A method for forming a sodium-ion battery containing a sodium supplement and the sodium-ion battery.
By optimizing SEI film formation through step-charging and dynamic current control formation methods, the problem of low coulombic efficiency in the first cycle of sodium-ion batteries was solved, improving cell energy density and cycle stability, and realizing efficient sodium-ion battery production.
Patent Information
- Application Number
- CN202611305484.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-17
AI Technical Summary
During the first charge and discharge cycle of a sodium-ion battery, the solid electrolyte interphase (SEI) film formed at the negative electrode consumes a large amount of sodium ions, resulting in low coulombic efficiency in the first cycle. The repeated rupture and regeneration of the SEI film during the cycle further exacerbates sodium loss, severely limiting the battery's energy density and cycle life.
A sodium-ion battery formation method with sodium supplementation agent is adopted. By using a step-by-step charging + dynamic current control strategy, the charging current and voltage window are precisely controlled, the SEI film formation process is optimized, and the capacity of sodium supplementation agent is efficiently released.
It improves the energy density and cycle stability of the battery cell, significantly increases the specific capacity of the battery cell, and shortens the formation time without affecting performance, thereby improving production efficiency.
Smart Images

Figure CN123120940A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sodium-ion battery technology, specifically to a sodium-ion battery formation method containing a sodium supplement and a sodium-ion battery. Background Technology
[0002] Sodium-ion batteries, as an important alternative technology to lithium-ion batteries, benefit from abundant sodium resources, low cost, and high safety, and have broad application prospects in energy storage, low-speed electric vehicles, and other fields. However, during the first charge and discharge process, the formation of a solid electrolyte interphase (SEI) film at the negative electrode consumes a large amount of sodium ions, resulting in low coulombic efficiency in the first cycle. During cycling, the repeated rupture and regeneration of the SEI film further exacerbates sodium loss, severely limiting the battery's energy density and cycle life.
[0003] Against this backdrop, sodium replenishment technology has become crucial for improving the performance of sodium-ion batteries. Sodium replenishment agents, by releasing active sodium during the formation stage, can effectively compensate for the sodium source consumed in SEI film formation, thereby increasing cell energy density and improving cycle stability.
[0004] Sodium-rich additives for the positive electrode are typically sodium-rich compounds with high irreversible charging (sodium removal) capacity (250-700 mAh / g), such as NaN3, Na3P, NaNO2, and Na2C4O4. Therefore, only a small amount needs to be added to the positive electrode slurry to induce irreversible decomposition during the first week of charging, releasing sufficient active sodium.
[0005] Based on this technical background, this invention studies a sodium-ion battery formation method containing a sodium supplement and a sodium-ion battery. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention provides a sodium-ion battery formation method containing a sodium supplement and a sodium-ion battery. This formation method utilizes a "step-by-step charging + dynamic current control" strategy to achieve efficient release of the sodium supplement capacity by precisely controlling the charging current and voltage window. At the same time, it optimizes the SEI film formation process, thereby improving the cell energy density and cycle stability.
[0007] To achieve the above objectives, a first aspect of the present invention provides a method for forming a sodium-ion battery containing a sodium supplement, comprising: Preparation of sodium-ion batteries containing sodium supplements; The sodium-ion battery is charged to above the film formation potential using a first charging current; The sodium-ion battery is charged to the upper limit of the system voltage using a second charging current; Calculate the third charging current, and use the third charging current to charge the sodium-ion battery in a stepwise manner to the upper limit voltage of the sodium replenisher; The third charging current is less than the first charging current, which is less than the second charging current.
[0008] A second aspect of the present invention provides a sodium-ion battery, wherein the sodium-ion battery is formed using the formation method described above.
[0009] The beneficial effects of this invention include: (1) The sodium-ion battery formation method containing sodium supplementation agent proposed in this invention utilizes the strategy of "step charging + dynamic current control" to achieve efficient release of sodium supplementation agent capacity by precisely controlling the charging current and voltage window, while optimizing the SEI film formation process and improving the cell energy density and cycle stability.
[0010] (2) The sodium-ion battery formation method containing sodium replenishing agent proposed in this invention, through a three-step charging strategy (small current film formation → large current activation → precise sodium replenishment), fully utilizes the sodium ions in the sodium replenishing agent, significantly improves the specific capacity of the cell, significantly improves the energy density, and also improves the cycle stability of the cell. In addition, the second charging current is large, which shortens the formation time and improves the production efficiency without affecting the cell performance.
[0011] Other features and advantages of the present invention will be described in detail in the following detailed description section. Attached Figure Description
[0012] The above and other objects, features and advantages of the present invention will become more apparent from the more detailed description of exemplary embodiments of the invention in conjunction with the accompanying drawings.
[0013] Figure 1 This is a schematic flowchart of the sodium-ion battery formation method containing a sodium supplement agent proposed in this invention.
[0014] Figure 2 This is a schematic diagram comparing cycle performance data in a specific embodiment of the sodium-ion battery formation method containing a sodium supplement agent proposed in this invention. Detailed Implementation
[0015] Preferred embodiments of the invention will now be described in more detail. While preferred embodiments of the invention are described below, it should be understood that the invention can be implemented in various forms and should not be limited to the embodiments set forth herein.
[0016] This invention provides a method for forming a sodium-ion battery containing a sodium supplement, such as... Figure 1 As shown, it includes: Preparation of sodium-ion batteries containing sodium supplements; The sodium-ion battery is charged to above the film formation potential using the first charging current; The sodium-ion battery is charged to the upper limit of the system voltage using a second charging current; Calculate the third charging current and use it to charge the sodium-ion battery in stages to the upper limit voltage of the sodium replenisher. Control the third charging current to be less than the first charging current and the second charging current.
[0017] In this invention, a "step-by-step charging + dynamic current control" strategy is used to achieve efficient release of sodium replenishment capacity by precisely controlling the charging current and voltage window. At the same time, the SEI film formation process is optimized, thereby improving the cell energy density and cycle stability.
[0018] According to the present invention, the magnitude of the first charging current is 0.05~0.2C; The second charging current is 0.33C~1C; The third charging current is 0.01~0.1C.
[0019] According to the present invention, when the sodium-ion battery is a layered oxygen system, the film formation potential is >2.8V and the upper limit of the voltage is 3.9-4.1V; When the sodium-ion battery uses a polyanion-type cathode material system, the film formation potential is >2.7V, and the upper limit of the voltage is 3.3~3.5V; The upper limit voltage for sodium supplementation is 3.6~4.1V.
[0020] According to the present invention, the formula for calculating the third charging current is:
[0021] Where C is the charging current of the sodium replenisher; a is the initial charge capacity of the sodium replenisher, in mAh / g; x is the percentage of the sodium replenisher compared to the main material, in %; b is the charge capacity of the main material, in mAh / g; and K is the initial efficiency of the full battery, in %.
[0022] According to the present invention, the charging current of the sodium replenishing agent is ≤0.5, which is used to ensure the full decomposition of the sodium replenishing agent material during the first charging process and release sodium ions.
[0023] In this invention, through a three-step charging strategy (small current film formation → large current activation → precise sodium replenishment), sodium ions in the sodium replenishment agent are fully utilized, resulting in a significant increase in the specific capacity of the battery cell and a substantial improvement in energy density. At the same time, it can also improve the cycle stability of the battery cell. Furthermore, the second charging current is relatively large, which shortens the formation time and improves production efficiency without affecting the performance of the battery cell.
[0024] According to the present invention, the preparation of a sodium-ion battery containing a sodium supplement includes: Prepare positive and negative electrode sheets containing sodium supplements; The positive electrode, negative electrode, and separator containing sodium supplement are assembled into a dry cell. The dry battery cells are baked and then injected with electrolyte. The dry cells after being injected with electrolyte are subjected to formation, aging, and capacity testing.
[0025] According to the present invention, the preparation of positive and negative electrode sheets containing sodium supplementation agents includes: A positive electrode sheet is prepared using a positive electrode material, a sodium supplement, a first conductive agent, and a first binder; A negative electrode sheet is prepared using a negative electrode material, a second conductive agent, a second binder, and a third adhesive.
[0026] According to the present invention, the mass ratio of the positive electrode material, the sodium supplement, the first conductive agent and the first binder is 93.5-95.5:1-2:1-2:2-3; The mass ratio of the negative electrode material, the second conductive agent, the second binder and the third binder is 94.7-96.7:0.5-1.5:0.8-1.8:1-3.
[0027] According to the present invention, the positive electrode material is at least one of polyanionic compounds, layered transition metal oxides, and Prussian blue analogues; The sodium supplement is at least one of sodium squartz, sodium oxalate, and sodium carbonate; The first conductive agent is at least one of conductive carbon black, carbon nanotubes, and graphene. The first adhesive is at least one of polyvinylidene fluoride, polyacrylonitrile, and polyimide; The negative electrode material is at least one of hard carbon, soft carbon, and expanded graphite; The second conductive agent is at least one of conductive carbon black, carbon nanotubes, and graphene. The second binder is at least one of sodium carboxymethyl cellulose, sodium alginate, and sodium polyacrylate; The third adhesive is at least one of styrene-butadiene rubber, polyacrylate, and polybutadiene rubber.
[0028] The present invention also provides a sodium-ion battery, which is formed using the above-described formation method.
[0029] The present invention will be described in more detail below through embodiments.
[0030] In the embodiments of the present invention, the positive electrode material is sodium iron pyrophosphate, a polyanionic material, and the sodium supplement is sodium squartzate.
[0031] Example 1
[0032] This embodiment provides a method for forming a sodium-ion battery containing a sodium supplement, specifically including: 1. Prepare a positive electrode sheet by mixing positive electrode material, sodium supplement, conductive agent, and binder in a ratio of 94.5:1.5:1.5:2.5; 2. Prepare a negative electrode sheet by mixing negative electrode material, conductive agent, and binder (sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR)) in a ratio of 95.7:1:1.3:2; 3. Assemble the above positive electrode, negative electrode and separator into a battery cell. After baking, the assembled battery cell is injected with electrolyte, formed, aged and tested for capacity. 4. The transformation process is as follows: a) Charge to 3.0V at 0.05C (first charging current), and let stand for 5 minutes; b) Charge at a constant current and constant voltage of 0.5C (second charging current) to 3.4V (0.05C), and let stand for 5 minutes; After reaching the upper limit of the system voltage, in order to meet the requirement that the charging current of the sodium supplement itself must be less than 0.5C in the formula, the initial charging specific capacity of the sodium supplement is 339mAh / g, the sodium supplement accounts for 1.56%, the specific capacity of the positive electrode is 95mAh / g, and the initial efficiency of the full battery is 83%. Substituting the above data into the formula:
[0033] According to the formula, the charging current in step three (i.e., the third charging current) must be ≤0.03C. To improve the formation efficiency and ensure the full release of sodium ions from the sodium supplement, a reverse step charging method is adopted, with currents selected at 0.03C, 0.015C, and 0.01C. The charging steps are as follows: c) Charge at 0.03C to 4.4V; let stand for 5 minutes; d) Charge to 4.4V at 0.015C; let stand for 5 minutes; e) Charge to 4.4V at 0.01C; let stand for 5 minutes; The formation temperature is 25°C and the formation pressure is 1000 kgf.
[0034] Example 2
[0035] 1. Prepare a positive electrode sheet by mixing positive electrode material, sodium supplement, conductive agent, and binder in a ratio of 93:3:1.5:2.5; 2. Prepare a negative electrode sheet by mixing negative electrode material, conductive agent, and binder (sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR)) in a ratio of 95.7:1:1.3:2; 3. Assemble the above positive electrode, negative electrode and separator into a battery cell. After baking, the assembled battery cell is injected with electrolyte, formed, aged and tested for capacity. 4. The transformation process is as follows: a) Charge to 3.0V at 0.05C (first charging current), and let stand for 5 minutes; b) Charge at a constant current and constant voltage of 0.5C (second charging current) to 3.4V (0.05C), and let stand for 5 minutes; After reaching the upper limit of the system voltage, in order to meet the requirement that the charging current of the sodium supplement itself must be less than 0.5C in the formula, the initial charge specific capacity of the sodium supplement is 339 mAh / g, the sodium supplement accounts for 3.12%, the specific capacity of the positive electrode is 95 mAh / g, and the initial efficiency of the whole battery is 83%; Substituting the above data into the formula:
[0036] According to the formula, the charging current in step three (i.e., the third charging current) should be ≤0.06C. To improve the formation efficiency and ensure the full release of sodium ions from the sodium supplement, a reverse step charging method is adopted, with currents selected at 0.03C, 0.015C, and 0.01C. The charging steps are as follows: c) Charge to 4.4V at 0.06C; let stand for 5 minutes; d) Charge to 4.4V at 0.03C; let stand for 5 minutes; e) Charge to 4.4V at 0.01C; let stand for 5 minutes; The formation temperature is 25°C and the formation pressure is 1000 kgf.
[0037] Comparative Example 1
[0038] 1. Prepare a positive electrode sheet by mixing positive electrode material, conductive agent, and binder in a ratio of 96:1.5:2.5; 2. Prepare a negative electrode sheet by mixing negative electrode material, conductive agent, and binder (sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR)) in a ratio of 95.7:1:1.3:2; 3. Assemble the above positive electrode, negative electrode and separator into a battery cell. After baking, the assembled battery cell is injected with electrolyte, formed, aged and tested for capacity. 4. The transformation process is as follows: a) Charge at 0.05C to 3.0V, let stand for 5 minutes; b) Charge at a constant current and constant voltage of 0.5C to 3.4V (0.05C), and let stand for 5 minutes; The formation temperature is 25°C and the formation pressure is 1000 kgf.
[0039] Table 1. Comparison data between Examples 1-2 and Comparative Example 1
[0040] Compare the data in Table 1 and Figure 2 A comparison of the cycle performance data shows that when the amount of sodium supplement is small, the specific capacity can be increased, thereby increasing the energy density of the cell, while the cycle performance does not change much; when the amount is increased to 3%, the specific capacity is not significantly improved, but the cycle performance is significantly improved.
[0041] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A method for forming a sodium-ion battery containing a sodium supplement, characterized in that, include: Preparation of sodium-ion batteries containing sodium supplements; The sodium-ion battery is charged to above the film formation potential using a first charging current; The sodium-ion battery is charged to the upper limit of the system voltage using a second charging current; Calculate the third charging current, and use the third charging current to charge the sodium-ion battery in a stepwise manner to the upper limit voltage of the sodium replenisher; The third charging current is controlled to be less than the first charging current and less than the second charging current.
2. The formation method according to claim 1, characterized in that, The magnitude of the first charging current is 0.05~0.2C; The magnitude of the second charging current is 0.33C~1C; The magnitude of the third charging current is 0.01~0.1C.
3. The formation method according to claim 1, characterized in that, When the sodium-ion battery is a layered oxygen system, the film formation potential is >2.8V, and the upper limit of the voltage is 3.9-4.1V; When the sodium-ion battery is a polyanion-type cathode material system, the film formation potential is >2.7V, and the upper limit of the voltage is 3.3~3.5V; The upper limit voltage of the sodium supplement is 3.6~4.1V.
4. The formation method according to claim 1, characterized in that, The formula for calculating the third charging current is: Where C is the charging current of the sodium replenisher; a is the initial charge capacity of the sodium replenisher, in mAh / g; x is the percentage of the sodium replenisher compared to the main material, in %; b is the charge capacity of the main material, in mAh / g; and K is the initial efficiency of the full battery, in %.
5. The formation method according to claim 4, characterized in that, The charging current of the sodium replenishing agent is ≤0.5, which is used to ensure that the sodium replenishing agent material is fully decomposed during the first charging process and releases sodium ions.
6. The formation method according to claim 1, characterized in that, The preparation of sodium-ion batteries containing sodium supplements includes: Prepare positive and negative electrode sheets containing sodium supplements; The positive electrode, negative electrode, and separator containing the sodium supplement are assembled into a dry cell. The dry battery cell is baked and then injected with electrolyte. The dry battery cells, after being immersed in electrolyte, undergo formation, aging, and capacity testing.
7. The formation method according to claim 6, characterized in that, The preparation of positive and negative electrode sheets containing sodium supplements includes: A positive electrode sheet is prepared using a positive electrode material, a sodium supplement, a first conductive agent, and a first binder; A negative electrode sheet is prepared using a negative electrode material, a second conductive agent, a second binder, and a third adhesive.
8. The formation method according to claim 7, characterized in that, The mass ratio of the positive electrode material, sodium supplement, first conductive agent, and first binder is 93.5-95.5:1-2:1-2:2-3; The mass ratio of the negative electrode material, the second conductive agent, the second binder, and the third adhesive is 94.7-96.7:0.5-1.5:0.8-1.8:1-3.
9. The formation method according to claim 7, characterized in that, The cathode material is at least one of polyanionic compounds, layered transition metal oxides, and Prussian blue analogues. The sodium supplement is at least one of sodium squartz, sodium oxalate, and sodium carbonate. The first conductive agent is at least one of conductive carbon black, carbon nanotubes, and graphene; The first adhesive is at least one of polyvinylidene fluoride, polyacrylonitrile, and polyimide; The negative electrode material is at least one of hard carbon, soft carbon, and expanded graphite; The second conductive agent is at least one of conductive carbon black, carbon nanotubes, and graphene; The second adhesive is at least one of sodium carboxymethyl cellulose, sodium alginate, and sodium polyacrylate; The third adhesive is at least one of styrene-butadiene rubber, polyacrylate, and polybutadiene rubber.
10. A sodium-ion battery, characterized in that, The sodium-ion battery is formed using the formation method described in any one of claims 1-9.