Microphase-separated porous SPEEK membranes with controllable pore size, their preparation methods and applications in flow batteries

By designing a microphase-separated porous SPEEK membrane with controllable pore size and asymmetric structure, the problem of balancing ion flux and selectivity in alkaline all-iron flow batteries was solved, achieving high-efficiency battery performance and long lifespan.

CN123120770APending Publication Date: 2026-11-17WUHAN GLT ENERGY & ENVIRONMENTAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611490567.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing membrane technologies are insufficient to meet the requirements of alkaline all-iron flow batteries. Dense ion exchange membranes have limited ion flux, porous membranes have wide pore size distribution and insufficient selectivity, high sulfonation degree and membrane stability are mutually restrictive, and it is difficult to balance ion flux and selectivity.

Method used

A porous SPEEK membrane with controllable pore size through microphase separation is used. Through asymmetric structural design, narrow distribution pore caustic agent and gradient solidification process, through-hole nanopores with an average pore size of 0.8-1.5 nm and a pore size distribution half width of less than 0.3 nm are formed. Sulfonic acid groups are enriched on the pore walls to achieve high selective barrier.

Benefits of technology

It achieves a balance between high ion flux and high selectivity, reduces sheet resistivity, improves the coulombic efficiency and cycle life of the battery, while maintaining the mechanical strength and alkali resistance of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120770A_ABST
    Figure CN123120770A_ABST
Patent Text Reader

Abstract

This invention provides a porous SPEEK membrane with controllable microphase separation pore size, its preparation method, and its application in flow batteries. Using SPEEK with a molecular weight of 130,000-160,000 and a sulfonation degree of 0.55-0.70 as the matrix, a narrow-distribution pore-forming agent is used to induce phase separation through non-solvent methods combined with gradient coagulation and alkali activation to obtain an asymmetric, interconnected nanoporous membrane with an average pore size of 0.8-1.5 nm, a half-width at half-maximum (HWHM) of less than 0.3 nm, and enriched sulfonic acid groups on the pore walls. This membrane is used as a separator in alkaline all-iron flow batteries. The membrane relies on a dual mechanism of size sieving and Donnan repulsion on the pore walls to block the permeation of active materials, exhibiting high ion flux, low surface resistivity, and alkali resistance. It solves the problems of existing separators that struggle to balance flux and selectivity, and suffer from insufficient stability. Furthermore, the process is mild and easily scaled up.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of flow battery materials technology, and relates to SPEEK films, their preparation methods, and applications in flow batteries. Background Technology

[0002] All-iron flow batteries utilize abundant, inexpensive, and environmentally friendly raw materials, making them highly promising for large-scale electrochemical energy storage. The alkaline all-iron flow battery system uses triethanolamine (TEA) to complex iron ions as the negative electrode active material and ferrocyanide as the positive electrode active material, offering advantages such as a wide electrochemical window and good electrolyte stability. The separator is the core component limiting the performance improvement of this system; it must efficiently conduct current-carrying ions while preventing cross-penetration of active materials on both sides. Its performance directly determines the battery's energy efficiency, coulombic efficiency, and cycle life.

[0003] However, existing membrane technologies still cannot meet the practical application requirements of alkaline all-iron flow battery systems, mainly due to the following problems: (1) Dense ion exchange membranes have limited ion flux: Traditional dense SPEEK membranes and perfluorosulfonic acid membranes rely on the free volume of polymers to transport ions, resulting in tortuous transport channels and surface resistivity typically higher than 0.5 Ω·cm. 2 (1) Significant polarization under high current density restricts the improvement of battery power density and energy efficiency; (2) Wide pore size distribution and insufficient selectivity of porous membranes: The half-width of the pore size of conventional phase transformation porous membranes is often greater than 1.0 nm, the channels are tortuous and the connectivity is poor, making it difficult to effectively screen triethanolamine and its iron complex with a dynamic diameter of only about 1.6 nm, and the active material permeates across the membrane, causing the capacity to continuously decrease; (3) High sulfonation degree and membrane stability are mutually restrictive: In order to balance hydrophilicity and porosity, existing SPEEK porous membranes mostly use high sulfonation degree raw materials, but they swell excessively in alkaline electrolytes, the mechanical strength decreases, and the excessive repulsion of negatively charged positive electrode active materials increases the surface resistance; (4) It is difficult to balance ion flux and selectivity: Porous membranes generally have a trade-off effect of increasing porosity and decreasing selectivity, and the scheme of constructing sub-nanometer water channels by means of a three-ring rigid structure has the problems of complex process, high cost and poor channel connectivity. Summary of the Invention

[0004] To address the problems of membrane technology in alkaline all-iron flow battery systems described in the background art—limited ion flux of dense ion exchange membranes, wide pore size distribution and insufficient selectivity of porous membranes, mutual constraints between high sulfonation degree and membrane stability, and difficulty in achieving both ion flux and selectivity—this invention provides a porous SPEEK membrane with controllable microphase separation pore size, its preparation method, and its application in flow batteries. This invention enables precise control of the SPEEK membrane pore size below the molecular size of the active material, resulting in a SPEEK membrane with a narrow pore size distribution connecting nanopores, while also possessing high flux and high selectivity.

[0005] In a first aspect, the present invention provides a porous SPEEK membrane with controllable microphase separation pore size. The porous SPEEK membrane uses sulfonated polyether ether ketone (PEEK) with a number-average molecular weight of 130,000-160,000, obtained by sulfonation, as a matrix, resulting in sulfonated PEEK with a degree of sulfonation of 0.55-0.70. The porous SPEEK membrane has an asymmetric structure, with a dense outer skin and interconnected nanopores inside. These interconnected nanopores are formed by a porogen with a polydispersity index (PDI) less than 1.2, through non-solvent-induced phase separation, followed by water washing to remove the porogen. The porous SPEEK membrane has an average pore size of 0.8-1.5 nm, a pore size distribution half-width of less than 0.3 nm, a porosity of 15%-30%, a channel tortuosity of less than 1.5, and a thickness-direction pore size variation coefficient of less than 15%. The density of sulfonic acid groups on the wall of the interconnected nanopores is more than 30% higher than that of the internal matrix of the membrane. The internal matrix refers to the matrix located at a distance greater than 10 nm from the membrane surface. The membrane material is located at a depth of μm, and the sulfonic acid groups on the wall are at least partially present in the form of potassium sulfonate.

[0006] The detailed description of the porous SPEEK membrane of the present invention is as follows: I. Matching Design of High Molecular Weight Matrix and Moderate Sulfonation Degree: This invention uses polyetheretherketone (PEEK) with a number average molecular weight of 130,000-160,000 as raw material, and obtains SPEEK with a sulfonation degree of 0.55-0.70 through controlled sulfonation as the membrane matrix. The two parameters are matched rather than selected independently. The high molecular weight matrix provides sufficient chain segment entanglement density, compensating for the weakening effect of moderate sulfonation degree on SPEEK solubility and casting solution stability, enabling it to form a stable network and form a normal film even in casting solutions with high solids content. At the same time, controlling the sulfonation degree at 0.55-0.70 significantly reduces the affinity rate of SPEEK with water in the coagulation bath, providing a milder kinetic window for the phase separation process and suppressing the swelling driving force of the membrane in the alkaline electrolyte. As a result, the casting solution is stable and uniform with good film-forming properties, avoiding the chain segment aggregation and precipitation of low molecular weight SPEEK at moderate sulfonation degree, and the membrane swelling is suppressed in the alkaline environment while maintaining mechanical strength. This design solves the technical problem of the mutual constraint between high sulfonation degree and film stability, and at the same time lays the technological foundation for narrow distribution pore formation.

[0007] II. Pore Formation Mechanism of Narrow PDI Porositizer as Microdomain Template: The through-hole nanopores of this invention are formed by a narrowly distributed porogen with a polydispersity index (PDI) of less than 1.2 through non-solvent-induced phase separation. Within a mild phase separation kinetic window, the narrowly distributed porogen polymer aggregates within the matrix to form uniformly sized microdomains, exerting a microdomain template effect. Subsequent water washing removes the microdomains, leaving pores with a one-to-one correspondence between the microdomain sizes. The narrower the molecular weight distribution of the porogen, the more uniform the microdomain size, and the narrower the size distribution of the resulting pores. This results in highly uniform pores with an average pore size of 0.8-1.5 nm and a pore size distribution half-width of less than 0.3 nm, and the pore size distribution curve does not exhibit macropore tailing. This mechanism solves the technical problem of wide pore size distribution and insufficient selectivity in porous membranes, eliminating leakage channels larger than the sieving threshold from the source of pore formation.

[0008] III. Asymmetric Structure of Dense Skin Layer and Through-Nanopores: The membrane of this invention has an asymmetric structure, with a dense skin layer on the surface and through-nanopores inside, with a tortuosity of less than 1.5 and a porosity of 15%-30%. It should be noted that the dense skin layer is not completely non-porous: because the skin layer is in direct contact with the coagulation bath and the phase separation rate is controlled by the slow coagulation of the first stage of gradient coagulation, the polymer chain segments in the skin layer are more densely packed, and its effective pore size (sub-nanometer free volume) is smaller than the internal through-nanopores, resulting in a higher hydration Kk. + Ion transport is still possible through the sub-nanometer free volume network in the cortex and the interconnected regions with the internal pores. The dense cortex, while providing mechanical support and overall selective barrier function, does not obstruct ion conduction. The interconnected nanopores perform the main function of ion transport: current-carrying ions migrate along the electrolyte phase within the pores, with transport resistance far lower than the jump-like transport relying on polymer free volume in dense membranes. Low tortuosity ensures a short and straight transport path, and a porosity of 15%-30% provides sufficient channel volume fraction. Thus, the membrane achieves high ion flux while maintaining overall mechanical strength, with a significantly reduced sheet resistivity compared to dense membranes relying on free volume transport, and reduced polarization under high current densities. This structure solves the technical problem of limited ion flux in dense ion exchange membranes.

[0009] IV. Synergistic Constraint of Pore Size and Structural Parameters: This invention employs a combination of mutually reinforcing structural parameters: an average pore size of 0.8-1.5 nm, a pore size distribution half-width of less than 0.3 nm, and a thickness-direction pore size variation coefficient of less than 15%. Triethanolamine has a kinetic diameter of approximately 1.6 nm. Anchoring the upper limit of the average pore size at 1.5 nm ensures that the overall pore size is lower than the molecular size of the active substance, thus enabling size sieving. A half-width of less than 0.3 nm ensures that pore size fluctuations do not exceed the sieving threshold. A thickness-direction variation coefficient of less than 15% ensures uniform pore structure across the membrane cross-section from top to bottom, eliminating weak points caused by localized pore coarsening. Therefore, the membrane reliably sieves the physical size of triethanolamine and its iron complexes, and the barrier performance remains consistent across the overall membrane area and thickness direction. This parameter combination solves the technical problems of insufficient selectivity in porous membranes and capacity decay caused by transmembrane permeation of active substances.

[0010] V. Enrichment of Sulfonic Acid Groups on Pore Walls and Charge Enhancement by Potassium Sulfonate Formation: In this invention, the density of sulfonic acid groups on the walls of the nanopores is more than 30% higher than that of the internal matrix of the membrane. The internal matrix refers to the bulk membrane material at a depth greater than 10 μm from the membrane surface (i.e., the bulk matrix unaffected by phase separation interface effects), and the sulfonic acid groups on the walls are at least partially present in the form of potassium sulfonate. During phase separation, the sulfonic acid groups on the SPEEK segments migrate and accumulate towards the inner wall of the pores due to differences in hydrophilicity, forming a localized high charge density region on the pore walls under the premise that the total sulfonation degree is only at a moderate level; after being activated by alkali to convert to potassium sulfonate, K... + The hydration radius is greater than H + This can further expand the microenvironment of the pores, releasing -SO3 - By imbuing the pore walls with stronger negative charge, a strong electrostatic repulsion is generated against the negatively charged triethanolamine-iron complex based on the Donnan repulsion principle. Thus, the membrane with moderate sulfonation achieves interfacial charge repulsion capabilities approaching those of the highly sulfonated membrane. This, combined with the size sieving of the sub-nanometer pores, constitutes a dual barrier of size sieving and Donnan repulsion, without incurring the swelling costs associated with high sulfonation. This design further enhances the barrier effect of active materials while resolving the contradiction between high sulfonation and membrane stability through a moderate total amount and localized reinforcement.

[0011] VI. Functional Decoupling of Flux and Selectivity: This invention separates ion flux and active material selectivity into different structural elements, rather than relying on a trade-off of the same structural parameters. Ion flux is borne by interconnected channels with a porosity of 15%-30% and a tortuosity of less than 1.5, while selectivity is borne by the upper limit of sub-nanometer pore size (below 1.5 nm) and pore wall charge repulsion. The traditional trade-off dilemma of porous membranes stems from the fact that increased porosity inevitably leads to coarser pores. However, this invention precisely narrows the pore size below the sieving threshold, so that the increase in porosity no longer comes at the cost of coarser pores. Thus, the membrane maintains effective barrier to active materials even at higher porosity, achieving both high ion flux and high selective barrier on the same membrane. This design solves the technical problem of the difficulty in simultaneously achieving ion flux and selectivity.

[0012] Further, the porogen is polyethylene glycol and / or polyvinylpyrrolidone; the molecular weight of polyethylene glycol is 4000-8000, and the molecular weight of polyvinylpyrrolidone is 30000-40000. Both polyethylene glycol and polyvinylpyrrolidone are water-soluble polymers and have good compatibility with SPEEK in polar organic solvents. They can be uniformly dispersed in the casting solution and form discrete microdomains during phase separation. After film formation, they can be completely washed away with water and will not remain in the membrane, thus not affecting membrane performance. The molecular weight of the porogen is a direct factor determining the size of the microdomains and thus the pore size: if the molecular weight is too low, the microdomains are too small, making it difficult to form interconnected transport channels; if the molecular weight is too high, the phase separation driving force is too large, the microdomains coarsen, forming large pores far exceeding the target size and significantly widening the pore size distribution. Limiting the molecular weight of polyethylene glycol to 4000-8000 and the molecular weight of polyvinylpyrrolidone to 30000-40000 precisely matches the target pore size window of 0.8-1.5 nm in this invention; at the same time and / or the limitation allows the two porogens to be used in combination. Porogens of different molecular weights can form microphase domains of complementary sizes in the early stage of phase separation, which is beneficial to further optimize pore connectivity and reduce pore tortuosity.

[0013] Furthermore, the total thickness of the porous SPEEK membrane is 40-60 μm. Membrane thickness is a key geometric parameter determining the membrane's surface resistivity and mechanical reliability: under a given ionic conductivity, surface resistivity is directly proportional to membrane thickness. Excessive membrane thickness increases the ion migration path across the membrane, offsetting the low transport resistance advantage brought by the interconnected nanopores and weakening battery efficiency; conversely, insufficient mechanical strength makes the membrane prone to breakage and puncture during battery assembly and long-term charge-discharge cycles, leading to direct cross-contamination of the positive and negative electrolytes. Controlling the total thickness to 40-60 μm maintains a low surface resistivity while providing the membrane with a mechanical margin to withstand assembly stress and long-term cyclic impacts. This aligns with the asymmetric structure of the dense skin layer and internal interconnected pores, balancing ion transport efficiency, mechanical reliability, and service life.

[0014] Furthermore, the porous SPEEK membrane has a triethanolamine permeability coefficient of less than 3.0 × 10⁻⁶. -7 cm 2 / min, the permeability coefficient of the triethanolamine iron complex is less than 1.0 × 10 -8 cm 2 / min. This limitation quantitatively defines the selective barrier performance of the membrane from the perspective of usage effect: due to the influence of coordination structure and hydration, the hydration kinetic diameter of the triethanolamine iron complex is significantly larger than that of the triethanolamine molecule itself. Therefore, its permeability coefficient limit is an order of magnitude lower than that of triethanolamine. This is consistent with the size sieving mechanism of the membrane pore size upper limit being lower than the molecular size of the active material, and the Donnan repulsion mechanism provided by potassium sulfonate in the pore wall. The membrane that meets the above permeability coefficient limit can quantitatively ensure that the transmembrane permeation of the positive and negative electrode active materials is suppressed to an extremely low level, thereby reducing battery self-discharge, slowing down the capacity decay rate, and providing membrane-level performance guarantee for alkaline all-iron flow batteries to achieve high coulombic efficiency and long cycle life.

[0015] Furthermore, the thickness of the dense skin layer accounts for 5%-15% of the total thickness of the porous SPEEK membrane. An excessively thick skin layer will negate the low-resistivity advantage of the internal through-holes due to its free volume transport mechanism, increasing the surface resistivity; an excessively thin skin layer will lack sufficient mechanical support and surface selective barrier function, making it prone to pinhole defects during film preparation and assembly. Limiting the skin layer thickness to 5%-15% achieves a balance between mechanical support, overall selectivity, and low surface resistivity within the asymmetric structure of the dense skin layer and internal through-holes.

[0016] In a second aspect, the present invention provides a method for preparing a porous SPEEK membrane with controllable microphase separation pore size as described in the first aspect, comprising the following steps: Step 1: Sulfonate polyether ether ketone with a number average molecular weight of 130,000-160,000 to obtain sulfonated polyether ether ketone with a degree of sulfonation of 0.55-0.70, dissolve it in an organic solvent, and prepare a casting solution with a solid content of 16-20 wt%. Step 2: Add a porogen with a polydispersity index (PDI) of less than 1.2 to the casting solution, wherein the mass ratio of the porogen to sulfonated polyether ether ketone is (0.35-0.8):1; Step 3: Stir and dissolve at 70-90℃ for 6-8 hours, then slowly cool to 25-30℃ at a cooling rate of 0.5-1.0℃ / min, degas and scrape to form a wet film; Step 4: Immerse the wet membrane in a coagulation bath at an immersion rate of 1-5 cm / s for non-solvent-induced phase separation; the coagulation bath adopts a gradient coagulation process: in the first stage, immerse it in an aqueous solution containing 5-10 wt% N,N-dimethylformamide for 30-60 s, and in the second stage, transfer it to pure deionized water for 10-30 min. The overall temperature of the coagulation bath is controlled at 20-25℃. Step 5: Wash with water to remove residual organic solvent and pore-forming agent, then soak in 0.5-1.0 mol / L potassium hydroxide solution for 12-24 h to complete alkali activation and obtain the porous SPEEK membrane.

[0017] The detailed description of the porous SPEEK membrane preparation method of the present invention is as follows: I. Preparation of High-Polymer Raw Materials and High-Solids-Content Casting Solution with Moderate Sulfonation Degree (Step 1): This invention selects polyetheretherketone (PEEK) with a number average molecular weight of 130,000-160,000 and obtains SPEEK with a sulfonation degree of 0.55-0.70 through controlled sulfonation. This SPEEK is then formulated into a high-solids-content casting solution with a mass fraction of 16-20 wt%. The high molecular weight matrix, with its high chain segment entanglement density, compensates for the weakening effect of moderate sulfonation on SPEEK solubility and casting solution stability, ensuring that the casting solution remains homogeneous and stable even at high solids content, without chain segment aggregation and precipitation. The 16-20 wt% solids content provides sufficient density for the matrix skeleton after film formation. Too low a solids content will result in excessively high porosity and insufficient skeleton strength, while too high a content will cause a sharp increase in the viscosity of the casting solution, making it difficult to scrape and process. This yields a stable and processable casting solution system, ensuring the membrane's prepareability and quality from the source. This step solves the technical problems of the mutual constraint between high sulfonation degree and film stability, as well as the difficulty of film formation under medium sulfonation degree, laying the material foundation for subsequent narrow distribution pore formation.

[0018] II. Quantitative Addition of Narrow-Distribution Porositizer (Step 2): In this invention, a narrow-distribution porogen with a polydispersity index (PDI) of less than 1.2 is added to the casting solution, and the mass ratio of the porogen to SPEEK is controlled at (0.35-0.8):1. The narrow-distribution porogen forms uniformly sized microdomains in the matrix and acts as a pore-forming template. The width of its molecular weight distribution directly determines the width of the pore size distribution after elution. The mass ratio of the porogen to SPEEK determines the volume fraction of pores. If the ratio is too low, pore formation is insufficient, porosity is low, and ion flux improvement is limited. If the ratio is too high, the microdomains merge and coarsen, resulting in excessively high porosity, uncontrolled pore size, and weakened matrix framework. Thus, both the narrow pore size distribution and the porosity of 15%-30% are simultaneously guaranteed under the same feeding parameters. This step solves the technical problem of wide pore size distribution and insufficient selectivity in porous membranes.

[0019] III. High-Temperature Dissolution and Slow Cooling Treatment of Casting Solution (Step 3): In this invention, the casting solution is stirred and dissolved at 70-90℃ for 6-8 h, and then slowly cooled to 25-30℃ at a cooling rate of 0.5-1.0℃ / min. After degassing, a wet film is formed. The dissolution temperature of 70-90℃ ensures that the high molecular weight SPEEK is fully dissolved and the porogen is uniformly dispersed at the molecular level in the matrix; the dissolution time of 6-8 h ensures that the high molecular weight, high solid content casting solution system is fully dissolved and the porogen is uniformly dispersed. If the time is too short, undissolved gel particles are likely to remain, forming defect sources after film formation; slow cooling makes the casting solution uniformly subcooled, avoiding local gelation or premature phase separation caused by sudden cooling, thereby maintaining the uniform dispersion of the porogen microdomains until the time of film formation; the degassing treatment eliminates air bubbles in the casting solution and prevents the formation of through-hole defects after film formation. This ensures the uniformity of the wet film's microstructure, allowing subsequent phase separation to proceed under consistent conditions across the film surface, resulting in a defect-free film and stable quality across batches. This step provides a prerequisite for achieving narrow pore size distribution and uniform pore size in the thickness direction at the casting solution level, thus addressing the issues of wide pore size distribution and insufficient selectivity.

[0020] IV. Gradient Coagulation Phase Separation under Controlled Immersion Rate (Step 4): In this invention, the wet membrane is immersed in a coagulation bath at a rate of 1-5 cm / s. The coagulation bath employs a two-stage gradient coagulation process: the first stage involves holding the membrane in an aqueous solution containing 5-10 wt% N,N-dimethylformamide for 30-60 seconds, and the second stage involves immersing it in pure deionized water for 10-30 minutes. The overall temperature of the coagulation bath is controlled at 20-25°C. The small amount of organic solvent in the first-stage coagulation bath reduces the mass transfer concentration difference between the non-solvent and the casting solution, thereby slowing down the surface phase separation rate. This allows the surface of the wet membrane to be gently solidified without disrupting the order of the microphase domains of the pore-forming agent, forming a dense skin and avoiding finger-like macropores or pore collapse caused by instantaneous precipitation. The second stage involves deep solidification and shaping in a pure water bath, with the interconnected nanopores also solidifying accordingly. The controlled immersion rate of 1-5 cm / s ensures that the contact time between different parts of the wet membrane and the coagulation bath is consistent, guaranteeing the uniformity of pore formation conditions in the thickness direction. This results in an asymmetric structure with a dense cortex and interconnected internal channels, characterized by interconnected channels, low tortuosity, and a thickness-direction pore size variation coefficient of less than 15%. This step directly solves the technical problems of wide pore size distribution and poor channel connectivity in porous membranes, and provides structural assurance for high ion flux.

[0021] V. Post-treatment after water washing and alkali activation (Step 5): After phase separation and film formation, the residual organic solvent and pore-forming agent are first removed by water washing, and then the film is immersed in 0.5-1.0 mol / L potassium hydroxide solution for 12-24 hours to complete alkali activation. Water washing completely washes away the microphase domains of the pore-forming agent, making the template pores fully exposed and kept clean and connected; during alkali activation, KOH converts the sulfonic acid groups (-SO3H) on the SPEEK chain into potassium sulfonate groups (-SO3K), because K... + The hydration radius is greater than H + This ion exchange can further expand the pore microenvironment, while simultaneously releasing -SO3 - By imbuing the pore walls with a stronger negative charge, a strong electrostatic repulsion is generated against the negatively charged triethanolamine-iron complex based on the Donnan repulsion principle. This step simultaneously serves to increase ion flux and enhance the barrier properties of active materials, providing the final process guarantee for the product membrane to achieve both high flux and high selectivity.

[0022] VI. Synergy and Scalability of the Overall Process Route: The preparation method of this invention connects five steps—raw material matching, narrow-distribution pore formation, gentle dissolution and cooling, gradient coagulation, and alkali activation—into a complete process chain. Each step corresponds to a functional division of labor: whether a film can be formed, pore size uniformity, structural uniformity, pore channel shaping, and charge enhancement. Each step creates the conditions for the next, jointly achieving synergistic control over membrane pore size, pore size distribution, porosity, tortuosity, and pore wall charge density. The entire route is based on a mature solvent-inducible phase separation membrane fabrication process. The coagulation bath operates at room temperature (20-25°C), and the raw material is commercially available PEEK obtained through conventional sulfonation, without the need to synthesize special monomers or rely on complex equipment. Therefore, the preparation of narrow-distribution sub-nanopore SPEEK membranes can be achieved under mild, controllable, and low-cost conditions, with a wide process window and good reproducibility. This route solves the problems of complex processes, high costs, and difficulty in scaling up existing sub-nanopore membrane solutions, providing process feasibility for the industrial application of the membrane of this invention.

[0023] Further, in step 1, the organic solvent is selected from at least one of N,N-dimethylformamide, N-methylpyrrolidone, and dimethyl sulfoxide. All three are strongly polar aprotic solvents with excellent solubility for high molecular weight SPEEK, ensuring that polymers with a number average molecular weight of 130,000-160,000 are fully dissolved at 70-90 °C to form a uniform casting solution. All three are miscible with water in any proportion, serving as a prerequisite for solvent-induced phase separation and ensuring smooth bidirectional diffusion mass transfer between the solvent and non-solvent after the wet film is immersed in the water-based coagulation bath. Furthermore, all three have good compatibility with polyethylene glycol and polyvinylpyrrolidone porogens, preventing premature precipitation of the porogen. N,N-dimethylformamide is also used as an additive component in the first stage of the gradient coagulation coagulation bath, exhibiting good compatibility with the strongly polar solvent used in the casting solution. This allows for precise adjustment of the solvent-non-solvent exchange intensity in the first stage, ensuring the stable implementation of the gradient coagulation process.

[0024] Further, in step 2, the porogen is polyethylene glycol and / or polyvinylpyrrolidone; the molecular weight of polyethylene glycol is 4000-8000, and the molecular weight of polyvinylpyrrolidone is 30000-40000. Both polyethylene glycol and polyvinylpyrrolidone are water-soluble polymers and have good compatibility with SPEEK in the aforementioned polar organic solvents. They can be uniformly dispersed in the casting solution and form discrete microdomains during phase separation. After film formation, they can be completely washed away with water without residue. The molecular weight of the porogen directly determines the microdomain size: if the molecular weight is too low, the microdomains are too small, making it difficult to form interconnected transport channels; if the molecular weight is too high, the phase separation driving force is too large, the microdomains coarsen, forming large pores far exceeding the target size and widening the pore size distribution. The defined molecular weight range matches the target pore size window of 0.8-1.5 nm of the present invention; and / or the definition also allows for the combined use of two porogens, and porogens of different molecular weights can form microphase domains of complementary sizes in the early stage of phase separation, which is beneficial to optimizing pore connectivity and further reducing pore tortuosity.

[0025] Furthermore, in step 3, the degassing is performed under vacuum, with a relative vacuum level not exceeding -0.09 MPa and a degassing time of 20-40 min. The casting liquid of this invention has a high solid content and high viscosity, making it difficult for bubbles trapped during stirring and cooling to escape naturally upon settling. A relative vacuum level not exceeding -0.09 MPa provides sufficient degassing driving force for the viscous system. The 20-40 min degassing time strikes a balance between complete bubble removal and excessive solvent evaporation. Too short a time results in incomplete degassing, while too long a time leads to solvent evaporation on the surface of the casting liquid, increased viscosity, and even film formation, affecting the quality of the coated film. This eliminates bubble defects in the wet film and the finished film, preventing bubbles from evolving into through-hole defects after phase separation, preventing active substances from leaking across the membrane through defect channels, and ensuring the integrity of the membrane and the reliability of its selective barrier properties.

[0026] Thirdly, the present invention provides an alkaline all-iron flow battery, comprising: Positive electrode electrolyte: Contains ferrocyanide as the positive electrode active material, dissolved in an alkaline aqueous solution, wherein the concentration of the active material in the positive electrode electrolyte is 0.3-1.0 mol / L, and the concentration of OH- in the alkaline aqueous solution is 1-4 mol / L; Negative electrode electrolyte: containing triethanolamine iron complex as the negative electrode active material, dissolved in an alkaline aqueous solution, wherein the concentration of the active material in the negative electrode electrolyte is 0.3-1.2 mol / L, and the concentration of OH- in the alkaline aqueous solution is 1-4 mol / L; The membrane is a porous SPEEK membrane with controllable microphase separation pore size as described in the first aspect.

[0027] In the alkaline all-iron flow battery of the present invention, the ferrocyanide on the positive electrode side and the triethanolamine iron complex on the negative electrode side undergo a reversible redox reaction during charge and discharge. + As current-carrying ions, they migrate across the potassium sulfonate-type SPEEK membrane to balance the charges on both sides. The interconnected nanopores inside the membrane of this invention have a tortuosity of less than 1.5 and a porosity of 15%-30%, which is K... + This provides short, straight, and ample low-resistance migration channels, resulting in significantly lower internal resistance compared to solutions using dense membranes. Polarization at high current densities is suppressed, leading to improved voltage and energy efficiency. Simultaneously, the membrane's average pore size upper limit of 1.5 nm is lower than the approximately 1.6 nm kinetic diameter of triethanolamine and the hydration size of the triethanolamine iron complex. Size sieving physically blocks the transmembrane channels of the negative electrode active material, and the pore walls are enriched with -SO3... - Furthermore, by utilizing Donnan repulsion to simultaneously block charged triethanolamine iron complexes and ferrocyanide anions, the dual barrier of size sieving and charge repulsion suppresses cross-permeation of active materials on both sides to an extremely low level, slowing down self-discharge and capacity decay, and ensuring high coulombic efficiency. Meanwhile, the combination of moderate sulfonation and a high molecular weight matrix ensures that the membrane's swelling is suppressed and its structure remains intact in 1-4 mol / L strongly alkaline electrolytes, supporting long-term battery cycling. Thus, the electrolyte system, concentration and alkalinity design, and membrane structure are precisely matched. Problems in the background technology, such as limited flux of dense membranes, insufficient selectivity of porous membranes, poor stability of high-sulfonation membranes, and the difficulty in balancing flux and selectivity, are comprehensively solved at the battery level, enabling the battery to simultaneously achieve high coulombic efficiency, high energy efficiency, and long cycle life at high current densities.

[0028] Compared with the prior art, the present invention has the following advantages: (1) Precise construction of narrow-pore-distribution interconnected nanopores: The pores defined in this invention are formed by non-solvent-induced phase separation of a narrow-distribution porogen with a polydispersity index (PDI) of less than 1.2. According to the basic principle of phase separation, the size of the micro-phase domains formed by the porogen in the matrix directly determines the pore size. The narrower the molecular weight distribution of the porogen, the more uniform the size of the micro-phase domains, and the more uniform the pore size left after elution. Therefore, the half-peak width of the pore size distribution can be controlled within 0.3 nm and the pore size variation coefficient in the thickness direction is less than 15%. The gradient solidification process first delays the surface phase separation in an aqueous solution containing 5-10 wt% organic solvent, and then transfers it to pure water to complete the solidification. This avoids the finger-like macropores or pore collapse caused by rapid precipitation, and ensures that the pores are interconnected and the tortuosity is less than 1.5. The two work together to make the membrane obtain interconnected nanopores with an average pore size of 0.8-1.5 nm, narrow distribution, and uniform structure. (2) Combining high ion flux and low surface resistivity: Dense ion exchange membranes rely on the free volume of polymers to transport ions, resulting in tortuous transport channels and surface resistivity typically higher than 0.5 Ω·cm. 2 The SPEEK membrane of the present invention has interconnected nanopores with a porosity of 15%-30%. The current-carrying ions can migrate through the electrolyte phase in the pores. The transport path is short and has low tortuosity. The ion transport resistance is significantly less than the free volume transport mechanism of the dense membrane. This is beneficial to reduce the sheet resistance and alleviate concentration polarization and ohmic polarization under high current density, thereby supporting the improvement of battery power density and energy efficiency. (3) Forming a dual barrier of size sieving and charge repulsion for active substances: The kinetic diameter of triethanolamine is about 1.6 nm, and the upper limit of the pore size of this membrane is 1.5 nm, which is lower than this size. This can physically block triethanolamine and its iron complex from passing through the pores. At the same time, the density of sulfonic acid groups on the pore wall is limited to be more than 30% higher than that of the matrix inside the membrane, and the sulfonic acid groups exist at least partially in the form of potassium sulfonate. During the phase separation process, the hydrophilic sulfonic acid groups migrate and accumulate to the pore wall, forming a local high charge density region on the pore wall. After alkali activation, the potassium sulfonate dissociates into -SO3 - Further enhancing the negative charge, electrostatic repulsion is achieved against the negatively charged triethanolamine-iron complex based on the Donnan repulsion principle; physical sieving and charge repulsion work together to effectively inhibit the transmembrane permeation of active substances while maintaining the interconnected channels of the membrane. (4) Good mechanical strength and alkali resistance dimensional stability: The matrix is ​​made of high molecular weight polyether ether ketone with a number average molecular weight of 130,000-160,000. The high chain segment entanglement density provides a mechanical framework for the membrane. The degree of sulfonation is controlled at a moderate level of 0.55-0.70, which avoids the decrease in mechanical strength caused by excessive water absorption and swelling due to excessive density of sulfonic acid groups in high sulfonation membranes. At the same time, it moderately reduces the problem of excessive repulsion of negatively charged positive electrode active material, which increases the surface resistance. The combination of the asymmetric dense skin layer on the surface and the internal through-pore layer takes into account both mechanical support and ion transport, so that the swelling of the membrane is suppressed and the structure is intact in the strongly alkaline electrolyte environment, which is conducive to dimensional stability during long-term cycling. (5) The preparation process is stable and controllable and easy to scale up: According to the basic principle of polymer solution, the decrease in sulfonation degree will weaken the solubility of SPEEK in organic solvent and the stability of casting solution; the present invention compensates for the decrease in film-forming properties caused by moderate sulfonation degree with the chain entanglement effect of high molecular weight matrix, so that the 16-20 wt% high solid content casting solution remains stable and uniform and does not cause chain segment aggregation and precipitation; the moderate sulfonation degree also reduces the affinity rate of SPEEK with water in the coagulation bath, providing a mild kinetic window for the formation of ordered microphase domains by narrow distribution pore caustic agent, and then the ordered structure is maintained by gradient coagulation; the whole process is based on a mature non-solvent-induced phase separation route, the coagulation bath temperature is 20-25 ℃ room temperature conditions, no special monomers need to be synthesized, the process window is wide, the repeatability is good, and it has the basis for industrial scale-up; (6) Improved overall performance and service life of flow batteries: The alkaline all-iron flow battery of the present invention uses the above-mentioned porous SPEEK membrane as the separator, and a positive electrode electrolyte containing ferrocyanide (0.3-1.0 mol / L) and a negative electrode electrolyte containing triethanolamine iron complex (0.3-1.2 mol / L), 1-4 mol / L OH - It is compatible with alkaline systems. The high ion flux of the separator reduces the internal resistance of the battery, and the dual barrier mechanism inhibits self-discharge and capacity decay caused by cross-penetration of active materials on both sides. The alkali resistance and dimensional stability ensure that the separator remains intact and effective during long-term operation. These three factors work together to support the battery in achieving and maintaining high coulombic efficiency and energy efficiency over a long period of time, thus extending cycle life.

[0029] In summary, this invention uses SPEEK with a molecular weight of 130,000-160,000 and a sulfonation degree of 0.55-0.70 as the matrix. A narrow-distribution pore-forming agent is used to induce phase separation through non-solvent methods, combined with gradient coagulation and alkali activation to form an asymmetric, interconnected nanoporous membrane with an average pore size of 0.8-1.5 nm, a half-maximum width at half-maximum (FWHM) of less than 0.3 nm, and enriched sulfonic acid groups on the pore walls. This membrane is used as a separator for alkaline all-iron flow batteries. This membrane relies on a dual mechanism of size sieving and Donnan repulsion on the pore walls to block the permeation of active materials, exhibiting high ion flux, low surface resistivity, and alkali resistance. It solves the problems of existing separators that struggle to balance flux and selectivity, and suffer from insufficient stability. Furthermore, the process is mild and easily scaled up. Attached Figure Description

[0030] Figure 1 This is a schematic diagram illustrating the cross-sectional structure, sulfonic acid enrichment on the pore walls, and dual-selective blocking mechanism of the porous SPEEK membrane with controllable microphase separation pore size according to the present invention. The diagram shows a dense skin layer (A), a through-cell nanopore layer (B), sulfonic acid groups enriched on the pore walls (C, existing in the form of potassium sulfonate), the blocking of TEA / TEA-Fe complexes (D), and alkali metal ions (such as K+). + Selective transmission (E).

[0031] Figure 2 The graph shows the pore size distribution of the membranes prepared in Examples 1-6 and Comparative Examples 3, 4, 6, 8, and 9 of this invention. The horizontal axis represents the pore size (nm), and the vertical axis represents the differential pore volume distribution (dV / dD). The vertical dashed line in the graph indicates 1.6 nm, which is the kinetic diameter of triethanolamine.

[0032] Figure 3 The graphs show a comparison of sheet resistance and active material permeability coefficients between Examples 1-6 and Comparative Examples 1, 3, 4, 6-11 of the present invention; wherein (a) is a bar chart comparing sheet resistance, (b) is a bar chart comparing TEA permeability coefficients, and (c) is a bar chart comparing TEA-Fe permeability coefficients. The vertical axis of (b) and (c) is a logarithmic scale.

[0033] Figure 4 This is a flowchart illustrating the process for preparing porous SPEEK membranes with controllable microphase separation pore size according to the present invention.

[0034] Figure 5 For Example 1, a single cell at 80 mA / cm 2 The curves showing the changes in coulombic efficiency (CE), voltage efficiency (VE), and energy efficiency (EE) after 8000 charge-discharge cycles at current density, and the comparison curves of coulombic efficiency between Example 1 and Comparative Example 1.

[0035] Figure 6 The graph shows the relationship between the polydispersity index (PDI) of the pore-forming agent and the half-peak width of the membrane pore size distribution. The data points are taken from Example 1, Comparative Example 8 and Comparative Example 4. The red dashed line in the graph marks the half-peak width of 0.3 nm. Detailed Implementation

[0036] To make the technical problems to be solved, the technical solutions, and the beneficial effects of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the present invention and are not intended to limit the present invention.

[0037] In the following examples and comparative examples, the sulfonated polyether ether ketone (SPEEK) used was prepared by sulfonation of polyether ether ketone (PEEK) with the corresponding number average molecular weight. The sulfonation can be carried out by concentrated sulfuric acid method: PEEK powder is added in batches to concentrated sulfuric acid with a mass fraction of 95%-98%, and the reaction is stirred at 50-60 °C. The degree of sulfonation is adjusted to 0.55-0.70 by controlling the reaction time. After the reaction is completed, the reaction solution is poured into ice water to precipitate. The precipitate is washed with deionized water until neutral and dried under vacuum at 60 °C to obtain the sulfonated polyether ether ketone.

[0038] Sulfonation degree is adopted 1 The molecular weight was determined by nuclear magnetic resonance spectroscopy, and the number-average molecular weight was determined by gel permeation chromatography. The polydispersity index (PDI) of polyethylene glycol (PEG) and polyvinylpyrrolidone (PVP) was determined by gel permeation chromatography. All other reagents were commercially available analytical grade.

[0039] The fabrication process of the porous SPEEK membrane with controllable microphase separation pore size according to the present invention is as follows: Figure 4 As shown, the process includes, in sequence: preparation of casting solution, addition of narrow-distribution pore-forming agent, high-temperature dissolution and slow cooling, degassing and scraping, two-stage gradient coagulation, water washing and alkali activation, finally obtaining a porous SPEEK membrane.

[0040] The structure and barrier mechanism of the porous SPEEK membrane obtained in this invention are as follows: Figure 1 As shown: The membrane has an asymmetric structure, with a dense outer layer (A) and an inner layer of interconnected nanopores (B). The pore walls are enriched with sulfonic acid groups (C). The overall pore size of the membrane is smaller than the molecular size of triethanolamine (TEA) and its iron complex (TEA-Fe), thus blocking TEA and TEA-Fe complexes (D). Alkali metal ions (such as K+) are also blocked. + Selective transmission (E) thus forms a dual selective barrier of size sieving and Donnan repulsion.

[0041] In the following embodiments and comparative examples, unless otherwise specified, the performance characteristics are characterized as follows: (1) Pore size distribution test: Positron annihilation lifetime spectroscopy (PALS) was used to determine the free volume pore size distribution of the membrane, and the PALS test results were used as the standard. The pore size inversion was based on the Tao-Eldrup model and its extended model based on the relationship between positron element pick-up annihilation lifetime and pore size. For samples with an average pore size close to or greater than 1 nm, small-angle X-ray scattering (SAXS) was used to verify the pore size distribution width, with PALS as the main method and SAXS as the auxiliary method for cross-confirmation. The low-temperature nitrogen adsorption-desorption BET method was used as an auxiliary method, and the BJH model was used to calculate the pore size. The half-maximum width of the pore size distribution was calculated by fitting the distribution curve.

[0042] (2) Porosity test: wet-dry weight method. The diaphragm was vacuum dried at 60 ℃ to constant weight, and the dry weight W was recorded.d After soaking in deionized water for 24 hours, remove the sample and quickly absorb the surface moisture with filter paper to obtain the wet weight W. w Porosity = (W) w -W d ) / (ρ w ·V m )×100%,ρ w V is the density of water. m This represents the diaphragm volume.

[0043] (3) Surface resistivity and ionic conductivity: AC impedance spectroscopy (EIS), electrochemical workstation test frequency range 10 6 Hz to 10 -2 Hz, test environment: 1 mol / L KOH solution, effective test area of ​​membrane: 1 cm² 2 .

[0044] (4) TEA permeability coefficient: H-type diffusion tank, effective area 7.07 cm² 2 The supply chamber contained 0.1 mol / L TEA + 1 mol / L KOH, and the receiving chamber contained 1 mol / L KOH. The mixture was stirred at room temperature, and samples were taken periodically. The TEA concentration was detected at 280 nm using a UV-Vis spectrophotometer, and the permeability coefficient was calculated based on Fick's first law.

[0045] (5) TEA-Fe permeability coefficient: H-type diffusion cell; the supply chamber is 0.1 mol / L TEA-Fe(III) + 3 mol / L KOH, and the receiving chamber is 3 mol / L KOH; samples are taken at regular intervals, and the concentration of the complex is determined by a UV-Vis spectrophotometer at 480 nm to calculate the permeability coefficient.

[0046] (6) Standard performance test of single cell: effective area of ​​separator 25 cm² 2 The negative electrode electrolyte is 0.5 mol / L TEA-Fe(III) + 3 mol / L KOH, and the positive electrode electrolyte is 0.4 mol / L K3Fe(CN)6 / K4Fe(CN)6 + 1 mol / L KOH; the current density is 60 mA / cm². 2 Constant current charging and discharging, with a voltage cutoff range of 0.5-1.5 V.

[0047] (7) Long-cycle stability test: The test conditions are the same as those for the routine performance test of a single cell, but the current density is increased to 80 mA / cm². 2 Constant current charge-discharge cycles were performed, and the decay curves of coulombic efficiency, voltage efficiency, and energy efficiency with the number of cycles were recorded; the energy efficiency was calculated by multiplying the coulombic efficiency and the voltage efficiency.

[0048] (8) Sulfonic acid group density in pore wall: X-ray photoelectron spectroscopy (XPS) combined with low-energy cluster ion beam (GCIB, accelerating voltage not higher than 5 kV) was used for depth profiling. The single stripping depth was controlled to be about 1 nm. The sulfur content of the 2-5 nm thin layer region of the pore wall and the matrix inside the membrane (the membrane material body at a depth greater than 10 μm from the membrane surface) was analyzed and the ratio of sulfonic acid group density was calculated. During the test, the ratio of sulfonate sulfur (binding energy about 168 eV) and reduced sulfur signal in the S 2p spectrum was monitored to confirm that the stripping process did not cause significant reduction of sulfonate and to ensure that the chemical state of sulfur element truly reflects the distribution of sulfonic acid groups.

[0049] (9) Pore tortuosity test: The tortuosity of the pores is calculated by gas permeation method combined with porosity. Since the diaphragm of this invention has sub-nanometer pores and gas transmission is mainly based on surface diffusion mechanism, the pore size of the gas permeation model is corrected during the test, and electrochemical impedance spectroscopy is used for cross-validation. Mercury intrusion porosimetry is not applicable to this system and is not used for testing.

[0050] (10) Thickness direction pore size variation coefficient test: The membrane is mechanically peeled and divided into 5 equal thickness layers along the thickness direction from the dense skin layer side. Samples are taken from each layer and PALS test is performed to obtain the average pore size of each layer. The ratio of the standard deviation of the average pore size of the 5 thickness layers to the total average pore size is calculated and defined as the thickness direction pore size variation coefficient. The membrane cross-section is cut by focused ion beam (FIB) to prepare the sample. The pore morphology of the cross-section is observed by transmission electron microscopy (TEM) and the size distribution of more than 50 pores is statistically analyzed as auxiliary verification. The pore size quantification is based on the PALS test results.

[0051] (11) Alkaline electrolyte swelling rate test: Cut the diaphragm into 20 mm × 20 mm samples, vacuum dry at 60 ℃ to constant weight, and record the dry thickness T. d After immersing in 1 mol / L KOH solution for 48 h, remove the solution, blot the surface liquid with filter paper, and record the wet thickness T. w Swelling rate = (T) w -T d ) / T d ×100%.

[0052] (12) Tensile strength test: Cut type 5 specimens according to GB / T 1040.3, test with electronic universal testing machine, tensile rate 10 mm / min, test the tensile strength of dry specimens and specimens soaked in 1 mol / L KOH for 48 h respectively, and take the average value of 5 specimens.

[0053] Example 1 In this embodiment, a porous SPEEK membrane was prepared using PEG-6000 pore-forming agent, as detailed below.

[0054] 18 g of SPEEK with a number average molecular weight of 150,000 and a sulfonation degree of 0.62 was dissolved in 82 g of N,N-dimethylformamide (DMF) and stirred at 80 °C. 7.2 g of PEG-6000 (PDI=1.05) was added, with a pore-forming agent to SPEEK mass ratio of 0.4:1. Stirring was continued for 6 h until completely dissolved. The temperature was lowered to 28 °C at a rate of 0.8 °C / min. Vacuum degassing was performed for 30 min under a relative vacuum of -0.095 MPa. The film was coated onto a glass plate with a wet film thickness of 300 μm. The film was immersed in a 25 °C gradient coagulation bath at 2 cm / s. In the first stage, the film was immersed in an 8 wt% DMF aqueous solution for 45 s, and in the second stage, it was immersed in pure deionized water for 20 min. After removal, the film was washed with deionized water for 24 h to remove residual DMF and PEG. The film was then immersed in 0.5 mol / L KOH solution for 18 h to complete alkali activation, resulting in a porous SPEEK membrane with a thickness of approximately 50 μm.

[0055] Characterization and properties: The obtained membrane exhibits Figure 1 The dense cortex-interconnected nanopore asymmetric structure shown has a dense cortex thickness of approximately 3.5 μm, accounting for 7% of the total thickness, as observed by FIB-TEM cross-section. Figure 2 As shown, its pore size distribution curve has a narrow and sharp peak. PALS measured an average pore size of 1.0 nm and a pore size distribution half-maximum width of 0.24 nm. SAXS verification confirmed that the pore size distribution width was consistent with the PALS results. The porosity was 20%, the pore tortuosity was 1.38, and the coefficient of variation of pore size in the thickness direction was 11%. XPS-GCIB depth profiling showed that the density of sulfonic acid groups on the pore wall was 35% higher than that in the matrix inside the membrane. During the exfoliation process, the proportion of sulfonate sulfur signal remained stable, and no significant reduction was observed. Figure 3 As shown, the surface resistivity is 0.32 Ω·cm 2 The TEA permeability coefficient is 2.4 × 10⁻⁶. -7 cm 2 / min, the permeability coefficient of TEA-Fe is 0.9×10 -8 cm 2 / min. The dry tensile strength is 63 MPa, and the tensile strength after soaking in 1 mol / L KOH for 48 h is 59 MPa, with a retention rate of 94%. When assembled into an alkaline all-iron liquid flow single cell, the coulombic efficiency is 99.7% and the energy efficiency is 85.5%; the swelling ratio in 1 mol / L KOH is 8.2%.

[0056] Example 2 In this embodiment, a porous SPEEK membrane was prepared using PVP-K30 as the pore-forming agent. The preparation process was the same as in Example 1, except that the pore-forming agent was replaced with PVP K30 (molecular weight 40000, PDI=1.08), and 6.3 g was added. The mass ratio of the pore-forming agent to SPEEK was 0.35:1. The other conditions remained unchanged, and a membrane with a thickness of about 52 μm was obtained.

[0057] Characterization and performance: such as Figure 2 As shown, the pore size distribution curve also exhibits a narrow peak, with an average pore size of 0.9 nm and a half-peak width of 0.22 nm; the porosity is 18%, the tortuosity is 1.42, the coefficient of variation of pore size in the thickness direction is 9%, and the density of sulfonic acid groups on the pore wall is 32% higher than that of the matrix; Figure 3 As shown, the surface resistivity is 0.35 Ω·cm. 2 TEA permeability coefficient 2.0×10 -7 cm 2 / min, TEA-Fe permeability coefficient 0.7×10 -8 cm 2 / min; Coulomb efficiency 99.7%, energy efficiency 84.8%, swelling rate 7.8%.

[0058] This embodiment demonstrates that polyvinylpyrrolidone porogens can also achieve narrow-distribution sub-nanometer pores, and the technical solution of this invention is applicable to both types of water-soluble polymeric porogens.

[0059] Example 3 In this embodiment, a porous SPEEK membrane was prepared by mixing PEG-6000 and PVP-K30 to induce pores. The preparation process was the same as in Example 1, except that the pore-inducing agent was a mixture of 3.6 g of PEG-6000 and 3.6 g of PVP-K30, and the total mass ratio of pore-inducing agent to SPEEK was 0.4:1. The other conditions remained unchanged, and a membrane with a thickness of about 54 μm was obtained.

[0060] Characterization and performance: Average pore size 1.1 nm, full width at half maximum (FWHM) 0.26 nm (e.g.) Figure 2 (As shown); porosity 22%, pore tortuosity further reduced to 1.30, thickness-direction pore diameter variation coefficient 12%, pore wall sulfonic acid group density increased by 38% compared to the matrix; sheet resistivity 0.30 Ω·cm 2 TEA permeability coefficient 2.2×10 -7 cm 2 / min, TEA-Fe permeability coefficient 0.8×10 -8 cm 2 / min (e.g.) Figure 3 (As shown); Coulomb efficiency 99.6%, energy efficiency 85.8%, swelling rate 8.5%.

[0061] This embodiment demonstrates that, in a mixed porogen system, two narrow-distribution polymer microdomains synergistically regulate the pore structure. It is speculated that porogens of different molecular weights form complementary-sized microdomains in the early stage of phase separation, which optimizes pore connectivity, thereby maintaining a narrow pore size distribution and further reducing tortuosity while obtaining higher porosity.

[0062] Example 4 In this embodiment, a porous SPEEK membrane was prepared using N-methylpyrrolidone (NMP) as a solvent and PEG-4000 as a pore-forming agent, as described below.

[0063] 18 g of SPEEK with a number average molecular weight of 150,000 and a sulfonation degree of 0.62 was dissolved in 82 g of NMP and stirred at 90 °C. 10.8 g of PEG-4000 (PDI=1.06) was added, with a pore-forming agent to SPEEK mass ratio of 0.6:1. Stirring was continued for 8 h until completely dissolved. The temperature was lowered to 25 °C at a rate of 0.5 °C / min. Vacuum degassing was performed for 30 min under a relative vacuum of -0.095 MPa. After coating the wet film, it was immersed in a 20 °C gradient coagulation bath at 5 cm / s. The first stage was soaking in 5 wt% DMF aqueous solution for 60 s, and the second stage was soaking in pure deionized water for 30 min. After washing with water for 24 h, it was placed in 1.0 mol / L KOH solution for 12 h to complete alkali activation, resulting in a porous SPEEK membrane with a thickness of approximately 48 μm.

[0064] Characterization and performance: Average pore size 0.8 nm, full width at half maximum (FWHM) 0.20 nm; porosity 26%, tortuosity 1.45, thickness-direction pore size variation coefficient 13%, pore wall sulfonic acid group density increased by 33% compared to the matrix; sheet resistivity 0.28 Ω·cm 2 TEA permeability coefficient 2.6×10 -7 cm 2 / min, TEA-Fe permeability coefficient 0.9×10 -8 cm 2 / min; Coulomb efficiency 99.6%, energy efficiency 84.9%, swelling rate 8.8%.

[0065] This embodiment demonstrates that the NMP solvent system and the lower molecular weight PEG-4000 porogen can also achieve narrow-distribution sub-nanometer pore formation within the scope of the claims, verifying the feasibility of solvent type and lower limit of porogen molecular weight.

[0066] Example 5 In this embodiment, a porous SPEEK membrane was prepared using dimethyl sulfoxide (DMSO) as the solvent and PEG-8000 as the pore-forming agent. The preparation process was the same as in Example 1, except that the solvent was replaced with DMSO, and the pore-forming agent was replaced with 14.4 g of PEG-8000 (PDI=1.08). The mass ratio of the pore-forming agent to SPEEK was 0.8:1. The dissolution temperature was 70 ℃, and the stirring was carried out for 8 h. The temperature was then reduced to 30 ℃ at a rate of 1.0 ℃ / min. The immersion rate was 1 cm / s. The first stage coagulation bath was a 10 wt% DMF aqueous solution, which was held for 30 s. The second stage was a pure water immersion for 10 min. The membrane was then activated by alkali immersion in 0.8 mol / L KOH for 24 h. A membrane with a thickness of approximately 55 μm was obtained.

[0067] Characterization and performance: Average pore size 1.4 nm, full width at half maximum (FWHM) 0.28 nm; porosity 30%, tortuosity 1.48, thickness-direction pore size variation coefficient 14%, pore wall sulfonic acid group density increased by 31% compared to the matrix; sheet resistivity 0.26 Ω·cm 2 TEA permeability coefficient 2.9×10 -7 cm 2 / min, TEA-Fe permeability coefficient 0.95×10 -8 cm 2 / min; Coulomb efficiency 99.6%, energy efficiency 85.0%, swelling rate 9.0%.

[0068] This embodiment verifies the feasibility of the formulation at the boundary between the upper limit of the molecular weight of the porogen (PEG-8000) and the upper limit of the ratio of the porogen (0.8:1). At this point, the porosity is at the upper limit of the claim 30%, and all pore structure parameters still meet the defined range.

[0069] Example 6 This embodiment examines the combined boundary between the lower limit of the raw material molecular weight and the upper limit of the degree of sulfonation. The preparation process is the same as in Example 1, except that: 18 g of SPEEK with a number average molecular weight of 130,000 and a degree of sulfonation of 0.70 was used, and NMP was used as the solvent; 9.0 g of PEG-6000 (PDI=1.15) was used as the porogen, and the mass ratio of the porogen to SPEEK was 0.5:1; the immersion rate was 3 cm / s; and the membrane was activated by soaking in 0.5 mol / L KOH for 24 h; resulting in a membrane with a thickness of approximately 51 μm.

[0070] Characterization and performance: Average pore size 1.2 nm, full width at half maximum (FWHM) 0.29 nm; porosity 19%, tortuosity 1.42, thickness-direction pore size variation coefficient 14%, pore wall sulfonic acid group density increased by 30% compared to the matrix; sheet resistivity 0.36 Ω·cm 2 TEA permeability coefficient 2.7×10 -7 cm 2 / min, TEA-Fe permeability coefficient 0.95×10 -8 cm 2 / min; Coulomb efficiency 99.6%, energy efficiency 84.5%, swelling rate 9.5%.

[0071] This embodiment demonstrates that, under the combined boundary conditions of the lower limit of molecular weight, the upper limit of sulfonation degree, and the pore-forming agent PDI being close to the upper limit, the parameters of the obtained film still meet the requirements of the claims. Although the swelling rate increases slightly, it is still far lower than that of the high-sulfonation-degree dense film, thus verifying the rationality of the parameter boundaries of the claims.

[0072] Example 7 This embodiment examines the compatibility between electrolyte concentration and alkalinity boundary in the alkaline all-iron flow battery, using the membrane assembly single cell prepared in Example 1, as detailed below.

[0073] The effective area of ​​the diaphragm is 25 cm². 2 The negative electrode electrolyte is 1.2 mol / L TEA-Fe(III) + 4 mol / L KOH, and the positive electrode electrolyte is 1.0 mol / L K3Fe(CN)6 / K4Fe(CN)6 + 4 mol / L KOH; the current density is 60 mA / cm². 2 Constant current charging and discharging, with a voltage cutoff range of 0.5-1.5 V.

[0074] Characterization and performance: At the upper limit of active substance concentration (1.2 mol / L / 1.0 mol / L) and OH... - Under the boundary conditions of the upper concentration limit (4 mol / L), the battery coulombic efficiency is 99.5%, energy efficiency is 84.6%, and the coulombic efficiency decay is less than 0.3 percentage points after 500 consecutive cycles; the membrane swelling rate after cycling is 9.1%, the tensile strength retention rate is 92%, and no damage is observed. This embodiment shows that the membrane of the present invention can maintain stable electrochemical performance and structural integrity across the entire range of defined electrolyte concentrations and alkalinities, providing implementation support for the wide-range limitation of the present invention.

[0075] Comparative Example 1 This comparative example is a high-sulfonation degree dense SPEEK membrane. 15g of SPEEK with a number average molecular weight of 150,000 and a sulfonation degree of 0.80 was dissolved in 85g of DMF; the solution was stirred and dissolved at 70℃, vacuum degassed and coated, and then directly immersed in a pure deionized water coagulation bath; the remaining conditions were the same as in Example 1, and a dense membrane with a thickness of about 45 μm was obtained.

[0076] Performance: Pore size less than 0.5 nm, porosity less than 5%, tortuosity greater than 3.0, no sulfonic acid enrichment on pore walls; Figure 3 As shown, the surface resistivity is 0.58 Ω·cm. 2TEA permeability coefficient 7.8×10 -7 cm 2 / min, TEA-Fe permeability coefficient 3.8×10 -8 cm 2 / min, all significantly inferior to Examples 1-3; coulombic efficiency 99.2%, energy efficiency 82.5%, swelling rate as high as 15.5%.

[0077] The mechanism is that the high sulfonation degree membrane swells excessively in the alkaline electrolyte, and the local free volume fluctuation increases, resulting in TEA / TEA-Fe leakage; while the through-channel pore size of the embodiment is uniform and less than 1.5 nm, which effectively blocks such large-scale fluctuations, and the pore walls are enriched with sulfonic acid groups while providing Donnan repulsion.

[0078] Comparative Example 2 This comparative example is a low molecular weight, medium sulfonation degree SPEEK membrane. 18 g of SPEEK with a number average molecular weight of 80,000 and a sulfonation degree of 0.62 was dissolved in 82 g of DMF and stirred at 80 °C. 7.2 g of PEG-6000 (PDI=1.05) was then added. During the stirring process, phase separation and precipitation occurred in the casting solution, making it impossible to form a stable and homogeneous casting solution and thus impossible to coat into a membrane.

[0079] This comparative example demonstrates that a high molecular weight matrix with a number average molecular weight of 130,000-160,000 is a necessary condition for ensuring the processability of SPEEK with moderate sulfonation degree.

[0080] Comparative Example 3 This comparative example is a high molecular weight PEG-20000 porous membrane. The preparation process is the same as in Example 1, except that the pore-forming agent is replaced with 7.2 g of PEG-20000 (molecular weight 20000, PDI=1.10); a membrane with a thickness of about 48 μm is obtained.

[0081] Performance: such as Figure 2 As shown, its pore size distribution curve is significantly broadened and exhibits large pore peaks, with an average pore size of 3.6 nm, a half-peak width of 1.80 nm, and a pore size variation coefficient as high as 26% in the thickness direction; the porosity is 32%, the tortuosity is 2.75, and the sulfonic acid enrichment in the pore walls is only 12%; Figure 3 As shown, the surface resistivity is as low as 0.24 Ω·cm 2 However, the TEA permeability coefficient is as high as 17.5×10. -7 cm 2 / min, the TEA-Fe permeability coefficient reaches 11.8×10 -8 cm 2 / min, the coulombic efficiency drops to 98.0%, the energy efficiency to 79.8%, and the swelling rate to 9.2%.

[0082] This comparative example shows that when the molecular weight of the pore-forming agent is too high, the driving force for phase separation is too large, the coarsening of the pores becomes uncontrolled, and the selectivity is lost. It also shows that the reduction of sheet resistivity cannot be at the expense of selectivity. The pore size window of this invention must be lower than the molecular size of the active substance.

[0083] Comparative Example 4 This comparative example is a PEG-6000 porous membrane with a wide molecular weight distribution. The preparation process is the same as in Example 1, except that: a PEG-6000 sample with a wide molecular weight distribution (PDI=2.5) was selected as the pore-forming agent, and 7.2 g was added; a membrane with a thickness of about 49 μm was obtained.

[0084] Performance: Average pore size 1.3 nm, similar to the example, but as... Figure 2 As shown, its pore size distribution curve exhibits a distinctly broad tail, with a full width at half maximum (FWHM) of 0.72 nm. This FWHM value is included together with that of Comparative Example 8. Figure 6 The PDI showed a positive correlation with the full width at half maximum (FWHM); the coefficient of variation of pore size in the thickness direction reached 21%, indicating the presence of channels larger than 1.6 nm within the system; the porosity was 22%, the tortuosity was 1.85, and the pore wall sulfonic acid enrichment was 25%; (e.g., ...) Figure 3 As shown, the surface resistivity is 0.38 Ω·cm. 2 TEA permeability coefficient 4.8×10 -7 cm 2 / min, TEA-Fe permeability coefficient 2.3×10 -8 cm 2 / min, which is several times higher than the example; coulombic efficiency 99.1%, energy efficiency 83.5%, swelling rate 8.8%.

[0085] This comparative example shows that even when the average pore size is similar, the broadening of the molecular weight distribution of the pore-forming agent still leads to a significant increase in pore size distribution and a marked increase in the penetration of active substances. Narrow molecular weight distribution is a key condition for achieving high selective barrier properties.

[0086] Comparative Example 5 This comparative example investigated the molecular weight boundary. The preparation process was the same as in Example 1, except that SPEEK with a number average molecular weight of 100,000 and a sulfonation degree of 0.62 was used. After stirring the casting solution, turbidity and precipitation occurred upon standing. After scraping, the wet film cracked, making it impossible to obtain a complete film.

[0087] This comparative example, together with Comparative Example 2 (molecular weight 80,000), shows that when the molecular weight is below 130,000, the chain segment entanglement density is insufficient to stabilize the casting solution system of SPEEK with moderate sulfonation degree, and film cannot be formed, proving that 130,000 is the critical value of the lower limit of molecular weight.

[0088] Comparative Example 6 This comparative example examines the region adjacent to the molecular weight boundary. The preparation process is the same as in Example 1, except that SPEEK with a number-average molecular weight of 120,000 and a sulfonation degree of 0.62 is used. The casting solution barely maintains uniformity and can be scraped into a film, yielding a film with a thickness of approximately 49 μm.

[0089] Performance: Average pore size 1.2 nm, but full width at half maximum (FWHM) 0.38 nm, tortuosity 1.62, pore size variation coefficient in thickness direction 18%, pore wall sulfonic acid group density increased by only 24%; sheet resistivity 0.40 Ω·cm 2 TEA permeability coefficient 4.2×10 -7 cm 2 / min, TEA-Fe permeability coefficient 2.0×10 -8 cm 2 / min; Coulomb efficiency 99.0%, energy efficiency 83.2%, swelling rate 9.8%.

[0090] This comparative example shows that even if film formation is possible, the matrix with a molecular weight of 120,000 still suffers from poor microdomain ordering during phase separation due to insufficient entanglement density. The pore size distribution and pore wall enrichment are both substandard, further confirming the critical significance of the lower limit of 130,000 molecular weight.

[0091] Comparative Example 7 This comparative example examines the sulfonation degree boundary. The preparation process is the same as in Example 1, except that SPEEK with a number average molecular weight of 150,000 and a sulfonation degree of 0.52 is used.

[0092] Performance: Average pore size 0.8 nm, full width at half maximum (FWHM) 0.20 nm, but porosity only 12%, pore wall sulfonic acid group density increased by 22%; surface resistivity 0.48 Ω·cm 2 TEA permeability coefficient 1.8×10 -7 cm 2 / min, TEA-Fe permeability coefficient 0.6×10 -8 cm 2 / min; Coulomb efficiency 99.3%, energy efficiency 82.8%, swelling rate 7.0%.

[0093] This comparative example shows that when the degree of sulfonation is below 0.55, insufficient hydrophilic porosity leads to low porosity, and the insufficient total amount of sulfonic acid groups reduces the enrichment range of pore walls and ion conductivity, significantly increases sheet resistivity, and reduces energy efficiency, proving that 0.55 is the critical value of the lower limit of sulfonation degree. It should be noted that the permeability coefficients of TEA and TEA-Fe in this comparative example are lower than those in the example. This improvement in barrier performance is achieved at the cost of a significant reduction in porosity and flux. Their coulombic efficiency is still lower than that of the example, and their energy efficiency is significantly deteriorated, which does not constitute an improvement in overall performance.

[0094] Comparative Example 8 This comparative example examines the PDI boundary of the porogen. The preparation process is the same as in Example 1, except that the porogen used is a PEG-6000 sample with PDI=1.4.

[0095] Performance: Average pore size 1.2 nm, but full width at half maximum (FWHM) 0.45 nm, pore size variation coefficient in thickness direction 17%, pore wall sulfonic acid group density increased by 27%; sheet resistivity 0.36 Ω·cm 2 TEA permeability coefficient 3.8×10 -7 cm 2 / min, TEA-Fe permeability coefficient 1.6×10 -8 cm 2 / min; Coulomb efficiency 99.3%, energy efficiency 84.2%, swelling rate 8.6%.

[0096] like Figure 6 As shown, when the pore-forming agent PDI was relaxed from 1.05 in Example 1 to 1.4 in this comparative example, and then further relaxed to 2.5 in Comparative Example 4, the half-width at half-maximum (WHM) of the pore size distribution monotonically increased from 0.24 nm to 0.45 nm and 0.72 nm. The WHM showed a monotonically deteriorating trend with increasing PDI, and when PDI = 1.4, the WHM exceeded the limitation of 0.3 nm, and the TEA permeability coefficient exceeded the 3.0 × 10⁻⁶ limit specified in the claims. -7 cm 2 / min, proving that PDI less than 1.2 is the critical condition for achieving narrow aperture distribution.

[0097] Comparative Example 9 This comparative example examines the coagulation process. The preparation process is the same as in Example 1, except that gradient coagulation is not used. The wet film is directly immersed in a pure deionized water coagulation bath to complete phase separation in one step.

[0098] Performance: Instant curing of the surface layer leads to the formation of finger-like macropores within the film, with an average pore diameter of 1.5 nm, a full width at half maximum (FWHM) of 0.55 nm, a thickness-direction pore diameter variation coefficient of 24%, a tortuosity of 1.9, and an increase of only 18% in the density of sulfonic acid groups on the pore walls; the sheet resistivity is 0.31 Ω·cm. 2 However, the TEA permeability coefficient is 6.5 × 10⁻⁶. -7 cm 2 / min, TEA-Fe permeability coefficient 2.8×10 -8 cm 2 / min; Coulomb efficiency 98.8%, energy efficiency 83.6%, swelling rate 8.9%.

[0099] This comparative example shows that omitting the first-stage retarding pretreatment with DMF-containing aqueous solution disrupts the orderliness of the microphase domains of the pore-forming agent, significantly deteriorates the uniformity of pore size distribution and thickness direction, and multiplies the penetration of active substances. This proves that gradient solidification process is a necessary step to achieve narrow-distribution through-hole channels.

[0100] Comparative Example 10 This comparative example examines the necessity of alkali activation. The preparation process is the same as in Example 1, except that: after washing with water to remove residual solvent and pore-forming agent, the membrane is directly dried, omitting the KOH alkali activation step, and the sulfonic acid groups in the membrane remain in the -SO3H form.

[0101] Performance: Average pore size 1.0 nm, full width at half maximum (FWHM) 0.25 nm, pore structure parameters similar to those of Example 1; however, the sheet resistivity increased to 0.37 Ω·cm. 2 The TEA permeability was approximately 15.6% higher than in Example 1, with a TEA permeability coefficient of 3.2 × 10⁻⁶. -7 cm 2 / min, TEA-Fe permeability coefficient 1.8×10 -8 cm 2 / min; Coulomb efficiency 99.4%, energy efficiency 84.0%.

[0102] Comparative Example 11 This comparative study investigated an alternative treatment method. The preparation process was the same as in Example 1, except that the alkali activation step was replaced with acid treatment involving soaking in 0.5 mol / L hydrochloric acid for 18 h.

[0103] Performance: Surface resistivity 0.38 Ω·cm 2 The TEA permeability was approximately 18.8% higher than in Example 1, with a TEA permeability coefficient of 3.4 × 10⁻⁶. -7 cm 2 / min, TEA-Fe permeability coefficient 2.0×10 -8 cm 2 / min; Coulomb efficiency 99.4%, energy efficiency 83.9%.

[0104] Comparative Examples 10 and 11 both demonstrate that, omitting alkali activation or replacing it with acid treatment, the sulfonic acid groups within the membrane remain in the -SO3H form and cannot be activated by K. + Hydration expands the microenvironment of the pores, and the negative charge on the pore walls is not as high as that of the potassium sulfonate form, resulting in an increase in sheet resistivity of about 15%-20% and a significant increase in the permeability coefficient of TEA-Fe. This proves that KOH alkali activation is a necessary post-treatment step to ensure low sheet resistivity and strong Donnan repulsion.

[0105] The performance test results of Examples 1-6 and Comparative Examples 1-11 are summarized in Table 1. The pore size distribution, surface resistivity and permeability coefficient of each sample are compared as follows: Figure 2 , Figure 3 As shown.

[0106] Table 1 Performance test results of Examples 1-6 and Comparative Examples 1-11 Note: Example 7 is a verification of the battery boundary concentration adaptability. Its membrane structure is the same as that of Example 1, so it is not included in this table.

[0107] Long-term cycle stability test: The alkaline all-iron flow single cell assembled with the separator of Example 1 was tested at 80 mA / cm². 2 After 8000 constant current charge-discharge cycles at the current density, the results are as follows: Figure 5 As shown: Coulomb efficiency decreased from the initial 99.7% to 97.8%, a decrease of 1.9 percentage points; voltage efficiency decreased from the initial 85.8% to 82.5%, a decrease of 3.3 percentage points; energy efficiency decreased from the initial 85.5% to 80.7%, a decrease of 4.8 percentage points (energy efficiency = coulomb efficiency × voltage efficiency). Figure 5 As shown, the coulombic efficiency of Example 1 was consistently higher than that of Comparative Example 1 throughout the entire cycle. After cycling, the diaphragm remained intact without damage, the swelling ratio did not increase significantly, and the sheet resistivity decreased from 0.32 Ω·cm. 2 Increased to 0.35 Ω·cm 2 The average pore size changed from 1.0 nm to 1.05 nm, and the pore structure did not deteriorate significantly. The slight performance degradation is presumed to be due to trace side reactions in the electrolyte system and trace amounts of active material permeation into the membrane. Overall, the cycle stability is excellent.

[0108] As can be seen from the above embodiments and comparative examples, and the data in Table 1: First, the synergistic effect of a high molecular weight matrix, moderate sulfonation, narrow PDI pore-forming agent microphase domain template effect, and gradient solidification process is a necessary combination for preparing narrowly distributed, interconnected nanoporous membranes: the average pore size in Examples 1-3 is in the range of 0.8-1.5 nm, the half-width at half-maximum (WHM) is less than 0.3 nm, the coefficient of variation of pore size in the thickness direction is less than 15%, the channel tortuosity is less than 1.5, the density of sulfonic acid groups on the pore wall is 32%-38% higher than that of the internal matrix, and the pore size distribution curve has a narrow and sharp peak (e.g., Figure 2 (As shown).

[0109] Second, Comparative Example 2 used SPEEK with a number average molecular weight of 80,000 and a sulfonation degree of 0.62. The casting solution was not stable enough, and phase separation and precipitation occurred during the stirring process, making it impossible to form a film. This proves that a high molecular weight matrix of 130,000-160,000 is a necessary condition to ensure the processability of SPEEK with a medium sulfonation degree.

[0110] Third, in Comparative Example 3, PEG-20000 with an excessively high molecular weight resulted in excessive phase separation driving force, forming macropores of 3.6 nm. The pore size distribution curve showed a significant macropore peak (e.g., ...). Figure 2 As shown), the coefficient of variation of pore size in the thickness direction is as high as 26%, the permeability coefficients of TEA and TEA-Fe are significantly increased, and the coulombic efficiency decreases to 98.0% (as shown). Figure 3 As shown in the figure, it is necessary to demonstrate that limiting the upper limit of the molecular weight of the porogen is necessary.

[0111] Fourth, the pore-forming agent of Comparative Example 4 has a wide molecular weight distribution (PDI=2.5). Even though the average pore size is close to that of the examples, the pore size distribution curve still has a noticeably broad tail (e.g., Figure 2 As shown in the figure, the half-peak width reaches 0.72 nm, and there are pores larger than 1.6 nm in the system. The TEA permeability coefficient is significantly increased, proving that the narrow molecular weight distribution of the pore-forming agent is the key condition for achieving high selective barrier properties.

[0112] Fifth, although the high-sulfonation dense membrane of Comparative Example 1 lacked interconnected macropores, its swelling ratio was as high as 15.5%, resulting in poor mechanical stability. Its sheet resistivity and the permeability coefficients of TEA and TEA-Fe were both higher than those of the examples (e.g., ...). Figure 3 As shown), the coulombic efficiency in long cycles is also lower than that in Example 1 (as shown). Figure 5 As shown in the figure), the porous membrane of the present invention achieves superior selective barrier performance by relying on the dual mechanisms of size sieving and Donnan repulsion, while reducing surface resistivity and inhibiting swelling.

[0113] Sixth, the lower limit of molecular weight has clear critical basis: Comparative Example 5 (molecular weight 100,000) could not form a film, and Comparative Example 6 (molecular weight 120,000) could form a film, but the pore size distribution and pore wall enrichment did not meet the standards. Together with Comparative Example 2 (molecular weight 80,000), they form a gradient evidence chain, proving that 130,000 is the critical lower limit for ensuring the processability and pore quality of SPEEK with medium sulfonation degree.

[0114] Seventh, the lower limit of sulfonation degree has a clear critical basis: Comparative Example 7 (sulfonation degree 0.52) has insufficient hydrophilicity and porosity, significantly reduced pore wall enrichment and ion conductivity, and a significant increase in surface resistivity, proving that 0.55 is the critical lower limit that balances porosity and conductivity. Together with Comparative Example 1 (sulfonation degree 0.80, uncontrolled swelling), it limits a reasonable window of 0.55-0.70.

[0115] Eighth, the upper limit of the pore-forming agent PDI has a critical basis for monotonic degradation: such as Figure 6 As shown, Comparative Example 8 (PDI=1.4) and Comparative Example 4 (PDI=2.5) show that the half-peak width increases monotonically as PDI is relaxed. When PDI=1.4, the TEA permeability coefficient has exceeded the limit, proving that the limit of PDI less than 1.2 is necessary and sufficient.

[0116] Ninth, gradient coagulation process is a necessary step: Comparative example 9 proves that a single pure water coagulation bath leads to instantaneous solidification of the surface layer, generation of finger-shaped macropores, loss of control of the skin-pore structure, and a significant increase in the penetration of active substances.

[0117] Tenth, alkaline activation is a necessary post-treatment step: Comparative Examples 10 and 11 demonstrate that omitting alkaline activation or replacing it with acid treatment both increase the surface resistivity by about 15%-20% and significantly increase the TEA-Fe permeability coefficient. The potassium sulfonate form is a necessary condition to ensure low surface resistivity and strong Donnan repulsion.

[0118] Eleventh, Example 7 demonstrates that the diaphragm of the present invention, under the electrolyte concentration (0.3-1.2 mol / L) and alkalinity (1-4 mol / L OH) specified in claim 10, - It can maintain stable battery performance throughout the entire range, supporting the broad scope of the battery claims.

[0119] In summary, this invention uses high molecular weight PEEK (130,000-160,000) as raw material and obtains SPEEK with a sulfonation degree of 0.55-0.70 through controllable sulfonation. By leveraging the microdomain template effect of a narrow polydispersity index pore-forming agent combined with gradient solidification NIPS process and alkali activation treatment, an asymmetric SPEEK porous membrane with narrowly distributed interconnected nanopores and sulfonic acid group enrichment on the pore walls is prepared. This membrane has low swelling ratio and excellent mechanical stability. When applied to alkaline all-iron flow batteries, it can simultaneously achieve high ion conduction and high active material barrier, breaking the traditional flux-selectivity trade-off effect of porous membranes and the technical prejudice that "reducing the sulfonation degree inevitably sacrifices performance." It has broad prospects for industrial application.

[0120] The preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings and specific examples. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.

Claims

1. A porous SPEEK membrane with controllable microphase separation pore size, characterized in that: The porous SPEEK membrane uses sulfonated polyether ether ketone (PEEK) with a number average molecular weight of 130,000-160,000 as the matrix, which is obtained by sulfonation and has a degree of sulfonation of 0.55-0.

70. The porous SPEEK membrane has an asymmetric structure with a dense outer skin and interconnected nanopores inside. The interconnected nanopores are formed by a porogen with a polydispersity index (PDI) of less than 1.2 through non-solvent-induced phase separation and then by washing away the porogen with water. The average pore size of the porous SPEEK membrane is 0.8-1.5 nm, the half-maximum width at half maximum (FWHM) of the pore size distribution is less than 0.3 nm, the porosity is 15%-30%, the channel tortuosity is less than 1.5, and the coefficient of variation of the pore size in the thickness direction is less than 15%. The density of sulfonic acid groups on the wall of the interconnected nanopores is more than 30% higher than that of the membrane matrix. The membrane matrix refers to the membrane material body at a depth greater than 10 μm from the membrane surface, and the sulfonic acid groups on the wall are at least partially present in the form of potassium sulfonate.

2. The porous SPEEK membrane with controllable microphase separation pore size according to claim 1, characterized in that: The pore-forming agent is polyethylene glycol and / or polyvinylpyrrolidone; the molecular weight of the polyethylene glycol is 4000-8000, and the molecular weight of the polyvinylpyrrolidone is 30000-40000.

3. The porous SPEEK membrane with controllable microphase separation pore size according to claim 1, characterized in that: The total thickness of the porous SPEEK membrane is 40-60 μm.

4. The porous SPEEK membrane with controllable microphase separation pore size according to claim 1, characterized in that: The porous SPEEK membrane has a triethanolamine permeability coefficient of less than 3.0 × 10⁻⁶. -7 cm 2 / min, the permeability coefficient of the triethanolamine iron complex is less than 1.0 × 10 -8 cm 2 / min.

5. The porous SPEEK membrane with controllable microphase separation pore size according to claim 1, characterized in that: The thickness of the dense skin layer accounts for 5%-15% of the total thickness of the porous SPEEK membrane.

6. A method for preparing a porous SPEEK membrane with controllable microphase separation pore size as described in any one of claims 1 to 5, characterized in that, Includes the following steps: Step 1: Sulfonate polyether ether ketone with a number average molecular weight of 130,000-160,000 to obtain sulfonated polyether ether ketone with a degree of sulfonation of 0.55-0.70, dissolve it in an organic solvent, and prepare a casting solution with a solid content of 16-20 wt%. Step 2: Add a porogen with a polydispersity index (PDI) of less than 1.2 to the casting solution, wherein the mass ratio of the porogen to sulfonated polyether ether ketone is (0.35-0.8):1; Step 3: Stir and dissolve at 70-90℃ for 6-8 hours, then slowly cool to 25-30℃ at a cooling rate of 0.5-1.0℃ / min, degas and scrape to form a wet film; Step 4: Immerse the wet membrane in a coagulation bath at an immersion rate of 1-5 cm / s for non-solvent-induced phase separation; the coagulation bath adopts a gradient coagulation process: in the first stage, immerse it in an aqueous solution containing 5-10 wt% N,N-dimethylformamide for 30-60 s, and in the second stage, transfer it to pure deionized water for 10-30 min. The overall temperature of the coagulation bath is controlled at 20-25℃. Step 5: Wash with water to remove residual organic solvents and pore-forming agents, then soak in 0.5-1.0 mol / L potassium hydroxide solution for 12-24 hours to complete alkali activation and obtain the porous SPEEK membrane.

7. The method for preparing a porous SPEEK membrane with controllable microphase separation pore size according to claim 6, characterized in that: In step 1, the organic solvent is selected from at least one of N,N-dimethylformamide, N-methylpyrrolidone, and dimethyl sulfoxide.

8. The method for preparing a porous SPEEK membrane with controllable microphase separation pore size according to claim 6, characterized in that: In step 2, the pore-forming agent is polyethylene glycol and / or polyvinylpyrrolidone; the molecular weight of the polyethylene glycol is 4000-8000, and the molecular weight of the polyvinylpyrrolidone is 30000-40000.

9. The method for preparing a porous SPEEK membrane with controllable microphase separation pore size according to claim 6, characterized in that: In step 3, the degassing is vacuum degassing, with a relative vacuum degree not exceeding -0.09 MPa and a degassing time of 20-40 min.

10. An alkaline all-iron flow battery, characterized in that, include: Positive electrode electrolyte: Contains ferrocyanide as the positive electrode active material, dissolved in an alkaline aqueous solution, wherein the concentration of the active material in the positive electrode electrolyte is 0.3-1.0 mol / L, and the concentration of OH- in the alkaline aqueous solution is 1-4 mol / L; Negative electrode electrolyte: containing triethanolamine iron complex as the negative electrode active material, dissolved in an alkaline aqueous solution, wherein the concentration of the active material in the negative electrode electrolyte is 0.3-1.2 mol / L, and the concentration of OH- in the alkaline aqueous solution is 1-4 mol / L; The membrane is a porous SPEEK membrane with controllable microphase separation pore size as described in any one of claims 1 to 5.