A negative electrode current collector, a negative electrode sheet, and a battery
By setting a first grain with a length greater than 2μm in the negative electrode current collector and controlling the proportion of small-angle grain boundaries, the grain structure of the metal foil layer was optimized, the breakage problem of the negative electrode current collector during battery cycling was solved, and the structural stability and cycle life of the battery were improved.
Patent Information
- Application Number
- CN202611359845.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-17
AI Technical Summary
The negative electrode current collector is prone to breakage during battery cycling, leading to rapid capacity decay and thermal runaway. Existing technologies struggle to address its structural stability issues.
By setting a first grain with a length greater than 2μm in the metal foil layer and controlling the number of layers and the distribution of grain boundaries in the thickness direction, a small-angle grain boundary ratio of 2%~30% is formed to optimize the grain structure and the microstructure distribution in the thickness direction, thereby enhancing fatigue resistance.
It improves the structural stability of the negative electrode current collector, reduces the risk of breakage, and enhances the cycle life and safety of the negative electrode sheet and battery.
Smart Images

Figure CN123120743A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of secondary batteries, and more particularly to a negative electrode current collector, a negative electrode sheet, and a battery. Background Technology
[0002] As a new generation of high-energy-density energy storage devices, secondary batteries have been widely used in consumer electronics (such as smartphones and laptops), electric vehicles, energy storage systems (such as home energy storage and grid-level energy storage), military and aerospace equipment (such as satellite power supplies and drones), and 5G communication base stations.
[0003] As an important battery component of secondary batteries, the negative electrode current collector has a direct impact on battery performance. However, during battery cycling, the negative electrode current collector is prone to breakage under stress, leading to rapid capacity decay or even thermal runaway.
[0004] Therefore, solving the current problem of negative electrode current collector fracture and improving the structural stability of the negative electrode current collector has become a key direction for breakthroughs in secondary battery technology. Summary of the Invention
[0005] The present invention provides a negative electrode current collector with a stable structure that is not prone to breakage.
[0006] The present invention provides a negative electrode sheet, which includes the above-mentioned negative electrode current collector and has excellent structural stability.
[0007] The present invention provides a battery comprising the above-mentioned negative electrode current collector or negative electrode sheet, which has good cycle stability.
[0008] In a first aspect, the present invention provides a negative electrode current collector, comprising a metal foil layer.
[0009] The metal foil layer includes grains;
[0010] Along the length direction of the metal foil layer, the grains include a first grain with a length greater than 2 μm;
[0011] When the test thickness of the metal foil layer is T μm, the number of layers of the first grain along the thickness direction of the metal foil layer is X layers;
[0012] The following conditions must be met: the layer coefficient X / T is 0.67~6.
[0013] As described above, in the negative electrode current collector, there are grain boundaries between any two adjacent grains.
[0014] The grain boundaries include small-angle grain boundaries with an included angle of 0 to 10°;
[0015] Based on the grain boundaries, the proportion of small-angle grain boundaries is 2% to 30%;
[0016] And / or, the test thickness is 15 μm;
[0017] And / or, the number of layers X layers of the first grain is 10 to 40 layers.
[0018] As described above, in the negative electrode current collector, along the length direction of the metal foil layer, the grains further include a second grain with a length of 0.1~2.0μm;
[0019] Wherein, the cross section of the metal foil layer along the thickness direction, the thickness of the metal foil layer is T1, and within any T1×20μm region, the number of the first grains is A, the number of the second grains is B, and A / B≥10;
[0020] Preferably, T1 is 15 μm, A is 100~240, and B is 5~10.
[0021] As described above, for the negative electrode current collector, based on the sum of the texture coefficients of the (111), (200), (220), (311), and (222) crystal planes of the negative electrode current collector, the texture coefficient of the (220) crystal plane accounts for ≥85%;
[0022] And / or, the sheet resistance of the negative current collector is 1~4mΩ / □.
[0023] As described above for the negative electrode current collector, the metal foil layer is copper foil;
[0024] The copper foil includes doping elements;
[0025] The doping element includes at least one of nickel and zirconium.
[0026] The copper foil satisfies at least one of the following conditions:
[0027] (1) Based on the copper foil, the content of the doping element is 230~1300ppm;
[0028] (2) The doping elements include nickel and zirconium; based on the copper foil, the content of nickel is 200~800ppm and the content of zirconium is 30~500ppm;
[0029] (3) The doping element also includes silicon, and the content of silicon is 1~50ppm based on the copper foil;
[0030] (4) The doping elements include nickel and silicon; based on the copper foil, the content of nickel is A1 and the content of silicon is A2, and A1 / A2≥4.
[0031] The negative electrode current collector described above satisfies at least one of the following conditions:
[0032] (1) After heat treatment at 260℃ for 30 min, the elongation of the negative electrode current collector along the MD direction is C1;
[0033] The direction at 45° to the MD direction is the second direction.
[0034] Along the second direction, the elongation of the negative electrode current collector is C2, 1.5% ≤ C1 - C2 ≤ 6%;
[0035] (2) The tensile strength of the negative electrode current collector is 350~700MPa;
[0036] (3) At 25±5℃, the elongation of the negative electrode current collector along the MD direction is 1%~4%;
[0037] (4) The fatigue life of the negative electrode current collector is 20,000 to 60,000.
[0038] The negative electrode current collector as described above includes a first surface and a second surface opposite to the first surface;
[0039] The negative electrode current collector satisfies at least one of the following conditions:
[0040] (1) The roughness of the first surface is D1, the roughness of the second surface is D2, and |D1-D2|≤0.4μm;
[0041] (2) The gloss of the first surface is E1, the gloss of the second surface is E2, and |E1-E2|≤100GU;
[0042] (3) The color difference between any two points on the surface of the negative electrode current collector is ≤5.
[0043] The negative electrode current collector described above, wherein the metal foil layer is a copper foil, and the negative electrode current collector further includes a polymer layer disposed on at least one surface of the copper foil;
[0044] The polymer layer comprises at least one of benzotriazole, benzotriazole derivatives, methylbenzotriazole, sodium mercaptobenzothiazole, benzimidazole, 2-mercaptobenzimidazole, and cerium salt;
[0045] The thickness of the polymer layer is 10~300nm.
[0046] In a second aspect, the present invention provides a negative electrode sheet, comprising a negative electrode current collector as described above and a negative electrode active layer disposed on at least one side surface of the negative electrode current collector;
[0047] The negative electrode active layer comprises a silicon-based material; the surface of the silicon-based material has several recessed structures;
[0048] The silicon-based material satisfies at least one of the following conditions:
[0049] (1) The major diameter of the silicon-based material is 5~20μm;
[0050] (2) The maximum depth of the recessed structure is 0.3~8μm;
[0051] (3) The ratio of the maximum depth of the recessed structure to the length-to-diameter ratio of the silicon-based material is 0.02 to 0.6;
[0052] (4) The recessed structure includes a first surface and a second surface arranged opposite to each other, and the angle between the first surface and the second surface is 30°~160°.
[0053] Thirdly, the present invention provides a battery, comprising a negative electrode current collector as described above or a negative electrode sheet and an electrolyte as described above;
[0054] The electrolyte comprises 8% to 35% fluoroethylene carbonate by weight percentage.
[0055] The negative electrode current collector structure provided by this invention is stable and not prone to breakage. By setting a first grain with a length greater than 2 μm along the length direction in the metal foil layer, and controlling the number of the first grain layers along the thickness direction to be X layers when the metal foil layer test thickness is T μm, and satisfying the layer number coefficient X / T being 0.67~6, the grain structure and microstructure distribution in the thickness direction of the metal foil layer can be optimized, reducing the adverse effects of high grain boundary density and orientation dispersion, enhancing the fatigue resistance of the negative electrode current collector under the stress caused by the volume change of the silicon-based negative electrode during charging and discharging, and thus improving the interface stability, cycle life and safety of the negative electrode sheet and battery. Attached Figure Description
[0056] Figure 1 This is a schematic diagram of the negative electrode current collector in a specific embodiment of the present invention;
[0057] Figure 2 This is a schematic diagram of the negative electrode sheet in a specific embodiment of the present invention;
[0058] Figure 3 This is a schematic diagram of the structure of the silicon-based material used in a specific embodiment of the present invention;
[0059] Figure 4 This is a schematic diagram of the structure of the positive electrode sheet in a specific embodiment of the present invention;
[0060] Figure 5 This is a schematic diagram of the battery structure provided in a specific embodiment of the present invention.
[0061] Explanation of reference numerals in the attached figures:
[0062] A - First side; B - Second side; 01 - Copper foil; 02 - Polymer layer; 11 - Negative electrode current collector; 12 - Negative electrode active layer; 21 - Positive electrode current collector; 22 - Positive electrode active layer. Detailed Implementation
[0063] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numerals in different drawings denote the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Rather, they are merely examples of apparatuses and methods consistent with some aspects of the invention as detailed in the appended claims.
[0064] In existing technologies, electrolytic copper foil is commonly used as the negative electrode current collector. The copper foil typically contains fine columnar grains with densely distributed grain boundaries and relatively dispersed grain orientation. When this type of copper foil is combined with silicon-based negative electrode materials, it continuously withstands stress caused by the volume changes of the silicon-based material during battery charging and discharging. The overall structure is maintained primarily through the deformation coordination between grains. However, due to the small grain size and insufficient distribution of effective long grains in existing copper foils, the stress transmission path in the thickness direction is discontinuous, easily leading to stress concentration at grain boundaries. This can induce grain boundary slip, crack initiation, and propagation. Especially under conditions of significant expansion and contraction of the silicon-based negative electrode, the copper foil is more prone to fatigue fracture and other problems.
[0065] Based on this, in a first aspect, the present invention provides a negative electrode current collector, comprising a metal foil layer.
[0066] The metal foil layer includes grains;
[0067] Along the length of the metal foil layer, the grains include a first grain with a length greater than 2 μm;
[0068] When the test thickness of the metal foil layer is T μm, the number of layers of the first grain along the thickness direction of the metal foil layer is X layers;
[0069] The following conditions must be met: the layer coefficient X / T is 0.67~6.
[0070] A negative electrode current collector is a sheet-like conductive substrate used to carry active materials and conduct electronic current on the negative electrode side of a battery. A metal foil layer is a thin conductive metal layer that constitutes the main body of the negative electrode current collector. It consists of multiple grains and performs current conduction and mechanical load-bearing functions, while also serving as a supporting framework for the negative electrode active material and isolating it from the external environment.
[0071] Grains refer to the metal structural units formed inside a metal foil layer. Their extension along the length of the metal foil layer determines the continuity of the force transmission path between layers, and affects the deformation coordination ability of the foil layer through the position and orientation distribution of grain boundaries.
[0072] The first grain refers to a grain unit with a length greater than 2 μm, which has a relatively large extension dimension along the length direction of the metal foil layer and is distributed in a layered manner in the thickness direction to form the first grain layer. Preferably, the first grain forms multiple relatively continuous layers in the thickness direction of the metal foil layer. When the distribution of these layers in the thickness direction matches the overall thickness of the metal foil layer, the stress transmission is no longer limited to local grain boundaries, but is jointly borne by multiple first grain layers, thereby reducing local stress concentration at the interface.
[0073] The test thickness T of the metal foil layer can be less than or equal to the thickness of a single metal foil layer, or it can be greater than the thickness of a single metal foil layer. When the test thickness T of the metal foil layer is greater than the thickness of a single metal foil layer, multiple metal foil layers can be stacked to obtain the test thickness before testing.
[0074] The number of layers X refers to the number of first grain layers counted at the same location along the thickness direction within the thickness range corresponding to the test thickness T of the metal foil layer. It reflects the layered distribution density of the first grains within the metal foil layer. The number of layers X can be determined based on metallographic cross-sectional observation, microstructure analysis, or image recognition statistics. In one possible embodiment, after sampling the cross-section of the metal foil layer, an arbitrary location is selected to identify and count the first grains with a length greater than 2 μm along the thickness direction layer by layer, and the average value is taken from 5 locations. In another possible embodiment, the statistics can also be achieved through image recognition.
[0075] The layer number factor X / T refers to the ratio between the number of first grain layers X and the test thickness T of the metal foil layer. The layer number factor X / T ranges from 0.67 to 6.
[0076] It should be noted that the layer number coefficient is calculated using only numerical values, without units. For example, if the test thickness is 8μm and the number of layers is 20, the layer number coefficient X / T is 20 / 8 = 2.5.
[0077] In detail, the layer coefficient includes, but is not limited to, a range of 0.67, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, or any two of these.
[0078] The negative electrode current collector provided in this application, during operation, has a metal foil layer that acts as a conductive framework for the negative electrode sheet, closely bonded to the negative electrode coating. Electron current is continuously conducted along the metal foil layer, while the volume change generated by the active material during charging and discharging is transmitted to the interior of the metal foil layer through the negative electrode coating. Because the metal foil layer contains first grains with a length greater than 2 μm, when the layer number factor is less than 0.67, it indicates that the first grains of the same thickness are too large, or the number of first grains is too low. According to the classical material theory of grain refinement strengthening, this will lead to lower current collector strength and easy breakage during cycling. Conversely, when the layer number factor is greater than 6, it means that there are too many first grain layers of the same thickness, i.e., a greater number of first grains. This results in more grain boundaries, making the negative electrode current collector prone to breakage along the grain boundaries under stress. When X / T is between 0.67 and 6, the metal foil layer forms interwoven and misaligned layered load-bearing units distributed along the thickness direction. This changes the stress transmission path from being dominated by a single grain boundary to being supported by multiple layers of first grains, thereby giving the negative electrode current collector excellent structural stability and making it less prone to breakage.
[0079] In some embodiments, the layer number coefficient is preferably 0.67 to 2.66.
[0080] In detail, the layer coefficient is preferably a range of 0.67, 0.80, 1.00, 1.20, 1.40, 1.60, 1.80, 2.00, 2.20, 2.40, 2.60, 2.66 or any two of these.
[0081] When the layer number coefficient is 0.67~2.66, the layered load-bearing unit of the metal foil layer can better achieve the stress mitigation effect and further improve the structural stability of the negative electrode current collector.
[0082] In some embodiments of the present invention, grain boundaries exist between any adjacent grains, and grain boundaries include small-angle grain boundaries with an included angle of 0 to 10°.
[0083] Based on grain boundaries, small-angle grain boundaries account for 2% to 30% of the total.
[0084] Small-angle grain boundaries and their proportion can be detected and distinguished using methods commonly used in the field, such as electron backscatter diffraction (EBSD) combined with orientation difference statistical analysis.
[0085] In some embodiments, the method for detecting the proportion of small-angle grain boundaries includes the following steps:
[0086] First, the sample surface undergoes rigorous argon ion polishing. Then, data is acquired using a scanning electron microscope equipped with an EBSD system to obtain crystallographic orientation information of the grains. Next, using professional analysis software, the orientation difference between adjacent grains is precisely measured, and interfaces with orientation differences in the range of 0~10° are automatically identified and marked as small-angle grain boundaries. Finally, the statistical analysis function of the software is used to directly calculate the proportion of small-angle grain boundaries in the total number of grain boundaries.
[0087] In detail, based on all grain boundaries, the percentage of small-angle grain boundaries includes, but is not limited to, 2%, 5%, 10%, 15%, 20%, 25%, 30%, or any combination thereof.
[0088] When the proportion of small-angle grain boundaries is in the range of 2% to 30%, the metal foil layer can achieve a better balance between grain boundary slip, dislocation transmission and stress redistribution, thereby improving the fatigue resistance and structural stability of the negative electrode current collector under the repeated expansion and contraction conditions of silicon-based negative electrode charging and discharging.
[0089] In some embodiments, the test thickness is 15 μm.
[0090] When the test thickness is 15μm, the microstructure observed along the thickness direction of the metal foil layer can more stably reflect the grain distribution characteristics under its actual service thickness, thus facilitating quantitative control of the number of the first grain layer.
[0091] In some embodiments, the test thickness is 15 μm, and the number of layers X layers of the first grain is 10 to 40 layers.
[0092] In detail, the number of layers of the first grain includes, but is not limited to, 10, 15, 20, 25, 30, 35, 40 layers or any combination thereof.
[0093] When the test thickness is 15μm, the number of layers X layers of the first grain is preferably 10 to 40 layers, so as to form a sufficiently continuous first grain bearing path in the thickness direction, while avoiding excessive grain coarsening that would lead to local unevenness of the structure.
[0094] In some embodiments, along the length direction of the metal foil layer, the grains further include a second grain with a length of 0.1~2.0 μm;
[0095] Wherein, the cross section of the metal foil layer along the thickness direction, the thickness of the metal foil layer is T1, and within any T1×20μm region, the number of the first grains is A, the number of the second grains is B, and A / B≥10;
[0096] Preferably, T1 is 15 μm, A is 100~240, and B is 5~10.
[0097] In this application, the second grain refers to a smaller grain with a length of 0.1 to 2.0 μm measured along the length of the metal foil layer. The second grain is usually distributed in the interstices of the first grain, at the grain junctions, or in the local recrystallization region, and forms a discrete and dispersed group of fine grains in the cross-sectional statistics along the thickness direction.
[0098] In one possible embodiment, the second grain may be in a near-equiaxed, short columnar, or irregular polygonal shape, and its material may be pure copper grain, copper grain whose growth has been suppressed by trace alloying elements, or fine recrystallized copper grain formed by rapid annealing.
[0099] Because the second grain is smaller, it is more suitable for providing deformation coordination and grain boundary pinning in local areas, and together with the first grain, it forms a composite grain system with both load-bearing and buffering capabilities.
[0100] When a section is cut along the thickness direction of the metal foil layer, the number of grains in any T1×20μm region is counted. The number of the first grains is denoted as A, and the number of the second grains is denoted as B. A / B≥10 means that the larger first grains dominate in the statistical region, thus ensuring that the load transfer in the thickness direction is mainly carried out along the continuous first grain path, while the second grains are embedded in a smaller number of them to refine the local structure without excessively increasing the grain boundary density.
[0101] Preferably, when the cross-section is taken along the thickness direction of the metal foil layer, the number of grains is counted in any 15×20μm region, where A is 100~240 and B is 5~10.
[0102] In detail, A includes, but is not limited to, a range of 100, 120, 140, 160, 180, 200, 220, 240 or any two of these; B includes, but is not limited to, a range of 5, 6, 7, 8, 9, 10 or any two of these.
[0103] At this ratio, the metal foil layer can maintain sufficient first grain continuity while retaining a small number of second grains to regulate grain boundary morphology and dislocation movement.
[0104] In some embodiments, based on the sum of the texture coefficients of the (111) crystal plane, (200) crystal plane, (220) crystal plane, (311) crystal plane, and (222) crystal plane of the negative electrode current collector, the texture coefficient of the (220) crystal plane accounts for ≥85%.
[0105] A Rigaku-type X-ray diffractometer can be used to characterize the phase and analyze the crystal planes of the copper foil current collector, thereby obtaining the proportion of the texture coefficient of the (220) crystal plane. The test method includes: disassembling the battery, removing the active layer on the negative electrode to expose the metal foil layer, cleaning the surface of the copper foil current collector with 10 vol.% dilute sulfuric acid and anhydrous ethanol solution in sequence, drying it with cold air, and then testing it; the test conditions include: using a copper Kα target (λ=0.15406 nm), the working voltage is 40 kV, the scanning angle range is 0~100°, the scanning rate is 0.02° / s, determining the (220) crystal plane in the obtained XRD spectrum, and using the integral intensity of the (220) peak as the basis to the sum of the texture coefficients of the (111) crystal plane, (200) crystal plane, (220) crystal plane, (311) crystal plane, and (222) crystal plane of the detected negative electrode current collector, calculating the proportion of the texture coefficient of the (220) crystal plane.
[0106] In detail, the texture factor of the (220) crystal plane is included, but is not limited to, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95% or any range ≥85%.
[0107] When the proportion of the texture coefficient of the (220) crystal plane in the negative electrode current collector is within the above range, the slip inside the grain and the stress release path near the grain boundary are more consistent. The periodic stress caused by external load and volume expansion of active material can be diffused more evenly in the metal foil layer and gradually dissipated, and it is not easy to form excessively high stress peaks in local areas.
[0108] In some embodiments, the sheet resistance of the negative current collector is 1~4mΩ / □.
[0109] In this invention, the sheet resistance of the negative electrode current collector is detected by a method comprising the following steps:
[0110] Sample preparation: Clean the foil surface to remove surface oil or other contaminants, ensuring good probe contact. Lay the sample flat on the insulating substrate, avoiding bending. Using a four-probe tester, arrange the probes at equal intervals (s) on the sample surface. Apply a constant current (I) to the two outer probes and measure the voltage drop (V) on the two inner probes. Input the sample thickness information and calculate the sheet resistance.
[0111] In detail, the sheet resistance of the negative current collector includes, but is not limited to, a range of 1Ω / □, 1.5Ω / □, 2Ω / □, 2.5Ω / □, 3Ω / □, 3.5Ω / □, 4Ω / □, or any two of these.
[0112] A metal foil layer with a sheet resistance of 1~4mΩ / □ can quickly and evenly conduct in-plane current to all parts of the electrode, thereby reducing local current density differences and better balancing battery performance such as temperature rise and rate performance.
[0113] In some current collectors, the metal foil layer is copper foil;
[0114] Copper foil includes doped elements;
[0115] The doping element includes at least one of nickel and zirconium.
[0116] In one possible embodiment, the copper foil can be prepared by electrolytic deposition followed by annealing, continuous casting followed by cold rolling and annealing, or a combination of direct rolling and heat treatment. Nickel, zirconium, and silicon can be introduced in the electrolyte, melt alloying, or subsequent surface diffusion treatment to meet the corresponding content ranges.
[0117] In some embodiments, based on copper foil, the content of doping elements is 230~1300ppm.
[0118] The content of doped elements can be detected using methods commonly used in the field, such as inductively coupled plasma optical emission spectrometry (ICP-OES).
[0119] In detail, based on copper foil, the content of doping elements includes, but is not limited to, a range of 230 ppm, 300 ppm, 400 ppm, 500 ppm, 600 ppm, 700 ppm, 800 ppm, 900 ppm, 1000 ppm, 1100 ppm, 1200 ppm, 1300 ppm, or any two of these.
[0120] The total content of doped elements in the copper foil is controlled between 230 and 1300 ppm to improve grain stability while ensuring high conductivity of the copper foil.
[0121] In some embodiments, the doping elements include nickel and zirconium; based on the copper foil, the nickel content is 200ppm to 800ppm and the zirconium content is 30ppm to 500ppm.
[0122] The content of nickel and zirconium can be determined using the methods described above.
[0123] Specifically, based on the copper foil, the nickel content includes, but is not limited to, a range of 200 ppm, 300 ppm, 400 ppm, 500 ppm, 600 ppm, 700 ppm, 800 ppm, or any two of these; the zirconium content includes, but is not limited to, a range of 30 ppm, 50 ppm, 100 ppm, 150 ppm, 200 ppm, 250 ppm, 300 ppm, 350 ppm, 400 ppm, 450 ppm, 500 ppm, or any two of these.
[0124] When copper foil contains both nickel and zirconium, and the mass percentages of nickel and zirconium are within the aforementioned range, the corrosion resistance and high-temperature resistance of the copper foil can be improved.
[0125] In some embodiments, the doping element also includes silicon, and the silicon content is 1 to 50 ppm based on the copper foil.
[0126] Specifically, based on the copper foil, the silicon content includes, but is not limited to, a range of 1 ppm, 10 ppm, 20 ppm, 30 ppm, 40 ppm, 50 ppm, or any two of these.
[0127] Silicon in copper foil may be introduced through methods such as adding it to the melt in the form of a Ni-Si intermediate alloy during the smelting process.
[0128] During the cycle, the silicon element in the copper foil will be lithium intercalated, repeatedly broken and formed into a film, which will damage the physical properties of the copper foil. Controlling the silicon element in the copper foil within the aforementioned low level range can further improve the structural stability of the negative electrode current collector.
[0129] In some embodiments, the doping elements include nickel and silicon; based on the copper foil, the nickel content is A1, the silicon content is A2, and A1 / A2≥4.
[0130] In detail, A1 / A2 includes, but is not limited to, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8 or any range ≥ 4.
[0131] When the mass ratio of Ni to Si is precisely controlled at 4:1, almost all Ni and Si atoms will participate in the reaction to form Ni2Si. There is not much residual Si in the copper matrix, so lithium will not be intercalated, which is beneficial to the stability of copper foil properties. A slightly higher Ni content can improve the corrosion resistance and high temperature resistance of copper foil.
[0132] In some embodiments, after heat treatment at 260°C for 30 min, the elongation of the negative electrode current collector along the MD direction is C1; the direction at 45° to the MD direction is the second direction, and the elongation of the negative electrode current collector along the second direction is C2, where 1.5%≤C1-C2≤6%.
[0133] The elongation of the negative electrode current collector in different directions was detected by a method including the following steps:
[0134] Using a special cutting knife, cut the sample into strips 15mm±0.1mm wide and 150±10mm long along the MD direction and at a 45° angle to the MD direction. Heat-treat the sample at 260℃ for 30min. Use a universal testing machine to tensile test the elongation rate. The gauge length is 50mm and the speed is 50mm / min. Statistical analysis of the test results yields the C1 and C2 values of the negative electrode current collector.
[0135] In detail, C1-C2 includes, but is not limited to, a range of 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, or any two of these.
[0136] When C1-C2 is in the range of 1.5% to 6%, it indicates that the elongation of the negative electrode current collector has high consistency in different directions, making it less prone to breakage.
[0137] In some embodiments, the tensile strength of the negative electrode current collector is 350~700 MPa.
[0138] The tensile strength of the negative electrode current collector was tested in accordance with SJ / T 11483-2014 "Electrolytic Copper Foil for Lithium-ion Batteries".
[0139] In detail, the tensile strength of the negative electrode current collector includes, but is not limited to, a range of 350 MPa, 400 MPa, 450 MPa, 500 MPa, 550 MPa, 600 MPa, 650 MPa, 700 MPa, or any combination thereof.
[0140] When the tensile strength of the negative electrode current collector is within the above range, it can effectively suppress the mechanical deformation and material shedding caused by the drastic volume expansion and contraction of the high silicon negative electrode or lithium metal negative electrode during charge and discharge cycles, thus significantly enhancing the battery's durability and cycle life.
[0141] In some embodiments, at 25±5°C, the elongation of the negative electrode current collector along the MD direction is 1%~4%.
[0142] In detail, the elongation of the negative electrode current collector includes, but is not limited to, a range of 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, or any two of these.
[0143] This moderate elongation can effectively buffer the mechanical stress in manufacturing processes such as coating and rolling, and can perfectly adapt to the volume expansion and contraction of high silicon-based or lithium metal anodes during charging and discharging, preventing electrode cracking, active material shedding or interface peeling caused by excessive stress concentration.
[0144] In some embodiments, the fatigue life of the negative electrode current collector is 20,000 to 60,000.
[0145] The fatigue life of the negative electrode current collector can be tested using methods commonly used in this field:
[0146] The negative electrode current collector was cut into 15mm*100mm strips, folded in half, and then rolled horizontally once with a 2kg stainless steel roller. The fatigue life cycle was then tested using a fatigue life cycle testing device. The fatigue life cycle testing conditions and methods were as follows: strain-life mode was used, with a test frequency of 5Hz, a strain of 0.1~0.8%, and a test temperature of 20℃~25℃. The fatigue life cycle was recorded until the negative electrode current collector strip experienced fatigue fracture.
[0147] In detail, the fatigue life of the negative electrode current collector includes, but is not limited to, a range of 20,000, 25,000, 30,000, 35,000, 40,000, 45,000, 50,000, 55,000, 60,000, or any combination thereof.
[0148] The negative electrode current collector has a high fatigue life of 20,000 to 60,000 cycles, which means that it can withstand repeated mechanical stress and volume deformation during long-term charge and discharge cycles of the battery, effectively avoiding the initiation and propagation of microcracks inside the material, and further preventing fracture.
[0149] In some embodiments, the negative current collector includes a first surface and a second surface opposite to the first surface.
[0150] Specifically, the first surface and the second surface are two working surfaces of the negative electrode current collector metal foil layer that face away from each other.
[0151] In some embodiments, the roughness of the first surface is D1, the roughness of the second surface is D2, and |D1-D2|≤0.4μm.
[0152] The roughness of the first and second surfaces can be tested using a three-dimensional optical profilometer or a contact profilometer, and then |D1-D2| can be calculated.
[0153] In detail, |D1-D2| includes, but is not limited to, a range of 0.4μm, 0.35μm, 0.3μm, 0.25μm, 0.2μm, 0.15μm, 0.1μm, 0.05μm, 0μm, or any two of these.
[0154] In some embodiments, the gloss of the first surface is E1, the gloss of the second surface is E2, and |E1-E2|≤100GU.
[0155] The gloss of the first and second surfaces can be tested using a multi-angle gloss meter, and then |E1-E2| can be calculated.
[0156] In detail, |E1-E2| includes, but is not limited to, a range consisting of 0 GU, 10 GU, 20 GU, 30 GU, 40 GU, 50 GU, 60 GU, 70 GU, 80 GU, 90 GU, 100 GU, or any two of these.
[0157] In some embodiments, the color difference between any two points on the surface of the negative electrode current collector is ≤5.
[0158] The color difference between any two points on the negative electrode current collector can be measured and calculated using a colorimeter. These two points can be on the same surface or on the first and second surfaces, respectively.
[0159] In detail, the color difference between any two points on the surface of the negative electrode current collector includes, but is not limited to, a range consisting of 5, 4, 3, 2, 1, 0, or any two of these.
[0160] When the roughness difference, gloss difference, and color difference are controlled within the above range, it usually means that the surface conditions on both sides of the negative electrode current collector are more balanced, which can achieve more consistent coating adhesion, interface wetting, and mechanical bonding effects when combined with silicon-based negative electrode materials in the future, and reduce the risk of local stress concentration, uneven coating thickness, and interface peeling caused by uneven surface conditions on both sides.
[0161] In some embodiments, such as Figure 1 As shown, the metal foil layer is copper foil 01, and the negative electrode current collector also includes a polymer layer 02 disposed on at least one side surface of the copper foil 01;
[0162] The polymer layer includes at least one of benzotriazole, benzotriazole derivatives, methylbenzotriazole, sodium mercaptobenzothiazole, benzimidazole, 2-mercaptobenzimidazole, and cerium salt;
[0163] The thickness of the polymer layer is 10~300nm.
[0164] The polymer layer is mainly used to passivate the chemical activity of the copper foil surface and to build a stable interface transition region between the negative electrode current collector and the silicon-based negative electrode active layer, thereby reducing the corrosion risk of the copper foil in the electrolyte environment and the degree of interface degradation under cyclic loading.
[0165] The polymer layer is usually disposed on at least one of the first and second surfaces of the copper foil, or it can be disposed on both surfaces simultaneously as required by the electrode structure. It can be attached to the copper foil surface by dip coating, roll coating, spray coating, chemical conversion, coupling deposition or other methods suitable for thin film formation, and forms a continuous cover layer after drying and curing.
[0166] The polymer layer includes at least one of benzotriazole, benzotriazole derivatives, methylbenzotriazole, sodium mercaptobenzothiazole, benzimidazole, 2-mercaptobenzimidazole, and cerium salt. These components can be used alone or compounded as needed to obtain a thin-layer structure that balances interfacial stability and film continuity. The polymer layer components described above can form strong coordination bonds with copper atoms, thereby forming a dense protective layer on the surface, effectively preventing the electrolyte from corroding the copper foil; furthermore, these polymer components are free of toxic heavy metals and are environmentally friendly.
[0167] The thickness of the polymer layer can be detected using methods commonly used in the field, such as using an ellipsometer to test the negative electrode current collector.
[0168] In detail, the thickness of the polymer layer includes, but is not limited to, a range of 10 nm, 20 nm, 40 nm, 60 nm, 80 nm, 100 nm, 120 nm, 140 nm, 160 nm, 180 nm, 200 nm, 220 nm, 240 nm, 260 nm, 280 nm, 300 nm, or any combination thereof.
[0169] When the thickness of the polymer layer is controlled within the range of 10~300nm, surface protection can be achieved without significantly increasing the thickness and internal resistance of the negative electrode current collector, while avoiding the obstruction of charge transport due to excessive coating thickness.
[0170] In some embodiments of the present invention, the negative electrode current collector is prepared by a method including the following steps:
[0171] Step 1: Smelting and Casting: Using high-purity cathode copper as raw material, silicon, nickel, zirconium, and tin elements are added to the molten copper during the smelting process. After smelting, the Ni content in the solution is controlled to be 200ppm–800ppm, the Si content to be 1ppm–50ppm, and the Ni / Si mass ratio to be controlled at 4.0–4.2:1. The resulting copper alloy liquid is then used for horizontal continuous casting or semi-continuous casting to produce copper billets.
[0172] Step 2: Hot Rolling and Milling: The copper billet is heated to 750–900℃ and hot rolled with a total reduction of not less than 85% to obtain hot-rolled copper strip. The hot-rolled copper strip is then milled on both sides to remove the surface oxide layer.
[0173] Step 3: Multi-pass cold rolling and differential speed rolling: The milled copper strip is subjected to multi-pass cold rolling, with a total cold rolling reduction of not less than 97%. In the cold rolling passes where the cumulative reduction reaches 30% to 70%, differential speed rolling is implemented with an upper and lower work roll linear speed ratio of 1.05 to 1.30, and the single-pass reduction is controlled at 30% to 60%.
[0174] Step 4: Segmented Annealing: During the cold rolling process, after the cumulative reduction reaches 40%–60%, segmented annealing is implemented. The segmented annealing regime is as follows: First segment: 200–350℃, holding for 1–3 hours; Second segment: 350–500℃, holding for 0.5–2 hours. The recrystallization volume fraction of the copper strip after annealing is controlled to be no higher than 30%, and the Vickers hardness decrease ΔHV is 10–35 HV.
[0175] Step 5: Finish rolling: The annealed copper strip is further cold rolled until the thickness reaches 4-15 μm to obtain rolled copper foil.
[0176] Step Six: Finished Product Annealing and Surface Treatment: The precision-rolled copper foil is annealed at 150–250℃ for 2–10 hours, followed by BTA passivation surface treatment to obtain a metal foil layer. A polymer layer is then coated onto the surface of the metal foil layer to obtain the negative electrode current collector.
[0177] Secondly, such as Figure 2 As shown, the present invention provides a negative electrode sheet, including a negative electrode current collector 11 as described above and a negative electrode active layer 12 disposed on at least one side surface of the negative electrode current collector 11;
[0178] The negative electrode active layer consists of silicon-based materials; the surface of the silicon-based materials has several recessed structures.
[0179] The negative electrode active layer uses a silicon-based material with a recessed structure on its surface, which can form a stress buffer and deformation release space on the particle surface, thereby more effectively absorbing the local stress generated by the volume expansion of the silicon-based material during charging and discharging.
[0180] In this invention, the parameters of the silicon-based material can be tested using high-resolution scanning electron microscopy combined with image analysis.
[0181] In some embodiments, the major axis of the silicon-based material is 5~20 μm.
[0182] In detail, the major diameter of silicon-based materials includes, but is not limited to, a range of 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, or any combination thereof.
[0183] By controlling the length and diameter of the silicon-based material within the range of 5~20μm, the specific surface area of the material is significantly reduced, effectively reducing the contact area with the electrolyte. This greatly suppresses the occurrence of side reactions and the excessive growth of the solid electrolyte interface film, improves the first coulombic efficiency, and reduces the consumption of active lithium.
[0184] In some embodiments, the maximum depth of the recessed structure is 0.3~8μm.
[0185] The maximum depth of the recessed structure includes, but is not limited to, a range of 0.3 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, or any combination thereof.
[0186] When the maximum depth of the recessed structure is too small (<0.3 μm), the liquid storage capacity is weak and the expansion is large; while when the maximum depth of the recessed structure is too large (>8 μm), the particle strength decreases and the particles are prone to breakage during the rolling process. When the maximum depth of the recessed structure is within the above range, it can effectively release internal mechanical stress, thereby significantly alleviating the problems of particle pulverization and electrode cracking, and significantly improving the cycle life of the battery.
[0187] In some embodiments, the ratio of the maximum depth of the recessed structure to the length-to-diameter ratio of the silicon-based material is 0.02 to 0.6.
[0188] The aspect ratio of the maximum depth of the recessed structure to the length-to-diameter ratio of the silicon-based material includes, but is not limited to, a range of 0.02, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, or any two of these.
[0189] The maximum depth of the recessed structure, with an aspect ratio to the silicon-based material ranging from 0.02 to 0.6, ensures both electrolyte retention and acceptable material structural stability. This helps to further reduce or even avoid damage to the protective layer on the copper foil surface caused by silicon particle expansion during rolling or during battery cycling, thereby improving the corrosion resistance of the copper foil and enhancing the cycle life and safety of the battery.
[0190] In some embodiments, such as Figure 3 As shown, the recessed structure includes a first surface A and a second surface B arranged opposite to each other, with the angle between the first surface A and the second surface B being 30° to 160°.
[0191] In detail, the angle between the first and second faces includes, but is not limited to, 30°, 40°, 50°, 60°, 70°, 80°, 90°, 100°, 110°, 120°, 130°, 140°, 150°, 160°, or any combination thereof.
[0192] The angle between the first and second surfaces is controlled between 30° and 160°, which helps to adjust the stress transmission path and reduce stress concentration at sharp parts. Therefore, it can reduce particle breakage, active layer pulverization and interface peeling.
[0193] Thirdly, the present invention provides a battery, comprising a negative electrode current collector as described above or a negative electrode sheet and an electrolyte as described above;
[0194] The electrolyte contains 8% to 35% fluoroethylene carbonate by weight percentage.
[0195] In detail, the mass percentage of fluoroethylene carbonate includes, but is not limited to, 8%, 10%, 15%, 20%, 25%, 30%, 35%, or any combination thereof.
[0196] By adding 8% to 35% fluoroethylene carbonate to the electrolyte, it can preferentially participate in film formation on the surface of the negative electrode, forming a dense and stable interface film, thereby reducing the continuous side reactions of the electrolyte on the surface of the silicon-based negative electrode.
[0197] In some embodiments, the electrolyte also includes common lithium salts. Appropriate lithium salts can be selected according to actual conditions, such as lithium hexafluorophosphate (LiPF6), lithium bisfluorosulfonylimide (LiFSI), lithium bistrifluoromethanesulfonylimide (LiTFSI), lithium perchlorate (LiClO4), lithium oxalate borate (LiBOB), lithium difluorooxalate borate (LiDFOB), lithium tetrafluoroborate (LiBF4), etc. Based on the electrolyte, the mass percentage of lithium salts is 10% to 30%.
[0198] The electrolyte may also include conventional linear carbonates, linear carboxylic acid esters, and other solvents, including but not limited to diethyl carbonate, dimethyl carbonate, methyl ethyl carbonate, propyl propionate, ethyl propionate, ethyl butyrate, 1,3-propanesulfonyl lactone, 1,4-butanesulfonyl lactone, ethyl acetate, 1,3-propanesulfonyl lactone, and propenyl-1,3-sulfonyl lactone. Based on the electrolyte, the mass percentage of the solvent is 10% to 80%.
[0199] In some embodiments, the electrolyte may also include boron-containing positive electrode protective additives, including but not limited to lithium difluorooxalate borate (LiDFOB), lithium bis(oxalate borate) (LiBOB), lithium tetrafluoroborate (LiBF4), etc.
[0200] Understandably, batteries also include a separator.
[0201] In some embodiments, the diaphragm includes a diaphragm base layer and a ceramic coating disposed on at least one side surface of the diaphragm base layer.
[0202] The ceramic coating includes inorganic particles and binders. The inorganic particles are selected from one or more of boehmite (γ-AlOOH), alumina (Al2O3), barium sulfate (BaSO4), magnesium oxide (MgO), magnesium hydroxide (Mg(OH)2), silicon dioxide (SiO2), tin oxide (SnO2), titanium oxide (TiO2), calcium oxide (CaO), zinc oxide (ZnO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), nickel oxide (NiO), cerium dioxide (CeO2), zirconium titanate (SrTiO3), barium titanate (BaTiO3), and magnesium fluoride (MgF2). The binder is selected from one or more of polyvinylidene fluoride, a copolymer of polyvinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, acrylate polymers, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polytetrafluoroethylene, or polyhexafluoropropylene.
[0203] The diaphragm may also include an adhesive layer located on the surface of the ceramic layer and / or the diaphragm base layer. The adhesive layer contains a polymer, which may be particulate or non-particulate. When it is a particulate polymer, it may be a mixture of polymers with the same particle size or polymers with different particle sizes, including one or more of acrylic acid, methacrylic acid, methyl acrylate, methyl methacrylate, ethyl acrylate, butyl acrylate, ethylhexyl acrylate, styrene, α-methylstyrene, vinyltoluene, ethylene, vinyl acetate, acrylonitrile, polytetrafluoroethylene, polyvinylidene fluoride, copolymers of vinylidene fluoride and hexafluoropropylene, polyimide, polyetherimide, and polyamideimide.
[0204] The battery also includes a positive electrode, such as in some embodiments. Figure 4 As shown, the positive electrode sheet includes a positive current collector 21 and a positive active layer 22 disposed on at least one side surface of the positive current collector 21. The positive active layer is not particularly limited and can include components such as a positive active material, a conductive agent, and a binder, according to conventional compositions in the art. The positive active material, conductive agent, and binder can all be conventional materials in the art. For example, the positive active material can be selected from one or more of lithium nickel oxide, lithium titanate, lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, and lithium manganese oxide; the conductive agent can be selected from one or more of conductive carbon black, carbon nanotubes, conductive graphite, and graphene; and the binder can be selected from one or more of polyvinylidene fluoride (PVDF), acrylic-modified PVDF, polyacrylate polymers, polyimide, styrene-butadiene rubber, and styrene-acrylic rubber.
[0205] In some embodiments, such as Figure 5 As shown, the battery is a wound battery.
[0206] The negative electrode current collector provided by the present invention will be described in detail below through specific embodiments.
[0207] Example 1
[0208] The battery preparation method provided in this embodiment includes the following steps:
[0209] 1. Preparation of positive electrode sheet
[0210] Lithium cobalt oxide, polyvinylidene fluoride (PVDF 500, Arkema) binder, and conductive material (acetylene black (Super P) and carbon nanotubes in a 2:1 mass ratio) were mixed in N-methylpyrrolidone (NMP) solvent at a weight ratio of 98:1:1. The mixture was continuously stirred under the action of a stirrer to form a homogeneous and fluid positive electrode slurry. Subsequently, the positive electrode slurry was coated onto an 8 μm thick aluminum foil and dried in a vacuum oven at 110 °C for 6 hours. After rolling and slitting, a surface density of 18 mg / cm³ was obtained. 2 The positive electrode plate.
[0211] 2. Preparation of negative electrode sheet
[0212] Preparation of negative electrode current collector:
[0213] Step 1: Smelting and Casting: Using high-purity cathode copper as raw material, silicon, nickel, and zirconium are added to the molten copper during the smelting process. After smelting, the Ni content in the solution is controlled to be 345 ppm, the Si content to be 22 ppm, and the Ni / Si mass ratio to be controlled at 15.68. The molten copper alloy obtained from smelting is then used to produce copper billets through horizontal continuous casting or semi-continuous casting.
[0214] Step 2: Hot Rolling and Milling: The copper billet is heated to 820℃ for hot rolling, with a total reduction rate of not less than 85%, to obtain hot-rolled copper strip. The hot-rolled copper strip is then milled on both sides to remove the surface oxide layer.
[0215] Step 3: Multi-pass cold rolling and differential speed rolling: The milled copper strip is subjected to multi-pass cold rolling, with a total cold rolling reduction rate of not less than 97%. In the cold rolling passes where the cumulative reduction rate reaches 65%, differential speed rolling is implemented with an upper and lower work roll linear speed ratio of 1.15, and the single-pass reduction rate is controlled at 45%.
[0216] Step 4: Segmented Annealing: During the cold rolling process, after the cumulative reduction reaches 65%, segmented annealing is implemented. The segmented annealing regime is as follows: First segment: 320℃ for 2.5 hours; Second segment: 460℃ for 1.2 hours. The recrystallization volume fraction of the copper strip after annealing is controlled to be no higher than 30%, and the Vickers hardness decrease ΔHV is 22HV.
[0217] Step 5: Finish rolling: The annealed copper strip is further cold rolled until the thickness reaches 8μm to obtain rolled copper foil.
[0218] Step 6: Finished product annealing and surface treatment: The finely rolled copper foil is annealed at 210℃ for 6 hours, followed by BTA passivation surface treatment.
[0219] When the cross-sectional thickness of the negative electrode current collector is 15 μm, the number of first grains with a length greater than 2 μm is 18, and the proportion of small-angle grain boundaries with an included angle of 0~10° is 8%. In a 15 μm × 20 μm region, the number A of first grains with a length exceeding 2 μm in the MD direction of the copper foil is 120, and the number B of second grains with a length between 0.1-2 μm is 8, with an A / B ratio of 15. Before and after treatment at 260℃ for 30 min, the elongation of the negative electrode current collector along the MD direction is C1; and compared with M... The direction at 45° from direction D is the second direction. Along the second direction, the elongation of the negative electrode current collector is C2, and C1-C2 is 4.5%; the texture coefficient of the (220) crystal plane of the grain accounts for 94%; the sheet resistance range of the negative electrode current collector is 2.1mΩ / □; the copper foil includes silicon, nickel, and zirconium, of which silicon is 22ppm, nickel is 345ppm, and zirconium is 200ppm; the tensile strength is 510, and the elongation is 2.1; the absolute value of the roughness difference between the first surface and the second surface is 0.34um, the gloss difference is 65GU, and the color difference is 1.3. The fatigue life of the negative electrode current collector is 31,000.
[0220] A polymer layer, comprising benzotriazole (BTA), is disposed on one side of the copper foil, and the polymer layer has a thickness of 25 nm.
[0221] The silicon-based material is a silicon-based material with a surface including a recessed structure. The major axis of the spherical silicon-based material is 12 μm; the maximum depth of the recessed structure is 4 μm; the ratio of the maximum depth of the recessed structure to the major axis of the silicon-based material is 0.34; and the angle α between the first surface and the second surface is 88°.
[0222] The aforementioned silicon-based material, graphite, styrene-diene rubber (SBR), sodium carboxymethyl cellulose, and conductive carbon black were mixed in a weight ratio of 34%:60%:3%:2%:1%. The mixture was dispersed in water and then subjected to a double planetary mixing process to obtain a negative electrode slurry. This slurry was coated onto a copper current collector, followed by rolling and drying to obtain an areal density of 5.85 mg / cm³. 2 The negative electrode plate.
[0223] 3. Selection of diaphragm
[0224] The standard ceramic diaphragm used in the industry consists of a 6μm thick polyethylene base membrane, a 2μm thick ceramic layer (mainly composed of boehmite) on one side of the base membrane, and an oil-based adhesive layer (1.5μm thick on each side, mainly composed of polyvinylidene fluoride:boehmite particles (mass ratio) = 4:6) on the ceramic layer surface and the other side of the base membrane.
[0225] 4. Preparation of electrolyte
[0226] The electrolyte is prepared by mixing ethylene carbonate (EC): ethyl propionate (EP): propyl propionate (PP): propylene carbonate (PC) in a volume ratio of 1:1:1:1. Then, 25% of the total electrolyte mass of fluoroethylene carbonate (FEC), 15% of the total electrolyte mass of lithium hexafluorophosphate, and 2% of the total electrolyte mass of adiponitrile (ADN) are added.
[0227] 5. Preparation of lithium-ion batteries
[0228] The positive electrode sheet, separator, and negative electrode sheet are stacked sequentially after fabrication and then wound to obtain a bare cell. The bare cell is placed in an aluminum-plastic film shell, and electrolyte is injected into the bare cell. After vacuum sealing, standing, formation (0.1C constant current charging to 4% SOC, then 0.2C constant current charging to 10% SOC), shaping, and capacity testing, a lithium-ion battery is obtained.
[0229] The battery preparation methods provided in Examples 2-20 and Comparative Examples 1-3 are basically the same, with the differences being that parameters such as the first grain, second grain, crystal face, grain boundary, and mechanical properties are controlled by adjusting the type and content of doping elements, hot rolling temperature, annealing temperature and time; polymer layer parameters are controlled by controlling the type of polymer layer material and coating process; silicon-based material parameters are controlled by controlling the selection of silicon-based materials; and battery electrolyte parameters are controlled by adjusting the electrolyte composition and its ratio. See Tables 1-1, 1-2, and 1-3 for details.
[0230] Test case
[0231] The relevant parameters of the negative electrode current collector and the battery were tested as follows:
[0232] 1. Number of floors coefficient
[0233] Two negative current collectors were stacked to achieve a test thickness of 15 μm. After sampling the cross-sectional EBSD image of the metal foil layer using a scanning electron microscope (SEM) with an EBSD accessory system, the first grain with a length greater than 2 μm in the length direction was identified and counted layer by layer along the thickness direction at the same location. The number of layers was obtained by counting, and the average value of 5 locations was taken. The layer number coefficient was calculated by using the ratio of the number of layers to the test thickness.
[0234] The test results are shown in Table 1-1.
[0235] 2. Proportion of small-angle grain boundaries
[0236] First, the sample surface undergoes rigorous electropolishing to obtain a stress-free and scratch-free mirror finish. Then, data is acquired using a scanning electron microscope equipped with an EBSD system to obtain crystallographic orientation information of the grains. Next, using professional analysis software, the orientation difference between adjacent grains is precisely measured, and interfaces with orientation differences in the range of 0~10° are automatically identified and marked as small-angle grain boundaries. Finally, the statistical analysis function of the software is used to directly calculate the proportion of small-angle grain boundaries in the total number of grain boundaries.
[0237] The test results are shown in Table 1-1.
[0238] 3. Number of first and second grains
[0239] The metal foil layers are stacked to achieve a test thickness greater than 15 μm. Within a region with a thickness of 15 μm and a width of 20 μm, the number of the first and second grains is counted, and A / B is calculated.
[0240] The test calculation results are shown in Table 1-1.
[0241] 4. (220) Proportion of crystal plane texture coefficient
[0242] A Rigaku-type X-ray diffractometer can be used to characterize the phase and analyze the crystal planes of the copper foil current collector, thereby obtaining the texture coefficient of the (220) crystal plane. The test method includes: disassembling the battery, removing the active layer on the negative electrode to expose the metal foil layer, cleaning the surface of the copper foil current collector with 10 vol.% dilute sulfuric acid and anhydrous ethanol solution in sequence, and then testing after drying with cold air; the test conditions include: using a copper Kα target (λ=0.15406 nm), the working voltage is 40 kV, the scanning angle range is 0~100°, the scanning rate is 0.02° / s, determining the (111) crystal plane, (200) crystal plane, (220) crystal plane, (311) crystal plane, and (222) crystal plane in the obtained XRD spectrum, and calculating the proportion of the texture coefficient of the (220) crystal plane based on the sum of the texture coefficients of the (111) crystal plane, (200) crystal plane, (220) crystal plane, (311) crystal plane, and (222) crystal plane of the negative electrode current collector.
[0243] The test results are shown in Table 1-1.
[0244] 5. Doping element content
[0245] First, the copper foil sample is pretreated by dissolution. Then, precise quantitative analysis is performed using inductively coupled plasma optical emission spectrometry (ICP-OES) or inductively coupled plasma mass spectrometry (ICP-MS) to obtain the content data of each element with ppm-level accuracy, and A1 / A2 is calculated.
[0246] The test calculation results are shown in Table 1-1.
[0247] 6. Thickness of the polymer layer
[0248] The thickness of the polymer layer was obtained by ellipsometer analysis.
[0249] The test calculation results are shown in Table 1-2.
[0250] 7. Silicon-based material parameters
[0251] High-resolution scanning electron microscopy combined with image analysis was used to test the silicon-based material and obtain its major diameter, maximum depth, and included angle.
[0252] The test calculation results are shown in Table 1-2.
[0253] 8. Square resistance
[0254] Sample preparation: Clean the foil surface to remove surface oil or other contaminants, ensuring good probe contact. Lay the sample flat on the insulating substrate, avoiding bending. Using a four-probe tester, arrange the probes at equal intervals (s) on the sample surface. Apply a constant current (I) to the two outer probes and measure the voltage drop (V) on the two inner probes. Input the sample thickness information and calculate the sheet resistance.
[0255] The test calculation results are shown in Table 1-3.
[0256] 9. Mechanical properties
[0257] Using a special cutting tool, cut strips with a width of 15mm±0.1mm and a length of 150±10mm along the MD direction and at a 45° angle to the MD direction for later use. Heat-treat the strips at 260℃ for 30min, and then use a universal testing machine to tensile test the elongation rate. The gauge length is 50mm and the speed is 50mm / min. The C1 and C2 of the negative electrode current collector are obtained from the test results.
[0258] The tensile strength and elongation at 25℃ were tested using the method described above.
[0259] The negative electrode current collector was cut into 15mm*100mm strips, folded in half, and then rolled horizontally once with a 2kg stainless steel roller. The fatigue life cycle was then tested using a fatigue life cycle testing device. The fatigue life cycle testing conditions and methods were as follows: strain-life mode was used, with a test frequency of 5Hz, a strain of 0.1~0.8%, and a test temperature of 20℃~25℃. The fatigue life cycle was recorded until the negative electrode current collector strip experienced fatigue fracture.
[0260] The test calculation results are shown in Table 1-3.
[0261] 10. Difference in roughness, gloss, and color difference at any point between the first and second surfaces.
[0262] The roughness of the first and second surfaces can be tested using a three-dimensional optical profilometer, and then |D1-D2| can be calculated.
[0263] The gloss of the first and second surfaces can be tested using a multi-angle gloss meter, and then |E1-E2| can be calculated.
[0264] The color difference between any two points of the negative electrode current collector can be measured and calculated using a colorimeter.
[0265] The test calculation results are shown in Table 1-3.
[0266] Table 1-1
[0267]
[0268] Note: " / " indicates that the substance or data does not exist.
[0269] Table 1-2
[0270]
[0271] Table 1-3
[0272]
[0273] 11. After 20 cycles, the negative electrode sheet fully charged and stretched:
[0274] The width values of the batteries to be assembled provided in each embodiment and comparative example were tested. Five sets of tests were taken for each embodiment and comparative example, and the average value was calculated and recorded as width A.
[0275] The batteries provided in each embodiment and comparative example were subjected to cycle tests: cycle performance test at room temperature of 25°C. The test process is as follows: first, 3C constant current charging to 4.2V, then constant voltage charging, cut-off current 0.05C, and finally 1C constant current discharge to 2.5V. This cycle test was repeated 20 times.
[0276] The battery, having completed the specified cycle, was disassembled in an inert gas environment while fully charged. The negative electrode was removed, and its width was tested. Five sets of tests were taken for each embodiment and comparative example, and the average value was calculated and recorded as width B. The 20T full-charge extension was calculated as width B - width A. The test calculation data is shown in Table 2.
[0277] 12. Negative electrode breakage test
[0278] The battery was disassembled, and the microstructure of the negative electrode edge and surface was observed directly using an optical microscope and a scanning electron microscope to check for microcracks, powder shedding, or brittle fracture marks that are not visible to the naked eye.
[0279] The test results are shown in Table 2.
[0280] 13. Cyclic performance test
[0281] The battery prepared above was subjected to cycle performance testing at room temperature of 25°C. The test process is as follows: first, it was charged to 4.2V at 3C constant current, then charged at constant voltage with a cutoff current of 0.05C, and finally discharged to 2.5V at 1C constant current. This cycle test was repeated until the capacity decayed to 92%. The test results are shown in Table 2.
[0282] Table 2
[0283]
[0284] As shown in Table 2, the negative electrode current collector structure provided in this application embodiment is stable and not prone to breakage. When the negative electrode current collector provided in the embodiment is used in a battery, the number of cycles with a capacity retention rate > 92% is no less than 920T, demonstrating excellent cycle performance.
[0285] Finally, it should be noted that other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This invention is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art not disclosed herein, and is not limited to the precise structures described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of the invention is limited only by the appended claims.
Claims
1. A negative electrode current collector, comprising a metal foil layer, characterized in that, The metal foil layer includes grains; Along the length direction of the metal foil layer, the grains include a first grain with a length greater than 2 μm; When the test thickness of the metal foil layer is T μm, the number of layers of the first grain along the thickness direction of the metal foil layer is X layers; The following conditions must be met: the layer coefficient X / T is 0.67~6.
2. The negative electrode current collector according to claim 1, characterized in that, Grain boundaries exist between any two adjacent grains. The grain boundaries include small-angle grain boundaries with an included angle of 0 to 10°; Based on the grain boundaries, the proportion of small-angle grain boundaries is 2% to 30%; And / or, the test thickness is 15 μm; And / or, the test thickness is 15 μm, and the number of layers X layers of the first grain is 10 to 40 layers.
3. The negative electrode current collector according to claim 1, characterized in that, Along the length of the metal foil layer, the grain further includes a second grain with a length of 0.1~2.0 μm; Wherein, the cross section of the metal foil layer along the thickness direction, the thickness of the metal foil layer is T1, and within any T1×20μm region, the number of the first grains is A, the number of the second grains is B, and A / B≥10; Preferably, T1 is 15 μm, A is 100~240, and B is 5~10.
4. The negative electrode current collector according to any one of claims 1-3, characterized in that, Based on the sum of the texture coefficients of the (111), (200), (220), (311), and (222) crystal planes of the negative electrode current collector, the texture coefficient of the (220) crystal plane accounts for ≥85%; And / or, the sheet resistance of the negative current collector is 1~4mΩ / □.
5. The negative electrode current collector according to any one of claims 1-4, characterized in that, The metal foil layer is copper foil; The copper foil includes doping elements; The doping element includes at least one of nickel and zirconium. The copper foil satisfies at least one of the following conditions: (1) Based on the copper foil, the content of the doping element is 230~1300ppm; (2) The doping elements include nickel and zirconium; Based on the copper foil, the nickel content is 200~800ppm, and the zirconium content is 30~500ppm; (3) The doping element also includes silicon, and the content of silicon is 1~50ppm based on the copper foil; (4) The doping elements include nickel and silicon; based on the copper foil, the content of nickel is A1 and the content of silicon is A2, and A1 / A2≥4.
6. The negative electrode current collector according to any one of claims 1-5, characterized in that, The negative electrode current collector satisfies at least one of the following conditions: (1) After heat treatment at 260℃ for 30 min, the elongation of the negative electrode current collector along the MD direction is C1; The direction at 45° to the MD direction is the second direction. Along the second direction, the elongation of the negative electrode current collector is C2, 1.5% ≤ C1 - C2 ≤ 6%; (2) The tensile strength of the negative electrode current collector is 350~700MPa; (3) At 25±5℃, the elongation of the negative electrode current collector along the MD direction is 1%~4%; (4) The fatigue life of the negative electrode current collector is 20,000 to 60,000.
7. The negative electrode current collector according to any one of claims 1-6, characterized in that, The negative electrode current collector includes a first surface and a second surface opposite to the first surface; The negative electrode current collector satisfies at least one of the following conditions: (1) The roughness of the first surface is D1, the roughness of the second surface is D2, and |D1-D2|≤0.4μm; (2) The gloss of the first surface is E1, the gloss of the second surface is E2, and |E1-E2|≤100GU; (3) The color difference between any two points on the surface of the negative electrode current collector is ≤5.
8. The negative electrode current collector according to any one of claims 1-7, characterized in that, The metal foil layer is copper foil, and the negative electrode current collector also includes a polymer layer disposed on at least one side surface of the copper foil; The polymer layer comprises at least one of benzotriazole, benzotriazole derivatives, methylbenzotriazole, sodium mercaptobenzothiazole, benzimidazole, 2-mercaptobenzimidazole, and cerium salt; The thickness of the polymer layer is 10~300nm.
9. A negative electrode sheet, characterized in that, Includes the negative electrode current collector as described in any one of claims 1-8 and the negative electrode active layer disposed on at least one side surface of the negative electrode current collector; The negative electrode active layer comprises a silicon-based material; the surface of the silicon-based material has several recessed structures; The silicon-based material satisfies at least one of the following conditions: (1) The major diameter of the silicon-based material is 5~20μm; (2) The maximum depth of the recessed structure is 0.3~8μm; (3) The ratio of the maximum depth of the recessed structure to the length-to-diameter ratio of the silicon-based material is 0.02 to 0.6; (4) The recessed structure includes a first surface and a second surface arranged opposite to each other, and the angle between the first surface and the second surface is 30°~160°.
10. A battery, characterized in that, Includes the negative electrode current collector as described in any one of claims 1-8 or the negative electrode sheet and electrolyte as described in claim 9; The electrolyte comprises 8% to 35% fluoroethylene carbonate by weight percentage.