-cycle thickness expansion of only 13.5%. It demonstrated high capacity retention, low impedance, and an intact negative electrode sheet without significant pulverization after 300 cycles.

[0120] In Experiment 2, increasing the content of TAIC multifunctional crosslinking monomers increased the crosslinking density of the three-dimensional crosslinked gel network, resulting in better stability of the three-dimensional carbon skeleton structure. However, excessively high crosslinking density may slightly reduce the flexibility of the three-dimensional carbon skeleton, thus its initial reversible specific capacity and cycling performance were slightly lower than those of Example 1. This result indicates that an appropriate content of multifunctional crosslinking monomers is beneficial to improving the stability of the three-dimensional carbon skeleton, but the crosslinking density needs to be controlled within a reasonable range.

[0121] In Experiment 3, the thickness expansion rate of the lithium-ion battery was further reduced after the content of KH-570 silane coupling monomer was increased. This indicates that the interface anchoring structure formed by KH-570 can enhance the bonding force between nano-silicon and the three-dimensional carbon skeleton, which is beneficial to suppressing the shedding and volume expansion of nano-silicon during cycling.

[0122] In Experiment 4, the increased MXene nanosheet content improved the 1C and 3C rate performance of the lithium-ion battery, and the initial impedance and post-cycle impedance were lower, indicating that MXene nanosheets can effectively construct MXene conductive bridging structures and improve electron transport capability.

[0123] In Experiment 5, the Joule heat treatment temperature was increased to 900℃ and the treatment time was shortened to 120s. The resulting silicon-based anode material exhibited good carbonization and conductivity. However, the higher temperature may have caused shrinkage of the three-dimensional carbon skeleton, reducing its ability to mitigate the expansion of nano-silicon. Therefore, the cyclic expansion was slightly higher than in Example 1. This result indicates that the Joule heat treatment temperature and time need to be controlled synergistically to achieve a suitable degree of carbonization while maintaining the integrity of the three-dimensional carbon skeleton.

[0124] Compared to Experimental Example 1, Comparative Example 1 did not employ microchannel continuous flow mixing and dispersion, but instead used ordinary mechanical stirring. This resulted in a decrease in the uniformity of dispersion of nano-silicon and MXene nanosheets. The resulting lithium-ion battery exhibited a capacity retention of only 76.5% after 300 cycles and a capacity retention of only 63.8% after 500 cycles, with a significant increase in thickness expansion after cycling. Comparative Example 1 did not utilize microchannel continuous flow mixing and dispersion; the mixing and dispersion of nano-silicon and MXene nanosheets relied primarily on macroscopic mechanical stirring. This method makes it difficult to achieve uniform microscale mixing of nano-silicon, MXene nanosheets, and the functional pre-emulsion, easily leading to localized agglomeration of nano-silicon and localized stacking of MXene nanosheets. This resulted in decreased uniformity and structural instability of the silicon-based anode material obtained after Joule heat treatment. Compared to Experimental Example 1, the lithium-ion battery obtained in Comparative Example 1 showed decreased initial coulombic efficiency, rate performance, and cycle capacity retention, while exhibiting an increased thickness expansion after cycling. The results demonstrate that the microchannel continuous flow mixing and dispersion process plays an important role in achieving uniform dispersion of nano-silicon and MXene nanosheets, constructing a uniform three-dimensional carbon framework, and improving the cycle stability of silicon-based anode materials.

[0125] Compared to Experimental Example 1, Comparative Example 2, although employing microchannel continuous flow mixing and dispersion, did not undergo gelation under strong shear conditions. During the transition from liquid to gel states in the reaction system, nano-silicon and MXene nanosheets still exhibited the potential for migration, sedimentation, and localized aggregation. Particularly during solvent evaporation and drying, nano-silicon particles easily migrated with the liquid phase and accumulated in localized areas, while MXene nanosheets were prone to re-stacking. Compared to Experimental Example 1, the silicon-based anode material obtained in Comparative Example 2 showed decreased uniformity of nano-silicon distribution and poor continuity of the three-dimensional carbon framework. This made the lithium-ion battery more susceptible to MXene conductive bridging structure breakage and localized electrode pulverization during cycling. These results demonstrate that strong shear gelation can rapidly fix nano-silicon and MXene nanosheets in a well-dispersed state, serving as a crucial step in confining nano-silicon and reducing cycling expansion.

[0126] Compared to Example 1, Comparative Example 3 did not include the KH-570 silane coupling monomer. The system lacked a silane coupling structure capable of hydrolytic condensation or coupling with the hydroxyl groups on the surface of the nano-silicon. The nano-silicon and the three-dimensional carbon framework primarily relied on physical coating, van der Waals interactions, or weak polar interactions for bonding, making it difficult to form a stable interface anchoring structure. During the charge-discharge cycle of the lithium-ion battery, the nano-silicon in the silicon-based anode material repeatedly expands and contracts in volume. Without an interface anchoring structure, the nano-silicon is more likely to detach locally from the three-dimensional carbon framework or MXene conductive bridging structure, leading to loss of active particles, SEI film rupture, and increased electrode thickness. Compared to Example 1, the lithium-ion battery obtained in Comparative Example 3 showed a decrease in cycle capacity retention, an increase in post-cycle thickness expansion, and a greater likelihood of localized cracks or active material detachment from the anode electrode after cycling. These results demonstrate that the interface anchoring structure introduced by the KH-570 silane coupling monomer plays a crucial role in improving the bonding stability between nano-silicon and the three-dimensional carbon framework, reducing cycle expansion, and enhancing the long-cycle performance of lithium-ion batteries.

[0127] Compared to Experimental Example 1, Comparative Example 4 did not include MXene nanosheets. The resulting material lacked a two-dimensional conductive bridging network, leading to decreased conductivity in both the powder and electrode, a significant reduction in the rate performance of the battery cell, and a more pronounced increase in impedance after cycling. This result demonstrates that MXene nanosheets can work with the three-dimensional carbon framework to maintain electron transport pathways during cycling, thereby improving material conductivity. In Comparative Example 4, although the functional pre-emulsion could form a certain three-dimensional carbon framework after Joule heating, the three-dimensional carbon framework might suffer from insufficient electron transport pathways in local areas. Especially when the nano-silicon undergoes volume changes during cycling, the lack of a flexible MXene conductive bridging structure can cause some nano-silicon to lose effective connection with the overall conductive network. Furthermore, since the MXene nanosheets did not participate in the Joule heating process, the electrothermal conversion channels within the gelation precursor were reduced, and the uniformity of Joule heating decreased. This could lead to inconsistent local carbonization of the silicon-based anode material, affecting the continuity and conductivity of the final three-dimensional carbon framework. Compared to Experimental Example 1, the silicon-based anode material obtained in Comparative Example 4 showed reduced conductivity, decreased rate performance of the lithium-ion battery, and a more significant increase in impedance after cycling.

[0128] Compared to Experimental Example 1, Comparative Example 5 used conventional tube furnace carbonization instead of Joule heat treatment. Conventional tube furnace carbonization is an outside-to-inside heat transfer method, with a long heating time. Temperature gradients easily exist between the inside and outside of the material, which can easily cause unevenness in the three-dimensional carbon framework structure. It also increases the risk of migration or aggregation of nano-silicon in local areas, and partially damages or re-stacks the MXene conductive bridging structure, thus affecting its conductive bridging function. Compared to Experimental Example 1, the three-dimensional carbon framework structure uniformity of the silicon-based anode material obtained in Comparative Example 5 decreased, and the lithium-ion battery cycle capacity retention and rate performance were lower than those of Experimental Example 1, while the thickness expansion rate after cycling was higher. These results indicate that Joule heat treatment can achieve rapid bulk phase heating through internal resistance heating, which is beneficial for shortening carbonization time, maintaining the integrity of the three-dimensional carbon framework structure, and improving the continuity of the three-dimensional carbon framework conductive network.

[0129] Compared to Experimental Example 1, Comparative Example 6 uses a traditional pre-emulsion system of styrene, acrylonitrile, and divinylbenzene. Styrene provides an aromatic carbon source, acrylonitrile provides a nitrogen-containing carbon source, and divinylbenzene provides a crosslinking structure. However, this system is mainly a general-purpose polymer carbon source system, lacking silane coupling monomers designed for anchoring at the nano-silicon interface, and also lacking TAIC multifunctional crosslinking monomers. This results in decreased rigidity of the formed three-dimensional carbon skeleton, which is prone to breakage during cycling. In the silicon-based anode material obtained in Comparative Example 6, the interfacial bonding between nano-silicon and the three-dimensional carbon skeleton is weak, making it more susceptible to nano-silicon particle shedding, SEI film rupture, and electrode expansion during cycling. The lithium-ion battery obtained in Comparative Example 6 is inferior to that of Experimental Example 1 in terms of initial coulombic efficiency, cycle retention, and expansion control. The results demonstrate that Experimental Example 1 of this invention utilizes a functional pre-emulsion system composed of furfuryl alcohol, 1-vinylimidazole, TAIC multifunctional crosslinking monomer, and KH-570 silane coupling monomer. Furfuryl alcohol forms the main framework of the three-dimensional carbon skeleton of the silicon-based anode material, 1-vinylimidazole forms the nitrogen-doped structure within the three-dimensional carbon skeleton, and TAIC forms the rigid supporting portion of the main framework. These three components synergistically form a stable three-dimensional carbon skeleton, constructing a continuous conductive network and effectively mitigating the volume expansion of nano-silicon. KH-570 forms a stable interface anchoring structure between the nano-silicon and the three-dimensional carbon skeleton, preventing the nano-silicon from detaching during cycling. This is not a simple replacement of traditional carbon sources, nitrogen sources, and crosslinking agents, but rather a synergistic design addressing the interface anchoring, conductive network construction, and volume expansion buffering requirements of silicon-based anode materials.

[0130] Based on the above experimental examples and comparative examples, it can be seen that the present invention, through an integrated preparation path of "functional pre-emulsion - microchannel continuous flow mixing and dispersion - strong shear gelation - Joule thermal carbonization," can obtain silicon-based anode materials with uniform and stable structure, low impedance, good conductivity, and stable cycle performance. Applying the silicon-based anode material of the present invention to lithium-ion batteries significantly improves the energy density, cycle life, and safety of the resulting lithium-ion batteries.

[0131] The foregoing has provided a detailed description of a silicon-based anode material, its preparation method, and a lithium battery disclosed in the embodiments of the present invention. Specific examples have been used to illustrate the principles and implementation methods of the present invention. The descriptions of the above embodiments are only for the purpose of helping to understand the method and core ideas of the present invention. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention. Any modifications, equivalent substitutions, and improvements made within the principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a silicon-based negative electrode material, characterized by, Specifically, the following steps are included: A polymerizable component is obtained by mixing a carbon source monomer, a nitrogen-containing functional monomer, a multifunctional crosslinking monomer, and a silane coupling monomer. The polymerizable component is then dissolved in an emulsion medium to obtain a functional pre-emulsion. Nano-silicon was mixed with a solvent to obtain a nano-silicon dispersion, and MXene nanosheets were mixed with a solvent to obtain an MXene nanosheet dispersion. The functional preemulsion, nano-silica dispersion, MXene nanosheet dispersion, and initiator were mixed and dispersed in a microchannel continuous flow to obtain a reaction mixture. The reaction mixture undergoes gelation under shearing to obtain a gelled precursor; as well as The gelled precursor was subjected to Joule heat treatment in an inert atmosphere to obtain silicon-based anode materials.

2. The method for preparing a silicon-based anode material as described in claim 1, characterized in that, The mass ratio of carbon source monomer, nitrogen-containing functional monomer, multifunctional crosslinking monomer, and silane coupling monomer is (20-70):(5-40):(1-30):(0.5-15).

3. The method for preparing a silicon-based anode material as described in claim 1, characterized in that, The carbon source monomer includes any one or more combinations of furan-based carbon source monomers, polyphenol-based carbon source monomers, benzoxazine-based carbon source monomers, phenolic resin carbon source monomers, and polyimide carbon source monomers; the nitrogen-containing functional monomer includes any one or more combinations of 1-vinylimidazolium, 4-vinylpyridine, 2-vinylpyridine, N-vinylpyrrolidone, acrylamide, methacrylamide, N-hydroxymethylacrylamide, melamine, cyanuric acid, and triazine monomers; and / or, the multifunctional crosslinking monomer includes any one or more combinations of triallyl isocyanurate, triallyl cyanurate, bismaleimide, ethylene glycol dimethacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, and phosphazene multifunctional crosslinking agents; and the silane coupling monomer includes any one or more combinations of γ-methacryloyloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, vinyltriethoxysilane, and vinyltrimethoxysilane.

4. The method for preparing a silicon-based anode material as described in claim 1, characterized in that, The particle size of the nanosilicon is 80 nm-120 nm, and the flake size of the MXene nanosheet is 2 pm-4 pm; and / or, the MXene nanosheet comprises Ti3C2T x MXene nanosheet, Ti2CT x MXene nanosheet, Nb2CT x MXene nanosheet, V2CT x MXene nanosheet, Nb2CT x represents a surface functional group, and x represents the average number of surface functional groups.

5. The method for preparing a silicon-based anode material as described in claim 1, characterized in that, The mass ratio of nano-silicon, MXene nanosheets, and polymerizable components is (96-105):(17-28):100; and / or the initiator includes any one or more combinations of azobisisobutyronitrile, benzoyl peroxide, ammonium persulfate, and potassium persulfate.

6. The method for preparing a silicon-based anode material as described in claim 1, characterized in that, In the microchannel continuous flow mixing and dispersion, the diameter of the microchannel is 50μm-1000μm, and the mixing and dispersion time is 5s-1800s; and / or, the microchannel includes any one or more combinations of T-shaped microchannels, Y-shaped microchannels, serpentine microchannels, spiral microchannels, staggered microchannels, diversion-convergence microchannels, or impinging flow microchannels.

7. The method for preparing a silicon-based anode material as described in claim 1, characterized in that, The shear rate of the shear treatment is 1000 s -1 -20000 s -1 The temperature of the gelation is 40-90℃, the time of the shear treatment is 5-120 min; and / or, the temperature of the Joule heat treatment is 500-1200℃, the time is 1-1800 s.

8. A silicon-based anode material, characterized in that, The silicon-based anode material is prepared by the silicon-based anode material preparation method according to claim 1. The silicon-based anode material includes nano-silicon, MXene conductive bridging structure and three-dimensional carbon skeleton. The nano-silicon is dispersed in the three-dimensional carbon skeleton. The MXene conductive bridging structure is interspersed in the interior or surface of the three-dimensional carbon skeleton. The MXene conductive bridging structure forms a conductive bridge between the three-dimensional carbon skeleton and the nano-silicon. There is an interface anchoring structure between the nano-silicon and the three-dimensional carbon skeleton.

9. A silicon-based anode material as described in claim 8, characterized in that, The three-dimensional carbon skeleton has a skeleton body, a nitrogen-doped structure, and a porous structure. The nitrogen-doped structure is distributed in the skeleton body, and the parts of the three-dimensional carbon skeleton that do not contain the skeleton body form the porous structure.

10. A lithium-ion battery, characterized in that, The lithium-ion battery includes a positive electrode, an electrolyte, and a negative electrode, wherein the negative electrode of the lithium-ion battery includes a silicon-based negative electrode material as described in any one of claims 8-9.