Composite materials and their preparation methods, optoelectronic devices and display devices

By using composite materials of metal oxides and transition metal sulfides in optoelectronic devices, the problem of poor stability of inorganic nanoparticles was solved, achieving high electron mobility and stability, and improving the performance and lifespan of optoelectronic devices.

CN123124587APending Publication Date: 2026-11-17GUANGZHOU TCL IND RESEARCH INSTITUTE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510626603.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Inorganic nanoparticles have poor stability, which affects the performance and lifespan of optoelectronic devices.

Method used

Composite materials, including metal oxides and transition metal sulfides, are used to form a stable crystal structure through covalent bonds, reducing oxygen vacancies and improving stability, while ligand linkages enhance the binding force.

Benefits of technology

High electron mobility and stability of composite materials were achieved, improving the luminous efficiency and lifespan of optoelectronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124587A_ABST
    Figure CN123124587A_ABST
Patent Text Reader

Abstract

This application discloses a composite material and its preparation method, as well as an optoelectronic device and display apparatus, relating to the field of display technology. The composite material includes metal oxides and transition metal sulfides, wherein the transition metal in the transition metal sulfide is selected from group IVB metals. The composite material provided in the embodiments of this application exhibits high stability and electron mobility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of display technology, and in particular to a composite material and its preparation method, optoelectronic devices and display apparatus. Background Technology

[0002] Nanoparticles are microscopic particles on the nanometer scale, with at least one dimension being smaller than 100 nanometers. Nanoparticles possess characteristics such as small size effect, surface and interface effect, strong adsorption capacity and chemical activity, and strong permeability, and are widely used in various fields.

[0003] Inorganic nanoparticles are typically chosen as materials for the carrier functional layer, but in related technologies, the stability of inorganic nanoparticles is poor and needs further improvement. Summary of the Invention

[0004] In view of this, this application provides a composite material and its preparation method, an optoelectronic device and a display device.

[0005] The embodiments of this application are implemented as follows: a composite material includes a metal oxide and a transition metal sulfide, wherein the transition metal in the transition metal sulfide is selected from group IVB metal elements.

[0006] Accordingly, this application also provides a method for preparing a composite material, comprising the following steps:

[0007] A mixture is provided, the mixture comprising a transition metal sulfide and a first solvent, wherein the transition metal in the transition metal sulfide is selected from group IVB metal elements;

[0008] A metal salt and an alkali are added to the mixture, and the mixture is reacted to obtain a composite material, which includes a metal oxide and the transition metal sulfide.

[0009] Accordingly, this application also provides an optoelectronic device, comprising an anode, a functional layer, and a cathode stacked sequentially, wherein the material of the functional layer includes the aforementioned composite material, or a composite material prepared by the aforementioned preparation method.

[0010] Accordingly, this application also provides a display device, which includes the above-mentioned optoelectronic device.

[0011] The composite material provided in this application has high stability and electron mobility. Attached Figure Description

[0012] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0013] Figure 1 This is a flowchart of the method for preparing composite materials provided in the embodiments of this application;

[0014] Figure 2 This is a schematic diagram of the structure of the optoelectronic device provided in the embodiments of this application;

[0015] Figure 3 This is a schematic diagram of the structure of another optoelectronic device provided in the embodiments of this application.

[0016] Figure label:

[0017] 100 - Optoelectronic device; 10 - Anode; 20 - Hole functional layer; 30 - Light-emitting layer; 40 - Electron functional layer; 50 - Cathode. Detailed Implementation

[0018] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application. Furthermore, it should be understood that the specific embodiments described herein are only for illustration and explanation of this application and are not intended to limit this application.

[0019] In this application, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of the device in its actual use or operating state, specifically the orientation shown in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". The terms first, second, third, etc., are used merely as illustrative purposes and do not impose numerical requirements or establish a numerical order.

[0020] In this application, "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural.

[0021] In this application, "at least one" means one or more, and "more than one" means two or more. "One or more", "at least one of the following", or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0022] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.

[0023] N-type oxide nanoparticles possess excellent electron transport properties and are commonly used as materials for the electronic functional layers in optoelectronic devices. These nanoparticles are generally synthesized using solution-based processes. The surface of N-type oxide nanoparticles easily retains adsorbed water (from molecular water generated during synthesis and adsorbed water in the product). These water molecules form adsorbed coordination compounds on the surface of the oxide nanoparticles, thereby altering their electrical properties (such as voltage reduction, mobility changes, and potential barrier changes). During the operation of optoelectronic devices, these changes in the electrical properties of oxide nanoparticles can increase the brightness of quantum dot luminescence and slow down lifetime decay; this effect is known as positive aging.

[0024] However, oxide nanoparticles have poor stability and their performance changes significantly with prolonged storage and changes in temperature and humidity, such as a decrease in electron mobility. The large number of oxygen vacancies in oxide nanoparticles is also one of the reasons for their poor stability, which can affect the performance of optoelectronic devices and cause problems such as efficiency degradation, large voltage fluctuations, and reduced lifespan.

[0025] The technical solution of this application is as follows:

[0026] In a first aspect, embodiments of this application provide a composite material comprising a metal oxide and a transition metal sulfide, wherein the transition metal in the transition metal sulfide is selected from group IVB metal elements.

[0027] It should be noted that transition metal sulfides (TMS) are a class of compounds composed of transition metal cations and sulfur anions. In transition metal sulfides, the transition metal and sulfur atoms are linked by covalent bonds, forming a stable crystal structure.

[0028] The composite material provided in this application comprises transition metal sulfides formed by group IVB metal elements, which possess certain charge migration capabilities and a certain band gap. Furthermore, the group IVB metal elements provide the transition metal sulfides with suitable conduction band positions and high chemical stability (including thermal and wet stability). The sulfur element in the transition metal sulfides can react with oxygen vacancies in the metal oxides, reducing the oxygen vacancy concentration and further improving stability. The transition metal sulfides can also form shallow donor levels, increasing electron concentration and lowering the electron transition barrier. This, combined with the metal oxides, promotes electron migration. When the composite material is used for electron injection, electrons can be transported within the transition metal sulfides and injected into the quantum dots from the metal oxide ends, thereby achieving high electron transport efficiency and high stability in the composite material. This also avoids denaturation caused by electron accumulation, further improving the stability of the composite material.

[0029] In some embodiments, the transition metal sulfide includes one or more of TiS (CAS: 12039-07-5), TiS2 (CAS: 12039-13-3), TiS3 (CAS: 12423-80-2), ZrS2 (CAS: 12039-15-5), and HfS2 (CAS: 18855-94-2).

[0030] In some embodiments, the transition metal sulfide comprises transition metal sulfide nanoparticles.

[0031] It should be noted that the shape of the transition metal sulfide nanoparticles can be a conventional shape in the art, such as spherical, rod-shaped, linear, or sheet-like.

[0032] In some embodiments, the average particle size of the transition metal sulfide nanoparticles is 2nm to 5nm, for example, it can be 2nm, 2.2nm, 2.5nm, 2.8nm, 3nm, 3.2nm, 3.5nm, 3.8nm, 4nm, 4.2nm, 4.5nm, 4.8nm, 5nm or any range between two of the above values.

[0033] It is understood that for spherical nanoparticles, the particle size range refers to the range of their diameter; for rod-shaped nanoparticles, the particle size range refers to the range of their length and / or diameter (at least one of length and diameter); for sheet-shaped nanoparticles, the particle size range refers to the range of their sheet diameter and / or thickness (at least one of sheet diameter and thickness).

[0034] For example, the average particle size of the spherical transition metal sulfide nanoparticles is 2 nm to 5 nm, such as 2 nm, 3 nm, 4 nm, 5 nm, or any range between two of the above values. It should be noted that in this application, the dimensions of the nanomaterials, such as particle size, length, diameter, sheet diameter, and thickness, are all obtained by transmission electron microscopy (TEM).

[0035] The average length of the rod-shaped transition metal sulfide nanoparticles is 3nm to 5nm, for example, it can be 3nm, 3.5nm, 4nm, 4.5nm, 5nm or any two of the above values; the average diameter of the rod-shaped transition metal sulfide nanoparticles is 2nm to 3nm, for example, it can be 2nm, 2.2nm, 2.5nm, 2.8nm, 3nm or any two of the above values.

[0036] The average diameter of the sheet-like transition metal sulfide nanoparticles is 3nm to 5nm, for example, it can be 3nm, 3.5nm, 4nm, 4.5nm, 5nm or any two of the above values; the average thickness of the sheet-like transition metal sulfide nanoparticles is 2nm to 3nm, for example, it can be 2nm, 2.2nm, 2.5nm, 2.8nm, 3nm or any two of the above values.

[0037] In some embodiments, the average particle size of the metal oxide is 3 nm to 5 nm, for example, it can be 3 nm, 3.5 nm, 4 nm, 4.5 nm, 5 nm, or any range between two of the above values. It should be noted that the shape of the metal oxide can also be spherical, rod-shaped, plate-shaped, etc.

[0038] In some embodiments, the metal oxide includes an N-type metal oxide.

[0039] Furthermore, the N-type metal oxide includes one or more of undoped N-type metal oxides or doped N-type metal oxides. The undoped N-type metal oxide and the doped N-type metal oxide each independently include one or more of ZnO, TiO2, SnO2, ZrO2, Ta2O5, and Al2O3.

[0040] In some embodiments, the doping element in the doped N-type metal oxide includes one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, cerium, indium, and gallium.

[0041] The molar doping amount of the dopant element in the doped N-type metal oxide is 0.1% to 20%, for example, it can be 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or any range between two of the above values.

[0042] In some embodiments, the mass ratio of the metal oxide to the transition metal sulfide is (1-10):100, for example, it can be 1:100, 2:100, 3:100, 4:100, 5:100, 6:100, 7:100, 8:100, 9:100, 10:100, or any range between two of the above values. Within the range of the mass ratio, it is beneficial for the metal oxide and the transition metal sulfide to work together, thereby improving the electron mobility and stability of the composite material.

[0043] Further, the mass ratio of the metal oxide to the transition metal sulfide is (1-5):100.

[0044] Furthermore, the mass ratio of the metal oxide to the transition metal sulfide is (1-2):100.

[0045] In some embodiments, the metal oxide and the transition metal sulfide are coordinated and linked in the composite material.

[0046] Specifically, the metal in the metal oxide and the sulfur in the transition metal sulfide are coordinated and connected.

[0047] In some embodiments, the composite material further includes a ligand coordinated to the transition metal sulfide and / or the metal oxide.

[0048] Furthermore, the ligand includes a hydroxyl ligand. The hydroxyl ligand can improve the dispersion and solubility of the composite material. In addition, the hydroxyl ligand can reduce the interfacial energy between the metal oxide and the transition metal sulfide, promoting close contact between the metal oxide and the transition metal sulfide, improving their binding force. Furthermore, the hydroxyl group can fill some sulfur vacancies in the transition metal sulfide and oxygen vacancies in the metal oxide, reducing the defect concentration of the composite material.

[0049] In some embodiments, the molar ratio of the transition metal sulfide to the ligand in the composite material is 100:(0.5–5), for example, it can be 100:0.5, 100:1, 100:1.5, 100:2, 100:2.5, 100:3, 100:3.5, 100:4, 100:4.5, 100:5, or any range between two of the above values. Within the range of the molar ratio, the ligand is beneficial in improving the solubility of the composite material.

[0050] Furthermore, the molar ratio of the transition metal sulfide to the ligand is 100:(1-3).

[0051] Secondly, please refer to Figure 1 This application also provides a method for preparing a composite material, comprising the following steps:

[0052] S11. Provide a mixture comprising a transition metal sulfide and a first solvent, wherein the transition metal in the transition metal sulfide is selected from group IVB metal elements;

[0053] S12. Add metal salt and alkali to the mixture and react to obtain a composite material, wherein the composite material comprises metal oxide and the transition metal sulfide.

[0054] In S11:

[0055] The transition metal sulfides mentioned above will not be repeated here.

[0056] In some embodiments, the first solvent comprises C1-C 10 Alcohol solvents. Further, the C1-C 10 The alcohol solvent is selected from one or more of methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, trimethoxybutanol, triethylene glycol monobutyl ether, and diethylene glycol dimethyl ether.

[0057] In some embodiments, the molar concentration of the transition metal sulfide in the mixture is 0.1 mmol / mL to 0.2 mmol / mL, for example, it can be 0.1 mmol / mL, 0.11 mmol / mL, 0.12 mmol / mL, 0.13 mmol / mL, 0.14 mmol / mL, 0.15 mmol / mL, 0.16 mmol / mL, 0.17 mmol / mL, 0.18 mmol / mL, 0.19 mmol / mL, 0.2 mmol / mL, or any range between two of the above values. Within the aforementioned molar concentration range, the dissolution and dispersion of the transition metal sulfide are favorable.

[0058] In S12:

[0059] In some embodiments, the metal cation in the metal salt includes one or more of zinc ions, titanium ions, tin ions, tantalum ions, and zirconium ions.

[0060] In some embodiments, the anions in the metal salt include one or more of acetate ions, sulfate ions, halide ions, and nitrate ions.

[0061] In some embodiments, the alkali includes one or more of potassium hydroxide, lithium hydroxide, sodium hydroxide, ammonium hydroxide, ethylenediamine, ethanolamine, diethanolamine, triethanolamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, and tetrabutylammonium hydroxide.

[0062] In some embodiments, the step of adding a metal salt and an alkali to the mixture and reacting to obtain a composite material includes:

[0063] S121. Add a metal salt solution to the mixture, wherein the metal salt solution includes the metal salt and a second solvent, and react to obtain an intermediate product.

[0064] S122. Add the alkaline solution to the intermediate product, the alkaline solution comprising the alkali and a third solvent, and react to obtain the composite material.

[0065] It should be noted that in step S121, the metal cations in the metal salt will undergo cation exchange with a small amount of transition metal elements in the transition metal sulfide, so that the metal salt is attached to the transition metal sulfide.

[0066] In some embodiments, the second solvent includes C1-C 10 Alcohol solvents. Further, the C1-C 10 The alcohol solvent is selected from one or more of methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, trimethoxybutanol, triethylene glycol monobutyl ether, and diethylene glycol dimethyl ether.

[0067] In some embodiments, the molar concentration of the metal salt in the metal salt solution is 0.05 mmol / mL to 0.1 mmol / mL, for example, it can be 0.05 mmol / mL, 0.06 mmol / mL, 0.07 mmol / mL, 0.08 mmol / mL, 0.09 mmol / mL, 0.1 mmol / mL, or any range between two of the above values. Within this molar concentration range, the dissolution and dispersion of the metal salt are beneficial.

[0068] In some embodiments, the metal salt solution further includes a doped metal salt.

[0069] Furthermore, the metal cations in the doped metal salt include one or more of aluminum ions, magnesium ions, lithium ions, manganese ions, yttrium ions, lanthanum ions, copper ions, nickel ions, cerium ions, indium ions, and gallium ions.

[0070] The anions in the doped metal salt include one or more of acetate ions, sulfate ions, halide ions, and nitrate ions.

[0071] In some embodiments, the molar ratio of the metal salt to the doped metal salt in the metal salt solution is (80-99.9):(0.1-20), for example, it can be 80:20, 85:15, 90:10, 95:5, 99.1:0.1 or any range between two of the above values.

[0072] In some embodiments, the mass ratio of the transition metal sulfide to the metal salt is 100:(1-20), for example, it can be 100:1, 100:2, 100:3, 100:4, 100:5, 100:6, 100:7, 100:8, 100:9, 100:10, 100:11, 100:12, 100:13, 100:14, 100:15, 100:16, 100:17, 100:18, 100:19, 100:20, or any range between two of the above values. Within the range of the mass ratio, it is beneficial for the metal salt to be stably attached to the transition metal sulfide, which facilitates the subsequent growth of metal oxides.

[0073] In some embodiments, in S121, the reaction temperature of the transition metal sulfide and the metal salt is 50°C to 60°C, for example, it can be 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, or any range between two of the above values; the reaction time of the transition metal sulfide and the metal salt is 4h to 6h, for example, it can be 4h, 4.5h, 5h, 5.5h, 6h, or any range between two of the above values. Thus, under the reaction conditions described above, it is advantageous for the metal salt to coordinate with the transition metal sulfide through metal-sulfur coordination, and it is also advantageous for the -OH groups in the first and second solvents to coordinate with the transition metal sulfide.

[0074] In some embodiments, the intermediate product comprises the coordinated-linked transition metal sulfide and the metal salt.

[0075] It should be noted that in step S122, the base provides OH- - It reacts with metal salts to form metal hydroxides, which are then dehydrated to form metal oxides.

[0076] In some embodiments, the third solvent comprises C1-C 10 Alcohol solvents. Further, the C1-C 10 The alcohol solvent is selected from one or more of methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, trimethoxybutanol, triethylene glycol monobutyl ether, and diethylene glycol dimethyl ether.

[0077] In some embodiments, the molar concentration of the alkali in the alkaline solution is 0.01 mmol / mL to 0.02 mmol / mL, for example, it can be 0.01 mmol / mL, 0.012 mmol / mL, 0.014 mmol / mL, 0.016 mmol / mL, 0.018 mmol / mL, 0.02 mmol / mL, or any range between two of the above values. Within this molar concentration range, the dissolution and dispersion of the alkali are beneficial.

[0078] In some embodiments, the molar ratio of the metal salt to the base is (1-3):(1-3), for example, it can be 1:1, 1:2, 1:3, 3:1, 2:1, or any range between two of the above ratios. Within the range of the molar ratio, the reaction between the metal salt and the base is favorable, resulting in the efficient formation of metal oxides.

[0079] In some embodiments, during step S122, the reaction temperature between the metal salt and the alkali is 50°C to 60°C, for example, it can be 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, or any range between two of the above values; the reaction time between the metal salt and the alkali is 4 hours to 6 hours, for example, it can be 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, or any range between two of the above values. Thus, under these reaction conditions, it is beneficial for the metal salt and the alkali to react fully, generating a metal oxide.

[0080] It should be noted that the first, second, and third solvents all contain hydroxyl groups, which can coordinate with transition metal sulfides and / or metal oxides in the form of ligands. Furthermore, the hydroxyl groups in the alcohol solvents promote the bonding between the metal oxides and transition metal sulfides in the metal salt and base reaction by lowering the interfacial energy, thereby improving the reaction efficiency.

[0081] It is understood that after obtaining the composite material, it can be further purified through operations such as centrifugation and washing.

[0082] Thirdly, please refer to Figure 2This application also provides an optoelectronic device 100, which includes an anode 10, a functional layer and a cathode 50 stacked sequentially, wherein the material of the functional layer includes the above-mentioned composite material or the composite material prepared by the above-mentioned preparation method.

[0083] It should be noted that the optoelectronic device 100 provided in the embodiments of this application can be an upright optoelectronic device 100 or an inverted optoelectronic device 100.

[0084] In some embodiments, the functional layer is an electronic functional layer 40, and the material of the electronic functional layer 40 includes the composite material.

[0085] The electronic functional layer 40 includes one or more of an electron injection layer and an electron transport layer, wherein the electron injection layer is located between the electron transport layer and the cathode 50.

[0086] The optoelectronic device 100 provided in this application embodiment uses a composite material with high electron migration performance and high stability in its electronic functional layer 40, which is beneficial to improving the luminous efficiency of the optoelectronic device 100, as well as the stability of the optoelectronic device 100 and extending the service life of the optoelectronic device 100.

[0087] In some embodiments, the thickness of the electronic functional layer 40 is 30 nm to 60 nm, for example, it can be 30 nm, 40 nm, 50 nm, 60 nm or any range between two of the above values. It should be noted that the thickness of the electronic functional layer 40 is obtained by a profilometer test.

[0088] In some embodiments, the optoelectronic device 100 includes a light-emitting diode.

[0089] In some embodiments, the functional layer further includes a light-emitting layer 30, which is located between the anode 10 and the electronic functional layer 40.

[0090] In some embodiments, please refer to Figure 3 The functional layer further includes a hole functional layer 20, which is located between the anode 10 and the light-emitting layer 30.

[0091] The hole functional layer 20 includes one or more of a hole injection layer and a hole transport layer, wherein the hole injection layer is located between the anode 10 and the hole transport layer.

[0092] In some embodiments, the optoelectronic device 100 includes an anode 10, a hole injection layer, a hole transport layer, a light-emitting layer 30, an electron transport layer, and a cathode 50 arranged sequentially, wherein the material of the electron transport layer includes the composite material.

[0093] In some embodiments, the anode 10 and the cathode 50 each independently include one or more of a metal electrode, a carbon electrode, a metal oxide electrode, and a composite electrode; the material of the metal electrode includes one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb, and Mg; the material of the carbon electrode includes one or more of graphite, carbon nanotubes, graphene, and carbon fibers; the material of the metal oxide electrode includes one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO, MoO3, and AMO; the composite electrode includes one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2, and TiO2 / Al / TiO2. In this context, " / " indicates a stacked structure. For example, AZO / Ag / AZO represents a composite electrode consisting of sequentially stacked AZO, Ag, and AZO layers.

[0094] In some embodiments, the material of the light-emitting layer 30 includes organic light-emitting materials or quantum dot materials.

[0095] The organic light-emitting material may be selected from, but is not limited to, one or more of the following: CBP:Ir(mppy)3(4,4'-bis(N-carbazole)-1,1'-biphenyl:tris[2-(p-tolyl)pyridinium(III)]), TCTX:Ir(mmpy)(4,4',4”-tris(carbazole-9-yl)triphenylamine:tris[2-(p-tolyl)pyridinium(III)]), diaromatic anthracene derivatives, stilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, TADF (thermally activated delayed) materials, polymers containing BN covalent bonds, HLCT (hybrid local charge transfer excited state) materials, and Exciplex (excitoplex) light-emitting materials.

[0096] The quantum dot material may be selected from, but is not limited to, one or more of single-structure quantum dots, core-shell structure quantum dots, and perovskite quantum dots.

[0097] The materials for the single-structure quantum dots, the core material of the core-shell quantum dots, and the shell material of the core-shell quantum dots can be selected from, but are not limited to, one or more compounds from group II-VI, group IV-VI, group III-V, and group I-III-VI. The shell of the core-shell quantum dots may consist of one or more layers. The group II-VI compounds may be selected from, but are not limited to, one or more of CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, and HgZnSTe. The IV-VI group compounds may be selected from, but are not limited to, one or more of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, and SnPbSTe. The group III-V compounds may be selected from, but are not limited to, one or more of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, and InAlPSb. The group I-III-VI compounds may be selected from, but are not limited to, one or more of CuInS2, CuInSe2, and AgInS2.

[0098] As an example, the core-shell structured quantum dots can be selected from, but are not limited to, one or more of CdSe / CdSeS / CdS, InP / ZnSeS / ZnS, CdZnSe / ZnSe / ZnS, CdSeS / ZnSeS / ZnS, CdSe / ZnS, CdSe / ZnSe / ZnS, ZnSe / ZnS, ZnSeTe / ZnS, CdSe / CdZnSeS / ZnS, and InP / ZnSe / ZnS. In the above descriptions of CdSe / ZnS, etc., the " / " indicates that the material after the " / " (as the shell) covers the material before the " / " (as the core).

[0099] The materials used for the perovskite quantum dots can be selected from, but are not limited to, doped or undoped inorganic perovskite semiconductors or organic-inorganic hybrid perovskite semiconductors. The general structural formula of the inorganic perovskite semiconductor is AMX3, where A is Cs. + Ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ Cu 2+ Ni 2+ Cd 2+ Cr 2+ Mn 2+ Co 2+ Fe 2+ 、Ge 2 + Yb 2+ Eu 2+ One or more of the following, where X is a halide anion selected from Cl... - ,Br - I - One or more of the following. The general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, where B is an organic amine cation selected from CH3(CH2). n-2 NH3 + Or [NH3(CH2)] n NH3] 2+ Where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ Cu 2+ Ni 2+ Cd 2+ Cr 2+ Mn 2+ Co 2+ Fe 2+ 、Ge 2+ Yb 2+ Eu 2+ One or more of the following, where X is a halide anion selected from Cl... - ,Br - I- One or more of them.

[0100] It is understood that the quantum dot material may also be coordinated with ligands known in the art, such as decaenoic acid, undecenoic acid, tetradecanoic acid, oleic acid, stearic acid, octaalkyl mercaptan, dodecyl mercaptan, octadecyl mercaptan, oleylamine, octadecylamine, octadecylamine, trioctylphosphine, trioctylphosphine oxide, phospholipids, lecithin, polyvinylpyridine, etc.

[0101] In some embodiments, the material of the hole functional layer 20 includes an organic p-type semiconductor material or an inorganic p-type semiconductor material, wherein the organic p-type semiconductor material includes 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4”-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro, N, N'-Di(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tris(N-carbazolyl)-triphenylamine, 4,4',4'-tris(carbazol-9-yl)triphenylamine, trichloroisocyanuric acid, terbium-doped phosphate-based green luminescent materials, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazabenzphenanthrene, 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl) -co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(4-butylphenyl-diphenylamine), poly[bis(4-phenyl)(4-butylphenyl)amine], polyaniline, polypyrrole, poly(p-)phenylenevinylene, poly(phenylenevinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene], poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylenevinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines, 4,4' -One or more of the following compounds: bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraarylbenzidine, PEDOT, PEDOT:PSS and its derivatives, PEDOT:PSS derivatives doped with s-MoO3, poly(N-vinylcarbazole) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-bis(naphthyl-1-yl)-N,N'-diphenylbenzidine, spironolactone (NPB), microcrystalline cellulose, and tetracyanoquinone dimethyl ester;The inorganic P-type semiconductor material comprises one or more of the following: nanocrystalline diamond, doped graphene, undoped graphene, doped metal oxide particles, undoped metal oxide particles, metal sulfides, metal selenides, and metal nitrides. The metal oxides in the doped and undoped metal oxide particles each independently comprise one or more of the following: MoO3, WO3, NiO, CrO3, CuO, and V2O5. The doping element in the doped metal oxide particles comprises one or more of the following: Mo, W, Ni, Cr, Cu, and V. The metal sulfide includes one or more of CuS, MoS3, and WS3; the metal selenide includes one or more of MoSe3 and WSe3; and the metal nitride includes p-type gallium nitride. The molar doping amount of the dopant element in the doped metal oxide particles is 0.1% to 20%, for example, it can be 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or any range between two of the above values.

[0102] Fourthly, embodiments of this application also provide a display device, which includes the aforementioned optoelectronic device 100.

[0103] The display device can be any electronic product with display function, including but not limited to smartphones, tablets, laptops, digital cameras, digital camcorders, smart wearable devices, smart weighing scales, in-vehicle displays, televisions, or e-book readers. Among them, smart wearable devices can be, for example, smart bracelets, smartwatches, virtual reality (VR) headsets, etc.

[0104] The present application will be specifically described below through specific embodiments. The following embodiments are only some embodiments of the present application and are not intended to limit the present application.

[0105] Composite Material Example 1

[0106] This embodiment provides a composite material comprising TiS2 and ZnO, wherein the mass ratio of TiS2 to ZnO is 100:5. The preparation method of the composite material includes the following steps:

[0107] Step S1: Disperse TiS2 spherical particles with an average particle size of 4 nm in ethanol to form a suspension, and stir to continue dispersing. The concentration of TiS2 is 0.1 mmol / mL.

[0108] Step S2: Add 0.05 mmol / mL of zinc acetate ethanol dispersion to the system of step S1, wherein the mass ratio of TiS2 to zinc acetate is 100:10, and heat to 60℃ and stir for 4 h.

[0109] Step S3: Add 0.01 mmol / mL of KOH ethanol dispersion to the system of step S2, wherein the molar ratio of zinc acetate to KOH is 1:1, and continue heating at 60°C for 4 hours to generate ZnO spherical particles with an average particle size of 4 nm, thus obtaining the composite material.

[0110] Composite Material Example 2

[0111] This embodiment is basically the same as Embodiment 1, except that TiS2 is replaced with ZrS2 in this embodiment.

[0112] Composite Material Example 3

[0113] This embodiment is basically the same as embodiment 1, except that TiS2 is replaced with HfS2 in this embodiment.

[0114] Composite Material Example 4

[0115] This embodiment is basically the same as Embodiment 1, except that the zinc acetate ethanol dispersion added in this embodiment also contains magnesium acetate, the molar ratio of zinc acetate to magnesium acetate is 95:5, and the composite material includes TiS2 and magnesium-doped zinc oxide, with a magnesium molar doping amount of 5%.

[0116] Composite Material Example 5

[0117] This embodiment is basically the same as Embodiment 1, except that zinc acetate is replaced with titanium sulfate in this embodiment, and the composite material includes TiS2 and TiO2.

[0118] Composite Material Example 6

[0119] This embodiment is basically the same as Embodiment 1, except that zinc acetate is replaced with tin nitrate in this embodiment, and the composite material includes TiS2 and SnO2.

[0120] Composite Material Example 7

[0121] This embodiment is basically the same as Embodiment 1, except that zinc acetate is replaced with zirconium chloride in this embodiment, and the composite material includes TiS2 and ZrO2.

[0122] Composite Material Example 8

[0123] This embodiment is basically the same as Embodiment 1, except that zinc acetate is replaced with tantalum chloride in this embodiment, and the composite material includes TiS2 and Ta2O5.

[0124] Composite Material Example 9

[0125] This embodiment is basically the same as Embodiment 1, except that the mass ratio of TiS2 to zinc acetate is 100:2 and the mass ratio of TiS2 to ZnO is 100:1.

[0126] Composite Material Example 10

[0127] This embodiment is basically the same as Embodiment 1, except that the mass ratio of TiS2 to zinc acetate is 100:20 and the mass ratio of TiS2 to ZnO is 100:10.

[0128] Composite Material Comparative Example 1

[0129] This comparative example provides a material comprising ZnO.

[0130] Composite Material Comparative Example 2

[0131] This comparative example provides a material comprising magnesium-doped zinc oxide, wherein the molar doping amount of magnesium is 5%.

[0132] Composite Material Comparative Example 3

[0133] This comparative example provides a material comprising TiO2.

[0134] Composite Material Comparative Example 4

[0135] This comparative example provides a material comprising SnO2.

[0136] Composite material comparative example 5

[0137] This comparative example provides a material comprising ZrO2.

[0138] Composite Material Comparative Example 6

[0139] This comparative example provides a material comprising Ta2O5.

[0140] Composite Material Comparative Example 7

[0141] This comparative example provides a material comprising TiS2.

[0142] Composite Material Comparative Example 8

[0143] This comparative example provides a material comprising ZrS2.

[0144] Composite Material Comparative Example 9

[0145] This comparative example provides a material comprising HfS2.

[0146] The electron mobility and stability of the composite materials in Examples 1-10 and Comparative Examples 1-9 were tested, and the results are shown in Table 1.

[0147] The electron mobility test method is as follows: The current density-voltage curve of the tested optoelectronic device (single electron transport thin film device, EOD) is obtained. The EOD structure is anode / emitting layer / electron transport layer / cathode. The anode material is ITO, the emitting layer material is CdSeS / ZnS, the electron transport layer material is the composite material used in Examples 1-10 and Comparative Examples 1-9, respectively, and the cathode material is Ag. The space charge confinement current (SCLC) region in the current density-voltage curve is obtained, and then the electron mobility is calculated using the formula J = (9 / 8)ε. r ε0μ e V 2 / d 3 Calculate the electron mobility, where J represents the current density in mA / cm². -2 ;ε r ε₀ represents the relative permittivity, and μ represents the vacuum permittivity. e Electron mobility is expressed in cm. 2 V -1 s -1 V represents the driving voltage, with units of V; d represents the film thickness, with units of m.

[0148] The method for testing the stability of composite materials is as follows: Store each of the above-mentioned devices at 85℃ and 85% relative humidity for one week, then test the electron mobility again. Calculate the stability using the following formula: Stability = Electron Mobility 85℃、85%RH Electron mobility 初始 ×100%.

[0149] Table 1

[0150]

[0151]

[0152] From Table 1, we can obtain:

[0153] As can be seen from Examples 1-10 and Comparative Examples 1-9, the composite material provided in this application has a higher electron mobility compared to Comparative Examples 7-9, and better stability in high temperature and high humidity environments compared to Comparative Examples 1-6. The combination of transition metal sulfides and metal oxides containing Group IVB metal elements significantly improves the stability of the composite material, promotes electron transport, and enhances stability.

[0154] Device Example 1

[0155] This embodiment of the device provides an optoelectronic device, the fabrication method of which is as follows:

[0156] Step S21: Provide ITO glass, use a cotton swab dipped in a small amount of soapy water to wipe the ITO surface to remove visible impurities, then use deionized water, acetone, ethanol and isopropanol for ultrasonic cleaning for 15 minutes, then blow dry with nitrogen gas and irradiate with UV for 15 minutes to form an ITO anode with a thickness of 120nm.

[0157] Step S22: Use a pipette to pick up PEDOT:PSS, where the molar ratio of PEDOT to PSS is 1:1, and drop it onto the ITO anode. Then start spin coating at 4000 rpm for 40 seconds. Then anneal at 100°C for 30 minutes to form a hole injection layer with a thickness of 80 nm.

[0158] Step S23: Use a pipette to draw 8 mg / mL of TFB solution and drop it onto the hole injection layer. Then start spin coating at 4000 rpm for 30 seconds. Then anneal at 100°C for 30 minutes to form a hole transport layer with a thickness of 70 nm.

[0159] Step S24: Place a 30 mg / mL n-octane dispersion of CdSeS / ZnS quantum dots on the hole transport layer. The surface of the CdSeS / ZnS quantum dots is connected to octane ligands, and each 1 mg of quantum dots contains 0.2 mmol of ligand. Spin-coat at 3000 rpm for 30 s, and then anneal at 80 °C for 10 min to form a light-emitting layer with a thickness of 70 nm.

[0160] Step S25: Dissolve the composite material of Example 1 in ethanol solvent. The concentration of the composite material is 20 mg / mL. Spin coat it onto the light-emitting layer at a speed of 3000 rpm for 30 seconds. Remove excess solvent by vacuuming for 5 minutes to form an electron transport layer with a thickness of 50 nm.

[0161] Step S26: After placing the object in a vacuum coating machine, Ag target material is vapor-deposited on the electron transport layer to form a cathode with a thickness of 60 nm.

[0162] Step S27: Encapsulate in an environment where both oxygen and water content are below 0.1 ppm to obtain the optoelectronic device.

[0163] Device Examples 2-10

[0164] Device Examples 2 to 10 are basically the same as Device Example 1, except that in step S25, the composite material of Composite Material Example 1 is replaced with the composite material of Composite Material Examples 2 to 10 to form an electron transport layer and obtain an optoelectronic device.

[0165] Device Comparison Examples 1-9

[0166] The devices in Comparative Examples 1 to 9 are basically the same as those in Device Example 1, except that in step S25, the composite material of Composite Material Example 1 is replaced with the composite material of Composite Material Comparative Examples 1 to 9 to form an electron transport layer and obtain an optoelectronic device.

[0167] The luminous efficiency CE (cd / A), stability (%), and lifetime T95@1000nit (h) of the optoelectronic devices of Device Examples 1-10 and Device Comparative Examples 1-9 were tested, and the test results are shown in Table 2.

[0168] The luminous efficacy (CE) was calculated using a Keithley 2400 high-precision digital source meter, an Ocean OpticUSB2000+ spectrometer, and an LS-160 luminance meter.

[0169] The method for testing the stability of optoelectronic devices is as follows: Store each device at 85℃ and 85% relative humidity for one week, then test the luminous efficiency (CE) again. Calculate the stability using the following formula: Stability = CE 85℃、85%RH / CE 初始 ×100%.

[0170] The test method for lifetime T95@1000nit is as follows: Under constant voltage drive, the time required for the brightness of the device to decrease to a certain percentage of its maximum brightness is defined as T95. This lifetime is the measured lifetime. To shorten the testing cycle, device lifetime testing is usually performed at high brightness by accelerating device aging, and the lifetime at high brightness is obtained by fitting the extended exponential decay brightness decay fitting formula. For example, the lifetime at 1000nit is measured as T95@1000nit. The specific calculation formula is as follows:

[0171]

[0172] Among them, T95 L For longer lifespan at low brightness, T95 H For the measured lifetime under high brightness, L H To accelerate the device to its maximum brightness, L L The value is 1000 nits, and A is the acceleration factor. In this experiment, the lifetime of several groups of QLED devices under rated brightness was measured, and the value of A was found to be 1.7.

[0173] Table 2

[0174]

[0175]

[0176] From Table 2, we can obtain:

[0177] As can be seen from Device Examples 1-3 and Device Comparative Examples 7-9, in Device Examples 1-3, composite materials are used as the material for the electron transport layer. Compared with Device Comparative Examples 7-9, which only use transition metal sulfides as the material for the electron transport layer, metal oxide modification of transition metal sulfides significantly improves the current efficiency of optoelectronic devices and greatly extends the service life of optoelectronic devices.

[0178] As can be seen from Device Examples 1, 4-8 and Device Comparative Examples 1-6, under the action of transition metal sulfides, the stability of Device Examples 1, 4-8 under high temperature and high humidity environments is significantly higher than that of Device Comparative Examples 1-6. The combination of transition metal sulfides and metal oxides promotes electron migration. Electrons are transported in the transition metal sulfides and injected into the quantum dots in the light-emitting layer from the metal oxide end, thereby promoting the effective recombination of electrons and holes and improving the current efficiency of optoelectronic devices.

[0179] As can be seen from Device Examples 1, 9-10 and Device Comparative Example 1, within the range of amounts of transition metal sulfides and metal oxides provided in this application, optoelectronic devices have high current efficiency, stability and long service life.

[0180] The technical solutions provided by the embodiments of this application have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A composite material, characterized in that, It includes metal oxides and transition metal sulfides, wherein the transition metal in the transition metal sulfide is selected from group IVB metal elements.

2. The composite material as described in claim 1, characterized in that, The mass ratio of the metal oxide to the transition metal sulfide is (1-10):100; optionally, the mass ratio of the metal oxide to the transition metal sulfide is (1-5):100; optionally, the mass ratio of the metal oxide to the transition metal sulfide is (1-2):100; and / or In the composite material, the metal oxide and the transition metal sulfide are coordinated and linked; and / or The composite material further includes a ligand coordinated to the transition metal sulfide and / or the metal oxide; the ligand includes a hydroxyl ligand; in the composite material, the molar ratio of the transition metal sulfide to the ligand is 100:(0.5-5), optionally, the molar ratio of the transition metal sulfide to the ligand is 100:(1-3).

3. The composite material as described in claim 1, characterized in that, The transition metal sulfides include one or more of TiS, TiS2, TiS3, ZrS2, and HfS2; The transition metal sulfide includes transition metal sulfide nanoparticles; the average particle size of the transition metal sulfide nanoparticles is 2 nm to 5 nm.

4. The composite material as described in claim 1, characterized in that, The metal oxide includes N-type metal oxides, which include one or more of undoped N-type metal oxides or doped N-type metal oxides. The undoped N-type metal oxide and the doped N-type metal oxide each independently include one or more of ZnO, TiO2, SnO2, ZrO2, Ta2O5, and Al2O3. The doping element in the doped N-type metal oxide includes one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, cerium, indium, and gallium. The molar doping amount of the doping element in the doped N-type metal oxide is 0.1% to 20%. The average particle size of the metal oxide is 3 nm to 5 nm.

5. A method for preparing a composite material, characterized in that, Includes the following steps: A mixture is provided, the mixture comprising a transition metal sulfide and a first solvent, wherein the transition metal in the transition metal sulfide is selected from group IVB metal elements; A metal salt and an alkali are added to the mixture, and the mixture is reacted to obtain a composite material, which includes a metal oxide and the transition metal sulfide.

6. The preparation method according to claim 5, characterized in that, The transition metal sulfides include one or more of TiS, TiS2, TiS3, ZrS2, and HfS2; The metal oxide includes N-type metal oxide, which includes one or more of undoped N-type metal oxide or doped N-type metal oxide. The undoped N-type metal oxide and the metal oxide in the doped N-type metal oxide each independently include one or more of ZnO, TiO2, SnO2, ZrO2, Ta2O5, and Al2O3. The metal cations in the metal salt include one or more of zinc ions, titanium ions, tin ions, tantalum ions, and zirconium ions; The anions in the metal salt include one or more of acetate ions, sulfate ions, halide ions, and nitrate ions. The alkali includes one or more of potassium hydroxide, lithium hydroxide, sodium hydroxide, ammonium hydroxide, ethylenediamine, ethanolamine, diethanolamine, triethanolamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, and tetrabutylammonium hydroxide; said first solvent comprises a Ci-C 10 alcoholic solvent; said Ci-C 10 alcoholic solvent is selected from one or more of methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, trimethoxybutanol, triethylene glycol monobutyl ether, diethylene glycol dimethyl ether; In the mixture, the molar concentration of the transition metal sulfide is 0.1 mmol / mL to 0.2 mmol / mL.

7. The preparation method according to claim 5, characterized in that, The process involves adding a metal salt and an alkali to the mixture, reacting, and obtaining a composite material, comprising: A metal salt solution, comprising the metal salt and a second solvent, is added to the mixture, and the mixture is reacted to obtain an intermediate product. The alkaline solution, comprising the alkali and a third solvent, is added to the intermediate product, and the mixture is reacted to obtain the composite material.

8. The preparation method according to claim 7, characterized in that, each of the second solvent, the third solvent independently comprises a Ci-C 10 alcoholic solvent, the Ci-C 10 alcoholic solvent is selected from one or more of methanol, ethanol, propanol, butanol, ethylene glycol, isopropanol, glycerol, trimethoxybutanol, triethylene glycol monobutyl ether, diethylene glycol dimethyl ether; The intermediate product includes the coordinated-linked transition metal sulfide and the metal salt; The metal salt solution further includes a doped metal salt; the metal cation in the doped metal salt includes one or more of aluminum ions, magnesium ions, lithium ions, manganese ions, yttrium ions, lanthanum ions, copper ions, nickel ions, cerium ions, indium ions, and gallium ions; the molar ratio of the metal salt to the doped metal salt is (80-99.9):(0.1-20); In the metal salt solution, the molar concentration of the metal salt is 0.05 mmol / mL to 0.1 mmol / mL; In the alkaline solution, the molar concentration of the alkali is 0.01 mmol / mL to 0.02 mmol / mL; The mass ratio of the transition metal sulfide to the metal salt is 100:(1-20); The molar ratio of the metal salt to the alkali is (1-3):(1-3); The reaction temperature of the transition metal sulfide and the metal salt is 50℃~60℃, and the reaction time is 4h~6h; The reaction temperature between the metal salt and the alkali is 50℃~60℃, and the reaction time is 4h~6h.

9. An optoelectronic device, characterized in that, It includes an anode, a functional layer, and a cathode stacked sequentially, wherein the material of the functional layer includes the composite material as described in any one of claims 1 to 4, or the composite material prepared by the preparation method as described in any one of claims 5 to 8.

10. The optoelectronic device as described in claim 9, characterized in that, The functional layer is an electronic functional layer, and the material of the electronic functional layer includes the composite material. The functional layer further includes a light-emitting layer located between the anode and the electronic functional layer; the material of the light-emitting layer includes organic light-emitting materials or quantum dot materials; the organic light-emitting material is selected from 4,4'-bis(N-carbazole)-1,1'-biphenyl:tris[2-(p-tolyl)pyridinium(III)], 4,4',4”-tris(carbazole-9-yl)triphenylamine:tris[2-(p-tolyl)pyridinium], diaromatic anthracene derivatives, stilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, and TBRb fluorescent materials. The quantum dot material is selected from one or more of the following: DBP fluorescent material, delayed fluorescence material, TTA material, TADF material, polymer containing BN covalent bonds, HLCT material, and Exciplex luminescent material; the quantum dot material is selected from one or more of the following: single-structure quantum dots, core-shell quantum dots, and perovskite quantum dots; the material of the single-structure quantum dot, the core material of the core-shell quantum dot, and the shell material of the core-shell quantum dot are respectively selected from one or more of the following: group II-VI compounds, group IV-VI compounds, group III-V compounds, and group I-III-VI compounds; the core... The shell structure of the quantum dots comprises one or more layers; the II-VI group compounds are selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, Cd ZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, and HgZnSTe; wherein the IV-VI compound is selected from one or more of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, and SnPbSTe;The III-V compounds are selected from one or more of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, and InAlPSb. Multiple types; the I-III-VI group compounds are selected from one or more of CuInS2, CuInSe2, and AgInS2; the core-shell structured quantum dots are selected from one or more of CdSe / CdSeS / CdS, InP / ZnSeS / ZnS, CdZnSe / ZnSe / ZnS, CdSeS / ZnSeS / ZnS, CdSe / ZnS, CdSe / ZnSe / ZnS, ZnSe / ZnS, ZnSeTe / ZnS, CdSe / CdZnSeS / ZnS, and InP / ZnSe / ZnS; the perovskite quantum dots are made of doped or undoped inorganic perovskite semiconductors or organic-inorganic hybrid perovskite semiconductors; the inorganic perovskite semiconductor has the general structural formula AMX3, where A is Cs; + Ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ Cu 2+ Ni 2+ Cd 2+ Cr 2+ Mn 2+ Co 2+ Fe 2+ 、Ge 2+ Yb 2+ Eu 2+ One or more of the following, where X is a halide anion selected from Cl... - ,Br - I - One or more of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, where B is an organic amine cation selected from CH3(CH2). n-2 NH3 + Or [NH3(CH2)] n NH3] 2+ Where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ Cu 2+ Ni 2+ Cd 2+ Cr 2+ Mn 2+ Co 2+ Fe 2+ 、Ge 2+ Yb 2 + Eu 2+ One or more of the following, where X is a halide anion selected from Cl... - ,Br - I - One or more of the following; The functional layer further includes a hole functional layer located between the anode and the light-emitting layer; the material of the hole functional layer includes organic P-type semiconductor materials or inorganic P-type semiconductor materials, wherein the organic P-type semiconductor materials include 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, and N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine. N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tris(N-carbazolyl)-triphenylamine, 4,4',4'-tris(carbazol-9-yl)triphenylamine, trichloroisocyanuric acid, terbium-doped phosphate-based green luminescent materials, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazabenzophenanthrene, 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9' -dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(4-butylphenyl-diphenylamine), poly[bis(4-phenyl)(4-butylphenyl)amine], polyaniline, polypyrrole, poly(p-)phenylenevinylene, poly(phenylenevinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene], poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylenevinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines Amines, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraarylbenzidine, PEDOT, PEDOT:PSS and its derivatives, PEDOT:PSS derivatives doped with s-MoO3, poly(N-vinylcarbazole) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-bis(naphthyl-1-yl)-N,N'-diphenylbenzidine, spironolactone (NPB), microcrystalline cellulose, and tetracyanoquinone dimethyl ester;The inorganic P-type semiconductor material includes one or more of the following: nanocrystalline diamond, doped graphene, undoped graphene, doped metal oxide particles, undoped metal oxide particles, metal sulfides, metal selenides, and metal nitrides. The metal oxides in the doped and undoped metal oxide particles each independently include one or more of MoO3, WO3, NiO, CrO3, CuO, and V2O5. The doping element in the doped metal oxide particles includes one or more of Mo, W, Ni, Cr, Cu, and V. The metal sulfide includes one or more of CuS, MoS3, and WS3. The metal selenide includes one or more of MoSe3 and WSe3. The metal nitride includes P-type gallium nitride. The molar doping amount of the doping element in the doped metal oxide particles is 0.1% to 20%. The anode and the cathode each independently include one or more of the following: a metal electrode, a carbon electrode, a metal oxide electrode, and a composite electrode; the material of the metal electrode includes one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb, and Mg; the material of the carbon electrode includes one or more of graphite, carbon nanotubes, graphene, and carbon fibers; the material of the metal oxide electrode includes one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO, MoO3, and AMO; the composite electrode includes one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2, and TiO2 / Al / TiO2.

11. The optoelectronic device as described in claim 9, characterized in that, The optoelectronic device includes an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, and a cathode arranged sequentially, wherein the material of the electron transport layer includes the composite material.

12. A display device, characterized in that, Including the optoelectronic device as described in any one of claims 9 to 11.