A broadband light-emitting perovskite device, its fabrication method and application

By fabricating high and low undulation patterns on the substrate to regulate stress accumulation in the perovskite layer, large-scale fabrication of STE broadband light-emitting perovskite devices under ambient temperature and pressure was achieved. This improved the self-trapped exciton luminescence intensity and the response range of the photodetector, making it suitable for applications such as photodetectors and anti-counterfeiting labels.

CN123124586APending Publication Date: 2026-11-17HARBIN INSTITUTE OF TECHNOLOGY (SHENZHEN) (INSTITUTE OF SCIENCE AND TECHNOLOGY INNOVATION HARBIN INSTITUTE OF TECHNOLOGY SHENZHEN)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611295462.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to fabricate broadband light-emitting perovskite devices on a large scale at room temperature and pressure, and existing methods may lead to a decrease in device stability and luminescence intensity.

Method used

Patterns with varying heights are prepared on the substrate. By controlling the stress accumulation inside the perovskite layer, lattice distortion is induced, which causes excitons to transform from free, weakly bound states to localized self-trapped states. Grooves that match the protrusions are formed on the substrate surface using laser direct writing or nanoimprinting, thus preparing periodically arranged hemispherical or striped structures.

Benefits of technology

Large-scale fabrication of STE broadband light-emitting perovskite devices under ambient temperature and pressure has been achieved, improving the self-trapped state exciton luminescence intensity and photoluminescence quantum yield. The devices exhibit significant Stokes shift and a high response range, making them suitable for applications such as photodetectors and anti-counterfeiting labels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention discloses a broadband light-emitting perovskite device, its fabrication method, and its applications, relating to the field of perovskite technology. The broadband light-emitting perovskite device provided by this invention includes a substrate and a perovskite layer. The surface of the substrate near the perovskite layer has several grooves, and the surface of the perovskite layer near the substrate has several protrusions. The protrusions on the surface of the perovskite layer are adapted to the grooves on the surface of the substrate. The protrusions on the surface of the perovskite layer are periodically arranged hemispheres or periodically arranged stripes. The periodically arranged stripes are parallel to a first direction on the surface of the perovskite layer, and the length of the stripes is equal to the length of a second direction on the surface of the perovskite layer. The first direction on the surface of the perovskite layer is perpendicular to the second direction. By fabricating undulating patterns on the substrate, this invention enables large-scale fabrication of STE broadband light-emitting perovskite devices at room temperature and pressure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of perovskite technology, specifically to a broadband light-emitting perovskite device, its fabrication method, and its application. Background Technology

[0002] Perovskites, as an emerging direct bandgap semiconductor, possess excellent properties, such as tunable bandgap covering the visible to near-infrared bands, high carrier mobility, low defect density, and high fluorescence quantum yield. Broadband radiation has been reported in some perovskite materials, demonstrating their potential for broadband luminescence.

[0003] Currently, there are three main technical approaches to achieve broadband light emission using perovskites: using Eu... 3+ 、Sm 3+ Lanthanide metal ion doping enables broadband emission based on energy transfer; organic molecular hybridization constructs heterojunction structures; and lattice structure modulation induces self-trapped exciton (STE) luminescence in perovskite materials. Among these, STE-based luminescence exhibits the highest external quantum efficiency, along with good device stability, a larger Stokes shift, and a higher photoluminescence quantum yield (PLQY). Therefore, the unique emission characteristics of STE have attracted widespread attention in optoelectronic fields such as photodetectors, high-energy particle scintillators, and LEDs.

[0004] Currently, STE (spatial electroluminescent perovskite) is mainly introduced through compositional and structural engineering techniques. In recent years, emerging superlattice structures and van der Waals interface engineering strategies have also provided new avenues for precisely controlling the photoelectric properties of STE. However, achieving large-scale fabrication of broadband luminescent STE perovskites at room temperature and pressure remains a significant challenge. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a broadband light-emitting perovskite device, its fabrication method, and its applications.

[0006] The above-mentioned objective of this invention is achieved through the following technical solution: A broadband light-emitting perovskite device includes a substrate and a perovskite layer. The surface of the substrate near the perovskite layer is provided with a plurality of grooves, and the surface of the perovskite layer near the substrate is provided with a plurality of protrusions. The plurality of protrusions on the surface of the perovskite layer are adapted to the plurality of grooves on the surface of the substrate. The ratio of the height of several protrusions on the surface of the perovskite layer to the thickness of the perovskite layer is (0.3-0.6):1; The protrusions on the surface of the perovskite layer are periodically arranged hemispheres or periodically arranged stripes. The periodically arranged stripes are parallel to a first direction on the surface of the perovskite layer, and the length of the stripes is equal to the length of a second direction on the surface of the perovskite layer. The first direction on the surface of the perovskite layer is perpendicular to the second direction. The periodically arranged stripes have a duty cycle of 0.5 and a period of 500 nm-5 μm; the periodically arranged hemispheres have a diameter of 10-30 μm, and any two adjacent hemispheres are in close contact.

[0007] The perovskite device provided in this application, by fabricating undulating patterns on a substrate, can control the stress accumulation within the perovskite layer, thereby causing lattice distortion in the perovskite crystal. This stress-driven lattice distortion significantly alters the interlayer structure of the perovskite, prompting excitons to transition from free, weakly bound states to localized self-trapped states. This increases the intensity and proportion of self-trapped exciton luminescence in the perovskite device, resulting in a more significant Stokes shift and higher PLQY. Furthermore, the micro-nano fabrication technology for patterning on the substrate is mature, enabling large-scale fabrication of STE broadband luminescent perovskite devices at room temperature and pressure.

[0008] It should be noted that the pattern on the substrate surface in this application (i.e., the pattern that perovskite can form) needs to meet specific conditions. The inventors have discovered that devices with STE broadband light emission characteristics can be obtained by constructing patterns using periodically arranged hemispheres or stripes, but the two different patterns each need to satisfy specific periodic structures. An inappropriate periodic pattern structure will lead to insufficient lattice strain gradient in the perovskite crystal, which will not effectively induce perovskite lattice distortion, resulting in the blockage of the formation path of self-trapped excitons.

[0009] It should be noted that the ratio of the height of the protrusions on the surface of the perovskite layer to the thickness of the perovskite layer needs to satisfy (0.3-0.6):1. If the ratio of the protrusion height to the thickness of the perovskite layer itself is too low, it cannot play a good role in stress transfer, so the intensity of self-trapped exciton luminescence will decrease. If the ratio of the protrusion height to the thickness of the perovskite layer itself is too high, it will lead to uneven coverage of the perovskite layer at the edge of the protrusions, local thinning, and even the formation of holes, cracks, or local defects, thereby increasing nonradiative recombination and reducing the luminescence intensity and stability of the device. In this application, the "thickness of the perovskite layer" refers to the thickness excluding the protrusion portion, and the "height of the protrusions on the surface of the perovskite layer" refers to the height from the surface of the perovskite layer excluding the protrusion portion to the surface of the protrusion.

[0010] In this application, the perovskite layer is rectangular, and the "first direction of the perovskite layer surface" is parallel to any rectangular side of the rectangular perovskite layer.

[0011] Preferably, the periodically arranged stripes have a period of 500 nm-1 μm.

[0012] Preferably, the height of the protrusions on the surface of the perovskite layer is 20-40 nm.

[0013] Preferably, the thickness of the perovskite layer is 50-100 nm.

[0014] Preferably, the perovskite layer comprises a 2D perovskite layer.

[0015] Preferably, the 2D perovskite layer includes a 2D perovskite material, wherein the 2D perovskite material includes (PEA)2PbI4.

[0016] Preferably, the substrate includes at least one of an ITO glass layer and a PEDOT:PSS layer.

[0017] More preferably, when the protrusions on the surface of the perovskite layer are periodically arranged hemispheres, the substrate includes an ITO glass layer. More preferably, the thickness of the ITO glass layer is 1-1.5 mm. In this application, the "thickness of the ITO glass layer" includes the thickness of the groove portion, that is, the length from the side of the surface away from the perovskite layer to the perovskite surface excluding the protrusion portion.

[0018] More preferably, when the protrusions on the surface of the perovskite layer are periodically arranged stripes, the substrate includes an ITO glass layer and a PEDOT:PSS layer. More preferably, the thickness of the ITO glass layer is 10-15 mm, and the thickness of the PEDOT:PSS layer is 20-30 nm. When the protrusions on the surface of the perovskite layer are periodically arranged stripes, the broadband light-emitting perovskite device sequentially includes an ITO glass layer, a PEDOT:PSS layer, and a perovskite layer. The surface of the PEDOT:PSS layer near the perovskite layer has several grooves, and the surface of the perovskite layer near the PEDOT:PSS layer has several protrusions. In this application, the "thickness of the PEDOT:PSS layer" includes the thickness of the groove portion, that is, the length from the side of the perovskite layer away from it to the perovskite surface excluding the protrusion portion.

[0019] This application also protects a method for fabricating the broadband light-emitting perovskite device, comprising the following steps: S1. Using laser direct writing and / or nanoimprinting, grooves are formed on the surface of the substrate to obtain a patterned substrate; S2. Coat the patterned substrate surface obtained in step S1 with a perovskite precursor solution, and anneal it to obtain the broadband light-emitting perovskite device.

[0020] Preferably, when the protrusions on the surface of the perovskite layer are periodically arranged hemispheres, step S1 uses a laser direct writing method to form grooves on the substrate surface that match the protrusions, thereby obtaining a patterned substrate. More preferably, the step of forming grooves on the substrate surface that match the protrusions using a laser direct writing method includes: performing direct writing processing on the quartz glass substrate using a 532 nm pulsed laser, with a pulse repetition frequency of 1 kHz, a pulse width of 50 μs, and a laser energy density of 4.5 J / cm². 2 The scanning speed is 300 mm / min.

[0021] Preferably, when the protrusions on the surface of the perovskite layer are periodically arranged stripes, step S1 uses nanoimprint lithography to form grooves on the substrate surface that match the protrusions, thus obtaining a patterned substrate. More preferably, the step of forming grooves on the substrate surface that match the protrusions using nanoimprint lithography includes: A1. Mix polydimethylsiloxane and curing agent at a mass ratio of (8-12):1, stir for 20-40 min, vacuum for 0.5-1.5 h, then pour into the template surface, heat to 60-100℃ and cure for 0.5-1.5 h, peel the cured product off the template to obtain a patterned PDMS film. A2. Add 1-2 wt% glycerol to the PEDOT:PSS solution, then stir at 400-600 rpm for 10-20 mins. Spin coat the PEDOT:PSS film onto the ITO glass surface at 3000-4000 rpm for 20-40 s using a spin coater. Lay the patterned PDMS film obtained in step A1 onto the surface of the PEDOT:PSS film and anneal at 60-100℃ for 1-10 min. Then peel the patterned PDMS film from the PEDOT:PSS film and continue to anneal the PEDOT:PSS film at 100-200℃ for 10-20 min.

[0022] Preferably, the concentration of the perovskite precursor solution in step S2 is 0.1-0.3 mol / L.

[0023] More preferably, the solvent of the perovskite precursor solution in step S2 is dimethylamide.

[0024] Preferably, the perovskite precursor in step S2 comprises PEAI (phenylethyl iodide) and PbI2 in a molar ratio of (1-3):1.

[0025] Preferably, the coating in step S2 is spin coating, and the spin coating speed is 3000-5000 rpm. More preferably, the spin coating time is 40-60 s.

[0026] Preferably, the annealing temperature in step S2 is 80-120°C and the time is 10-30 min.

[0027] The preferred conditions in step S2 described above are beneficial for controlling the nucleation and growth process of perovskite crystals, making full use of the stress amplification process provided by the matrix surface pattern to coarsen the grains and generate lattice distortion.

[0028] This application also protects the application of the broadband light-emitting perovskite device in photoconductive detectors.

[0029] This application also protects the application of the broadband light-emitting perovskite device in anti-counterfeiting labels and information storage.

[0030] Compared with the prior art, the present invention has the following beneficial effects: The perovskite device provided in this application can regulate the stress accumulation inside the perovskite layer by fabricating undulating patterns on the substrate, thereby causing lattice distortion in the perovskite crystal and promoting the transformation of excitons from free, weakly bound states to localized self-trapped states. Furthermore, the micro-nano fabrication technology for fabricating patterns on the substrate is mature, thus enabling large-scale fabrication of STE broadband light-emitting perovskite devices at room temperature and pressure. The resulting devices have characteristics such as wide response range and dual-mode emission, and have broad application prospects in fields such as photodetectors and anti-counterfeiting labels. Attached Figure Description

[0031] Figure 1 The figures shown are schematic diagrams of the vertical cross-section and normalized steady-state spectra of the broadband light-emitting perovskite devices in Examples 1-2 of this application. Figure 1 A is a schematic diagram of the vertical cross-section of the perovskite device in Example 2. Figure 1 B is a schematic diagram of the vertical cross-section of the perovskite device in Example 1. Figure 1 C represents the normalized steady-state spectrum of the perovskite device in Example 2. Figure 1 D represents the normalized steady-state spectrum of the perovskite device in Example 1.

[0032] Figure 2 These are schematic diagrams of the groove patterns on the substrate surface of the broadband light-emitting perovskite devices in Examples 1-2 of this application, and SEM images of the perovskite crystals. Figure 2 A is a schematic diagram of the groove pattern on the substrate surface of the perovskite device in Example 2. Figure 2 B is a schematic diagram of the groove pattern on the substrate surface of the perovskite device in Example 1. Figure 2 C is a SEM image of the perovskite crystal in the perovskite device of Example 2. Figure 2 D is a SEM image of the perovskite crystal of the perovskite device in Example 1.

[0033] Figure 3These are optical fluorescence photographs, steady-state spectra, fluorescence quantum yield comparison diagrams, and steady-state absorption ratio diagrams of the perovskite devices in Example 1 and Comparative Example 1 of this application. Figure 3 A shows the optical fluorescence image and steady-state spectrum of the perovskite device in Comparative Example 1. Figure 3 B shows the optical fluorescence photograph and steady-state spectrum of the perovskite device in Example 1. Figure 3 C is a comparison graph of fluorescence quantum yield between Example 1 and Comparative Example 1 (Narrow emission is Comparative Example 1). Figure 3 D is a schematic diagram of the steady-state absorption ratio of Example 1 and Comparative Example 1 (Narrow emission is Comparative Example 1).

[0034] Figure 4 To illustrate the comparison of self-trapped exciton photocurrent measurement and transient absorption of the photoconductive detector in Example 1 of this application, the diagram shows... Figure 4 A represents the optical power density at a bias voltage of 5 V and an optical power density of 2.36 × 10⁻⁶. -6 mW / μm 2 Under illumination conditions, the periodic photocurrent switching response curve of the device, Figure 4 B shows the transient absorption normalized kinetic curves and fitting results of the control sample at a detection wavelength of 521 nm, and the patterned substrate sample at detection wavelengths of 521 nm and 567 nm. Figure 4 C represents the relationship between the responsivity of the patterned substrate sample and the control sample as a function of laser power at a bias voltage of 5 V. Figure 4 D represents the optical power density at 2.9 × 10⁻⁶. -7 W / μm 2 Under certain conditions, a comparison of the photocurrent changes with bias voltage between devices with and without broadband emission.

[0035] Figure 5 This is a schematic diagram illustrating the use of the perovskite device from Example 1 in pumping light emission, as shown in Example 2 of this application. Figure 5 A; Scale bar: 300 micrometers) and the relationship between near-field fluorescence images and pump power ( Figure 5 B, Scale: 100 micrometers). Detailed Implementation

[0036] The present invention will be further described below with reference to specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise stated, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.

[0037] Example 1 A broadband light-emitting perovskite device includes a substrate ITO glass layer with a thickness of 1.1 mm and a 2D perovskite layer. The 2D perovskite layer is made of 2D perovskite material, specifically (PEA)₂PbI₄. The substrate surface near the perovskite layer has several grooves, and the perovskite layer surface near the substrate has several protrusions. The protrusions on the perovskite layer surface are adapted to the grooves on the substrate surface. The height of the protrusions on the surface of the perovskite layer is 30 nm, and the ratio of the height to the thickness of the perovskite layer is 30:100. The surface of the perovskite layer has several protrusions arranged in periodic hemispheres with a diameter of 20 μm, and any two adjacent hemispheres are in close contact.

[0038] The fabrication method of the broadband light-emitting perovskite device described in this embodiment includes the following steps: S1. A patterned substrate is obtained by forming grooves on the substrate surface that match the protrusions using a laser direct writing method. The laser direct writing includes the following steps: using a 532 nm pulsed laser to perform direct writing processing on the quartz glass substrate, with a pulse repetition frequency of 1 kHz, a pulse width of 50 μs, and a laser energy density of 4.5 J / cm². 2 The scanning speed is 300 mm / min; S2. Dissolve PEAI and PbI2 in dimethylamide (DMF) at a molar ratio of 2:1, stir for 12 h, and filter to obtain a 0.16 mol / L perovskite precursor solution; drop 40 μL of the perovskite precursor solution onto the patterned substrate obtained in step S1, spin coat it at 4000 rpm for 50 s on a spin coater, and then anneal it at 100℃ for 15 minutes to obtain a broadband light-emitting perovskite device.

[0039] Example 2 A broadband light-emitting perovskite device includes a 13 nm thick ITO glass layer, a 30 nm thick PEDOT:PSS layer, and a 2D perovskite layer. The 2D perovskite layer is made of 2D perovskite material, specifically (PEA)₂PbI₄. A substrate has several grooves on its surface near the perovskite layer, and the perovskite layer has several protrusions on its surface near the substrate. The protrusions on the surface of the perovskite layer are adapted to the grooves on the surface of the substrate. The height of the protrusions on the surface of the perovskite layer is 30 nm, and the ratio of the height to the thickness of the perovskite layer is 30:100. The surface of the perovskite layer has several protrusions arranged in a periodic pattern of stripes. The periodic stripes are parallel to a first direction on the surface of the perovskite layer, and the length of the stripes is equal to the length of a second direction on the surface of the perovskite layer. The first direction on the surface of the perovskite layer is perpendicular to the second direction. The periodic stripes have a width of 350 nm, a period of 700 nm, and a duty cycle of 0.5.

[0040] The fabrication method of the broadband light-emitting perovskite device described in this embodiment differs from that in Example 1 only in that: Step S1 involves forming a groove on the substrate surface that matches the protrusion using nanoimprint lithography, and includes the following steps: A1. Mix polydimethylsiloxane and curing agent at a mass ratio of 10:1, stir for 30 min, vacuum for 1 h, then pour onto the template surface, heat to 80℃ and cure for 1 h, peel the cured product off the template to obtain a patterned PDMS film. A2. Add 1.5 wt% glycerol to the PEDOT:PSS solution, then stir at 500 rpm for 15 min. Spin coat the PEDOT:PSS film onto the ITO glass surface at 3500 rpm for 30 s using a spin coater. Lay the patterned PDMS film obtained in step A1 onto the surface of the PEDOT:PSS film and anneal at 80°C for 5 min. Then peel the patterned PDMS film from the PEDOT:PSS film and anneal the PEDOT:PSS film at 150°C for 15 min to obtain the patterned substrate.

[0041] Example 3 A broadband light-emitting perovskite device, which differs from Example 2 only in that: The perovskite layer surface has periodically arranged stripes with a period of 1 μm.

[0042] The fabrication method of the broadband light-emitting perovskite device described in this embodiment is basically the same as that in Embodiment 2, except that a template with a different period is used in step A1.

[0043] Example 4 A broadband light-emitting perovskite device, which differs from Example 2 only in that: The perovskite layer surface has periodically arranged stripes with a period of 5 μm.

[0044] The fabrication method of the broadband light-emitting perovskite device described in this embodiment is basically the same as that in Embodiment 2, except that a template with a different period is used in step A1.

[0045] Comparative Example 1 A perovskite device includes a substrate ITO glass layer with a thickness of 1.1 mm and a 2D perovskite layer with a thickness of 75 nm. The 2D perovskite layer is made of 2D perovskite material, which is (PEA)2PbI4.

[0046] The fabrication method of the broadband light-emitting perovskite device described in this comparative example differs from that in Example 1 only in that: Step S1 is skipped; the perovskite precursor solution is directly spin-coated onto the ITO glass layer, and subsequent steps are performed.

[0047] Performance testing I. Intrinsic Characteristic Testing of Perovskite Devices The proportion of self-trapped exciton luminescence intensity I FE / I STE Test: The ratio of free exciton luminescence intensity to self-trapped state exciton luminescence intensity (I) FE / I STE The emission spectra were obtained using steady-state PL spectroscopy. Under 405 nm continuous-wave laser (CW) excitation, PL emission spectra of each sample were acquired at the same excitation power density, integration time, and spectral acquisition parameters. After background signal subtraction, the peak intensities of the narrow-band emission peak of free excitons and the broadband emission peak of self-trapped excitons were read, and the ratio of their peak intensities was defined as I. FE / I STE .

[0048] PLQY and Stokes Shift Measurements: PLQY was performed using an integrating sphere system for absolute photoluminescence quantum yield measurement. The perovskite film was placed inside the integrating sphere, and measurements were conducted under the same excitation wavelength and power density. The number of absorbed and emitted photons was recorded, and PLQY was calculated based on the ratio of emitted to absorbed photons. The Stokes shift was obtained by comparing the absorption peak position of the sample's absorption spectrum with the emission peak position of the steady-state PL spectrum, characterized by the energy difference between the two.

[0049] The results of the above performance tests are shown in Table 1 and Figure 1-3 As shown: Table 1. From Table 1 and Figure 1-3 As shown, the perovskite device provided in this application has broadband light emission characteristics, and the broadband light emission is dominated by STE self-trapped excitons. FE / I STE The ratio is below 12:1, and the PLQY reaches over 17%. According to... Figure 3C. Under the same excitation intensity, the broadband emission effect of self-trapped excitons (STEs) on the patterned substrate significantly improved the PLQY of the perovskite film, increasing it from 14.5% in Comparative Example 1 to 37.23% in Example 1, representing a significant 2.5-fold enhancement. This PLQY enhancement can be attributed to a dual mechanism: firstly, the intrinsic properties of the perovskite self-trapped excitons, which form stable potential wells due to localization effects, resulting in higher thermal quenching activation energies compared to free excitons, effectively suppressing non-radiative recombination paths caused by thermal excitation and thus improving carrier recombination efficiency; secondly, the substrate modulates the waveguide mode of the perovskite film, improving the fluorescence extraction efficiency by disrupting the original waveguide mode confinement effect. For samples with broadband emission characteristics, the free exciton recombination fluorescence peak remains significant and shows a slight broadening towards lower energies. Figure 3 (D), revealing the induced traps generated by lattice distortion in the low-energy region.

[0050] II. Application Performance Testing of Perovskite Devices The broadband light-emitting perovskite device obtained in Example 1 of this application was used in photoconductive detectors and pumped light emission, respectively, as shown in Example 1-2.

[0051] Example of an effect 1. Using the broadband luminescent perovskite device obtained in Example 1 as the photosensitive layer of a photoconductive photodetector, optical signal detection is achieved by monitoring the current change before and after incident light irradiation under an applied bias voltage. The broadband emission-correlated low-energy states extend the device's response range to low-energy photons outside the bandgap, thereby broadening the effective operating spectral range of the detector.

[0052] The application effect of the broadband light-emitting perovskite device obtained in Example 1 of this application when used as a photoconductive detector is as follows: Figure 4As shown in the figure. Experimental results show that, regardless of the presence of the self-trapped exciton effect, the device exhibits extremely low dark current at a bias voltage of 5 V. This is because the presence of the organic layer results in very low conductivity of the two-dimensional perovskite along the out-of-plane direction, effectively suppressing the dark current (10−11 A). Subsequently, the stability of the device's photoelectric performance was tested under 633 nm laser irradiation. Through a 5-minute continuous photocurrent switching characteristic test (2.36×10−6 mW / um2), experimental data showed that the photocurrent response amplitude fluctuation was <2%, demonstrating excellent electrical stability. Even outside the absorption bandgap, there is still a significant on / off ratio Ion / Ioff ~10. Compared to the perovskite sample that only exhibits free exciton luminescence, the broadband emission film shows less bleaching at 520 nm, but an additional negative signal appears near 567 nm. The weak bleaching on the low-energy side can be attributed to the trapping effect of local low-energy states caused by lattice distortion on charge carriers. In the low-energy region outside the bandgap, due to phonon-assisted absorption, the responsivity R at 633 nm increases from 4.4 × 10⁻⁴ mA / W to 1.5 × 10⁻³ mA / W, thus widening the detector's operating range to the sub-bandgap range.

[0053] Example of effect 2. Using the broadband light-emitting perovskite device obtained in Example 1 as a pump-driven tunable light-emitting unit, the green and orange-red light emission states can be switched by adjusting the pump power of the 405 nm continuous laser. This device can be used for optical anti-counterfeiting and information storage.

[0054] The application effect of the broadband light-emitting perovskite device obtained in Example 1 of this application when used for pumped light emission is as follows: Figure 5 As shown, based on the nonlinear optical response characteristics of self-trapped excitons, the device provided in this application exhibits unique power-dependent multicolor emission characteristics. At low pump power (<2.06 mW / um²) with a 405 nm continuous laser, the perovskite emits predominantly green light; at high pump power (>24.06 mW / um²), it emits orange-red light. Its dual-mode emission characteristics have significant application potential in anti-counterfeiting labels and information storage.

[0055] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A broadband light-emitting perovskite device, comprising a substrate and a perovskite layer, characterized in that, The surface of the substrate near the perovskite layer has several grooves, and the surface of the perovskite layer near the substrate has several protrusions; the protrusions on the surface of the perovskite layer are adapted to the grooves on the surface of the substrate. The ratio of the height of several protrusions on the surface of the perovskite layer to the thickness of the perovskite layer is (0.3-0.6):1; The protrusions on the surface of the perovskite layer are periodically arranged hemispheres or periodically arranged stripes. The periodically arranged stripes are parallel to a first direction on the surface of the perovskite layer, and the length of the stripes is equal to the length of a second direction on the surface of the perovskite layer. The first direction on the surface of the perovskite layer is perpendicular to the second direction. The periodically arranged stripes have a duty cycle of 0.5 and a period of 500 nm-5 μm; the periodically arranged hemispheres have a diameter of 10-30 μm, and any two adjacent hemispheres are in close contact.

2. The broadband light-emitting perovskite device as described in claim 1, characterized in that, The height of the protrusions on the surface of the perovskite layer is 20-40 nm, and / or the thickness of the perovskite layer is 50-100 nm.

3. The broadband light-emitting perovskite device as described in claim 1, characterized in that, The perovskite layer includes a 2D perovskite layer.

4. The broadband light-emitting perovskite device as described in claim 3, characterized in that, The 2D perovskite layer includes a 2D perovskite material, which includes (PEA)2PbI4.

5. The broadband light-emitting perovskite device as described in claim 1, characterized in that, The substrate includes at least one of an ITO glass layer and a PEDOT:PSS layer.

6. The method for fabricating the broadband light-emitting perovskite device according to any one of claims 1-5, characterized in that, Includes the following steps: S1. Using laser direct writing and / or nanoimprinting, grooves are formed on the surface of the substrate to obtain a patterned substrate; S2. Coat the patterned substrate surface obtained in step S1 with a perovskite precursor solution, and anneal it to obtain the broadband light-emitting perovskite device.

7. The method for fabricating the broadband light-emitting perovskite device as described in claim 6, characterized in that, The concentration of the perovskite precursor solution in step S2 is 0.1-0.3 mol / L, and / or the perovskite precursor in step S2 includes PEAI and PbI2 in a molar ratio of (1-3):

1.

8. The method for fabricating the broadband light-emitting perovskite device as described in claim 6, characterized in that, The coating in step S2 is spin coating, with a spin coating speed of 3000-5000 rpm, and / or the annealing temperature in step S2 is 80-120℃, and the time is 10-30 min.

9. The application of the broadband light-emitting perovskite device according to any one of claims 1-5 in a photoconductive detector.